Zero-dimensional copper (I)-based halide flexible luminescent material and preparation method and application thereof
The synthesis of zero-dimensional copper (I)-based halides by low-temperature solvent thermal method, combining surfactants and polymer materials, solve the high temperature and high pressure problem of X-ray scintillators in the prior art, achieve efficient flexible scintillation performance, and promote medicine and applications in the field of radiation monitoring.
Patent Information
- Application Number
- CN202410901224.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing X-ray scintillators are synthesized under high temperature and high pressure, which is costly, poorly stable, and difficult to achieve flexible high-quality scintillation films. The toxicity and low light yield of lead-based materials limit medical imaging applications.
The zero-dimensional copper (I)-based halide was synthesized by low-temperature solvent thermal method, and the nanocrystal size was controlled by surfactant to mix with polymer materials to prepare flexible luminescent materials with high resolution and low detection limits to achieve high-efficiency X-ray scintillation performance .
It has achieved high photoluminescence quantum yield, low detection limit and high radiation resistance, demonstrated the potential of high-performance flexible X-ray imaging, highlighted the multiple advantages of cuprous halide, and promoted medical diagnosis and radiation monitoring applications.
Smart Images

Figure CN118879306A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a zero-dimensional copper (I)-based halide flexible luminescent material and a preparation method and application thereof. Background Art
[0002] X-ray scintillators can convert high-energy photons into visible light photons and have been widely used in radiation exposure monitoring, safety testing, nondestructive testing, medical imaging and other fields. Several key factors determine the practical application value of scintillators, such as high light yield, low cost, high response rate and high stability. At present, various inorganic scintillators, such as NaI:Tl, CsI:Tl, YAlO3:Ce, Bi4Ge3O 12 Crystals have been developed and widely used commercially due to the advantages of high light yield and stability. However, these inorganic scintillators are synthesized by a harsh Czochralski method at extremely high temperature and pressure, resulting in high energy consumption and cost. In addition, large crystal size and grain boundaries hinder the fabrication of high-quality scintillator films for flexible X-ray imaging. To address these problems, some organic scintillators have been developed, but they still suffer from the disadvantage of blocking X-rays due to their low absorption coefficient. Given the importance of dynamic X-ray flexible imaging for real-time monitoring of curved structures inside complex devices, it remains urgent and challenging to develop high-performance X-ray scintillators with high X-ray absorption coefficient, simple synthesis process, controllable crystal size, and excellent processing performance.
[0003] Considering the basic requirements of scintillators for high X-ray absorption and photoluminescence quantum yield (PLQY), three-dimensional (3D) perovskite nanocrystals of CsPbX3 (X = Cl, Br, I) have attracted extensive attention due to their mild synthesis conditions, high absorption coefficient, low defect density, long carrier diffusion length, and high PLQYs. Since the first scintillator based on 3D perovskite CsPbX3 (X = Cl, Br, I) was reported in 2018, perovskite-based scintillators have been widely developed and achieved great success. However, Pb 2+ The toxicity of 3D CsPbX3 and its sensitivity to humidity and oxygen have hindered the further application of 3D CsPbX3 in medical X-ray imaging. In addition, the low light yield and severe aggregation-induced luminescence quenching effect further severely restrict practical applications. Even more unfortunately, the limited types of A-site cations and B-site metal ions lead to a lack of structural diversity and difficulties in tunable scintillation properties. Therefore, it is of great significance to develop new perovskite-associated scintillators that are non-toxic, highly stable, low-cost, and have high X-ray absorption coefficients and light yields.
[0004] Recently, lead-free zero-dimensional (0D) organic-inorganic metal halides (OIMHs) have emerged as one of the promising scintillators. Compared with DCsPbX3 perovskites, 0D OIMHs have richer structural flexibility due to the collaboration of multifunctional organic parts and inorganic metal halide centers, resulting in diverse photophysical properties. In addition, the inorganic units are periodically embedded into a large organic matrix with a large dielectric constant, which induces a strong quantum confinement effect and highly localized excitons, leading to large exciton binding energy and high PLQY. Most importantly, the soft lattice of 0D OIMHs is easily structurally deformed under photoexcitation due to strong electron-phonon coupling, generating excited-state defects and trapping photogenerated excitons to form self-trapped excitons (STEs). Therefore, 0D OIMHs tend to show broadband light emission with large Stokes shift and negligible self-absorption characteristics. In summary, 0D OIMHs have the characteristics of high exciton binding energy, large Stokes shift, wide full width at half maximum, and high PLQY, which make 0D OIMHs excellent candidates for high-quality scintillators.
[0005] In the OIMH family, 0D OIMHs based on manganese (II), zinc (II), indium (III) and antimony (III) have shown good scintillation performance. However, there are still some problems to be solved. For example, manganese-based halide scintillators usually emit ions originating from tetrahedral [MnX4] 2- The single green radiative emission of the dd electron transition of the unit is very small, and it is difficult to adjust the emission spectrum range. As for zinc (II), indium (III) or antimony (III) based OIMHs, the low light yield of the scintillator still needs to be improved. Relatively speaking, copper (I) based 0D halides have received the most attention among X-ray scintillators due to their multiple advantages such as environmental protection, earth abundance, structure and luminescence diversity. For example, (R, S-2mpip)2Cu2I6 (mpip = methylpiperazinium) single crystals show green radiative luminescence (RL) with a light yield of about 47,000 photons·MeV -1 . In addition, the emission spectral range of OIMHs can be tailored across the entire visible spectrum by regulating the anionic cuprous salt unit through the structure-directing effect of organic cations. Of course, 0D Cu(I)-based OIMH scintillator screens still face challenges of poor uniformity, transparency, and stability due to bulk crystal size, and few flexible scintillator screens have been explored for dynamic X-ray imaging. Summary of the invention
[0006] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a zero-dimensional copper (I)-based halide flexible luminescent material and a preparation method and application thereof. By adding a surfactant to control the size of the crystal to the micrometer-nanometer level, the synthesized nanocrystals are mixed with a polymer material to prepare a zero-dimensional copper (I)-based halide flexible luminescent material with high resolution, low detection limit, excellent foldability, high crack resistance and excellent X-ray scintillation luminescence performance.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A method for preparing a zero-dimensional copper (I)-based halide flexible luminescent material comprises the following steps:
[0009] The cuprous salt and KBr are mixed, and then a hypophosphorous acid reducing agent is added, the hypophosphorous acid reducing agent prevents cuprous oxidation, and the cuprous salt and the halogen are coordinated to form an anion skeleton, thereby obtaining a solution containing an anion skeleton;
[0010] The polyvinyl pyrrolidone solution is dissolved in ethanol to obtain a polyvinyl pyrrolidone mixed solution, and a solution containing an anion skeleton is added to the above solution under stirring. Since the polyvinyl pyrrolidone molecular structure is large, after coordination with inorganic anions, steric hindrance is increased, so that the anion units can be diffused, and the diffused anion units are combined with organic cations to avoid accumulation and growth into large crystals;
[0011] reacting an organic amine with a hydrohalic acid to form a protonated organic amine, reacting the organic amine with a halogen to protonate the organic amine to form an organic cation, then adding the protonated organic amine to the diffused anion skeleton solution, stirring at room temperature, and obtaining a zero-dimensional copper (I)-based halide nanocrystalline material;
[0012] EVA is dissolved in cyclohexane to obtain a mixed solution, the zero-dimensional copper (I)-based halide nanocrystalline material and ethanol are mixed and added to the mixed solution, and a fluid is obtained after stirring, and the fluid is post-processed to obtain a zero-dimensional copper (I)-based halide flexible luminescent material with high-efficiency X-ray scintillation luminescence performance.
[0013] The requirements for selecting polymer compounds in the present invention are as follows: polymer materials generally require certain conditions to be melted into liquid state and mixed with the luminescent material of the present invention, and then formed into a film after cooling; the luminescent material of cuprous halide is easily oxidized and not resistant to high temperature, so the melting temperature of the selected polymer material cannot be too high, and the luminescence of the halide cannot be affected after mixing. In addition, the polymer material must be environmentally friendly and non-toxic. Therefore, there are two reasons for selecting EVA in the present invention: first, because EVA is soluble in cyclohexane at 60 degrees, it will not affect the luminescent properties of the halide, and it will form a film immediately after cooling; second, because the EVA material has good flexibility, good stretchability and can be restored.
[0014] In a preferred embodiment of the present invention, the cuprous salt is cuprous bromide, and only cuprous bromide compounds can grow into nanocrystals at room temperature with the assistance of polyvinyl pyrrolidone, and the organic amine is N-aminoethylpiperazine.
[0015] In a preferred embodiment of the present invention, the usage ratio of cuprous salt to KBr is 1 mmol:2-3 mL.
[0016] In a preferred embodiment of the present invention, the dosage of polyvinyl pyrrolidone and ethanol is 1 g:100 mL, and the dosage ratio of polyvinyl pyrrolidone to cuprous salt is 1 g:1 mmol.
[0017] In a preferred embodiment of the present invention, in the protonated organic amine, the volume ratio of the organic amine to the hydrohalic acid is 1:10, and the dosage ratio of the organic amine to the cuprous salt is 0.1 mL:1 mmol.
[0018] In a preferred embodiment of the present invention, the volume ratio of hypophosphorous acid to organic amine is 1:1.5-2.
[0019] In a preferred embodiment of the present invention, the usage ratio of EVA to cyclohexane is 100 mg: 4-5 mL.
[0020] In a preferred embodiment of the present invention, the usage ratio of nanocrystals to ethanol is 50 mg:1 mL, and the mass ratio of nanocrystals to EVA is 1:2.
[0021] Another object of the present invention is to provide a zero-dimensional copper (I)-based halide flexible luminescent material prepared by any of the preparation methods described above.
[0022] The third object of the present invention is to provide an application of the above-mentioned zero-dimensional copper (I)-based halide flexible luminescent material in the field of wearable radiation imaging and industrial X-ray detection.
[0023] Before preparing nanocrystals, the present invention first prepares single crystal materials and verifies that single crystal materials have excellent luminescence properties. Therefore, it is considered to prepare them into flexible films for use in wearable radiation imaging and industrial X-ray detection. It is difficult for ordinary organic-inorganic hybrid material compounds to be sized to the nanometer level. The smaller the size of the luminescent material, the more uniformly it is mixed and dispersed with the polymer material, and the finer the film produced. The resolution of the scintillator screen made for scintillator imaging will be higher.
[0024] The preparation method of the zero-dimensional copper (I)-based halide single crystal material comprises the following steps:
[0025] The cuprous salt and the organic amine are dissolved in a halogen acid and an organic solvent, and then hypophosphorous acid is added, stirred and dissolved, and a solvothermal reaction is performed to obtain a zero-dimensional copper (I)-based halide single crystal material;
[0026] In a preferred embodiment of the present invention, the organic amine is N-aminoethylpiperazine, the cuprous salt is cuprous bromide, the hydrohalic acid is hydrobromic acid, and the organic solvent is sec-butyl alcohol; when the cuprous salt is cuprous iodide, the hydrohalic acid is hydroiodic acid, and the solvent is water.
[0027] In a preferred embodiment of the present invention, when the cuprous salt is cuprous bromide, the molar ratio of the organic amine to cuprous bromide is 1:1-2; when the cuprous salt is cuprous iodide, the hydrohalic acid is hydroiodic acid, and the solvent is deionized water, the molar ratio of the organic amine to cuprous bromide is 1:1-2.
[0028] In a preferred embodiment of the present invention, the volume ratio of hypophosphorous acid to N-aminoethylpiperazine is 1:1.5-2.
[0029] In a preferred embodiment of the present invention, when the cuprous salt is cuprous bromide, the solvent thermal reaction temperature is 80°C and the reaction time is 48 to 72 hours; when the cuprous salt is cuprous iodide, the solvent thermal reaction temperature is 100°C and the reaction time is 48 to 72 hours.
[0030] In a preferred embodiment of the present invention, the organic amine is N-aminoethylpiperazine, when the cuprous salt is cuprous bromide, the hydrohalic acid is hydrobromic acid, and the organic solvent is sec-butyl alcohol, the molecular formula of the obtained zero-dimensional copper (I)-based halide single crystal material is [AEPipz]CuBr3·Br·H2O, the crystal system space group is P21 / c, and the unit cell parameters are α=90°,β=97.670(2)°,γ=90°,Z=4,the unit cell volume is When the cuprous salt is cuprous iodide, the hydrohalic acid is hydroiodic acid, and the organic solvent is deionized water, the molecular formula of the resulting zero-dimensional copper (I)-based halide single crystal material is [AEPipz]CuI3·I·H2O, the crystal system space group is P21 / c, and the unit cell parameters are α=90°,γ=98.575(4),β=90°,Z=4,the unit cell volume is
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The present invention mixes cuprous salt and KBr, then adds hypophosphorous acid reducing agent, and the cuprous salt and halogen coordinate to form an anion skeleton to obtain a solution containing an anion skeleton; polyvinyl pyrrolidone solution is added to ethanol to obtain a polyvinyl pyrrolidone mixed solution, and under stirring, the solution containing an anion skeleton is added to the polyvinyl pyrrolidone mixed solution. Since the molecular structure of polyvinyl pyrrolidone is large, after coordination with inorganic anions, steric hindrance is increased, so that the anion unit can be diffused, and the diffused anion unit is combined with organic cations to avoid accumulation and growth into large crystals; organic amine and hydrogen halide are added to the mixture to form an anion skeleton. Acid is added to the diffused anion skeleton solution, and the organic amine reacts with the halogen to protonate the organic amine to form an organic cation. The solution is stirred at room temperature to obtain a zero-dimensional copper (I)-based halide nanocrystalline material. The size of the crystal is controlled to the micrometer-nanometer level by adding a surfactant, and the synthesized nanocrystals are mixed with a polymer material to prepare a zero-dimensional copper (I)-based halide flexible luminescent material with high resolution, low detection limit, excellent foldability, high crack resistance and excellent X-ray scintillation luminescence performance. High spatial resolution can be achieved in X-ray imaging, demonstrating potential applications in wearable radiation radiography.
[0033] 2. In order to solve the problems of low light yield, high toxicity and high temperature and high pressure of traditional inorganic scintillators in the synthesis of lead halide perovskite nanocrystals, the present invention can prepare zero-dimensional hybrid copper-based halide single crystals by a low-temperature solvothermal method. In view of the importance of dynamic X-ray flexible imaging for real-time monitoring of the internal curved structure of complex devices, it is still urgent and challenging to develop high-performance X-ray scintillators with high X-ray absorption coefficient, simple synthesis process, controllable crystal size and excellent processing performance. The present invention controls the size of the crystal by adding a surfactant, and then mixes the nanocrystals with polymer materials to prepare a zero-dimensional copper (I)-based halide flexible luminescent material with high-efficiency X-ray scintillation luminescence performance. These two halides have ultra-high photoluminescence quantum yield as broadband cyan light emitters. As expected, the high quantum yield and large Stokes shift make these two halides high-performance X-ray scintillators with a maximum light yield of 62,400 photons·MeV -1 The minimum detection limit is 95.7 nGyair·s -1 , far superior to commercially available scintillators. Significantly, [AEPipz]·CuBr3·Br·H2O, with the assistance of polyvinylpyrrolidone (PVP), can be controlled from millimeter-scale single crystals to nanometer-scale powder crystals, which is conducive to the construction of high-quality flexible films. Therefore, the present invention can assemble a highly transparent, well-distributed and stable film as a flexible scintillator screen with a spatial resolution of up to 17.4lp·mm -1, demonstrating the obvious advantages of high-performance flexible X-ray imaging. These combined advantages, including high cost-effectiveness, large-scale assembly, excellent scintillation performance, strong radiation resistance and great flexibility, fully demonstrate the unique advantages of low-dimensional cuprous halide as a high-performance scintillator. This invention not only highlights the multiple advantages of cuprous halide scintillators, but also promotes advanced applications in cutting-edge radiation industries such as medical diagnosis, non-destructive testing and radiation monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the crystal structure of compound 1-2 prepared in Example 1-2 of the present invention, wherein (a) and (c) are the anion [Cu2Br6] of compound 1-2, respectively. 4- and [Cu2I6] 4- Structural diagram, (b) is the cation [AEPipz] 3+ Structural schematic diagram, (d) is the zero-dimensional structural schematic diagram of compound 1, and (e) is the zero-dimensional structural schematic diagram of compound 2.
[0035] Figure 2 This is the X-ray powder diffraction pattern of compound 1-2 prepared in Example 1-2 of the present invention.
[0036] Figure 3 It is the solid-state UV-visible absorption spectrum of compound 1-2 prepared in Example 1-2 of the present invention, wherein (a) is the solid-state UV-visible absorption spectrum of compound 1, and (b) is the solid-state UV-visible absorption spectrum of compound 2.
[0037] Figure 4 The excitation spectrum and emission spectrum of the crystal of compound 1-2 prepared in Example 1-2 of the present invention at room temperature, wherein (a) is the excitation spectrum and emission spectrum of compound 1, and (b) is the excitation spectrum and emission spectrum of compound 2.
[0038] Figure 5 This is the time-resolved PL decay curve of compound 1-2 according to Example 1-2 of the present invention.
[0039] Figure 6 is the photoluminescence quantum yield of compound 1-2 prepared in Example 1-2 of the present invention.
[0040] Figure 7 The fluorescence emission spectra of the crystals, nano-solutions, nano-microcrystals and flexible films of Compound 1 prepared in Example 1 of the present invention are shown.
[0041] Figure 8 The quantum yield of a flexible film made from the nanocrystals of Compound 1 obtained in Example 1 of the present invention.
[0042] Fig. 9The fluorescence emission spectrum of the compound 1-2 crystal prepared in Example 1-2 of the present invention is compared with the fluorescence emission spectrum intensity of the crystal exposed to air for more than one year.
[0043] Fig.10 The X-ray powder diffraction spectrum of the compound 1-2 crystal prepared in Example 1-2 of the present invention and the X-ray powder diffraction spectrum of the crystal exposed to air for more than one year.
[0044] Fig.11 This is the thermogravimetric analysis diagram of compound 1-2 prepared in Example 1-2 of the present invention.
[0045] Fig.12 Temperature-dependent PL emission spectrum (a), fitting relationship between emission intensity and reciprocal temperature (b), and fitting relationship between half-peak width and temperature (c) of compound 1 prepared in Example 1 of the present invention.
[0046] Fig.13 The temperature-dependent PL emission spectrum (a), the fitting relationship between the emission intensity and the reciprocal temperature (b), and the fitting relationship between the half-peak width and the temperature (c) of the compound 2 prepared in Example 2 of the present invention.
[0047] Fig.14 The energy band structure and orbital density diagram of compound 1 prepared in Example 1 of the present invention are obtained by theoretical calculation, wherein (a) is the energy band structure of compound 1, and (b) is the orbital density diagram of compound 1.
[0048] Fig.15 The band structure and orbital density of states diagram of compound 2 prepared in Example 2 of the present invention obtained by theoretical calculation, wherein (a) is the band structure of compound 1, and (b) is the orbital density of states diagram of compound 1.
[0049] Fig.16 Schematic diagram of the luminescence mechanism in the configuration coordination of compound 1-2 prepared in Example 1-2 of the present invention.
[0050] Fig.17 Absorption coefficient of compound 1-2 prepared in Example 1-2 of the present invention as a function of photon energy from 1 to 1000 KeV (a) and radiant luminescence spectrum (b).
[0051] Fig.18 Radiation emission spectra (a) of Compound 1 prepared in Example 1 of the present invention at different dose rates and integrated scintillation intensity as a linear function of X-ray dose rate (b).
[0052] Fig.19 Radiation emission spectra (a) of Compound 2 prepared in Example 2 of the present invention at different dose rates and integrated scintillation intensity as a linear function of X-ray dose rate (b).
[0053] Fig. 20 This is an afterglow image of compound 1-2 prepared in Example 1-2 of the present invention after stopping X-ray irradiation.
[0054] Fig.21 The radiant luminescence emission intensity curve of the compound 1 prepared in Example 1 of the present invention under constant X-ray irradiation and the radiant luminescence emission intensity curve after 20 consecutive switching cycles.
[0055] Fig. 22 This is the MTF curve of the crystalline scintillating screen of compound 1 prepared in Example 1 of the present invention.
[0056] Fig.23 The powder X-ray diffraction spectrum of compound 3 prepared in comparative example 1 of the present invention.
[0057] Fig.24 It is the excitation spectrum and emission spectrum of compound 3 prepared in comparative example 1 of the present invention at room temperature.
[0058] Fig.25 It is the quantum yield of compound 3 prepared in comparative example 1 of the present invention at room temperature.
[0059] Fig.26 It is the radioluminescence spectrum of compound 3 prepared in comparative example 1 of the present invention under X-ray.
[0060] Fig. 27 The powder X-ray diffraction spectrum of compound 4 prepared in comparative example 2 of the present invention.
[0061] Fig.28 These are the excitation spectrum and emission spectrum of compound 4 prepared in comparative example 2 of the present invention at room temperature.
[0062] Fig.29 It is the quantum yield of compound 4 prepared in comparative example 2 of the present invention at room temperature.
[0063] Fig.30 It is the radioluminescence spectrum of compound 4 prepared in comparative example 2 of the present invention under X-ray.
[0064] Fig.31 The powder X-ray diffraction spectrum of compound 5 prepared in comparative example 3 of the present invention.
[0065] Fig.32 These are the excitation spectrum and emission spectrum of compound 5 prepared in comparative example 3 of the present invention at room temperature.
[0066] Fig.33 It is the quantum yield of compound 5 prepared in comparative example 3 of the present invention at room temperature.
[0067] Fig.34It is the radioluminescence spectrum of compound 5 prepared in comparative example 3 of the present invention under X-ray. DETAILED DESCRIPTION
[0068] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0069] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0070] The raw materials used in the embodiments of the present invention are all provided by Aladdin Reagent Company: cuprous bromide (purity 99.9%), cuprous iodide (purity 99.9%), N-aminoethylpiperazine (99%), hydrobromic acid, hydroiodic acid, hypophosphorous acid, ethanol, sec-butyl alcohol, PVP (polyvinyl pyrrolidone), EVA (polyethylene-co-vinyl acetate); the reaction container is a 25 mL glass bottle that can withstand temperatures below 120°C.
[0071] Instruments and detection methods
[0072] The electric heating blast drying oven was provided by Shanghai Yiheng Scientific Instrument Co., Ltd., model DHG-9140.
[0073] The crystal structure was determined by single crystal X-ray diffractometer (SMART APEXII, Bruker, Germany).
[0074] The powder diffraction was measured by X-ray powder diffractometer (Bruker D8 ADVANCE), and the UV-visible absorption spectrum was measured by UV-visible spectrophotometer (PE Lambda 900).
[0075] PL spectroscopy was performed on a F4700 fluorescence spectrometer.
[0076] The photoluminescence quantum yield was achieved by adding an integrating sphere to the FLS980 fluorescence spectrometer.
[0077] The photoluminescence lifetime was measured on an Edinburgh FLS980 fluorescence spectrometer.
[0078] The thermal stability test was performed by thermogravimetric analysis (TGA) on a Mettler TGA / SDTA 851 thermal analyzer in the temperature range of 30-800°C under the constant protection of N2 atmosphere flow.
[0079] RL spectra were obtained using a 1000 fluorescence spectrometer equipped with a Mini-X-ray tube.
[0080] Example 1
[0081] The preparation method of [AEPipz]CuBr3·Br·H2O (compound 1) comprises the following steps:
[0082] (1) 1 Mmol of N-aminoethylpiperazine and 1 Mmol of cuprous bromide were mixed and dissolved in a mixed solvent of 1 mL of hydrobromic acid and 4 mL of sec-butyl alcohol, and stirred thoroughly until dissolved, and then 0.5 mL of hypophosphorous acid was added to obtain a mixed solution, which was added to a reaction container;
[0083] (2) The sealed reaction solvent was placed in an electric heated forced air drying oven with programmable temperature control for hydrothermal reaction at 80°C for 72 h. After the reaction was completed, it was naturally cooled to room temperature, allowed to stand for 1 day, washed, and dried to obtain the target compound 1, recorded as [AEPipz]CuBr3·Br·H2O.
[0084] Example 2
[0085] The preparation method of [AEPipz]CuI3·I·H2O (compound 2) comprises the following steps:
[0086] (1) 1 mmol of N-aminoethylpiperazine and 1 mmol of cuprous iodide were mixed and dissolved in a mixed solvent of 1 mL of hydroiodic acid and 4 mL of deionized water, and stirred thoroughly until dissolved, and then 0.5 mL of hypophosphorous acid was added to obtain a mixed solution, which was added to a reaction container;
[0087] (2) The sealed reaction vessel was placed in an electric heating forced air drying phase with programmable temperature control to carry out a hydrothermal reaction at a reaction temperature of 100°C for a reaction time of 72 h. After the reaction was completed, it was naturally cooled to room temperature, allowed to stand for 1 day, washed, and dried to obtain the target compound 2, which was recorded as [AEPipz]CuI3·I·H2O.
[0088] Example 3
[0089] [AEPipz] A method for preparing a CuBr3·Br·H2O flexible film comprises the following steps:
[0090] (1) 1 mmol CuBr and 2 mL KBr aqueous solution (concentration: 1.45 mol / L) were mixed, and 0.05 mL hypophosphorous acid was added dropwise to the CuBr / KBr aqueous solution to obtain a solution containing an anion skeleton;
[0091] (2) 1 g of polyvinylpyrrolidone (PVP) is dissolved in 100 mL of ethanol to obtain a PVP / ethanol solution. Then, the solution containing the anionic skeleton is slowly added to the PVP / ethanol solution under continuous stirring to immediately form a turbid white solution. Subsequently, 0.2 mL of protonated N-aminoethylpiperazine is quickly injected into the white solution and stirred for 24 hours; the protonated N-aminoethylpiperazine is prepared by adding 1 mL of hydrobromic acid to 0.1 mL of N-aminoethylpiperazine.
[0092] (3) centrifuging at a low speed of about 2000 rpm to collect the suspension, and then centrifuging the collected suspension at a high speed of about 6000 rpm for more than 10 minutes to further collect microcrystals with a size of nanometers;
[0093] (4) 100 mg of EVA was completely dissolved in 5 mL of cyclohexane and stirred at 60° C. for 1 hour to form a solution. 50 mg of the nano-scale microcrystals prepared in step (3) and 1 mL of ethanol mixed solution were added to the solution formed in step (3) and stirred thoroughly until a uniform and viscous fluid was formed. The fluid was evenly applied on the glass and slowly evaporated in a fume hood at room temperature to finally obtain a flexible film with high-efficiency X-ray scintillation luminescence performance.
[0094] Comparative Example 1
[0095] The preparation method of the zero-dimensional hybrid cuprous material comprises the following steps:
[0096] 1 mmol of cuprous iodide and 2 mmol of benzyltriphenylphosphonium bromide were mixed in 1 mL of hydroiodic acid and 4 mL of ethanol solvent, and 0.5 mL of hypophosphorous acid was added dropwise. The raw materials were dissolved under heating and constant magnetic stirring until the suspension became clear, and then allowed to stand at room temperature for 3 days. Compound 3 was obtained after washing and drying.
[0097] Comparative Example 2
[0098] The preparation method of the zero-dimensional hybrid cuprous material comprises the following steps:
[0099] 1 mmol of cuprous bromide and 1 mmol of 1-ethylpyridinol bromide were added to a mixed solution of 5 mL of ethanol, 0.5 mL of hydrobromic acid and 0.5 mL of hypophosphorous acid; the suspension was heated and stirred continuously at 80°C for about 5 minutes until it became clear, and then allowed to stand at room temperature for 5 days, after which the mixture was filtered to obtain a large amount of colorless compound 4.
[0100] Comparative Example 3
[0101] The preparation method of the zero-dimensional cuprous halide material comprises the following steps:
[0102] 1 mmol of tetrapropylamine and 1 mmol of cuprous iodide were mixed, dissolved in a mixed solvent of hydroiodic acid and isobutyl alcohol, and stirred thoroughly until dissolved, followed by adding 0.5 mL of hypophosphorous acid to obtain a mixed solution; the reaction was placed in an electric heated blast drying oven at a reaction temperature of 60°C for a reaction time of 72 h; after the reaction was completed, the mixture was naturally cooled to room temperature, and compound 5 was obtained after washing and drying.
[0103] Results Analysis
[0104] The molecular formula of the compound 1 prepared in Example 1 of the present invention is [AEPipz]CuBr3·Br·H2O (AEPipz = N-Aminoethylpiperazine), the crystal system space group is P21 / c, and the unit cell parameters are α=90°,β=97.670(2)°,γ=90°,Z=4,the unit cell volume is
[0105] The molecular formula of compound 2 prepared in Example 2 is [AEPipz]CuI3·I·H2O, the crystal system space group is P21 / c, and the unit cell parameters are α=90°,γ=98.575(4),β=90°,Z=4, the unit cell volume is
[0106] Figure 1 Schematic diagram of the crystal structure of compound 1 and compound 2. Figure 1 As shown, the single crystal X-ray diffraction test results show that each Cu atom is coordinated by four Br or I atoms as [CuX4] 3- Tetrahedron, further interconnected by edge-sharing two Br atoms to form [Cu2X6] 4- The Cu-Br and Cu-I bond distances are and Between the two [Cu2X6] 4- are periodically embedded in large organic matter[AEPipz] 3+ The two adjacent [Cu2X6] 4- The closest distances between dimer clusters are and Such a long distance effectively reduces the adjacent [Cu2X6] 4- Energy transfer between dimers is conducive to efficient luminescence.
[0107] like Figure 2 As shown, the diffraction peaks of the X-ray powder diffraction patterns of Compound 1 and Compound 2 are completely consistent with the diffraction peaks of the single crystal structure simulation, indicating the high purity of Compound 1 and Compound 2.
[0108] like Figure 3 As shown, the UV-visible spectrum exhibits strong absorption in the range of 300-500 nm, and based on Tauc's function fitting, the indirect band gaps of compound 1 and compound 2 are determined to be 2.84 eV and 3.47 eV, respectively.
[0109] like Figure 4 As shown, under an excitation wavelength of 292 nm, compound 1 exhibits broadband emission from 400 nm to 650 nm, with a wide FWHM of 93 nm and a large Stokes shift of 208 nm; under excitation at 287 nm, the maximum peak of the emission spectrum of compound 2 is about 469 nm, the FWHM is 90 nm and the large Stokes shift is 182 nm, and it exhibits similar broadband light emission as compound 1. The larger Stokes shift indicates that the self-absorption characteristics can be ignored, which is conducive to efficient scintillation performance.
[0110] like Figure 5 As shown, time-resolved PL decay curves of compound 1 and compound 2 were collected at 300 K to understand their photodynamics. The PL decay curves were fitted with a single exponential function, and the lifetimes of compound 1 and compound 2 were 121.7 μs and 3.42 μs, respectively. The long lifetimes of compound 1 and compound 2 were attributed to the radiative recombination of triplet self-trapped exciton emission.
[0111] In order to better understand the performance of zero-dimensional halides in the field of luminescence, the quantum yields of compounds 1 and 2 were tested.
[0112] from Figure 6 As shown, the quantum yields of compounds 1 and 2 under UV excitation are 92.10% and 89.20%, respectively. It is worth noting that the highest photoquantum yield of compound 1 has exceeded all reported zero-dimensional copper-based (I) halides. For example, [ETPP]CuBr2 (65.2%), [(C3H7)4N]2Cu2I4 (91.9%), [BAPMA]Cu2Br5 (53.4%), (TBA)CuBr2 (80.5%), PEA4Cu4I4 (73.6%).
[0113] like Figure 7-8 As shown, the emission spectrum of the flexible film made of the nanoparticles synthesized in Example 3 is consistent with that of the crystal of Compound 1, both of which are cyan emission. In addition, the flexible film has good luminescence performance, and its quantum yield is as high as 62.55%.
[0114] In addition to excellent photoluminescence performance, compound 1-2 has sufficient structural and luminescence stability in air.
[0115] like Figure 9-10 As shown, the PXRD patterns and PL emission spectra of compounds 1-2 were not significantly changed after being exposed to air for one year.
[0116] Fig.11 Thermogravimetric analysis shown shows that compound 1-2 has good thermal stability.
[0117] To further investigate the mechanism of the broadband light emission, temperature-dependent PL measurements from 80 K to 300 K were performed for both halides.
[0118] like Fig.12 (a) and 13(a), in the entire temperature range, there is only one emission peak without any splitting, indicating that the emission should come from the same excited state in all phases. As the temperature decreases, the weakened thermally activated non-radiative recombination causes the PL intensity to increase monotonically. Thermal activation energy (exciton binding energy) can be used to evaluate the degree of excitation recombination, that is, large energy means strong binding ability of electron-hole pairs, which is conducive to the formation of stable bound excitons. Fig.12 As shown in (b) and 13(b), during the cooling process, the weakened thermal non-radiative recombination rate leads to a monotonically increasing emission intensity. According to the Arrhenius-type equation, the relevant thermal activation energy (E) can be extracted from the temperature-dependent emission intensity. a ). For compounds 1-2, the evaluated Ea values are 33.7meV and 31.9meV, respectively, which are greater than the thermal decomposition energy of free excitons at room temperature (26meV), indicating the formation of stable STE. The higher energy barrier ensures the formation of stable excitons to overcome thermal decomposition and subsequently produce strong luminescence at room temperature. In addition, the FWHM gradually narrows with decreasing temperature, which is generally due to the weakening of the electron-phonon coupling strength, further strongly confirming the nature of self-trapped exciton emission. Here, the electron-phonon coupling strength can be evaluated by the Huang Kun factor. The Huang Kun factor and the phonon frequency can be obtained by fitting the temperature-dependent FWHM, such as Fig.12 As shown in (c) and 13(c), the estimated Huang-Kun factor values of compounds 1-2 are 60.4 and 62.6, respectively, which are larger than those of all-inorganic copper halides, such as Rb2CuBr3 (37.17) and Cs3Cu2I5 (40.33), indicating a softer organic-inorganic hybrid lattice and stronger electron-phonon coupling.
[0119] To gain a deeper understanding of the unique PL behavior, the band structure and predicted density of states were performed based on DFT calculations.
[0120] like Fig.14 a and Fig.15As shown in a, the band gaps between the valence band maximum (VBM) and conduction band minimum (CBM) of compounds 1 and 2 are 2.50 eV and 2.81 eV, respectively. Due to the limitations of DFT calculations, the calculated band gaps are slightly lower than the experimental results of UV spectroscopy. This phenomenon has been widely reported in other semiconductor materials. In addition, the band structure shows that the valence band is quite flat and the dispersion is negligible, while the conduction band shows significant dispersion. In order to gain a deeper understanding of this phenomenon, the predicted density of states was further calculated. As shown in Fig.12 b and Fig.13 As shown in b, the VBM is mainly contributed by the Cu-3d and Xp orbitals of the two halides, resulting in a rather flat band. This can be understood by the fact that due to the adjacent [Cu2X6] 4- The ultra-long distance between clusters has a strong quantum confinement effect, and the Cu-3d orbital is quite confined. In addition to some Cu-3d orbitals, the CBM is mainly contributed by the Xs state. In addition, for both halides, the electron distribution of the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) is mostly located in [Cu2X6] 4- On the dimer, this also verifies that the highly recombination center captures excitons and dominates the luminescence properties of the hybrid halide.
[0121] Taking into account the wide half-peak width, large Stokes shift, microsecond lifetime and DFT calculation results, we attribute these broadband light emissions to the radiative recombination of STEs caused by strong electron-phonon coupling in the 0D soft lattice. Fig.16 As shown. Under the photoexcitation of high-energy UV light, electrons are rapidly excited from the ground state to the excited state to form free excitons (FE). At the same time, due to the strong exciton-phonon interaction in the soft 0D lattice, the free excitons are rapidly captured to form low-energy STEs through intersystem crossing (ISC). Ultimately, the recombination of excitons from the triplet excited state to the ground state produces broadband light emission with a large Stokes shift.
[0122] Considering the importance of scintillators to X-ray attenuation, the present invention first plotted the absorption coefficients of compound 1-2 and commercially available scintillator LuAG:Ce at different photon energies.
[0123] like Fig.17 As shown in (a), the X-ray absorption coefficient of compound 1-2 is slightly lower than that of commercial LuAG:Ce scintillator, indicating that it has high absorption rate of X-ray in a wide energy range. Fig.17As shown in (b), similar to the PL properties under UV radiation, compounds 1 and 2 emit the same cyan emission under X-ray radiation. The almost identical RL and PL spectral distributions indicate the same luminescence mechanism. The light yield, a key parameter of scintillator materials, is determined by comparing the integrated area of the RL emission spectrum with that of commercial LuAG:Ce as a reference, which has a standard light yield of 25,000 photons MeV. -1 The light yields of compound 1 and compound 2 are 62,400 MeV respectively. -1 Photons and 49,300 MeV -1 photons, outperforming most state-of-the-art commercially available inorganic scintillators such as NaI:Tl (38,000 photons MeV -1 ), CsI:Tl (54,000 photons MeV -1 ), BGO (9,000 photons MeV -1 )wait.
[0124] At the same time, the detection limit is another important parameter of X-ray scintillation. The RL emission intensity at different doses is measured to evaluate the sensitivity of the response to X-rays. Fig.18 (a) and 19(a), the RL intensity increases with the X-ray dose from 5000 to 50000 μGyair·s -1 The linear increase of RL intensity demonstrated the potential application of compound 1-2 as a scintillator at high doses. At the same time, the detection limit was evaluated by fitting the relationship between RL intensity and X-ray dose. Fig.18 As shown in (b) and 19(b), when the signal-to-noise ratio (SNR) is equal to 3, the detection limits of compound 1 and compound 2 are calculated to be 95.7 nGyair·s -1 and 94.0nGyair·s -1 , which is 5.5μGyair·s higher than the normal X-ray dose required for medical diagnosis -1 The ultra-high light yield and low detection limit are better than most well-designed Cu(I) halide-based scintillators, further demonstrating the multiple advantages of cuprous halide-based scintillators.
[0125] In order to explore the potential applications of compound 1 in medical imaging, industrial X-ray detection, etc., the present invention has made the following explorations on its imaging technology.
[0126] like Fig. 20 As shown, after the X-ray was cut off, the relative afterglow intensities of compound 1 and compound 2 decreased rapidly to the background level (0.1%) within 53.6 ms and 39.1 ms, respectively.
[0127] like Fig.21As shown, considering the high light yield, the stability of the scintillation performance of compound 1-2 was evaluated by switching on / off and continuously irradiating X-rays. The results showed that the RL intensity remained unchanged within 20 irradiation on / off cycles within 100 min, indicating its excellent X-ray resistance. -1 After continuous irradiation for 2 hours at a wide range of X-ray dose rates, the RL intensity only weakened by 4.3%, further confirming the robust stability. In summary, the present invention has high light yield, low detection limit and ultra-high stability, and is an ideal scintillator material for X-ray imaging.
[0128] Finally, the flexible film synthesized by Example 3 was used as a flexible scintillator screen to evaluate the X-ray imaging capability on a homemade X-ray imaging optical device. When the metal ring sealed in the box was irradiated with X-rays, the metal ring inside the box could be clearly distinguished on the CCD camera due to the large difference in X-ray absorption capacity between the box and the ring. The same result was observed for the metal pendant sealed in a polytetrafluoroethylene box. In addition, in X-ray imaging, delicate circuit board details can still be clearly displayed with sufficient contrast. The resolution of X-ray imaging was roughly determined using a standard X-ray resolution test pattern plate, where ≈14-18lp mm can be observed. -1 High resolution. Fig. 22 To further evaluate the image quality, the modulation transfer function (MTF) was calculated based on the slant edge method. At an MTF value of 0.2, the spatial resolution is 17.25 lp / mm, which is consistent with the resolution limit observed from the standard line pair card. This value is close to some reported metal halide perovskite scintillator screens and far exceeds that of commercial scintillators based on CsI:Tl (10 lp mm -1 ). In general, the zero-dimensional mixed cuprous halide prepared by the present invention has high light yield, low detection limit, strong radiation resistance, good flexibility and high spatial resolution. These excellent X-ray imaging properties expand the application in the fields of wearable radiation radiography, industrial X-ray detection, etc.
[0129] The molecular formula of compound 4 prepared in comparative example 1 is [BzTPP]2Cu2I4, the crystal system space group is C2 / c, and the unit cell parameters are α=90°,β=110.259°,γ=90°,Z=8,the unit cell volume is
[0130] like Fig.23 As shown, the powder diffraction pattern of compound 3 is consistent with the data of single crystal structure simulation, indicating the high purity of compound 3. Fig.24As shown, under 362 nm excitation, compound 3 exhibits broadband light emission in the entire visible light range, with the maximum emission peak located at around 529 nm. These broadband light emissions are manifested by a wide half-peak width of 101 nm and a large Stokes shift of 167 nm.
[0131] like Fig.25 As shown, the quantum yield of compound 3 is 44.24%, and the fluorescence intensity is lower than that of Example 1 (92.1%) and Example 2 (89.2%).
[0132] like Fig.26 As shown, the light yield of compound 3 (27706 photons MeV -1 ) is the standard sample LuAG:Ce (25000 photons MeV -1 ) is 1.1 times that of Example 1 (62,400 photons MeV -1 ) and Example 2 (49300 photons MeV -1 ). The photoluminescence and radioluminescence properties of the compound 1-2 of the present invention are better than those of the compound 3 prepared in comparative example 1.
[0133] The molecular formula of compound 4 prepared in Comparative Example 2 is [BAPMA]Cu2Br5, the crystal system space group is P-1, and the unit cell parameters are α=83.0260°,β=70.9060°,γ=74.1900°,Z=2,unit cell volume is
[0134] like Fig. 27 As shown, the diffraction peaks of X-ray powder diffraction of compound 4 are consistent with the diffraction peaks of single crystal structure simulation, indicating the high purity of compound 4.
[0135] like Fig.28 As shown, under 282 nm excitation, compound 4 exhibits broadband light emission in almost the entire visible light range, with the maximum emission peak located at around 526 nm. These broadband light emissions are manifested by a wide half-peak width of 101 nm and a large Stokes shift of 244 nm.
[0136] like Fig.29 As shown, the quantum yield of compound 5 is 53.4%, and the fluorescence intensity is lower than that of Example 1 (92.1%) and Example 2 (89.2%).
[0137] like Fig.30 As shown, the light yield of compound 4 (43744 photons MeV -1 ) is the standard sample LuAG:Ce (25000 photons MeV -1 ) is 1.7 times lower than that of Example 1 (62,400 photons MeV -1) and Example 2 (49300 photons MeV -1 ). Therefore, the photoluminescence and radioluminescence properties of the compound 1-2 of the present invention are better than those of the compound 4 prepared in comparative example 2.
[0138] The molecular formula of compound 5 prepared in comparative example 3 is [TPA]CuBr2, the crystal system space group is P-1, and the unit cell parameters are α=94.6937°,β=107.9969°,γ=109.4976°,Z=2,the unit cell volume is
[0139] like Fig.31 As shown, the diffraction peaks of X-ray powder diffraction of compound 5 are consistent with the diffraction peaks of single crystal structure simulation, indicating the high purity of compound 5. Fig.32 As shown, under 323 nm excitation, compound 5 exhibits broadband light emission within 400-800 nm, with the maximum emission peak at around 596 nm. These broadband light emissions are manifested by a wide half-peak width of 106 nm and a large Stokes shift of 176 nm.
[0140] like Fig.33 As shown, the quantum yield of compound 5 is 15%, and the fluorescence intensity is much lower than that of Example 1 (92.1%) and Example 2 (89.2%).
[0141] like Fig.34 The light yield of compound 5 (8750 photons MeV -1 ) is the standard sample LuAG:Ce (25000 photons MeV -1 ) is 0.35 times that of Example 1 (62,400 photons MeV -1 ) and Example 2 (49300 photons MeV -1 ). The photoluminescence and radioluminescence properties of the compound 1-2 of the present invention are much better than those of the compound 5 prepared in comparative example 3, so it has no application prospect in X-ray imaging.
[0142] In summary, in order to solve the low light yield, high toxicity and high temperature and high pressure harsh synthesis problems of lead halide perovskite nanocrystals and traditional inorganic scintillators, the present invention can prepare zero-dimensional hybrid copper-based halide single crystals by a low-temperature solvothermal method. In view of the importance of dynamic X-ray flexible imaging for real-time monitoring of the internal curved structure of complex devices, it is still urgent and challenging to develop high-performance X-ray scintillators with high X-ray absorption coefficient, simple synthesis process, controllable crystal size and excellent processing performance. The present invention controls the size of the crystal by adding a surfactant, and then mixes the nanocrystals with a polymer material to prepare a zero-dimensional copper (I)-based halide flexible luminescent material with high-efficiency X-ray scintillation luminescence performance. These two halides have ultra-high photoluminescence quantum yields as broadband cyan light emitters. As expected, the high quantum yield and large Stokes shift make these two halides high-performance X-ray scintillators with a maximum light yield of 62,400 photons·MeV -1 The minimum detection limit is 95.7 nGyair·s -1 , far superior to commercially available scintillators. Significantly, [AEPipz]·CuBr3·Br·H2O, with the assistance of polyvinylpyrrolidone (PVP), can be controlled from millimeter-scale single crystals to nanometer-scale powder crystals, which is conducive to the construction of high-quality flexible films. Therefore, the present invention can assemble a highly transparent, well-distributed and stable film as a flexible scintillator screen with a spatial resolution of up to 17.4lp·mm -1 , demonstrating the obvious advantages of high-performance flexible X-ray imaging. These combined advantages, including high cost-effectiveness, large-scale assembly, excellent scintillation performance, strong radiation resistance and great flexibility, fully demonstrate the unique advantages of low-dimensional cuprous halide as a high-performance scintillator. This invention not only highlights the multiple advantages of cuprous halide scintillators, but also promotes advanced applications in cutting-edge radiation industries such as medical diagnosis, non-destructive testing and radiation monitoring.
[0143] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0144] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a zero-dimensional copper (I)-based halide flexible luminescent material, characterized in that: The following steps are involved: The cuprous salt and KBr are mixed, and then a hypophosphorous acid reducing agent is added, and the cuprous salt and the halogen are coordinated to form an anion skeleton, thereby obtaining a solution containing an anion skeleton; Dissolving polyvinyl pyrrolidone in ethanol to obtain a polyvinyl pyrrolidone mixed solution, adding the polyvinyl pyrrolidone mixed solution to a solution containing an anion skeleton to diffuse the anion skeleton; reacting an organic amine with a hydrohalic acid to form a protonated organic amine, thereby forming an organic cation, and then adding the protonated organic amine to the diffused anion skeleton solution, stirring at room temperature, to obtain a zero-dimensional copper (I)-based halide nanocrystalline material; EVA is dissolved in cyclohexane to obtain a mixed solution, the zero-dimensional copper (I)-based halide nanocrystalline material and ethanol are mixed and added to the mixed solution, and a fluid is obtained after stirring, and the fluid is post-treated to obtain a zero-dimensional copper (I)-based halide flexible luminescent material.
2. The method for preparing a zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The cuprous salt is cuprous bromide, the organic amine is N-aminoethylpiperazine, and the hydrohalic acid is hydrobromic acid.
3. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The usage ratio of cuprous salt to KBr is 1mmol:2~3mL.
4. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The dosage ratio of polyvinyl pyrrolidone to ethanol is 1 g:100 mL, and the dosage ratio of polyvinyl pyrrolidone to cuprous salt is 1 g:1 mmol.
5. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: In the protonated organic amine, the volume ratio of the organic amine to the hydrohalic acid is 1:10, and the dosage ratio of the organic amine to the cuprous salt is 0.1 mL:1 mmol.
6. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The volume ratio of hypophosphorous acid to organic amine is 1:1.5-2.
7. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The usage ratio of EVA to cyclohexane is 100 mg:4-5 mL.
8. The method for preparing the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 1, characterized in that: The dosage ratio of nanocrystals to ethanol was 50 mg:1 mL, and the mass ratio of nanocrystals to EVA was 1:
2.
9. A zero-dimensional copper (I)-based halide flexible luminescent material prepared by the preparation method according to any one of claims 1 to 8.
10. An application of the zero-dimensional copper (I)-based halide flexible luminescent material according to claim 9 in the fields of wearable radiation imaging and industrial X-ray detection.
Citation Information
Cited By
Organic-inorganic hybrid copper-based halide crystal material as well as preparation method and application thereof
CN120797211A