Steel plate with yield strength of 690 MPa for crude oil storage tank and manufacturing method of steel plate
Through the design and process of specific chemical compositions, steel plates for crude oil storage tanks with bainite tempering structure are formed, which solves the problem of insufficient strength and welding performance of the steel plate in the existing technology, and achieves a combination of high yield strength and good welding performance. Improved production efficiency.
Patent Information
- Application Number
- CN202411043854.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-31
Smart Images

Figure BDA0004973001760000071 
Figure BDA0004973001760000081 
Figure BDA0004973001760000082
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a steel plate for a crude oil storage tank with a yield strength of 690 MPa and a manufacturing method thereof. Background Art
[0002] Oil is an important energy pillar for the development of every country, and strategic oil reserves are the main way to ensure oil security. Oil affects the development of my country's national economy and the improvement of people's quality of life in all aspects. Among them, crude oil has a large demand and a wide range of demand, and it itself has the characteristics of flammability, explosion, and volatility, so its transportation and storage are always accompanied by risks. Storage tanks have the advantages of small surface area, light weight, short manufacturing cycle and small footprint. They are a kind of gas and liquid storage container widely used in the petrochemical industry. Therefore, with the steady growth of my country's oil demand and the continuous strengthening of oil reserves, the construction of reserve depots and large crude oil storage tanks has also ushered in an unprecedented peak.
[0003] As the domestic industrial production technology and large tank manufacturing technology of steel for crude oil storage tanks have basically matured, but as crude oil storage tanks gradually develop towards large-scale and high-parameter directions, the construction of 150,000 cubic meters of super-large oil storage tanks is imminent, but the high-strength steel for crude oil storage tanks still uses the previous grades of high-strength steel, which will cause the steel plate to be too thick, difficult to weld, and inconvenient to build crude oil storage tanks. In addition, the production of steel plates wastes the production capacity of the existing advanced medium and thick plate rolling mills on the production line, increasing the process cost and delivery time of the steel plates. Therefore, based on demand, it is necessary to develop a new type of steel plate for crude oil storage tanks that not only requires high strength and toughness, but also has good comprehensive performance. At present, the existing domestic steel plates for crude oil storage tanks cannot meet the high strength requirements, so it has become an urgent task for the steel industry to study a steel plate for crude oil storage tanks with a yield strength of 690MPa.
[0004] The patent document "Heat Treatment Method for Thin-gauge Quenched and Tempered 12MnNiVR Steel Plate" (CN108265161A) adopts a conventional quenching + tempering heat treatment process, and its yield strength is difficult to reach 690MPa, which cannot meet the demand;
[0005] Patent document "High-strength and toughness steel plate for crude oil storage tank with low welding crack sensitivity coefficient and manufacturing method thereof with resistance to high temperature PWHT softening and high strength and toughness" (CN105671436A) has the following chemical composition: C 0.07-0.12%, Si 0.15-0.30%, Mn 1.40-1.60%, S≤0.010%, P≤0.015%, Mo 0.05-0.15%, Ni0.20-0.35%, Nb 0.015-0.035%, V0.030-0.060%, Ti 0.010-0.030%, Alt0.015-0.045%, and the rest is Fe and unavoidable trace impurities. The steel produced by its designed composition and manufacturing process cannot meet the yield strength of 690MPa, and the heat treatment time is long, which affects the production efficiency.
[0006] Patent document "Large Thickness Ultra-Low Temperature High Toughness Steel Plate for Spherical Tanks and Rolling Method Thereof" (CN112795839A) designs the chemical composition C: 0.06-0.09%, Si≤0.55%, Mn 1.30-1.60%, P≤0.012%, S≤0.005%, Ni 0.40-0.70%, Nb 0.020-0.030%, Alt 0.020-0.050%, balance Fe and other elements. The strength of the designed thick steel plate is lower than the designed yield strength of 690MPa, and the mechanical properties of the thick steel plate are difficult to guarantee after post-weld heat treatment, which affects subsequent processing.
[0007] Therefore, in view of the above situation, it is urgent to develop a new type of high-strength steel by adjusting the manufacturing method and designing new components, and to develop a steel plate for crude oil storage tanks with a yield strength of 690MPa and its manufacturing method. Summary of the invention
[0008] The purpose of the present invention is to overcome the above problems and shortcomings and provide a steel plate for crude oil storage tanks with a yield strength of 690MPa and a manufacturing method thereof, which has a bainite tempered structure, eliminates the damage of ferrite to the strength of the steel plate, has a good strength-toughness ratio, and good high-wire energy welding performance.
[0009] The object of the invention is achieved in this way:
[0010] A steel plate for crude oil storage tanks with a yield strength of 690 MPa. The components of the steel plate are as follows by weight percentage: C: 0.05%-0.10%, Si: 0.10%-0.30%, Mn: 1.00%-2.00%, P: ≤0.010%, S: ≤0.005%, V: 0.10%-0.20%, Ti: 0.05%-0.10%, Al: 0.0025%-0.0045%, N: 0.002%-0.006%, B: 0.0005%-0.0015%, W: 0.002%-0.004%, and the balance is Fe and unavoidable impurities.
[0011] Furthermore, in the steel plate, V / C=1.5 to 3.5.
[0012] Furthermore, the microstructure of the steel plate is a bainite tempered structure, and the size of carbides in the structure is 1 to 4 μm.
[0013] Furthermore, the thickness of the steel plate is 10 to 50 mm, and the yield strength R eL ≥700MPa, tensile strength R m :800~920MPa, elongation A≥18%, -20℃KV 2 ≥100J; simulated mechanical yield strength Re of steel plate after post-weld heat treatment L ≥690MPa, tensile strength R m :780~900MPa, elongation A≥18%, -20℃KV 2 ≥100J.
[0014] Furthermore, the heat affected zone properties of the steel plate after large wire welding with a large wire energy of 70-110kJ / cm: yield strength R eL ≥690MPa, tensile strength R m :750~880MPa, elongation A≥18%, -20℃KV 2 ≥80J.
[0015] The design reason of the present invention is:
[0016] C: C forms various carbides or solid solutions with alloy elements in steel to strengthen it. It is an element that directly improves the strength of steel plates. Too high C content will lead to too high Pcm and CEV, resulting in poor toughness and welding performance of steel. Therefore, in order to ensure that the steel plate has good low-temperature toughness, high strength and welding performance during use, the C content is limited to 0.05-0.10%.
[0017] Si: Si is an element that increases carbon activity in steel, can inhibit the coarsening of carbides, and can be dissolved in ferrite to increase the strength of the steel plate and the hardenability of the steel. It can also reduce the ductile-brittle transition temperature within a certain range and improve the plasticity of the steel. Therefore, the Si content is limited to 0.10-0.30%.
[0018] Mn: Mn can achieve excellent deoxidation effect in combination with Si in steel. Mn improves the strength of steel plate through solid solution strengthening, improves its toughness, hot working performance and sulfide distribution morphology, and prevents the formation of hot cracks; and with the increase of Mn content, the stability of austenite in steel is improved, the critical cooling rate is reduced, the hardenability is significantly improved, and the stability of tempered structure is improved. Appropriate Mn content can make the welding heat affected zone have higher strength and toughness, so Mn is limited to 1.00-2.00%.
[0019] P: P is a harmful element in steel, which has a great impact on low temperature impact toughness and is also an element that is very easy to segregate. The present invention controls P within a relatively low range, so the content of P is controlled to be below 0.010%.
[0020] S: S is also a harmful element in steel. It is easy to form MnS in steel, which is easy to become the source of hot cracks during welding and has a great impact on the toughness of the heat-affected zone of welding. Therefore, S is controlled below 0.005%.
[0021] V: V, as the main element of the present invention, can be dissolved into austenite at high temperature, and after solid solution, it can play a strengthening role and improve the hardenability and strength of steel; the increase of V (C, N) precipitation can also inhibit grain boundary movement and grain growth, and further improve the toughness and tempering stability of steel. Among them, V and C atoms have a very strong affinity, and the formed V-containing carbides play a role in improving the strength of steel, and have high-temperature stability, so that the steel can still maintain a fine-grained structure at a higher temperature, greatly reducing the overheating sensitivity of steel and improving the welding performance of steel plates; if the V content is too high, the carbide size will be too large, so V is limited to 0.10-0.20%, V / C: 1.5~3.5.
[0022] Ti: Ti, as the main element of the present invention, can significantly refine the grains. Ti has a strong affinity with C and N, and the formed carbides, nitrides or carbonitrides have a very high dissolution temperature. During the heating process, the undissolved small carbonitride particles increase the nucleation points of austenite and hinder the growth of austenite grains at high temperatures; the fine nitrides greatly inhibit the coarsening of austenite grains at high welding temperatures, and during the cooling process, the organization of the welding heat-affected zone is refined and the toughness is improved. Therefore, the Ti content is limited to 0.05-0.10%.
[0023] Al: Al can deoxidize and fix N elements in steel, improve the toughness of steel, and refine the grain structure; Al can also reduce the formation of BN in steel and increase the content of solid solution B in steel; appropriate Al can improve the yield and tensile strength of the heat affected zone of welding, but too much Al will lead to the formation of larger oxides and reduce the low-temperature impact toughness of the steel plate. Therefore, the Al content is limited to 0.0025-0.0045%.
[0024] N: N in steel mainly precipitates VN or V(CN) when austenite transforms into ferrite, which inhibits the growth of austenite grains and improves the strength and low-temperature toughness of steel. Therefore, the N content is limited to 0.002-0.006%.
[0025] B: During the two-stage rolling process, B causes the segregation of solid-solution boron on the original austenite grain boundary to occupy the nucleation position of ferrite on the original austenite grain boundary, inhibiting the formation of ferrite; B can promote the transformation of bainite structure, thereby improving the hardenability of the steel plate; and B can inhibit grain boundary sliding and grain growth, enhance grain boundary strengthening, and ensure fine grains in the weld structure. Therefore, B is limited to 0.0005-0.0015%.
[0026] W: As the main element of the present invention, W forms refractory carbides in steel, increases hardenability, reduces thermal sensitivity of the steel plate, and ensures that the welding heat-affected zone of the steel plate has a higher strength; at the same time, it can refine the grains and improve the tempering resistance of the steel plate. Therefore, the W content is limited to 0.002-0.004%.
[0027] The second technical solution of the present invention is to provide a method for manufacturing a steel plate for a crude oil storage tank with a yield strength of 690 MPa, comprising smelting, continuous casting, heating, rolling, and heat treatment;
[0028] (1) Smelting: Use molten iron pretreatment, the molten iron temperature is 1350-1410℃; during refining treatment, LF time is 25-35min, RH time is 25-35min, and vacuum degree is ≤5.0mbar.
[0029] (2) Continuous casting: The casting temperature of the molten steel in the tundish is 1340-1400°C. The light reduction technology is preferably used in the continuous casting process, and the reduction amount is controlled at 2-4 mm; the billet drawing speed is 0.70-0.85 m / min, the secondary cooling water is 5500-6000 L / min, the superheat is 20-35°C, and the straightening temperature is 970-990°C. The light reduction technology is used to slightly reduce the center segregation of the billet at the point where the billet is about to solidify.
[0030] (3) Heating: The continuous casting billet heating is divided into preheating section, heating section and soaking section; the temperature range of the heating section is 1170-1210℃; the temperature range of the soaking section is 1160-1200℃; the total time in the furnace is 150-200min. By heating the billet in three stages, the temperature of the core of the billet reaches 1160-1200℃, ensuring that the billet structure is completely austenitic.
[0031] (4) Rolling: After the billet is discharged from the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. The starting rolling temperature in the rough rolling stage is 1130-1170°C, the roller speed is 0.6-0.8 m / s, and the single-pass reduction rate is 11%-16%; the starting rolling temperature in the finishing rolling stage is 840-900°C, the final rolling temperature is 790-850°C, the roller speed is 0.5-0.6 m / s, and the single-pass reduction rate is 13%-18%; the starting cooling temperature in the cooling stage is 750-810°C, and the final cooling temperature is 450-500°C; after cooling, the steel plate is straightened, and the straightening speed is controlled at 1.0-1.8 m / s; finally, the steel plates are stacked and slowly cooled, the slow cooling temperature is 400-450°C, and the slow cooling time is 1000-1200 min. Through two-stage rolling, large reduction and slow roll speed rolling are adopted, the deformation storage energy in the structure is increased, the time for dynamic recrystallization behavior to occur is prolonged, and the grains are refined; by controlling cooling, the ferrite transformation is suppressed and the bainite structure transformation is promoted to be complete; by straightening the steel plate, the residual stress generated inside the steel plate due to cooling is eliminated, ensuring the good shape of the steel plate.
[0032] (5) Heat treatment: After stacking and slow cooling, the steel plate is tempered at a temperature of 610-630°C and the holding time is 100-250 minutes to ensure that the steel plate structure is fully transformed into a bainite tempered structure. Through tempering heat treatment, the steel plate structure is uniform and is a bainite tempered structure, and the mechanical properties of the steel plate can be improved.
[0033] The beneficial effects of the present invention are:
[0034] 1. The composition design of the present invention is simple. On the basis of a relatively low carbon content, sufficient amounts of V and Ti elements are added to ensure that the steel plate has sufficient strength by using precipitation strengthening. V can be dissolved into austenite at high temperature to improve the hardenability of steel. Stable and refractory carbides formed by V and C during the smelting process can refine the grains and reduce the overheating sensitivity of steel. At the same time, the precipitation strengthening and dispersion strengthening effects of V elements are used to ensure that the steel plate has sufficient strength and toughness, and can significantly refine the grains. Ti has a strong affinity with C and N, and the formed compound has a very high dissolution temperature. During the heating process, the undissolved carbonitride small particles increase the nucleation points of austenite and hinder the growth of austenite grains at high temperatures. During the cooling process, the organization of the weld and the heat-affected zone is refined, and the toughness is improved. In addition, W and B elements are added to refine the grains, improve the hardenability and tempering resistance of the steel plate. The above-mentioned composition involves ensuring that the steel plate has good high-heat input welding performance.
[0035] 2. The manufacturing method of the present invention is reasonable. By adopting controlled rolling and controlled cooling combined with tempering heat treatment, the finished product structure is ensured to be a bainite tempered structure. The carbide size in the structure is between 1 and 4 μm and is evenly distributed, eliminating the damage of blocky ferrite to the strength of the steel plate, so that the steel plate has a good strength-toughness ratio, and still has excellent strength and toughness after simulated post-weld heat treatment. By straightening the steel plate, the unevenness of the steel plate is controlled between 1 and 4 mm.
[0036] 3. The thickness of the steel plate of the present invention is 10 to 50 mm, and the yield strength of the steel plate is R eL ≥700MPa, tensile strength R m :800~920MPa, elongation A≥18%, -20℃KV 2 ≥100J. The properties of the steel plate after simulated post-weld heat treatment are ReL≥690MPa, Rm:780~900MPa, A≥18%, -20℃KV2≥100J.
[0037] 4. The heat affected zone performance of the steel plate after large wire welding with a large wire energy of 70-110 kJ / cm: yield strength R eL ≥690MPa, tensile strength R m :750~880MPa, elongation A≥18%, -20℃KV 2 ≥80J. DETAILED DESCRIPTION
[0038] The present invention will be further described below by way of examples.
[0039] (1) Heating: The continuous casting billet heating is divided into preheating section, heating section and soaking section; the temperature range of the heating section is 1170-1210°C; the temperature range of the soaking section is 1160-1200°C; the total time in the furnace is 150-200 minutes;
[0040] (2) Rolling: After the billet is out of the furnace, a two-stage controlled rolling and controlled cooling technology is adopted. The starting rolling temperature of the rough rolling stage is 1130-1170°C, the roller speed is 0.6-0.8m / s, and the single-pass reduction rate is 11%-16%; the starting rolling temperature of the finishing rolling stage is 840-900°C, the final rolling temperature is 790-850°C, the roller speed is 0.5-0.6m / s, and the single-pass reduction rate is 13%-18%; the starting cooling temperature of the cooling stage is 750-810°C, and the final cooling temperature is 450-500°C; after cooling, the steel plate is straightened, and the straightening speed is controlled at 1.0-1.8m / s; then the steel plates are stacked and slowly cooled, the slow cooling temperature is 400-450°C, and the slow cooling time is 1000-1200min;
[0041] (3) Heat treatment: After stacking and slow cooling, the steel plate is tempered at a temperature of 610-630°C and the holding time is 100-250 min.
[0042] Further; smelting: using molten iron pretreatment, the molten iron temperature is 1350 ~ 1410 ℃; during refining treatment, LF time is 25 ~ 35min, RH time is 25 ~ 35min, vacuum degree is ≤5.0mbar.
[0043] Further; continuous casting: tundish molten steel casting temperature 1340 ~ 1400 ℃, billet drawing speed 0.70 ~ 0.85m / min, secondary cooling water 5500 ~ 6000L / min, superheat 20 ~ 35 ℃, straightening temperature 970 ~ 990 ℃.
[0044] Furthermore, a light reduction technique is used during the continuous casting process, and the reduction amount is controlled within 2 to 4 mm.
[0045] The embodiment of the present invention is smelted, continuously cast, heated, rolled and heat treated according to the component ratio of the technical solution. The composition of the steel of the embodiment of the present invention is shown in Table 1. The main process parameters for smelting and casting of the steel of the embodiment of the present invention are shown in Table 2. The main process parameters for heating and rolling of the steel of the embodiment of the present invention are shown in Table 3. The process parameters for cooling, slow cooling and heat treatment of the steel of the embodiment of the present invention are shown in Table 4. The properties of the steel of the embodiment of the present invention are shown in Table 5. The properties of the steel of the embodiment of the present invention after simulating post-weld heat treatment are shown in Table 6. The mechanical properties of the heat-affected zone after high-energy line welding of the embodiment of the present invention are shown in Table 7.
[0046] Table 1 Composition of steel according to the present invention (wt%)
[0047] Example C Si Mn P S V Ti N B W Al V / C 1 0.09 0.13 1.03 0.001 0.001 0.12 0.05 0.002 0.0005 0.002 0.0025 1.3 2 0.05 0.16 1.80 0.002 0.002 0.16 0.08 0.003 0.0009 0.002 0.0025 3.2 3 0.05 0.27 1.19 0.001 0.001 0.10 0.06 0.003 0.0007 0.002 0.0038 2.0 4 0.06 0.16 1.97 0.007 0.005 0.19 0.07 0.006 0.0014 0.003 0.0029 3.2 5 0.06 0.14 1.71 0.007 0.005 0.18 0.10 0.002 0.0006 0.002 0.0026 3.0 6 0.07 0.28 1.62 0.004 0.003 0.13 0.06 0.005 0.0015 0.004 0.0040 1.9 7 0.05 0.17 1.57 0.01 0.005 0.10 0.10 0.003 0.001 0.003 0.0031 2.0 8 0.07 0.28 1.53 0.006 0.005 0.12 0.06 0.005 0.0014 0.004 0.0035 1.7 9 0.08 0.22 1.09 0.001 0.002 0.20 0.10 0.002 0.0006 0.003 0.0033 2.5 10 0.05 0.20 1.46 0.008 0.005 0.10 0.10 0.003 0.0008 0.002 0.0032 2.0 11 0.08 0.29 1.35 0.002 0.002 0.17 0.09 0.004 0.0012 0.004 0.0037 2.1 12 0.09 0.15 1.3 0.005 0.004 0.18 0.09 0.004 0.0011 0.004 0.0028 2.0 13 0.10 0.30 1.27 0.003 0.003 0.15 0.08 0.005 0.0013 0.004 0.0039 1.5 14 0.10 0.23 1.88 0.009 0.005 0.17 0.09 0.002 0.0007 0.004 0.0027 1.7 15 0.09 0.25 1.48 0.006 0.004 0.19 0.06 0.006 0.0013 0.003 0.0039 2.1
[0048] Table 2 Main process parameters of steel smelting and casting in the embodiment of the present invention
[0049]
[0050] Table 3 Main process parameters of heating and rolling of steel in the embodiment of the present invention
[0051]
[0052] Table 4 Process parameters for cooling, slow cooling and heat treatment of steel according to the present invention
[0053]
[0054] Table 5 Properties of steel according to the present invention
[0055]
[0056] Table 6 Mechanical properties of steel after heat treatment in the present invention
[0057]
[0058] Note: The heat treatment temperature of mold welding is 560-640℃, and the holding time is 120-240min.
[0059] Table 7 Mechanical properties of heat affected zone after high heat input welding in the embodiment of the present invention
[0060]
[0061] Note: The maximum welding energy is 70-110 kJ / cm.
[0062] The microstructure of the steel plate produced by the present invention is a bainite tempered structure. The thickness of the steel plate is 10 to 50 mm, and the yield strength R eL ≥700MPa, tensile strength R m :800~920MPa, A≥18%, -20℃KV 2 ≥100J. Mechanical properties of steel plate after simulated post-weld heat treatment Yield strength R eL ≥690MPa, tensile strength R m :780~900MPa, A≥18%, -20℃KV 2 ≥100J. Steel plate welding heat affected zone performance yield strength R eL ≥690MPa, tensile strength R m :750~880MPa, A≥18%, -20℃KV 2 ≥80J.
[0063] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A steel plate for crude oil storage tanks with a yield strength of 690 MPa, It is characterized in that The components of the steel plate are as follows by weight percentage: C: 0.05% to 0.10%, Si: 0.10% to 0.30%, Mn: 1.00% to 2.00%, P: ≤0.010%, S: ≤0.005%, V: 0.10% to 0.20%, Ti: 0.05% to 0.10%, Al: 0.0025% to 0.0045%, N: 0.002% to 0.006%, B: 0.0005% to 0.0015%, W: 0.002% to 0.004%, and the balance is Fe and unavoidable impurities.
2. The steel plate for crude oil storage tanks with a yield strength of 690 MPa according to claim 1, It is characterized in that In the steel plate, V / C=1.5-3.
5.
3. The steel plate for crude oil storage tanks with a yield strength of 690 MPa according to claim 1, It is characterized in that The microstructure of the steel plate is a bainite tempered structure, and the size of carbides in the structure is 1 to 4 μm.
4. The steel plate for crude oil storage tanks with a yield strength of 690 MPa according to claim 1, It is characterized in that The thickness of the steel plate is 10 to 50 mm, and the yield strength R eL ≥700MPa, tensile strength R m :800~920MPa, elongation A≥18%, -20℃KV 2 ≥100J; the heat affected zone performance of the steel plate after large-line welding with a welding energy of 70-110kJ / cm is the yield strength R eL ≥690MPa, tensile strength R m :750~880MPa, elongation A≥18%, -20℃KV 2 ≥80J.
5. A method for manufacturing a steel plate for a crude oil storage tank with a yield strength of 690 MPa as claimed in any one of claims 1 to 4, comprising smelting, continuous casting, heating, rolling and heat treatment; Features: (1) Heating: The continuous casting billet heating is divided into preheating section, heating section and soaking section; the temperature range of the heating section is 1170-1210°C; the temperature range of the soaking section is 1160-1200°C; the total time in the furnace is 150-200 minutes; (2) Rolling: After the billet is discharged from the furnace, a two-stage controlled rolling and controlled cooling technology is adopted; the starting rolling temperature in the rough rolling stage is 1130-1170°C, the roller speed is 0.6-0.8 m / s, and the single-pass reduction rate is 11%-16%; the starting rolling temperature in the finishing rolling stage is 840-900°C, the final rolling temperature is 790-850°C, the roller speed is 0.5-0.6 m / s, and the single-pass reduction rate is 13%-18%; the starting cooling temperature in the cooling stage is 750-810°C, and the final cooling temperature is 450-500°C; after cooling, the steel plate is straightened, and the straightening speed is controlled at 1.0-1.8 m / s; After that, the steel plates are stacked and slowly cooled at a temperature of 400-450°C and a time of 1000-1200 minutes. (3) Heat treatment: After stacking and slow cooling, the steel plate is tempered at a temperature of 610-630°C and the holding time is 100-250 min.
6. The method for manufacturing a steel plate for a crude oil storage tank with a yield strength of 690 MPa according to claim 5 is characterized by: smelting: using molten iron pretreatment, the molten iron temperature is 1350-1410°C; during the refining treatment, the LF time is 25-35 minutes, the RH time is 25-35 minutes, and the vacuum degree is ≤5.0 mbar.
7. The method for manufacturing a steel plate for a crude oil storage tank having a yield strength of 690 MPa according to claim 5, Features: Continuous casting: tundish molten steel casting temperature 1340 ~ 1400 ℃, billet drawing speed 0.70 ~ 0.85m / min, secondary cooling water 5500 ~ 6000L / min, superheat 20 ~ 35 ℃, straightening temperature 970 ~ 990 ℃.
8. The method for manufacturing a steel plate for a crude oil storage tank having a yield strength of 690 MPa according to claim 7, Features: During the continuous casting process, light reduction is adopted, and the reduction amount of light reduction is 2 to 4 mm.
Citation Information
Patent Citations
An economical high-strength steel plate with a yield strength of 690 MPa and its manufacturing method
CN102260823A
Low-carbon bainite construction steel with yield ratio of less than 0.8 and production method thereof
CN103667963A
High-toughness steel plate with high-temperature PWHT softening resistance and low welding crack sensitivity coefficient for crude oil storage tank and manufacturing method of high-toughness steel plate
CN105671436A
690MPa-grade steel plate with excellent low-temperature ductility and manufacturing method
CN116875903A
Ultrahigh-strength steel plate for ship in ice area and manufacturing method of ultrahigh-strength steel plate
CN116891975A