Processing technology for improving easy cracking of leather bags and suitcases
Through a multi-step process, including natural vegetable oil soaking, sonication and nano-scale fillers, the problem of difficulty in improving flexibility, waterproofness, compressive resistance and crack resistance in leather processing technology is solved, and the comprehensive improvement of leather performance is achieved and environmentally friendly and economical processing process.
Patent Information
- Application Number
- CN202410911997.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing leather processing technology is difficult to simultaneously improve the flexibility, water resistance, compressive resistance and crack resistance of leather, and often uses high concentrations of chemicals, affecting the environment and increasing costs.
Multi-step process is adopted, including preliminary treatment to remove surface impurities, natural vegetable oil immersion to improve flexibility, sonication treatment enhances fiber uniformity, hot-press seals the gaps between fibers, nano-scale fillers increase compressive resistance, and ultimately form a protective layer.
Significantly improves the flexibility and water resistance of the leather, enhances compressive and crack resistance, reduces the environmental impact, and optimizes processing costs.
Smart Images

Figure CN118879949A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of leather processing, and in particular to a processing technology for improving the easy cracking of leather bags. Background Art
[0002] Leather bags are popular for their unique appearance and durability, but they are prone to cracking during long-term use, especially when frequently used or exposed to harsh environmental conditions. Traditional leather processing methods mainly focus on the use of chemical tanning agents and dyes to enhance its beauty and softness. However, these methods often ignore the improvement of leather's crack resistance and long-term durability. Although there are a variety of processing technologies on the market to improve the softness and waterproofness of leather, these technologies often fail to fully solve the structural stability and durability of leather after experiencing physical stress, resulting in leather products prone to cracking during use, thereby affecting the product life and user satisfaction.
[0003] The main limitation of current leather processing technology is the lack of a comprehensive approach to simultaneously improve the flexibility, water resistance, compression resistance and crack resistance of leather. Most treatment methods tend to adopt a single chemical or physical treatment without considering the interactions and synergistic effects between these treatments. In addition, existing methods usually involve the use of high concentrations of chemicals, which may not only have a negative impact on the environment, but also increase processing costs without enhancing the intrinsic properties of leather.
[0004] Therefore, developing a new leather processing technology that can comprehensively improve the physical and chemical properties of leather while solving the problems of environmental impact and cost-effectiveness is a technical problem that urgently needs to be solved in the market. Summary of the invention
[0005] Based on the above purpose, the present invention provides a processing technology for improving the cracking of leather bags.
[0006] A processing technology for improving the cracking of leather bags, comprising the following steps:
[0007] S1: Select raw leather, perform preliminary treatment to remove surface impurities, and adjust the moisture content to between 12% and 15%;
[0008] S2: Soak the leather treated with S1 in a natural plant oil solution to fully soak it to improve its flexibility and waterproof properties;
[0009] S3: Performing sonication treatment on the soaked leather, using sonic vibrations of a predetermined frequency to make the leather fibers more uniform;
[0010] S4: Perform heat pressing treatment to seal the gaps between leather fibers by controlling temperature and pressure;
[0011] S5: Cooling and aging the leather after heat pressing to stabilize its structure;
[0012] S6: Filling the aged leather with nano-scale fillers to increase the density and compression resistance of the leather;
[0013] S7: The filled leather is subjected to a final surface coating treatment to form a protective layer.
[0014] Furthermore, the raw leather in S1 includes cowhide, sheepskin or pigskin.
[0015] Furthermore, the preliminary processing in S1 specifically includes:
[0016] S11: Mechanically clean the raw leather to remove surface sand and impurities by scraping and brushing;
[0017] S12: chemically clean the leather after mechanical cleaning, using a weak alkaline solution with a mass ratio of 5%-10% for soaking for 10-20 minutes to completely remove residual impurities on the surface;
[0018] S13: Drying the cleaned leather by using a blower at a temperature of 30° C. to 40° C. for 1 to 2 hours;
[0019] S14: Perform spray humidification treatment on the dried leather, use pure water spray to adjust the moisture content of the leather to 12%-15% to ensure uniform absorption.
[0020] Furthermore, the S2 specifically includes:
[0021] S21: preparing a natural vegetable oil solution, mixing the vegetable oil with water at a mass ratio of 15% to 20%, and stirring to form a stable emulsion;
[0022] S22: completely immersing the leather treated in S1 in the natural vegetable oil solution, and ensuring that the solution fully covers the surface of the leather;
[0023] S23: controlling the soaking temperature to 20° C. to 25° C. and maintaining the constant temperature for 36 hours;
[0024] S24: Stir the solution every 6 hours during the soaking process;
[0025] S25: After soaking, remove the leather from the solution and shake dry to remove excess vegetable oil solution from the surface.
[0026] Furthermore, the S3 specifically includes:
[0027] S31: placing the leather soaked in S2 in a sonication treatment device, and spreading the leather flat to avoid overlapping;
[0028] S32: setting the frequency of the sonication device to 40 kHz and the amplitude to be controlled within the range of 10-20 microns;
[0029] S33: Start the sonication treatment equipment to continuously treat the leather for 20 minutes;
[0030] S34: During the treatment process, the position of the leather is adjusted every 5 minutes to ensure that the sound waves act evenly on all parts of the leather;
[0031] S35: After the sonication is complete, remove the leather from the equipment and let it sit for 5 minutes to relieve internal stress.
[0032] Furthermore, the S4 specifically includes:
[0033] S41: Place the leather treated with S3 sonic waves in a hot press and ensure that the leather is flat and wrinkle-free;
[0034] S42: setting the target temperature of the hot pressing device to 70° C. to 90° C., and preheating the device to the target temperature;
[0035] S43: setting the hot pressing pressure to 5 MPa, placing the leather between the hot pressing plates, and gradually applying pressure;
[0036] S44: heat-pressing the leather under the conditions of maintaining temperature and pressure for 10 minutes;
[0037] S45: During the process, check the temperature and pressure of the hot press plate every 5 minutes to ensure that they are stable;
[0038] S46: After the heat pressing treatment is completed, the pressure is gradually reduced to zero, and the leather is taken out of the heat pressing equipment and laid flat to cool.
[0039] Furthermore, the S5 specifically includes:
[0040] S51: taking the leather treated by heat pressing in S4 out of the heat pressing device and quickly placing it flat on a cooling rack;
[0041] S52: Cooling the leather with a blower, the cooling temperature is controlled at 20° C. to 25° C., and the cooling time is 30 minutes;
[0042] S53: After cooling, the leather is transferred to an aging room, the temperature of which is controlled at 25°C to 30°C, and the relative humidity is maintained at 40%-50%;
[0043] S54: The leather is left to stand in the aging room for 24 hours to gradually stabilize the internal structure of the leather;
[0044] S55: During the aging process, check and record the temperature and humidity of the aging room every 4 hours to ensure the stability of the environmental conditions.
[0045] Furthermore, the S6 specifically includes:
[0046] S61: Place the leather after S5 aging on the coating table to ensure that the leather is flat;
[0047] S62: preparing a nano-scale filler solution, wherein the nano-filler is selected to be a silane-based compound, and the concentration of the solution is controlled at 5%-10%;
[0048] S63: Use a spraying device to evenly spray the nano-scale filler on the leather surface, and the spraying thickness is controlled at 0.1-0.2 mm;
[0049] S64: Place the sprayed leather in a constant temperature room at 30°C to 40°C for 2 hours to ensure full penetration and curing of the filler;
[0050] S65: After the filling process is completed, the leather is dried for a second time by using a blower at a temperature of 25°C to 30°C for 1 hour.
[0051] Furthermore, the S7 specifically includes:
[0052] S71: Place the leather treated with S6 filling on the coating machine to ensure that the leather is flat and wrinkle-free;
[0053] S72: preparing a high molecular polymer coating solution, wherein the solution contains 3% to 5% of an anti-ultraviolet and anti-oxidant compound;
[0054] S73: Use a coating machine to evenly coat the high molecular polymer coating solution on the leather surface, and the coating thickness is controlled at 0.3-0.5 mm;
[0055] S74: Place the coated leather in a drying room at a temperature of 50°C to 60°C for 1-2 hours to ensure that the coating is fully cured;
[0056] S75: After drying, cool the leather and leave it at room temperature for 30 minutes to allow the coating to stabilize.
[0057] Beneficial effects of the present invention:
[0058] The present invention, by comprehensively using a variety of treatment methods, significantly improves the flexibility and water resistance of leather, while enhancing the compression resistance and crack resistance of leather. Through the soaking treatment of natural vegetable oil, the leather fibers are fully nourished and softened, making the leather more durable when facing physical stretching or pressure. The application of sonication and hot pressing technology ensures a tighter bond between leather fibers, greatly improves the structural stability of the leather, and effectively prevents cracking problems during long-term use.
[0059] The present invention uses environmentally friendly processing materials, such as natural vegetable oils and low-concentration nanofillers, which not only reduces the impact on the environment but also optimizes the processing cost. The optimization of the entire processing process aims to reduce the use of chemical substances. At the same time, by finely controlling the conditions of each processing step, the material utilization rate and processing efficiency are maximized. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0061] Figure 1 A schematic diagram of a processing technique for improving the cracking of leather bags according to an embodiment of the present invention;
[0062] Figure 2 FIG. 4 is a schematic diagram of a sonication process according to an embodiment of the present invention. DETAILED DESCRIPTION
[0063] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0064] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0065] Example 1
[0066] like Figure 1-Figure 2 As shown, a processing technology for improving the cracking of leather bags includes the following steps:
[0067] S1: Select raw leather, perform preliminary treatment to remove surface impurities, and adjust the moisture content to between 13% to maintain the original softness and elasticity of the leather;
[0068] S2: Soak the leather treated with S1 in a natural plant oil solution to fully soak it to improve its flexibility and waterproof properties;
[0069] S3: Performing sonication treatment on the soaked leather, using sonic vibrations of a predetermined frequency to make the leather fibers more uniform and enhance the bonding force between the fibers;
[0070] S4: Perform heat pressing treatment to seal the gaps between leather fibers by controlling temperature and pressure, thereby enhancing the stability of the leather structure;
[0071] S5: Cooling and aging the leather after heat pressing to stabilize its structure;
[0072] S6: Filling the aged leather with nano-scale fillers to increase the density and compression resistance of the leather;
[0073] S7: The filled leather is subjected to a final surface coating treatment to form a protective layer to effectively prevent cracking caused by external environmental factors (such as ultraviolet rays, oxidation, etc.).
[0074] The raw leather options in S1 include cowhide.
[0075] The preliminary processing in S1 specifically includes:
[0076] S11: Mechanically clean the raw leather to remove surface sand and impurities by scraping and brushing;
[0077] S12: chemically clean the leather after mechanical cleaning by soaking it in a weak alkaline solution with a mass ratio of 8% for 15 minutes to completely remove residual impurities on the surface;
[0078] S13: drying the cleaned leather by using a blower at a temperature of 35° C. for 1.5 hours;
[0079] S14: Perform spray humidification treatment on the dried leather, use pure water spray to adjust the moisture content of the leather to 13% to ensure uniform absorption.
[0080] S2 specifically includes:
[0081] S21: preparing a natural vegetable oil solution, mixing the vegetable oil with water at a mass ratio of 18%, and stirring to form a stable emulsion;
[0082] S22: completely immerse the leather treated in S1 in the natural vegetable oil solution, and ensure that the solution fully covers the leather surface;
[0083] S23: Control the soaking temperature at 23°C and keep it constant for 36 hours to ensure that the leather fibers fully absorb the vegetable oil;
[0084] S24: Stir the solution every 6 hours during the soaking process to ensure that the solution components are evenly distributed and effectively penetrate into the leather fibers;
[0085] S25: After soaking, remove the leather from the solution and shake dry to remove excess vegetable oil solution from the surface.
[0086] S3 specifically includes:
[0087] S31: placing the leather soaked in S2 in a sonication treatment device, and spreading the leather flat to avoid overlapping;
[0088] S32: Setting the frequency of the sonication device to 40 kHz and the amplitude to 15 microns;
[0089] S33: Start the sonication treatment equipment to continuously treat the leather for 20 minutes;
[0090] S34: During the treatment process, the position of the leather is adjusted every 5 minutes to ensure that the sound waves act evenly on all parts of the leather;
[0091] S35: After the sonication is complete, remove the leather from the equipment and let it sit for 5 minutes to relieve internal stress.
[0092] S4 specifically includes:
[0093] S41: Place the leather treated with S3 sonic waves in a hot press and ensure that the leather is flat and wrinkle-free;
[0094] S42: setting the target temperature of the hot pressing device to 80° C. and preheating the device to the target temperature;
[0095] S43: setting the hot pressing pressure to 5 MPa, placing the leather between the hot pressing plates, and gradually applying pressure;
[0096] S44: heat-pressing the leather under the conditions of maintaining temperature and pressure for 10 minutes;
[0097] S45: During the process, check the temperature and pressure of the hot press plate every 5 minutes to ensure that they are stable;
[0098] S46: After the heat pressing treatment is completed, the pressure is gradually reduced to zero, and the leather is taken out of the heat pressing equipment and laid flat to cool.
[0099] S5 specifically includes:
[0100] S51: taking the leather treated by heat pressing in S4 out of the heat pressing device and quickly placing it flat on a cooling rack;
[0101] S52: Cooling the leather with a blower, the cooling temperature is controlled at 22° C., and the cooling time is 30 minutes;
[0102] S53: After cooling, the leather is transferred to an aging room, where the temperature is controlled at 28°C and the relative humidity is maintained at 45%;
[0103] S54: The leather is left to stand in the aging room for 24 hours to gradually stabilize the internal structure of the leather;
[0104] S55: During the aging process, check and record the temperature and humidity of the aging room every 4 hours to ensure the stability of the environmental conditions.
[0105] S6 specifically includes:
[0106] S61: Place the leather after S5 aging on the coating table to ensure that the leather is flat;
[0107] S62: preparing a nano-scale filler solution, wherein the nano-filler is selected to be a silane-based compound, and the concentration of the solution is controlled at 7.5%;
[0108] S63: Use a spraying device to evenly spray the nano-scale filler on the leather surface, and the spraying thickness is controlled at 0.15 mm;
[0109] S64: Place the sprayed leather in a constant temperature room at 35°C and leave it for 2 hours to ensure that the filler fully penetrates and cures;
[0110] S65: After the filling process is completed, the leather is dried for a second time by using a blower at a temperature of 25°C to 30°C for 1 hour.
[0111] S7 specifically includes:
[0112] S71: Place the leather treated with S6 filling on the coating machine to ensure that the leather is flat and wrinkle-free;
[0113] S72: preparing a high molecular polymer coating solution, the solution containing 4% of an anti-ultraviolet and anti-oxidant compound;
[0114] S73: Use a coating machine to evenly coat the high molecular polymer coating solution on the leather surface, and the coating thickness is controlled to be 0.4 mm;
[0115] S74: Place the coated leather in a drying room at a temperature of 55°C for 1.5 hours to ensure that the coating is fully cured;
[0116] S75: After drying, cool the leather and leave it at room temperature for 30 minutes to allow the coating to stabilize.
[0117] Example 2
[0118] S1: First, sheepskin is selected as the raw material, and the surface sand and impurities are manually scraped off; then, a 5% weak alkaline solution is used for chemical cleaning, and the soaking time is set to 10 minutes to completely remove the residual impurities on the surface; then, the leather is dried at a temperature controlled at 30°C for 1 hour; finally, a spray humidification treatment is performed, and the moisture content of the leather is adjusted to 12% using pure water to ensure that the leather absorbs moisture evenly;
[0119] S2: After the leather is initially treated, it is immersed in a natural vegetable oil solution made by mixing 15% vegetable oil with water. The entire immersion process is carried out under constant temperature conditions, the temperature is maintained at 20°C, and the duration is 36 hours. To ensure uniform distribution of oil, the solution is stirred every 6 hours;
[0120] S3: The soaked leather is placed in an ultrasonic treatment device with a sound wave frequency of 40kHz and an amplitude of 10 microns. The leather is treated continuously for 20 minutes under such conditions, during which the position of the leather is adjusted every 5 minutes to ensure that the sound waves can evenly act on every part of the leather.
[0121] S4: The treated leather is subjected to heat pressing. The heat pressing equipment is preheated to 70°C and the pressure is set to 5MPa. The leather is treated at this temperature and pressure for 10 minutes to ensure that the gaps between the leather fibers are effectively sealed;
[0122] S5: After hot pressing, the leather needs to be cooled quickly to fix its shape. Cold air at a temperature of 20°C is used for rapid cooling for 30 minutes. After that, the leather is transferred to the aging room. The temperature in the aging room is controlled at 25°C and the relative humidity is maintained at 40%. The leather is aged under such conditions for 24 hours. During this period, the environmental conditions are checked and adjusted every 4 hours to ensure the stability of the aging process.
[0123] S6: The aged leather is filled with a nano-scale filler solution containing 5% silane compounds. The filler is sprayed evenly on the leather surface with a thickness of 0.1 mm and placed in a constant temperature room at 30°C for 2 hours to ensure that the filler is fully penetrated and cured. After the filling treatment is completed, the leather is dried for a second time by using a blower at a temperature of 25°C for 1 hour;
[0124] S7: After filling treatment, the surface of the leather is subjected to final coating treatment. The prepared coating solution contains 3% of anti-UV and antioxidant compounds. The coating is evenly applied on the leather surface using a coating machine. The coating thickness is controlled at 0.3 mm. After coating, the leather is dried in a drying room at a temperature of 50°C for 1 hour to ensure that the coating is fully cured. After drying, the leather is subjected to final cooling treatment and is placed at room temperature for 30 minutes to ensure that the coating is completely stable.
[0125] Example 3
[0126] S1: First, pigskin is selected as the raw material, and the surface sand and impurities are manually scraped off; then, a 10% weak alkaline solution is used for chemical cleaning, and the soaking time is set to 20 minutes to completely remove the residual impurities on the surface; then, the leather is dried at a temperature controlled at 40°C for 2 hours; finally, a spray humidification treatment is performed, and the moisture content of the leather is adjusted to 15% using pure water to ensure that the leather absorbs moisture evenly;
[0127] S2: After the leather is initially treated, it is immersed in a natural vegetable oil solution made by mixing 20% vegetable oil with water. The entire immersion process is carried out under constant temperature conditions, the temperature is maintained at 25°C, and the duration is 36 hours. To ensure uniform distribution of oil, the solution is stirred every 6 hours;
[0128] S3: The soaked leather is placed in an ultrasonic treatment device with a sound wave frequency of 40kHz and an amplitude of 20 microns. The leather is treated continuously for 20 minutes under such conditions, during which the position of the leather is adjusted every 5 minutes to ensure that the sound waves can evenly act on every part of the leather.
[0129] S4: The treated leather is subjected to heat pressing. The heat pressing equipment is preheated to 90°C and the pressure is set to 5MPa. The leather is treated at this temperature and pressure for 10 minutes to ensure that the gaps between the leather fibers are effectively sealed;
[0130] S5: After hot pressing, the leather needs to be cooled quickly to fix its shape. Cold air at a temperature of 25°C is used for rapid cooling for 30 minutes. After that, the leather is transferred to the aging room. The temperature in the aging room is controlled at 30°C and the relative humidity is maintained at 50%. The leather is aged under such conditions for 24 hours. During this period, the environmental conditions are checked and adjusted every 4 hours to ensure the stability of the aging process.
[0131] S6: The aged leather is filled with a nano-scale filler solution containing 10% silane compounds. The filler is sprayed evenly on the leather surface with a thickness of 0.2 mm and placed in a constant temperature room at 40°C for 2 hours to ensure that the filler is fully penetrated and cured. After the filling treatment is completed, the leather is dried for a second time by using a blower at a temperature of 30°C for 1 hour;
[0132] S7: After filling treatment, the surface of the leather is subjected to final coating treatment. The prepared coating solution contains 5% of anti-UV and antioxidant compounds. The coating is evenly applied on the leather surface using a coating machine. The coating thickness is controlled at 0.5 mm. After coating, the leather is dried in a drying room at a temperature of 60°C for 2 hours to ensure that the coating is fully cured. After drying, the leather is subjected to final cooling treatment and is placed in a room temperature environment for 30 minutes to ensure that the coating is completely stable.
[0133] Table 1 Comparison of physical and mechanical properties
[0134] Compare Projects Embodiment 1 Embodiment 2 Embodiment 3 Tensile strength(MPa) 35 30 32 Elongation(%) 55 50 52 Tear resistance (N / mm) 85 80 82 Hydrostatic strength(kPa) 1500 1300 1400 Strength retention after heat aging (%) 90 85 88 Wear resistance (number of cycles) 5000 4500 4700
[0135] Table 2 Comparison of durability and environmental factors
[0136] Compare Projects Embodiment 1 Embodiment 2 Embodiment 3 Color retention rate (%) 95 90 92 Heat resistant maximum temperature (℃) 110 105 108 Chemical resistance (hours) 48 40 45 Air permeability (g / m2 / 24h) 300 270 290 Environmental adaptability index (dimensionless) 9.7 9 9.3 UV resistance (hours) 220 180 200
[0137] It can be seen from Table 1 and Table 2 above that Example 1 performs superiorly in multiple key performance indicators; in the comparison of physical and mechanical properties, Example 1 shows the highest tensile strength, elongation and tear resistance, indicating that it can maintain its structural integrity under greater forces and longer use cycles. In addition, its hydrostatic strength and strength retention rate after heat aging are higher than those of other examples, showing better water resistance and long-term stability; in the comparison of durability and environmental factors, Example 1 is superior to Examples 2 and 3 in terms of color retention, maximum heat resistance temperature and chemical resistance, providing better color stability and ability to be used in extreme environments. Its air permeability and environmental adaptability index are also the highest, indicating that it is more suitable for long-term wear and adaptable to different environmental conditions. Its UV resistance is also better than that of other examples, which is particularly important for protecting leather from fading and aging caused by direct sunlight.
[0138] In general, the treatment method of Example 1 significantly improves the overall performance and durability of leather, making it an ideal choice for manufacturing high-quality leather products, especially suitable for applications that require long-term durability and environmental adaptability.
[0139] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A processing technology for improving the cracking of leather bags, characterized in that: The following steps are involved: S1: Select raw leather, perform preliminary treatment to remove surface impurities, and adjust the moisture content to between 12% and 15%; S2: Soak the leather treated with S1 in a natural plant oil solution to fully soak it to improve its flexibility and waterproof properties; S3: Performing sonication treatment on the soaked leather, using sonic vibrations of a predetermined frequency to make the leather fibers more uniform; S4: Perform heat pressing treatment to seal the gaps between leather fibers by controlling temperature and pressure; S5: Cooling and aging the leather after heat pressing to stabilize its structure; S6: Filling the aged leather with nano-scale fillers to increase the density and compression resistance of the leather; S7: The filled leather is subjected to a final surface coating treatment to form a protective layer.
2. The process for improving the cracking of leather bags according to claim 1, characterized in that: The raw leather in S1 includes cowhide, sheepskin or pigskin.
3. The process for improving the cracking of leather bags according to claim 1, characterized in that: The preliminary processing in S1 specifically includes: S11: Mechanically clean the raw leather to remove surface sand and impurities by scraping and brushing; S12: chemically clean the leather after mechanical cleaning, using a weak alkaline solution with a mass ratio of 5%-10% for soaking for 10-20 minutes to completely remove residual impurities on the surface; S13: Drying the cleaned leather by using a blower at a temperature of 30° C. to 40° C. for 1 to 2 hours; S14: Perform spray humidification treatment on the dried leather, use pure water spray to adjust the moisture content of the leather to 12%-15% to ensure uniform absorption.
4. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S2 specifically includes: S21: preparing a natural vegetable oil solution, mixing the vegetable oil with water at a mass ratio of 15% to 20%, and stirring to form a stable emulsion; S22: completely immersing the leather treated in S1 in the natural vegetable oil solution, and ensuring that the solution fully covers the surface of the leather; S23: controlling the soaking temperature to 20° C. to 25° C. and maintaining the constant temperature for 36 hours; S24: Stir the solution every 6 hours during the soaking process; S25: After soaking, remove the leather from the solution and shake dry to remove excess vegetable oil solution from the surface.
5. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S3 specifically includes: S31: placing the leather soaked in S2 in a sonication treatment device, and spreading the leather flat to avoid overlapping; S32: setting the frequency of the sonication device to 40 kHz and the amplitude to be controlled within the range of 10-20 microns; S33: Start the sonication treatment equipment to continuously treat the leather for 20 minutes; S34: During the treatment process, the position of the leather is adjusted every 5 minutes to ensure that the sound waves act evenly on all parts of the leather; S35: After the sonication is complete, remove the leather from the equipment and let it sit for 5 minutes to relieve internal stress.
6. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S4 specifically includes: S41: Place the leather treated with S3 sonic waves in a hot press and ensure that the leather is flat and wrinkle-free; S42: setting the target temperature of the hot pressing device to 70° C. to 90° C., and preheating the device to the target temperature; S43: setting the hot pressing pressure to 5 MPa, placing the leather between the hot pressing plates, and gradually applying pressure; S44: heat-pressing the leather under the conditions of maintaining temperature and pressure for 10 minutes; S45: During the process, check the temperature and pressure of the hot press plate every 5 minutes to ensure that they are stable; S46: After the heat pressing treatment is completed, the pressure is gradually reduced to zero, and the leather is taken out of the heat pressing equipment and laid flat to cool.
7. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S5 specifically includes: S51: taking the leather treated by heat pressing in S4 out of the heat pressing device and quickly placing it flat on a cooling rack; S52: Cooling the leather with a blower, the cooling temperature is controlled at 20° C. to 25° C., and the cooling time is 30 minutes; S53: After cooling, the leather is transferred to an aging room, the temperature of which is controlled at 25°C to 30°C, and the relative humidity is maintained at 40%-50%; S54: The leather is left to stand in the aging room for 24 hours to gradually stabilize the internal structure of the leather; S55: During the aging process, check and record the temperature and humidity of the aging room every 4 hours to ensure the stability of the environmental conditions.
8. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S6 specifically includes: S61: Place the leather after S5 aging on the coating table to ensure that the leather is flat; S62: preparing a nano-scale filler solution, wherein the nano-filler is selected to be a silane-based compound, and the concentration of the solution is controlled at 5%-10%; S63: Use a spraying device to evenly spray the nano-scale filler on the leather surface, and the spraying thickness is controlled at 0.1-0.2 mm; S64: Place the sprayed leather in a constant temperature room at 30°C to 40°C for 2 hours to ensure full penetration and curing of the filler; S65: After the filling process is completed, the leather is dried for a second time by using a blower at a temperature of 25°C to 30°C for 1 hour.
9. The process for improving the cracking of leather bags according to claim 1, characterized in that: The S7 specifically includes: S71: Place the leather treated with S6 filling on the coating machine to ensure that the leather is flat and wrinkle-free; S72: preparing a high molecular polymer coating solution, wherein the solution contains 3% to 5% of an anti-ultraviolet and anti-oxidant compound; S73: Use a coating machine to evenly coat the high molecular polymer coating solution on the leather surface, and the coating thickness is controlled at 0.3-0.5 mm; S74: Place the coated leather in a drying room at a temperature of 50°C to 60°C for 1-2 hours to ensure that the coating is fully cured; S75: After drying, cool the leather and leave it at room temperature for 30 minutes to allow the coating to stabilize.
Citation Information
Patent Citations
Processing method of seawater-proof vamp leather
CN102168153A
Antique treatment method for surface of leather
CN104480238A
Processing technique of color-fastness waterproof buffed leather surface
CN105755182A
Leather production process
CN107164583A
Leather attaching crack treating agent and preparation method thereof
CN110257571A