6xxx series aluminum alloy material for automobile covering part as well as preparation method and application of 6xxx series aluminum alloy material

By short-term peak aging treatment of 6xxx series aluminum alloy materials, the strength and rebound problems in complex forming and recycling processes are solved, and efficient forming and homogeneous recycling of automotive cover parts materials is achieved, reducing production and Recycling costs.

CN118880133APending Publication Date: 2024-11-01CHONGQING NATIONAL INNOVATION INSTITUTE OF LIGHT ALLOYS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411368707.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The strength increase of 6xxx aluminum alloy is affected by natural aging effects before stamping, which increases processing time and cost. At the same time, it is easy to rebound and crack when complex structures such as the door inner panel are formed, which limits its application, and the door inner panel, Different materials on the outer plate are difficult to separate and process during the recycling process, which increases the cost of recycling and environmental pollution risks.

Method used

Aluminum alloy materials with natural aging or pre-aging state are used for short-term peak aging treatment. They are heated up to 200~260℃ through box furnace or electromagnetic induction heating, and are insulated for 20~40s, so as to achieve coordinated shape control, suitable for complex forming Process, reduces rebound and cracking problems and simplifies the recycling process.

Benefits of technology

Improve the forming performance of 6xxx series aluminum alloy materials, the material strength reaches yield strength >225MPa, tensile strength >280MPa, and elongation >20%, reducing production difficulty and energy consumption costs, simplifying the equipment procurement and recycling process, and improving the Product yield and recycling efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a 6xxx series aluminum alloy material for an automobile covering part and a preparation method and application thereof.The 6xxx series aluminum alloy material is obtained by conducting short-time peak aging treatment on an aluminum alloy material in a natural aging state or a pre-aging state, and the aluminum alloy material in the natural aging state or the pre-aging state comprises, by mass, 0.4%-1.85% of Si, 0.2%-1.5% of Mg, smaller than or equal to 0.4% of Cu, smaller than or equal to 0.5% of Mn, smaller than or equal to 0.3% of Zn, smaller than or equal to 0.35% of Cr, smaller than or equal to 0.5% of Fe, smaller than or equal to 0.35% of Ti, smaller than or equal to 0.05% of single other impurities and the balance Al. The total amount of other impurities is smaller than or equal to 0.15%; the short-time peak aging treatment adopts box-type furnace heating treatment or electromagnetic induction heating treatment. The plate provided by the invention has high formability and high strength, and is suitable for preparation of aluminum alloy parts such as automobile inner and outer covering parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum alloy materials, and in particular relates to a 6xxx series aluminum alloy material for automobile covering parts, a preparation method and application thereof. Background Art

[0002] Aluminum alloy materials have the characteristics of low density, high specific strength and easy processing, and are widely used in the manufacture of parts for automobile engines, transmissions, brakes and other components. In recent years, cast aluminum alloys have been widely used in the manufacture of engines, transmission housings, etc., while various series of deformed aluminum alloy materials manufactured by rolling, extrusion and forging are mainly used for automobile body panels, heat exchangers and chassis systems. Among them, 5xxx series aluminum alloys are work-hardening aluminum alloys, and the main alloy component is magnesium, which makes it have high tensile strength and elongation. It can be directly stamped and formed, and is usually used to manufacture complex door inner panels. 6xxx series aluminum alloys are aging-hardened aluminum alloys, mainly containing two alloy elements, magnesium and silicon. The strength of the material can be significantly improved by baking paint after solid solution, pre-aging and stamping treatment. Although complex structure forming cannot be achieved, it is particularly suitable for automobile outer panels, hoods and other automotive outer panels that do not have high forming requirements but need to withstand external impact.

[0003] However, 6xxx series aluminum alloys will be parked for a period of time before stamping due to unavoidable factors such as logistics. During this period, due to the natural aging effect, its strength increment after painting will be adversely affected to a certain extent. Therefore, the industry usually adopts the pre-aging method for regulation, but this method will increase the processing time of aluminum processing enterprises by about 10 hours, and increase the raw material procurement cost of the main engine factory. In addition, the inner and outer panels of the door are made of different aluminum alloy materials, which need to be separated during the recycling process after the vehicle is scrapped. However, since the two are already closely integrated in the door structure, additional equipment and process support are required. The separation process is relatively complicated and time-consuming. At the same time, since the market value of different aluminum alloys may vary, recyclers need to conduct detailed classification and evaluation when handling these materials, which will significantly increase the recycling cost. In addition, during the recycling process, if improperly handled, the dust and waste liquid generated during the crushing and sorting process will also pollute the environment. Therefore, in order to more efficiently promote the recycling process of automobile waste aluminum, the demand for homogenization of the inner and outer panels of the door is becoming increasingly urgent. However, 6xxx series aluminum alloy sheets often face industry problems such as springback and cracking during cold stamping. This problem is particularly prominent when stamping parts with complex structures such as door inner panels, which limits their application in related fields. Summary of the invention

[0004] The purpose of the present invention is to provide a 6xxx series aluminum alloy material for automobile covering parts, a preparation method and application thereof. The 6xxx series aluminum alloy material of the present invention can adapt to complex forming processes and achieve coordinated control of shape and properties while maintaining the existing grade composition, which is of great significance to promoting the homogeneous application of 6xxx series aluminum alloys in automobile covering parts materials.

[0005] The present invention provides a 6xxx series aluminum alloy material for automobile covering parts, which is obtained by subjecting a naturally aged or pre-aged aluminum alloy material to a short-time spike aging treatment:

[0006] The aluminum alloy material in the naturally aged state or pre-aged state includes the following components in mass fraction:

[0007] Si 0.4~1.85%, Mg 0.2~1.5%, Cu ≤0.4%, Mn ≤0.5%, Zn ≤0.3%, Cr≤0.35%, Fe≤0.5%, Ti ≤0.35%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al;

[0008] The short-time peak aging treatment adopts box furnace heating treatment or electromagnetic induction heating treatment.

[0009] The box-type furnace heating treatment comprises: heating the naturally aged or pre-aged aluminum alloy material to 200-260° C. at a heating rate of 5-10° C. / s;

[0010] The electromagnetic induction heating treatment comprises: heating the aluminum alloy material in a natural aging state or a pre-aging state to 200-260° C. at a heating rate of 35-70° C. / s, and keeping the temperature for 20-40s.

[0011] Preferably, the aluminum alloy material in the naturally aged state or pre-aged state comprises the following components in mass fractions:

[0012] Si 1.0~1.5%, Mg 0.25~0.6%, Cu ≤0.2%, Mn ≤0.2%, Zn ≤0.2%, Cr ≤0.1%, Fe≤0.5%, Ti ≤0.15%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al.

[0013] Preferably, the set temperature of the box furnace is 420-480° C., and the heating time is 20-60 s.

[0014] The present invention provides a method for preparing the 6xxx series aluminum alloy material for automobile covering parts as described above, comprising the following steps:

[0015] A) melting and casting the raw materials to obtain ingots;

[0016] B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment, and then natural aging or pre-aging treatment to obtain a naturally aged or pre-aged aluminum alloy material;

[0017] C) The naturally aged or pre-aged aluminum alloy material is subjected to short-time spike aging treatment to obtain a 6xxx series aluminum alloy material for automotive covering parts.

[0018] Preferably, the casting is performed by a spray deposition method;

[0019] The homogenization process comprises the following steps:

[0020] First, heat the temperature to 540-570°C at a heating rate of 20-80°C / h and keep it at that temperature for 4-25 hours;

[0021] The homogenization process also includes a cooling and heat preservation process, wherein the temperature of the cooling and heat preservation process is 500-530° C., and the cooling and heat preservation time is 1.5-18 hours.

[0022] Preferably, the hot rolling start temperature is 490-530°C, and the final rolling temperature is 240-360°C.

[0023] Preferably, the temperature of the solution treatment is 510-560° C., and the time of the solution treatment is 10-150 s.

[0024] Preferably, the pre-aging treatment comprises: heating the aluminum alloy material after the solid solution treatment to 60-100° C., then coiling and cooling naturally;

[0025] The temperature of the natural aging treatment is 0-40°C.

[0026] The present invention provides an automobile covering part, which is obtained by cold stamping and baking varnish treatment of 6xxx aluminum alloy material;

[0027] The 6xxx aluminum alloy material is the 6xxx series aluminum alloy material for automobile covering parts mentioned above.

[0028] Preferably, the automobile covering comprises an automobile door outer panel and an automobile door inner panel; the thickness of the automobile covering is 0.2-2 mm.

[0029] The present invention provides a 6xxx series aluminum alloy material for automobile covering parts, which is obtained by subjecting a naturally aged or pre-aged aluminum alloy material to a short-time spike aging treatment: the naturally aged or pre-aged aluminum alloy material comprises the following components in mass fraction: Si 0.4-1.85%, Mg 0.2-1.5%, Cu ≤0.4%, Mn ≤0.5%, Zn ≤0.3%, Cr ≤0.35%, Fe ≤0.5%, Ti ≤0.35%, other impurities individually ≤0.05%, other impurities in total ≤0.15%, and the balance is Al; the short-time spike aging treatment adopts box furnace heating treatment or electromagnetic induction heating treatment, and the box furnace heating treatment includes: heating the naturally aged or pre-aged aluminum alloy material to 200~260℃ at a heating rate of 5~10℃ / s; the electromagnetic induction heating treatment includes: heating the naturally aged or pre-aged aluminum alloy material to 200~260℃ at a heating rate of 35~70℃ / s, and keeping it warm for 20~40s.

[0030] The present invention has the following beneficial effects:

[0031] 1. The aluminum alloy material of the present invention is suitable for T4 / T4P state 6xxx series aluminum alloy sheet and its preparation process for automobile cover parts based on aging forming integrated stamping process, and the material strength can reach yield strength>225MPa, tensile strength>280MPa, elongation>20%, while significantly improving the material forming performance and ensuring that its performance is not lower than that of 6xxx aluminum alloy parts obtained by conventional cold and hot stamping processing;

[0032] 2. The T4 / T4P state 6xxx series aluminum alloy sheet for automobile cover parts based on the aging forming integrated stamping process and its preparation process described in the present invention can be implemented based on conventional cold stamping equipment and dies to produce related parts and products, and the equipment procurement cost is significantly lower than that of hot stamping related equipment and dies;

[0033] 3. The T4 / T4P state 6xxx series aluminum alloy sheet for automobile covering parts based on the aging forming integrated stamping process and its preparation process described in the present invention only need to heat the sheet to 200~260℃, compared with hot stamping which requires long-term heating at more than 450℃ to achieve solid solution to ensure high-quality forming, thereby significantly reducing production difficulty and energy consumption cost.

[0034] 4. The T4 / T4P state 6xxx series aluminum alloy sheet for automobile covering parts based on the short-time peak aging forming integrated stamping process and its preparation process described in the present invention can effectively reduce problems such as springback and cracking compared with conventional cold stamping, thereby improving the product yield when stamping parts such as door inner panels with complex structures, and the performance after painting is higher than that of cold stamping.

[0035] 5. The T4 / T4P state 6xxx series aluminum alloy sheet for automobile covering parts based on the short-time peak aging forming integrated stamping process and its preparation process described in the present invention can be realized by differential temperature heating in a conventional box-type annealing furnace, the temperature is easier to control and stabilize, and the process feasibility is better.

[0036] 6. The present invention has conducted a detailed study on the stability of natural aging / pre-aging clusters of 6xxx series aluminum alloys with different compositions and different initial states at various temperatures and the relationship between remelting and re-precipitation, proposed an aluminum alloy peak aging (medium temperature short-time heating) process window for different natural aging / pre-aging cluster precipitation conditions, and clarified the differences in the preparation process of aluminum alloy plates in different natural aging states or pre-aging states.

[0037] 7. It will help to achieve homogeneous recycling in the future. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0039] Figure 1 This is a photo of a stamped automobile door inner panel of the pre-aged 6xxx series aluminum alloy sheet of Example 1 of the present invention after being formed by peak aging (medium temperature short time heating);

[0040] Figure 2 This is a photo of an automobile door inner panel stamping part formed from the pre-aged 6xxx series aluminum alloy sheet of comparative example 2 of the present invention after peak aging (medium temperature short-time heating). DETAILED DESCRIPTION

[0041] The present invention provides a 6xxx series aluminum alloy material for automobile covering parts, which is obtained by subjecting a naturally aged or pre-aged aluminum alloy material to a short-time spike aging treatment:

[0042] The aluminum alloy material in the naturally aged state or pre-aged state includes the following components in mass fraction:

[0043] Si 0.4~1.85%, Mg 0.2~1.5%, Cu ≤0.4%, Mn ≤0.5%, Zn ≤0.3%, Cr≤0.35%, Fe≤0.5%, Ti ≤0.35%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al;

[0044] The short-time peak aging treatment adopts box furnace heating treatment or electromagnetic induction heating treatment.

[0045] The box-type furnace heating treatment comprises: heating the naturally aged or pre-aged aluminum alloy material to 200-260° C. at a heating rate of 5-10° C. / s;

[0046] The electromagnetic induction heating treatment comprises: heating the aluminum alloy material in a natural aging state or a pre-aging state to 200-260° C. at a heating rate of 35-70° C. / s, and keeping the temperature for 20-40° C.s.

[0047] In the present invention, the aluminum alloy material in the natural aging state (T4) or the pre-aging state (T4P) includes the following components in mass fractions:

[0048] Si 0.4~1.85%, Mg 0.2~1.5%, Cu ≤0.4%, Mn ≤0.5%, Zn ≤0.3%, Cr≤0.35%, Fe≤0.5%, Ti ≤0.35%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al.

[0049] In the present invention, the mass fraction of Si is preferably 0.5~1.8%, such as 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.85%, preferably a range value with any of the above values ​​as the upper or lower limit.

[0050] In the present invention, the mass fraction of Mg is preferably 0.5-1.2%, such as 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, preferably a range value with any of the above values ​​as the upper or lower limit.

[0051] In the present invention, the mass fraction of Cu is preferably ≤0.4%, more preferably ≤0.3%, such as Cu≤0.4%, Cu≤0.3%, Cu≤0.2%, Cu≤0.1%.

[0052] In the present invention, the mass fraction of Mn is preferably ≤0.5%, more preferably ≤0.4%, such as Mn≤0.5%, Mn≤0.4%, Mn≤0.3%, Mn≤0.2%, and Mn≤0.1%.

[0053] In the present invention, the mass fraction of Zn is preferably ≤0.3%, more preferably ≤0.2%, such as Zn≤0.3%, Zn≤0.2%, Zn≤0.1%.

[0054] In the present invention, the mass fraction of Cr is preferably ≤0.35%, more preferably ≤0.3%, such as Cr≤0.35%, Cr≤0.3%, Cr≤0.25%, Cr≤0.2%, Cr≤0.15%, Cr≤0.1%.

[0055] In the present invention, the mass fraction of Fe is preferably ≤0.5%, more preferably ≤0.4%, such as Fe≤0.5%, Fe≤0.4%, Fe≤0.3%, Fe≤0.2%, Fe≤0.1%.

[0056] In the present invention, the mass fraction of Ti is preferably ≤0.35%, more preferably ≤0.3%, such as Ti≤0.35%, Ti≤0.3%, Ti≤0.25%, Ti≤0.2%, Ti≤0.15%, Ti≤0.1%, and Ti≤0.05%.

[0057] Preferably, Si 1.0-1.5%, Mg 0.25-0.6%, Cu ≤0.2%, Mn ≤0.2%, Zn ≤0.2%, Cr ≤0.1%, Fe ≤0.5%, Ti ≤0.15%, other impurities individually ≤0.05, other impurities total ≤0.15%, and the balance is Al.

[0058] More preferably, Si 1.2-1.5%, Mg 0.25-0.5%, Cu≤0.1%, Mn≤0.2%, Zn≤0.05%, Cr≤0.1%, Fe≤0.3%, Ti≤0.05%, other impurities individually ≤0.05%, total ≤0.15%, and the balance is Al.

[0059] In the present invention, the short-time peak aging adopts box furnace heating treatment or electromagnetic induction heating treatment. In the present invention, the box furnace heating treatment is differential temperature heating. The heating rate of the box furnace heating is preferably 5-10°C / s, more preferably 6-9°C / s, such as 5°C / s, 6°C / s, 7°C / s, 8°C / s, 9°C / s, 10°C / s, preferably a range value with any of the above values ​​as the upper or lower limit; the box furnace heating treatment is heated to 200-260°C, preferably 220-260°C, such as 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, preferably a range value with any of the above values ​​as the upper or lower limit, the temperature refers to the aluminum alloy The temperature actually reached by the gold material, the heating of the aluminum alloy material is stopped after reaching this temperature, and the set temperature of the box furnace is set to 420-480°C, more preferably 430-470°C, such as 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, preferably a range value with any of the above values ​​as the upper or lower limit; the box furnace is set at this temperature, and the naturally aged aluminum alloy material or the pre-aged aluminum alloy material in the furnace is heated from room temperature to the heating temperature at a rate of 5-10°C / s, and the materials successively experience different temperature ranges from low to high, which can make a part of the particles effectively nucleate during the heating process and precipitate during the paint baking process without almost increasing the yield strength of the material before stamping, and finally improve the paint baking strength through the β'' strengthening precipitation phase with higher number density. The heating time is preferably 20 to 60 s, more preferably 30 to 50 s, such as 20 s, 25 s, 30 s, 35 s, 40 s, 45 s, 50 s, 55 s, 60 s, preferably a range value with any of the above values ​​as the upper or lower limit.

[0060] In the present invention, the electromagnetic induction heating is an isothermal heating device, and the heating rate of the electromagnetic induction heating is preferably 35-70°C / s, more preferably 40-50°C / s, such as 35°C / s, 40°C / s, 45°C / s, 50°C / s, 55°C / s, 60°C / s, 65°C / s, 70°C / s, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the insulation temperature of the electromagnetic induction heating is preferably 200-260°C, more preferably 220-240°C, such as 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the insulation time is preferably 20-40s, more preferably 25-35s.

[0061] Compared with other alloys (such as 7xxx alloys), the clusters formed by natural aging of the 6xxx alloy involved in the present invention not only increase the yield strength of the material before stamping and affect the forming, but also have a significant adverse effect on the strength of the subsequent baking varnish treatment. The naturally aged or pre-aged sheet in the present invention is softened and formed by short-time spike aging (short-time heating at medium temperature), and then the baking varnish treatment is performed. The yield strength of the final sheet (taking 6016 as an example) is greater than 225MPa, the tensile strength is greater than 280MPa, and the elongation is greater than 20%.

[0062] The present invention provides a method for preparing the 6xxx series aluminum alloy material for automobile covering parts as described above, comprising the following steps:

[0063] A) melting and casting the raw materials to obtain ingots;

[0064] B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment, and then natural aging or pre-aging treatment to obtain a naturally aged or pre-aged aluminum alloy material;

[0065] C) The naturally aged or pre-aged aluminum alloy material is subjected to short-time spike aging treatment to obtain a 6xxx series aluminum alloy material for automotive covering parts.

[0066] In the present invention, the raw materials used for smelting can be selected from corresponding pure metal or alloy raw materials according to the composition and content of the 6xxx series aluminum alloy material for automobile covering parts described above, and the present invention will not be elaborated herein.

[0067] In the present invention, the smelting temperature is preferably 740-760°C, more preferably 750-755°C, the ingot is preferably manufactured by industrial semi-continuous ingot casting, preferably prepared by spray deposition; the casting temperature is preferably 720-740°C, more preferably 730-735°C.

[0068] In the present invention, the temperature of the homogenization treatment is 540-570°C, more preferably 550-560°C, such as 540°C, 545°C, 550°C, 555°C, 560°C, 565°C, 570°C, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit; the holding time of the homogenization treatment is preferably 4-25 hours, more preferably 8-20 hours; the heating rate of the homogenization treatment is preferably 20-80°C / h, more preferably 30-70°C / h, such as 20°C / h, 30°C / h, 40°C / h, 50°C / h, 60°C / h, 70°C / h, 80°C / h, preferably a range value with the above arbitrary numerical values ​​as the upper or lower limit.

[0069] After the homogenization treatment, the present invention performs a cooling and heat preservation treatment on the homogenized blank, and the heat preservation temperature is preferably 500-530°C, more preferably 510-520°C, and the heat preservation time is preferably 1.5-18h, more preferably 3-15h, such as 1.5h, 3h, 5h, 10h, 15h, 18h, preferably a range value with any of the above values ​​as the upper or lower limit.

[0070] The present invention sequentially hot-rolls, cold-rolls and curls the material after cooling and heat preservation to obtain a cold-rolled plate with a thickness of 0.2-0.2 mm.

[0071] In the present invention, the hot rolling start temperature is preferably 490-530°C, more preferably 500-520°C, such as 490°C, 495°C, 500°C, 505°C, 510°C, 515°C, 520°C, 525°C, 530°C, preferably a range value with any of the above values ​​as the upper or lower limit; the hot rolling finish temperature is preferably 240-360°C, more preferably 280-320°C, such as 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, preferably a range value with any of the above values ​​as the upper or lower limit. After hot rolling, a hot-rolled material with a thickness of 4-8 mm is obtained.

[0072] In the present invention, the cold rolling temperature is preferably room temperature, such as 0-40°C, more preferably 20-30°C.

[0073] After obtaining the cold-rolled sheet, the present invention performs solid solution treatment and water cooling on the cold-rolled sheet to obtain a solution-treated sheet.

[0074] In the present invention, the temperature of the solution treatment is preferably 510~560℃, more preferably 520~550℃, such as 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, preferably a range value with the above arbitrary numerical value as the upper or lower limit, and the time of the solution treatment is preferably 10~150s, more preferably 30~120s, such as 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, preferably a range value with the above arbitrary numerical value as the upper or lower limit.

[0075] After water cooling, the present invention preferably performs natural aging or pre-aging treatment on the plate. In the present invention, the pre-aging treatment includes the following steps:

[0076] The plate after water cooling is heated to the pre-aging temperature and then the heating is stopped. The coil is coiled and slowly cooled naturally at room temperature to achieve pre-aging treatment. The pre-aging treatment temperature is preferably 60-100°C, more preferably 70-90°C, such as 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, preferably a range value with any of the above values ​​as the upper or lower limit.

[0077] In the present invention, the natural aging treatment is to leave the aluminum alloy material in a naturally aged state at room temperature (between 0°C and 40°C) for any period of time. The present invention has no special restrictions on the time of the natural aging treatment.

[0078] The present invention subjects the aluminum alloy material in the natural aging state or the pre-aging state to short-time spike aging treatment to obtain a 6xxx series aluminum alloy material for automobile covering parts.

[0079] In the present invention, the short-time spike aging treatment is consistent with the short-time spike aging treatment described above, and the present invention will not be repeated here.

[0080] The present invention also provides an automobile covering part, which is obtained by cold stamping and baking varnish treatment of the 6xxx aluminum alloy material mentioned above.

[0081] In the present invention, the cold stamping is a commonly used forming method in the art, which can be implemented using conventional cold stamping equipment and molds, and the present invention will not be repeated here. In the present invention, the cold stamping refers to stamping at a conventional room temperature, such as 0-40°C.

[0082] In the present invention, the temperature of the baking varnish treatment is preferably 170-190° C., more preferably 175-185° C., and the time of the baking varnish treatment is preferably 20-60 min, more preferably 20-40 min.

[0083] In the present invention, the automobile covering parts include automobile door outer panels and automobile door inner panels, that is, the 6xxx series aluminum alloy material in the present invention can not only be used to prepare automobile door outer panels, but also can be used to prepare automobile door inner panels with more complex punching structures, laying the foundation for the homogeneous application of automobile covering materials.

[0084] The present invention uses short-time spike aging to fully dissolve the clusters precipitated during natural aging or pre-aging, then stamps the material, and further performs baking varnish treatment. The final sheet (6016) has a yield strength of >225MPa, a tensile strength of >280MPa, and an elongation of >20%, which are higher than the corresponding performance of conventional cold stamping and baking varnish sheets. The sheet provided by the present invention has both high formability and high strength, and is suitable for the preparation of aluminum alloy parts such as automotive interior and exterior covers.

[0085] In order to further illustrate the present invention, a 6xxx series aluminum alloy material for automobile covering parts provided by the present invention, its preparation method and application are described in detail below in combination with embodiments, but it should not be understood as limiting the protection scope of the present invention.

[0086] Example 1

[0087] The alloy ingot is prepared according to the composition ratio, and the ingot is prepared by industrial semi-continuous casting.

[0088] After the alloy ingot is prepared, a homogenization treatment and a cooling and insulation integrated treatment are carried out: the homogenization-cooling and insulation integrated treatment includes a homogenization heat treatment and a cooling and insulation treatment carried out in sequence, wherein the temperature of the homogenization heat treatment is 555±15°C, the time is 15±5h, and the heating rate is 30±10°C / h; the temperature of the cooling and insulation treatment is 515±15°C, and the time is 2±0.5h.

[0089] The starting temperature of hot rolling is 510±20℃, and the final rolling temperature is 300±60℃; the thickness of the hot rolled material is 4 ~ 8mm.

[0090] The 4-8 mm alloy hot-rolled coils are cold-rolled and coiled to obtain alloy cold-rolled sheets (foils) with a thickness of 1.2 mm.

[0091] The 1.2 mm thick cold rolled coil is subjected to solution treatment at a temperature of 545 ± 15 ° C for 25 ± 10 s (the process production uses an air cushion furnace for solution treatment), and then water-cooled, and then heated to 90 ± 10 ° C, coiled and naturally cooled, and the pre-aging treatment is completed to obtain a 1.2 mm thick cold rolled coil in a pre-aged state. The aluminum alloy coil used in this embodiment is in a pre-aged T4P state, and the alloy composition and thickness state are shown in Table 1.

[0092] The peak aging (medium temperature short-time heating) forming process is: using a box furnace for differential temperature heating, the box furnace temperature is set to 450°C, heating for 30s and then taking it out of the furnace (actual material temperature 240°C), using a cold stamping die for stamping, and the paint baking system is 180°C for 30min. The sample has a good stamping forming effect and does not crack.

[0093] Example 2

[0094] The aluminum alloy plate was prepared according to the steps in Example 1. The difference from Example 1 is that the heating method is different. The sample is heated by electromagnetic induction, and the temperature is quickly raised to 240°C at a heating rate of 50°C / s and then kept warm for about 40s.

[0095] Example 3

[0096] The difference from Example 1 is that: the alloy composition is different, see Table 1 for details; the heating method is different, the sample adopts electromagnetic induction heating, and the temperature is quickly raised to 240°C at a heating rate of 50°C / s and then kept warm for about 40s.

[0097] Example 4

[0098] The difference from Example 1 is that the alloy composition is different, see Table 1 for details.

[0099] Embodiment 5~7

[0100] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the heating process before forming is different, see Table 2 for details.

[0101] Example 8

[0102] The difference from Example 1 is that: the alloy composition is slightly different, the foil thickness is 0.3 mm, see Table 1 for details; the heating process before forming is different, see Table 2 for details.

[0103] Embodiment 9, 10

[0104] The difference from Example 1 is that: the alloy composition is different, see Table 1 for details; the ingot is prepared by injection molding, see Table 2.

[0105] Comparative Example 1

[0106] The difference from Example 1 is that the alloy composition is different, see Table 1 for details.

[0107] Comparative Examples 2~3

[0108] The difference from Example 1 is that: the alloy composition is slightly different, see Table 1 for details; the peak aging (medium temperature short time heating) process is different, see Table 2 for details.

[0109] Table 1 Plate composition (wt%) thickness state

[0110]

[0111] Table 2 Measured data of comparative examples and embodiments

[0112]

[0113] As can be seen from Table 2, the alloys in the embodiments of the present invention all have good mechanical properties and are well compatible with the aging forming integrated process. After forming and baking varnish treatment, the plates in the embodiments all reach a yield strength of >225MPa, a tensile strength of >280MPa, and an elongation of >20%. Among them, the peak aging (medium temperature short-time heating) treatment can not only dissolve the natural aging clusters that are unfavorable to stamping into solute atoms or smaller clusters, but also form a certain number of nucleation particles in the matrix, so that they can be quickly converted into strengthening precipitation phases in the subsequent baking varnish process, thereby improving the baking varnish response of the material.

[0114] Specifically:

[0115] In Examples 1 to 4, the performance of the formed components is good, the strength gradually increases due to the increase in the degree of alloying, and it is well adapted to the peak aging forming integrated process. The plate still maintains a good elongation index after forming.

[0116] Examples 5 to 7 use different peak aging (medium temperature short time heating) processes before forming, and the process window is wide, which is convenient for various component processing plants to perform process screening.

[0117] Example 8 is a 0.3 mm thick foil prepared using a peak aging forming integrated process to produce aluminum performance. This thickness of foil can be used in 3C electronic products such as mobile phones.

[0118] The ingots of Examples 9 and 10 were prepared by injection molding, and the performance of the formed plates was significantly improved compared with the ingots produced by conventional semi-continuous casting.

[0119] The alloy composition of Comparative Example 1 does not fall within the scope of the present invention, and the strength of the sheet after forming is insufficient.

[0120] The peak aging (medium temperature short time heating) processes of Comparative Examples 2 and 3 do not fall within the scope of the present invention, and cracking occurs during the sheet forming process.

[0121] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A 6xxx series aluminum alloy material for automobile covering parts, obtained by subjecting a naturally aged or pre-aged aluminum alloy material to a short-time spike aging treatment, The aluminum alloy material in the naturally aged state or pre-aged state includes the following components in mass fraction: Si 0.4~1.85%, Mg 0.2~1.5%, Cu ≤0.4%, Mn ≤0.5%, Zn ≤0.3%, Cr≤0.35%, Fe ≤0.5%, Ti ≤0.35%, other impurities individually ≤0.05%, other impurities total ≤0.15%, the balance is Al; The short-time peak aging treatment adopts box furnace heating treatment or electromagnetic induction heating treatment. The box-type furnace heating treatment comprises: The aluminum alloy material in the natural aging state or pre-aging state is heated to 200-260°C at a heating rate of 5-10°C / s; The electromagnetic induction heating treatment comprises: heating the aluminum alloy material in a natural aging state or a pre-aging state to 200-260° C. at a heating rate of 35-70° C. / s, and keeping the temperature for 20-40s.

2. The 6xxx series aluminum alloy material for automobile covering parts according to claim 1, characterized in that: The aluminum alloy material in the naturally aged state or pre-aged state includes the following components in mass fraction: Si 1.0~1.5%, Mg 0.25~0.6%, Cu ≤0.2%, Mn ≤0.2%, Zn ≤0.2%, Cr ≤0.1%, Fe ≤0.5%, Ti ≤0.15%, other impurities individually ≤0.05, other impurities total ≤0.15%, the balance is Al.

3. The 6xxx series aluminum alloy material for automobile covering parts according to claim 1, characterized in that: The set temperature of the box furnace is 420-480° C., and the heating time is 20-60 seconds.

4. A method for preparing the 6xxx series aluminum alloy material for automobile covering parts as claimed in claim 1, comprising the following steps: A) melting and casting the raw materials to obtain ingots; B) subjecting the ingot to homogenization treatment, hot rolling, cold rolling, solution treatment, and then natural aging or pre-aging treatment to obtain a naturally aged or pre-aged aluminum alloy material; C) The naturally aged or pre-aged aluminum alloy material is subjected to short-time spike aging treatment to obtain a 6xxx series aluminum alloy material for automotive covering parts.

5. The preparation method according to claim 4, characterized in that: The casting is carried out by a spray deposition method; The homogenization process comprises the following steps: First, heat the temperature to 540-570°C at a heating rate of 20-80°C / h and keep it at that temperature for 4-25 hours; The homogenization process also includes a cooling and heat preservation process, wherein the temperature of the cooling and heat preservation process is 500-530° C., and the cooling and heat preservation time is 1.5-18 hours.

6. The preparation method according to claim 4, characterized in that: The hot rolling starting temperature is 490-530°C, and the final rolling temperature is 240-360°C.

7. The preparation method according to claim 4, characterized in that: The temperature of the solution treatment is 510-560° C., and the time of the solution treatment is 10-150 s.

8. The preparation method according to claim 4, characterized in that: The pre-aging treatment comprises: heating the aluminum alloy material after the solid solution treatment to 60-100° C., then coiling and cooling naturally; The temperature of the natural aging treatment is 0-40°C.

9. An automobile cover is obtained by cold stamping and baking varnish treatment of 6xxx aluminum alloy material; The 6xxx aluminum alloy material is the 6xxx series aluminum alloy material for automobile covering parts described in any one of claims 1 to 3 or the 6xxx series aluminum alloy material for automobile covering parts prepared by the preparation method described in any one of claims 4 to 7.

10. The automobile covering member according to claim 9, characterized in that: The automobile covering part comprises an automobile door outer panel and an automobile door inner panel; The sheet thickness of the automobile covering part is 0.2-2 mm.