Copper alloy with excellent oxidation resistance and preparation method thereof

By adding cobalt, silicon, phosphorus and calcium elements to the copper alloy, the calcium-phosphorus phase is formed, and the problem of oxidation of copper alloy at high temperatures is solved through a specific preparation process, and high conductivity, high strength and excellent resistance are achieved The combination of oxidation properties is suitable for applications such as electronic connectors in high temperature environments.

CN118880108APending Publication Date: 2024-11-01NINGBO POWERWAY ALLOY MATERIAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965933.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing copper alloys are difficult to have good oxidation resistance while having high conductivity and high strength, resulting in easy oxidation in high temperature environments, affecting the reliability and service life of the connector.

Method used

By adjusting the composition of the copper alloy, adding appropriate amounts of cobalt, silicon, phosphorus and calcium elements, the Ca3P2 and CaP phases are formed as the main functional phases, and cobalt is controlled through specific preparation process flows, such as hot rolling, solid solution quenching and aging treatment. The distribution of silicon, cobalt and phosphorus phases and the presence of free states of calcium and phosphorus form a protective film to improve antioxidant properties.

Benefits of technology

It realizes the oxidation resistance of copper alloys while maintaining high conductivity and high strength, and the mass loss rate per unit area is reduced to ≤0.01 mg/mm2 at 600℃, extending the service life of the material, and is suitable for electronic connectors. and connectors and other high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004951778970000061
    Figure BDA0004951778970000061
  • Figure BDA0004951778970000071
    Figure BDA0004951778970000071
  • Figure BDA0004951778970000081
    Figure BDA0004951778970000081
Patent Text Reader

Abstract

The invention discloses a copper alloy with excellent oxidation resistance and a preparation method thereof, the copper alloy comprises the following components in percentage by mass: 0.5-3.0 wt% of Co, 0.1-1.0 wt% of Si, 0.01-0.3 wt% of P, 0.001-0.1 wt% of Ca and the balance of copper and inevitable impurities, the mass ratio of Co to (Si + P) is more than or equal to 3 and less than or equal to 5, the mass ratio of Si to P is more than or equal to 2 and less than or equal to 10, and the mass ratio of P to Ca is more than or equal to 5 and less than or equal to 20. The microstructure of the copper alloy contains a calcium-phosphorus phase with Ca3P2 and CaP phases as main bodies, the Ca3P2 and CaP phases serve as main functional phases, a cobalt-silicon phase and a cobalt-phosphorus phase serve as main strengthening phases, the copper alloy has excellent oxidation resistance while keeping high strength and high conductivity, the requirements of the market for high-strength, high-conductivity and excellent-oxidation-resistance materials are met, and the application prospect is wide. The method can be applied to products such as electronic connectors, connectors, lead frames and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of copper alloys and applications thereof, and particularly relates to a copper alloy with excellent anti-oxidation performance and a preparation method thereof. Background Art

[0002] With the popularity of electric vehicles, fast charging technology has developed rapidly in recent years. The performance requirements of copper alloys used in electronic materials in the automotive, connector and other industries are getting higher and higher, especially the conductivity, strength and high temperature resistance, which will directly determine whether the copper alloy material can meet the use requirements.

[0003] In the copper matrix, the solid solution amount of Co element is less than that of Ni element. Therefore, under the condition of ensuring the same strength, Cu-Co-Si alloy is easier to achieve the advantage of high conductivity than Cu-Ni-Si alloy, and is more suitable for scenes with large working current such as car charging piles. However, the current maximum working current of the connector for electric vehicle charging piles has reached 300A. When the working current is large, the copper alloy used as a connector will produce a significant thermal effect, causing the working temperature of the connector to rise abnormally. Once severe oxidation occurs, the resistance and thermal resistance of the connector will increase rapidly, eventually leading to connector failure.

[0004] Therefore, according to the current market development trend analysis, a copper alloy with good oxidation resistance while maintaining high conductivity and high strength is needed. Therefore, the present invention studies a copper-cobalt-silicon alloy containing low calcium and low phosphorus to meet the market demand. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a copper alloy with excellent antioxidant properties and a preparation method thereof. The copper alloy has good antioxidant properties while maintaining high conductivity and high strength, and the copper alloy is non-toxic and meets environmental protection requirements. The material can obtain a combination of different conductive properties and mechanical properties by adjusting the preparation process.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: a copper alloy with excellent antioxidant performance, the mass percentage composition of the copper alloy is: Co: 0.5wt%~3.0wt%, Si: 0.1wt%~1.0wt%, P: 0.01wt%~0.3wt%, Ca: 0.001wt%~0.1wt%, and the rest is composed of copper and inevitable impurities, wherein the Co / (Si+P) mass ratio is 3≤Co / (Si+P)≤5, the Si / P mass ratio is 2≤Si / P≤10, and the P / Ca mass ratio is 5≤P / Ca≤20, and the microstructure of the copper alloy contains calcium-phosphorus phases with Ca3P2 and CaP phases as the main body.

[0007] The present invention adds 0.5wt% to 3.0wt% of cobalt by mass, and after adding it simultaneously with silicon and phosphorus, cobalt-silicon and cobalt-phosphorus phases can be formed, which helps to improve the electrical conductivity and mechanical properties of the material. When the cobalt content is less than 0.5wt%, it cannot form a certain amount of second phase with silicon and phosphorus elements. Although the copper alloy has a high electrical conductivity, the mechanical properties do not meet the use requirements, which limits its application in the market. When the cobalt content is greater than 3.0wt%, due to the limited content of the added silicon and phosphorus elements, the cobalt element cannot completely form a second phase with them, and a part of it still remains in the copper matrix, affecting the electrical conductivity of the copper alloy. If too much silicon and phosphorus are added, a large amount of brittle compounds will be formed, resulting in deterioration of the bending performance of the material. Therefore, the cobalt content in the copper alloy of the present invention is 0.5wt% to 3.0wt%, preferably 0.7wt% to 2.5wt%.

[0008] In the present invention, 0.1wt% to 1.0wt% silicon is added, and the addition of silicon can form a cobalt-silicon phase to precipitate, thereby improving the strength and electrical conductivity of the material. When the silicon content is less than 0.1wt%, the amount of precipitated cobalt-silicon phase is too small, and the mechanical properties cannot meet the use requirements. When the silicon content is greater than 1wt%, too much cobalt-silicon phase is precipitated, and although the strength can be improved, the scattering effect of the second phase particles on the electron wave is enhanced, resulting in a significant decrease in the electrical conductivity of the copper alloy of the present invention. Therefore, the silicon content in the copper alloy of the present invention is 0.1wt% to 1.0wt%, preferably 0.15wt% to 0.9wt%.

[0009] In the present invention, 0.01wt% to 0.3wt% of phosphorus is added by mass, and the added phosphorus element can form a cobalt-phosphorus phase with the cobalt element to improve the electrical conductivity and mechanical properties of the copper alloy. However, when the phosphorus content is less than 0.01wt%, too little cobalt-phosphorus phase is precipitated, and the strengthening effect is not obvious, which affects the performance of the copper alloy. Because in the copper alloy of the present invention, the influence of the cobalt-silicon phase on the mechanical properties of the material exceeds that of the cobalt-phosphorus phase, the phosphorus content is controlled below 0.3wt%. If it exceeds 0.3wt%, it will lead to excessive cobalt-phosphorus phase and reduced cobalt-silicon phase, which is not conducive to the mechanical properties of the material. At the same time, part of the phosphorus element exists in the copper matrix in a free state. As a deoxidizer, the phosphorus element can effectively improve the antioxidant properties of the copper alloy. Therefore, the phosphorus content in the copper alloy of the present invention is 0.01wt% to 0.3wt%, preferably 0.05wt% to 0.25wt%.

[0010] In the present invention, calcium is added in a mass percentage of 0.001wt% to 0.1wt%, and the calcium element can form a calcium-phosphorus phase with the phosphorus element, which serves as a functional phase in the copper alloy of the present invention. The calcium-phosphorus phase can be decomposed into Ca and P single atoms at high temperature, combined with oxygen to form a continuous protective film, thereby playing a role in protecting the matrix. At the same time, part of the calcium element is in a free state in the copper matrix, which can inhibit oxygen from diffusing from the alloy surface to the inside through the grain boundary, thereby improving the oxidation resistance of the copper alloy of the present invention. When the calcium content is lower than 0.001wt%, the calcium-phosphorus phase and the free calcium element formed are too small, and the improvement of the oxidation resistance of the copper alloy is not obvious. When the calcium content is higher than 0.1wt%, a large amount of coarse brittle second phase is easily generated, resulting in loose organization, and cracking problems may occur during rolling, which has an adverse effect on the processing and performance of the copper alloy. Therefore, the calcium content in the copper alloy of the present invention is 0.001wt% to 0.1wt%, preferably 0.005wt% to 0.06wt%.

[0011] After calculation and test verification, in the copper alloy of the present invention, when the weight percentages of Co, Si, and P satisfy 3≤Co / (Si+P)≤5, 2≤Si / P≤10, the comprehensive performance of the copper alloy of the present invention can be improved to the greatest extent. If the values ​​of the above three elements are far from the above range values, one of the elements will be excessive, and the element existing in the copper matrix in the solute state will not significantly improve the strength, but will cause the conductivity of the copper alloy to decrease.

[0012] In the copper alloy of the present invention, when the weight percentage of P and Ca elements satisfies 5≤P / Ca≤20, the synergistic effect of the two elements can be maximized to improve the oxidation resistance of the copper alloy of the present invention. At the same time, the addition of P element can effectively inhibit the rolling cracking problem caused by Ca element and eliminate the copper alloy processing and manufacturing related problems caused by the addition of Ca.

[0013] The microstructure of the copper alloy of the present invention contains calcium-phosphorus phases mainly composed of Ca3P2 and CaP phases. The Ca3P2 and CaP phases are dispersed in the copper matrix as the main functional phases and can be decomposed into free Ca and P atoms at high temperatures to supplement the Ca and P elements consumed by oxygen in the copper matrix as calcium and phosphorus sources, thereby greatly improving the anti-oxidation performance of the copper alloy while strengthening the copper matrix.

[0014] Preferably, in the microstructure of the copper alloy of the present invention, more than 90% of the calcium-phosphorus phase particles have a particle size distribution between 0.1 and 5 μm, and a surface density of 1×10 3 ~1×10 5 Pieces / mm 2The particle distribution of the calcium-phosphorus phase has an important influence on the oxidation resistance of the copper alloy of the present invention. By controlling the particle size and surface density of the calcium-phosphorus phase, the oxidation resistance of the material can be effectively improved. If the particle size of the calcium-phosphorus phase is too small or the surface density is too low, the oxidation resistance will not be significantly improved; if the particle size of the calcium-phosphorus phase is too large or the surface density is too high, the conductivity and strength of the material will be affected, thereby reducing the overall performance of the material.

[0015] Preferably, in the microstructure of the copper alloy of the present invention, the cobalt-silicon phase and the cobalt-phosphorus phase are the main strengthening phases, and in the cobalt-silicon phase, the surface density of particles with a particle size distribution between 5 and 100 nm is 1×10 6 ~1×10 9 Pieces / mm 2 In the cobalt-phosphorus phase, the surface density of particles with a particle size distribution between 100 and 1000 nm is 1×10 4 ~1×10 6 Pieces / mm 2 . In the copper alloy of the present invention, the particle size and surface density of the cobalt-silicon phase and the cobalt-phosphorus phase have an important influence on the electrical conductivity and strength of the material. By controlling the particle distribution of the cobalt-silicon phase and the cobalt-phosphorus phase, the electrical conductivity and strength of the copper alloy can be improved. In the copper alloy of the present invention, it is ensured that fine and dispersed cobalt-silicon phase particles are formed first to strengthen the matrix and improve the electrical conductivity. If the number of small-sized particles is insufficient, the electrical conductivity and strength of the material will be reduced. On this basis, relatively large-sized cobalt-phosphorus phase particles are precipitated to further improve the strength and electrical conductivity of the material. If the number of large-sized particles is too large, the plastic deformation ability of the material will be affected, thereby reducing the overall performance of the material.

[0016] Preferably, in the mass percentage composition of the copper alloy of the present invention, part of the calcium element and part of the phosphorus element are present in the copper matrix in a free state, and the sum of the mass percentages of the free calcium element and the phosphorus element is not less than 0.01wt%. The free calcium element and the phosphorus element are present in the copper matrix lattice in the form of replacement atoms. Since the atomic radius of the free calcium element and the phosphorus element is much different from that of the copper atom, the lattice distortion can be caused, which plays a role in solid solution strengthening; at the same time, the affinity of the calcium atom and the phosphorus atom with the oxygen atom is relatively large, and the oxygen atom preferentially combines with the calcium and phosphorus atoms at high temperature, thereby playing a role in protecting the matrix. If the sum of the mass percentages of the free calcium element and the phosphorus element is less than 0.01wt%, the effect of improving the strength and oxidation resistance of the copper alloy is limited; on the contrary, if the content of the free calcium element and the phosphorus element is too high, the electrical conductivity of the copper alloy is greatly damaged.

[0017] Preferably, the mass loss rate per unit area of ​​the copper alloy of the present invention after being kept at 600°C for 8 hours is ≤0.01 mg / mm 2 This excellent anti-oxidation property can greatly expand the application range of copper alloys.

[0018] Preferably, the copper alloy of the present invention further comprises one or more elements of Be, Mn, Ti, Zr, Cr, In, Zn, Al, Ni, B, Mg, Fe, Ag, Sn and RE in a total amount not exceeding 2wt%. The above alloying elements are added to the copper alloy mainly to enter the copper matrix by solid solution to play a role, thereby improving the electrical conductivity, strength and high temperature resistance of the copper alloy. However, the amount of the above alloying elements added should not be too high, otherwise it will not only reduce the electrical conductivity of the copper alloy, but also have an adverse effect on the processing and manufacturing performance of the copper alloy.

[0019] The invention also discloses a method for preparing the copper alloy with excellent oxidation resistance, which comprises the following process flow: batching→melting and casting→hot rolling→surface milling→rough rolling→solution quenching→intermediate rolling→aging treatment→cleaning→finishing rolling→hood annealing.

[0020] The hot rolling starting temperature is 950°C to 1000°C, the holding time is 2h to 6h, the total processing rate of hot rolling is greater than 90%, and the hot rolling final rolling temperature is 800°C to 840°C.

[0021] After the hot rolled strip is milled, rough rolling is performed to adjust the thickness, and then solution quenching is performed. The solution temperature is 950℃~1050℃, the cooling medium is water, and the cooling rate exceeds 150℃ / s.

[0022] After solution quenching, intermediate rolling is carried out, and the total processing rate of intermediate rolling is 50% to 70%.

[0023] The aging temperature of the aging treatment after intermediate rolling is 400°C to 550°C. The aging temperature and holding time of the aging treatment are respectively denoted as Ts and Hs. Then Ts and Hs satisfy the relationship: Hs=20-(0.02-0.03)×Ts, where the unit of Ts is degrees Celsius and the unit of Hs is hours.

[0024] By adjusting the relationship between the aging temperature and the holding time, the calcium-phosphorus phase can be decomposed into calcium and phosphorus atoms and the total amount of calcium and phosphorus elements in the copper matrix in the form of free state can be controlled, thereby improving the oxidation resistance of the copper alloy. At the same time, by controlling the relationship between the aging temperature and the holding time, the particle size and surface density of the cobalt-silicon phase and cobalt-phosphorus phase particles can be avoided to affect the comprehensive performance of the material.

[0025] The total processing rate of the finishing rolling after aging treatment is 10% to 40%. Preferably, the total processing rate from intermediate rolling to finishing rolling does not exceed 80%.

[0026] The annealing temperature of the hood annealing before the finished product is 350°C to 450°C. The annealing temperature and holding time of the hood annealing are respectively recorded as Tz and Hz. Then Tz and Hz respectively satisfy the relationship: Hz=20-(0.02~0.03)×Tz, where the unit of Tz is degrees Celsius and the unit of Hz is hours.

[0027] Furthermore, the preparation method of the present invention controls the annealing temperature Tz of the hood annealing and the aging temperature Ts of the aging treatment to satisfy: Tz-Ts≤0. The use of a higher aging temperature Ts is conducive to the nucleation and precipitation of a large number of cobalt silicon phases and cobalt phosphorus phases, while regulating their proportions and sizes, and playing a role in dispersion strengthening; while the use of a lower annealing temperature Tz of the hood annealing can further promote the precipitation of the cobalt silicon phase and the cobalt phosphorus phase, while avoiding the abnormal growth of the second phase precipitated during the aging treatment, and can ensure that the sum of the mass percentages of free calcium and phosphorus in the copper matrix is ​​above 0.01wt%.

[0028] Compared with the prior art, the advantages of the present invention are:

[0029] 1. Cobalt, silicon, calcium and phosphorus are added to the copper alloy of the present invention at the same time. The microstructure of the copper alloy contains calcium-phosphorus phases with Ca3P2 and CaP phases as the main body. The Ca3P2 and CaP phases are dispersed in the copper matrix as the main functional phases and can be decomposed into free Ca and P atoms at high temperature. They can be used as calcium sources and phosphorus sources to supplement the Ca and P elements consumed by oxygen in the copper matrix, thereby greatly improving the oxidation resistance of the copper alloy while strengthening the copper matrix. At the same time, the copper alloy uses cobalt-silicon phases and cobalt-phosphorus phases as the main strengthening phases, thereby significantly improving the electrical conductivity and mechanical properties of the material while further improving the oxidation resistance of the material.

[0030] 2. The mass loss rate per unit area of ​​the copper alloy of the present invention after being kept at 600°C for 8 hours is ≤0.01mg / mm 2 The copper alloy of the present invention has relatively excellent anti-oxidation performance while maintaining high strength and high conductivity, meeting the market demand for high-strength, high-conductivity and excellent anti-oxidation performance materials, and can be applied to electronic connectors, connectors, lead frames and other products. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is clearly and completely described below through specific embodiments.

[0032] 24 examples and 4 comparative examples of alloys were selected, and the specific compositions are shown in Table 1. All of them were processed into finished strips with a thickness of 0.2 mm using the preparation method of the present invention, and the key process parameters were controlled as shown in Table 2. The preparation process of the copper alloy strip of this embodiment is: batching → melting and casting → hot rolling → milling → rough rolling → solution quenching → intermediate rolling → aging treatment → cleaning → finishing rolling → hood annealing, which specifically includes the following steps:

[0033] 1) Batching and melting and casting: Raw materials are prepared and batched according to the alloy chemical composition shown in Table 1, and smelting is carried out in an induction furnace. Casting is carried out after the composition meets the requirements and is fully degassed and deslaged. The melting temperature is 1350°C to 1450°C, and the casting temperature is 1180°C to 1200°C.

[0034] 2) Hot rolling: After keeping the temperature at 950℃~1000℃ for 2h~6h, hot rolling is carried out to open the blank, the total processing rate is greater than 90%, and the final rolling temperature is 800℃~840℃.

[0035] 3) Rough rolling: The hot rolled strip is milled and then subjected to rough rolling, with the total rough rolling processing rate being 70% to 85%.

[0036] 4) Solution quenching: The strip after rough rolling is subjected to solution quenching treatment. The solution temperature and holding time are shown in Table 2. The cooling medium is water, and the cooling rate exceeds 150°C / s.

[0037] 5) Intermediate rolling: The strip after solution quenching is subjected to intermediate rolling, and the total processing rate of intermediate rolling is 50% to 70%.

[0038] 6) Aging treatment: The strip after intermediate rolling is subjected to aging treatment. The parameters of the aging treatment are shown in Table 2, wherein the aging temperature Ts and the holding time Ts satisfy the relationship: Hs=20-(0.02-0.03)×Ts, wherein the unit of Ts is degrees Celsius and the unit of Hs is hours.

[0039] 7) Finish rolling: After cleaning the strip after aging treatment, finish rolling is performed with a processing rate of 20% to 40%.

[0040] 8) Hood annealing: The strip after finish rolling is subjected to hood annealing. The parameters of the hood annealing are shown in Table 2, wherein the hood annealing temperature Tz and the holding time Hz satisfy the relationship: Hz=20-(0.02-0.03)×Tz, wherein the unit of Tz is degrees Celsius and the unit of Hz is hours.

[0041] The electrical conductivity, yield strength, oxidation resistance and microstructure of the alloy strips of Examples 1 to 24 and Comparative Examples 1 to 4 of the present invention were evaluated according to the methods specified in the relevant national standards and industry standards, specifically:

[0042] The conductivity is tested in accordance with GB / T 32791-2016 Eddy Current Test Method for Electrical Conductivity of Copper and Copper Alloys. The sample thickness is 0.2 mm. Three samples are superimposed for measurement. The test frequency is 480 KHz. The results are expressed in % IACS.

[0043] The yield strength is tested on an electronic universal mechanical properties testing machine in accordance with "GB / T 228.1-2021 Metal Materials Tensile Test Part 1: Room Temperature Test Method" at a tensile speed of 5 mm / min.

[0044] The anti-oxidation performance is expressed by the mass loss rate per unit area. The original mass of the sample is weighed before the test. After the test, the sample is cleaned and weighed after removing the surface oxide film. The lost mass is divided by the surface area of ​​the sample to obtain the mass loss rate per unit area. During the test, the sample is placed in a muffle furnace with a heating rate of >300℃ / hour, a heating temperature of 600℃, a holding time of 8h, and an atmospheric environment.

[0045] The microstructure of the sample was observed perpendicular to the cross section of the sample using a field emission scanning electron microscope (TESCAN S9000GMH), and more than ten SEM photos were taken. The elemental composition and atomic ratio of the second phase were determined by energy spectrum technology to distinguish the calcium-phosphorus phase from the cobalt-phosphorus phase. Since the cobalt-silicon phase is small and distributed at the nanometer level, a transmission electron microscope (FEI Talos F200X) was used to observe perpendicular to the plane of the plate and strip, and more than ten STEM photos were taken. The phase composition was determined by energy spectrum surface distribution technology. Finally, the image processing software ImageJ was used to count the particle size and number of each second phase. The surface density was calculated based on the number of precipitated phases in the photo divided by the area represented by the photo. The final particle size and surface density of the second phase were the average of the statistical results of ten photos.

[0046] The EDS spectrometer (model: ULTIM MAX 40, quantitative analysis software: AZtec Symmetry 3000) was used to measure the sum of the mass percentages of calcium and phosphorus in the copper matrix. The energy spectrum point measurement mode was selected. During the measurement, care should be taken to avoid the calcium-phosphorus phase and the cobalt-phosphorus phase (the second phase is in obvious granular form). The clean grain area in the copper matrix was selected for component analysis. More than 10 points were measured in each field of view, and a total of 10 fields of view were counted. The sum of the mass percentages of calcium and phosphorus was finally taken as the average of all the point measurement results in the ten fields of view.

[0047] The performance and microstructure test results of each embodiment and comparative example are shown in Table 3. From the performance of the embodiment, it can be seen that the copper alloy of the present invention has excellent oxidation resistance while maintaining high strength and high conductivity, and the unit area mass loss rate after being kept at 600°C for 8 hours is ≤0.01mg / mm 2 , which can better meet the requirements of copper alloy performance in more fields.

[0048] Table 1 Chemical compositions of the embodiments of the present invention and comparative examples

[0049]

[0050]

[0051] Table 2 Key process parameter control and performance test results of the embodiments of the present invention and the comparative examples

[0052]

[0053] Table 3 Test results of the embodiments of the present invention and the comparative examples

[0054]

Claims

1. A copper alloy having excellent oxidation resistance, characterized in that: The copper alloy has a mass percentage composition of: Co: 0.5wt% to 3.0wt%, Si: 0.1wt% to 1.0wt%, P: 0.01wt% to 0.3wt%, Ca: 0.001wt% to 0.1wt%, and the rest is composed of copper and inevitable impurities, wherein the Co / (Si+P) mass ratio is 3≤Co / (Si+P)≤5, the Si / P mass ratio is 2≤Si / P≤10, and the P / Ca mass ratio is 5≤P / Ca≤20. The microstructure of the copper alloy contains calcium-phosphorus phases with Ca3P2 and CaP phases as the main body.

2. The copper alloy having excellent oxidation resistance according to claim 1, characterized in that: More than 90% of the calcium-phosphorus phase has a particle size distribution between 0.1 and 5 μm, and a surface density of 1×10 3 ~1×10 5 Pieces / mm 2 .

3. The copper alloy having excellent oxidation resistance according to claim 1, characterized in that: In the microstructure of the copper alloy, cobalt-silicon phase and cobalt-phosphorus phase are the main strengthening phases. In the cobalt-silicon phase, the surface density of particles with a particle size distribution between 5 and 100 nm is 1×10 6 ~1×10 9 Pieces / mm 2 In the cobalt-phosphorus phase, the surface density of particles with a particle size distribution between 100 and 1000 nm is 1×10 4 ~1×10 6 Pieces / mm 2 .

4. The copper alloy having excellent oxidation resistance according to claim 1, characterized in that: In the mass percentage composition of the copper alloy, part of the calcium element and part of the phosphorus element exist in the copper matrix in a free state, and the sum of the mass percentages of the free calcium element and the phosphorus element is not less than 0.01wt%.

5. The copper alloy having excellent oxidation resistance according to claim 1, characterized in that: The copper alloy comprises the following mass percentages: Co: 0.7wt% to 2.5wt%, Si: 0.15wt% to 0.9wt%, P: 0.05wt% to 0.25wt%, Ca: 0.005wt% to 0.06wt%, and the rest is copper and inevitable impurities.

6. The copper alloy having excellent oxidation resistance according to claim 1, characterized in that: The mass loss rate per unit area of ​​the copper alloy after being kept at 600℃ for 8h is ≤0.01mg / mm 2 .

7. The copper alloy having excellent oxidation resistance according to any one of claims 1 to 6, characterized in that: The copper alloy also includes one or more elements selected from the group consisting of Be, Mn, Ti, Zr, Cr, In, Zn, Al, Ni, B, Mg, Fe, Ag, Sn and RE in a total amount not exceeding 2wt%.

8. The method for preparing a copper alloy having excellent oxidation resistance according to any one of claims 1 to 7, characterized in that: The process includes the following steps: batching→melting→hot rolling→milling→rough rolling→solution quenching→intermediate rolling→aging treatment→cleaning→finishing rolling→hood annealing; the aging temperature of the aging treatment is 400°C to 550°C, the annealing temperature of the hood annealing is 350°C to 450°C, the aging temperature and the holding time of the aging treatment are respectively recorded as Ts and Hs, and the annealing temperature and the holding time of the hood annealing are respectively recorded as Tz and Hz, wherein the units of Ts and Tz are both degrees Celsius, and the units of Hs and Hz are both hours, then Ts and Hs, Tz and Hz respectively satisfy the relationship: Hs=20-(0.02~0.03)×Ts Hz=20-(0.02~0.03)×Tz.

9. The method for preparing a copper alloy with excellent oxidation resistance according to claim 8, characterized in that: Tz-Ts≤0.

10. The method for preparing a copper alloy with excellent oxidation resistance according to claim 8, characterized in that: The hot rolling temperature is 950° C. to 1000° C., the heat preservation time is 2 h to 6 h, and the total processing rate of the hot rolling is greater than 90%.