Bridge cable high-temperature heating preparation method

By using stepping heating furnace to adjust the high-temperature heating process in bridge cable production, the heating temperature and time are improved, and the problem of excessive residence time in the high-temperature section in the existing technology is solved, capacity improvement and cost reduction are achieved, and customers are met need.

CN118879998APending Publication Date: 2024-11-01QINGDAO SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750358.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing bridge cable production process has stayed in the high-temperature section for too long, resulting in insufficient production, which is difficult to meet the sales orders for large-scale products, and has a high production cost.

Method used

The stepping heating furnace is used for high-temperature heating, adjust the temperature and time of heating section one section, heating section two sections and heating sections, increase the temperature of heating section one section to 1150-1200℃, and the temperature of heating section two sections and heating sections to 1180-1230℃. And move forward in the high temperature section to reduce the total furnace time.

Benefits of technology

The production of high-temperature sections without parking and waiting for temperature is achieved, reducing the furnace time of billet decarbonization sensitive sections, improving production capacity, meeting customer needs, and reducing fixed costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879998A_ABST
    Figure CN118879998A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature heating preparation method for a bridge cable, which is characterized in that the method for heating a continuous casting billet in a stepping heating furnace comprises the following steps of: controlling the temperature of a first heating section to be 1150-1200 DEG C, controlling the temperature of a second heating section and the temperature of a soaking section to be 1180-1230 DEG C, and controlling the time of the first heating section, the second heating section and the soaking section in the furnace to be 80-85 minutes. Compared with an original process, the high-temperature section does not need to be stopped for temperature holding, meanwhile, the in-furnace time of a decarburization sensitive section, larger than or equal to 1000 DEG C, of a steel billet is shortened, decarburization layer control is facilitated, high-temperature section forward movement is adopted in the walking beam furnace, the high-temperature diffusion time is not shortened, the total in-furnace time is shortened, the method is applied to a steel product QS87Mn for the bridge cable with the section being 180 mm * 240 mm for the first time, batch production is successful, and the production cost is reduced. The use requirements of customers are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a high-temperature heating preparation method for bridge cables. Background Art

[0002] The current production status of QS87Mn steel products for bridge cables is: to ensure that the residence time in the high temperature section (heating section 2 and soaking section) is controlled at 80 minutes, and after 42 steel pieces are produced per hour, the steel is stopped for 30 minutes to wait for the temperature. According to the output of 1,000 tons, the waiting time for the temperature is 327 minutes, which seriously affects the output and makes it difficult to meet the sales orders of large-size products. Therefore, it is urgent to increase production capacity to meet the needs of product structure adjustment and to allow the production line to digest more billets as much as possible to reduce the company's overall expenses. For this reason, the focus of research and development is to increase production capacity and reduce production costs. Summary of the invention

[0003] The present invention aims to provide a high-temperature heating preparation method for bridge cables in order to address the problem that traditional production processes cannot meet production capacity requirements.

[0004] In order to achieve the above-mentioned object, the present invention adopts the following technical solution: a high-temperature heating preparation method for bridge cables, the method comprising the following steps in sequence:

[0005] The method is a method for heating the continuous casting billet in a walking beam heating furnace: the temperature of the first heating stage is controlled at 1150-1200°C, the temperature of the second heating stage and the temperature of the soaking stage are both controlled at 1180-1230°C, and the time of the first heating stage, the second heating stage and the soaking stage in the furnace is controlled at 80-85 minutes.

[0006] Preferably, the method further comprises the steps of high-pressure water dephosphorization and rolling. After the continuous casting billet is heated in a walking beam heating furnace, high-pressure water dephosphorization is performed and then rolling is performed. The starting rolling temperature is 1080-1100°C.

[0007] Preferably, the rolling process is 1#-7# rough rolling→1# flying shear→8#-13# medium rolling→2# flying shear→14#-21# pre-finishing rolling→1# water tank cooling→3# flying shear→22#-29# finishing rolling→2# water tank cooling→4# flying shear→30#-33# sizing reduction→3# water tank cooling→spinning.

[0008] Preferably, the temperature of the finishing mill in the pre-finishing rolling step is 900±10°C.

[0009] Preferably, the temperature of the sizing mill in the sizing step is 900±10°C.

[0010] Preferably, the spinning temperature in the spinning step is 920±10°C.

[0011] Compared with the prior art, the advantages and positive effects of the present invention are:

[0012] The present invention adopts an innovative high-temperature heating process: the temperature of the first heating stage is increased from 1030-1060°C to 1150-1200°C, the temperature of the second heating stage and the soaking stage are increased from 1130-1160°C to 1180-1230°C, and the high-temperature stage (heating stage one + second heating stage + soaking stage) time is 80-85min. Compared with the original process, the high-temperature stage does not need to be stopped for temperature waiting, and at the same time, the furnace time of the decarburization sensitive section of the steel billet ≥1000°C is reduced, which is beneficial to the control of the decarburization layer. The present invention adopts the method of moving the high-temperature section forward in the walking-beam heating furnace, does not reduce the high-temperature diffusion time, and reduces the total furnace time. It is firstly applied to the 180mm×240mm section bridge cable steel product QS87Mn, and is successfully mass-produced to meet the customer's requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a box plot comparing the net carbon produced by Example 1 with the original process;

[0014] Figure 2 It is a box plot comparing the segregation of Example 1 and the original process;

[0015] Figure 3 It is a box plot comparing the decarburized layer produced by Example 1 with the original process. DETAILED DESCRIPTION

[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] Example 1

[0018] Reference Figure 1, this embodiment provides a high-temperature heating preparation method for producing ∮14mm bridge cable steel product QS87Mn, the steps of which are: 180mm*240mm continuous casting billet → walking beam heating furnace → high-pressure water descaling → 1#-7# rough rolling → 1# flying shear → 8#-13# medium rolling → 2# flying shear → 14#-21# pre-finishing rolling → 1# water tank cooling → 3# flying shear → 22#-29# finishing rolling → 2# water tank cooling → 4# flying shear → 30#-33# sizing reduction → 3# water tank cooling → spinning → air-cooled roller cooling → collection → bundling → weighing → listing → storage. The heating process of the walking-beam heating furnace was adjusted to a preheating temperature of 663.7°C and a furnace time of 37 minutes. The temperature of the first heating stage was controlled at 1172-1194°C and a furnace time of 25 minutes. The temperature of the second heating stage was controlled at 1197-1217°C and a furnace time of 33 minutes. The temperature of the soaking section was controlled at 1198-1219°C and a furnace time of 26 minutes. The total furnace time of the first, second and soaking sections was 84 minutes. The starting rolling temperature is 1080-1100°C, the temperature of the pre-finishing rolling step entering the finishing mill is 896-908°C, the temperature of the sizing reduction step entering the sizing reduction mill is 892-906°C, the spinning temperature of the wire-spinning step is 916-924°C, the rolling speed is 32m / s, the opening degrees of 1-14# fans are all 100%, the opening degree of 15# fan is 80%, the opening degree of 16# fan is 60%, and the opening degrees of other fans are all 0.

[0019] Comparative Example

[0020] Preparation method of comparative example ( Figure 1-3 Normal production shown in Example 1 Figure 1-3 The difference between the test production shown in the figure is that the heating process of the step-beam heating furnace is different. The temperature of the first heating stage is 1030-1060°C, the temperature of the second heating stage and the soaking stage are both 1130-1160°C, and the high temperature stage (second heating stage + soaking stage) time is 80-85min.

[0021] By attaching Figure 1-3 It can be seen that from the test sample results produced by the method of Example 1, the decarburization layer, segregation, and carbon mesh detected in the test samples meet the requirements of the internal control standards, and are consistent with the various indicators of the products produced by the original rolling process. After testing and mass promotion production inspection, the expected results of the test were achieved, among which decarburization was better than the original heating process. Compared with the original process, the high-temperature section of Example 1 does not need to be stopped for temperature, and the machine-hour output of the high-temperature steel grade QS87Mn bridge cable product is increased from 74.4t / h to 115t / h, the machine-hour output is increased by 54.56%, and the fixed cost per ton of steel is reduced by 49 yuan / ton. Not only does it reduce the fixed cost per ton of steel, but it also generates benefits by increasing production.

[0022] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes and apply it to other fields. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high temperature heating preparation method for bridge cables, characterized in that: The method is a method for heating the continuous casting billet in a walking beam heating furnace: the temperature of the first heating stage is controlled at 1150-1200°C, the temperature of the second heating stage and the temperature of the soaking stage are both controlled at 1180-1230°C, and the time of the first heating stage, the second heating stage and the soaking stage in the furnace is controlled at 80-85 minutes.

2. The high temperature heating preparation method for bridge cables according to claim 1, characterized in that: The method also includes the steps of high-pressure water dephosphorization and rolling. After the continuous casting billet is heated in a walking beam heating furnace, high-pressure water dephosphorization is performed and then rolling is performed. The starting rolling temperature is 1080-1100°C.

3. The high temperature heating preparation method for bridge cables according to claim 2, characterized in that: The rolling process is 1#-7# rough rolling→1# flying shear→8#-13# medium rolling→2# flying shear→14#-21# pre-finishing rolling→1# water tank cooling→3# flying shear→22#-29# finishing rolling→2# water tank cooling→4# flying shear→30#-33# sizing reduction→3# water tank cooling→spinning.

4. The high temperature heating preparation method for bridge cables according to claim 3 is characterized in that: The temperature of the finishing mill in the pre-finishing rolling step is 900±10°C.

5. The high temperature heating preparation method for bridge cables according to claim 3, characterized in that: The temperature of the sizing mill in the sizing reduction step is 900±10°C.

6. The high temperature heating preparation method for bridge cables according to claim 3, characterized in that: The spinning temperature in the spinning step is 920±10°C.