By adding microalloy elements W to the rolling roll and performing differential temperature quenching + tempering heat treatment, the problem of insufficient thermal cracking and wear resistance of the roll surface in large steel rolling is solved, extending the service life of the roll and improving the rolling performance.
Patent Information
- Application Number
- CN202410890173.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-01
AI Technical Summary
During the rolling process of large-scale steel, the rolling rolls bear high loads and high deformation resistance, resulting in a large tendency for thermal cracking on the roll surface, insufficient wear resistance, high risk of breaking the roll, and high requirements for the surface quality and service cycle of the roll. The existing rolls are available. It is difficult to meet the rolling needs of high-quality steel.
High-strength long roller-operated BD rollers are used, and their chemical compositions are C: 0.4-0.7%, Si: 0.2-0.6%, Mn: 0.5-1.0%, Cr: 0.5-3.5%, Ni: 0.2-1.7%, Mo: 0.1-0.8%, W: 0.1-0.4%, Cu: ≤0.3%, by combining arc furnace oxidation and LF refining, microalloy element W is added, VD vacuum degassing and near-final forging, combined with differential temperature quenching + Tempering heat treatment improves the wear resistance of the roll and the roll surface heat crack resistance.
Effectively improve the wear resistance of BD rollers and the heat crack resistance of the roller surface, extend the service cycle of BD rollers, improve the comprehensive rolling performance, and meet the needs of high-quality steel rolling.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing high-alloy forged steel rolls, and in particular relates to a high-strength long roll BD roll and a preparation method thereof. Background Art
[0002] With the rapid development of the national economy, the demand for large-scale steel and heavy rails for large-scale construction, lifting and transportation, oil platforms and other industries is increasing. Due to its large cross-sectional size and high material strength, large-scale steel has the characteristics of high rolling load, deep hole groove and strong deformation resistance during the billet rolling process. First of all, the deep hole groove will lead to large heat storage of the roller. In the case of insufficient cooling, the roller surface has a high tendency to thermal cracking; secondly, due to the high strength of the rolled material, the rolling load on the roller is also increased accordingly, and the axial extrusion pressure on the hole is also increased, which greatly increases the risk of roller breakage; in addition, due to the high precision of the rolled material, the surface quality requirements of the roller are high, and due to continuous production, the service life of the roller is also higher. Therefore, in order to ensure the quality of the rolled material of the steel and extend the service life of the billet roll, a high-strength long-roll BD roller with higher roller body strength, stronger wear resistance and better roller surface resistance to thermal cracking and its preparation method are now needed. Summary of the invention
[0003] The purpose of the present invention is to provide a high-strength long-life BD roller and a preparation method thereof, which can effectively improve the wear resistance of the BD roller and the heat crack resistance of the roller surface, thereby extending the on-machine roll service of the BD roller, improving the comprehensive rolling performance of the BD roller, and meeting the high-quality steel rolling requirements.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] A high-strength long roller BD roller, the chemical composition of the high-strength long roller BD roller is as follows: C: 0.4-0.7%, Si: 0.2-0.6%, Mn: 0.5-1.0%, Cr: 0.5-3.5%, Ni: 0.2-1.7%, Mo: 0.1-0.8%, W: 0.1-0.4%, Cu: ≤0.3%, [H]: ≤2ppm, [O]: ≤15ppm, [N]: ≤70ppm, P and S are both ≤0.025%, and the balance is Fe and unavoidable impurities.
[0006] A further improvement of the technical solution of the present invention is that forging a high-strength long roll BD roll comprises the following steps:
[0007] Step S1: Selecting furnace materials, using scrap steel, pig iron and alloy materials;
[0008] Step S2: using an arc furnace oxidation method to perform primary smelting of molten steel, and ensuring that P≤0.01% is the end point before steel tapping;
[0009] Step S3: The molten steel after primary refining is transferred to the LF refining furnace. The whole LF refining process is white slag operation. The alloy material and micro-alloy material are added in batches according to the chemical composition of the high-strength long roll BD roll;
[0010] Step S4: After LF refining is completed, VD vacuum degassing operation is performed in a VD vacuum degassing furnace after heating;
[0011] Step S5: heating after VD vacuum degassing, and then casting using a large-taper steel ingot mold hanging ladle;
[0012] Step S6: After the steel ingot is demoulded, it is hot-transferred to forging, and the blank is forged by using the near-net-shape forging method according to the hole shape finished product drawing, and the single-side machining allowance of the blank in the diameter direction at the hole shape position is ≤25mm;
[0013] Step S7: Rough machining the blank according to the hole pattern finished product drawing and the heat treatment allowance principle, and the blank at the rough machining hole position is made to have a single side allowance of 5-10 mm in the diameter direction;
[0014] Step S8: Performance heat treatment: using differential temperature quenching + tempering, the quenching temperature is 850-1000°C, and the tempering temperature is 500-600°C;
[0015] Step S9: After the heat treatment is completed, the forging is subjected to performance testing.
[0016] A further improvement of the technical solution of the present invention is that in step S3, at the end of LF refining, W element is added in batches at different positions evenly distributed on the surface of molten steel, with a single addition amount not exceeding 0.10 kg / t molten steel, and the W content is between 0.1-0.4%.
[0017] A further improvement of the technical solution of the present invention is that the near-net-shape forging method in step S6 comprises the following steps:
[0018] Step S601: designing a forging drawing of the forging pass according to the finished pass and classifying and designing the machining allowance of the pass: classifying and designing the machining allowance of the pass diameter and length according to the roll body diameter, the total length of the roll and the shape of the finished corner;
[0019] Step S602: Designing the margin reserve of the BD roller pass;
[0020] Step S603: designing the spacing distance of the BD roller pass profile and the length of the groove side of the roller body edge;
[0021] Step S604: Determine the corresponding length of the blank at the hole position before the imprinting station and perform hole forging on the blank.
[0022] The technical solution of the present invention is further improved in that: in step S602, the length margin of the BD roller hole is designed to be 35-40 mm on one side, and the diameter margin is 15-25 mm on one side. When the depth of the finished hole is ≥100 mm, the length margin and the diameter margin are both increased by 10-15%.
[0023] A further improvement of the technical solution of the present invention is that in step S603, the spacing distance between the BD roller pass profiles is designed to be ≥300 mm, and the groove length of the roller body edge is ≥220 mm.
[0024] A further improvement of the technical solution of the present invention is that in step S604, the blank length required for engraving is first calculated based on the principle of conservation of blank volume and weight, and then the blank length is determined by engraving at both ends of the corresponding position, and finally the engraved blank is forged through a clamping table to form a hole-shaped recess.
[0025] A further improvement of the technical solution of the present invention is that the blank length required for engraving is ≥100 mm.
[0026] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:
[0027] The high-strength long-service BD roller and the preparation method thereof of the present invention can effectively improve the wear resistance of the BD roller and the thermal crack resistance of the roller surface, thereby extending the on-machine service life of the BD roller, improving the comprehensive rolling performance of the BD roller, and meeting the high-quality steel section rolling requirements.
[0028] The present invention improves the wear resistance and thermal fatigue performance of the roll by adding the microalloying element W to the microalloyed structure during the solidification process of the molten steel. This is because the W element can form fine carbides or nitrides in the molten steel as a microalloying element. These precipitates can significantly improve the strength, toughness and wear resistance of the steel. At the same time, the fine carbides have a high melting point. These carbides can stably exist during the heat treatment of the steel, thereby hindering the growth of the grains at the microscopic level, resulting in grain boundary strengthening and precipitation strengthening. Therefore, it is also helpful to refine the grains during the cooling process, thereby improving the overall performance of the steel.
[0029] The present invention adopts a near-net-shape forging method during the forging process, can forge a blank of similar shape according to a hole profile finished product drawing, reduce the blank processing allowance, and can maximize the retention of the excellent structure of the outer layer of the roller blank.
[0030] The present invention performs rough processing according to the hole type finished product drawing and the heat treatment reserve principle before the performance heat treatment, reduces the processing amount after the heat treatment, and maximizes the retention of the excellent structure of the hardened layer. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with embodiments:
[0032] The invention provides a high-strength long roll BD roll, which is made of high-alloy pure steel and has the following chemical composition ranges: C: 0.4-0.7%, Si: 0.2-0.6%, Mn: 0.5-1.0%, Cr: 0.5-3.5%, Ni: 0.2-1.7%, Mo: 0.1-0.8%, W: 0.1-0.4%, Cu: ≤0.3%, [H]: ≤2ppm, [O]: ≤15ppm, [N]: ≤70ppm, P and S are both ≤0.025%, and the remainder is Fe and unavoidable impurities.
[0033] A method for preparing a high-strength long roll BD roll comprises the following steps:
[0034] Step S1: Select the furnace charge, use scrap steel, pig iron and alloy materials: do not allow non-pure furnace charge to enter the furnace, the residual elements of scrap steel, pig iron and alloy materials must meet the requirements of the chemical composition of the finished product, especially control the harmful elements P, Sn and Sb that affect the performance;
[0035] Step S2: electric furnace smelting by oxidation method: the molten steel is initially smelted by electric arc furnace oxidation method, and the end point before tapping is ensured to be P≤0.01%;
[0036] Step S3: LF refining: The molten steel after primary refining is transferred to the LF refining furnace. The LF refining furnace should be cleaned before use, without residual steel and slag. Slag should be strictly prevented during the whole process of steel tapping. White slag operation is performed during the whole process of LF refining. Alloy materials and micro-alloy materials are added in batches according to the chemical composition of the high-strength long roll BD roll, the refining time is extended, the slag-making batches are increased, the purity of the molten steel is improved, and the harmful elements are ensured to meet the process requirements;
[0037] At the end of LF refining, W element is added to achieve microalloying of molten steel, thereby improving the strength and toughness of the roll. The added W content is between 0.1-0.4%;
[0038] The content of W should be neither too high nor too low. If the content of W is too low, the carbides or nitrides formed will not be sufficient to effectively prevent grain growth and improve strength. In this case, the effect of microalloying will not be obvious, and the purpose of improving the toughness of the roll cannot be achieved. On the other hand, if the content of W is too high, the following problems may occur: 1. Increased alloy cost: W is an expensive alloying element, and excessive content will significantly increase production costs; 2. Phase change problem: Excessive W may cause unnecessary phase changes, such as the formation of unfavorable carbide structures, which may not be completely dissolved or excessively dissolved during heat treatment, thereby affecting the performance of the steel; 3. Impact on welding performance: Excessive microalloying elements may affect the welding performance of steel, resulting in welding cracks or other welding defects; 4. Poisoning effect: In some cases, excessive W may have a poisoning effect on the steelmaking process, affecting the dissolution and performance of other alloying elements;
[0039] At the end of refining, W element is added in batches at different positions evenly distributed on the surface of molten steel to ensure that W element can be evenly distributed in the molten steel. The single addition amount shall not exceed 0.10kg / t molten steel.
[0040] W element can be used as a microalloying element to form fine carbides or nitrides in molten steel. These precipitates can significantly improve the strength, toughness and wear resistance of steel. At the same time, fine carbides have a high melting point. These carbides can stably exist during the heat treatment of steel, thereby hindering the growth of grains at the microscopic level, resulting in grain boundary strengthening and precipitation strengthening. Therefore, it also helps to refine the grains during the cooling process, thereby improving the overall performance of the steel.
[0041] Step S4: VD vacuum degassing: After LF refining is completed, VD vacuum degassing operation is performed in a VD vacuum degassing furnace after heating;
[0042] Step S5: heating after VD vacuum degassing, and then casting using a large-taper steel ingot mold hanging ladle;
[0043] Step S6: After the steel ingot is demoulded, it is hot-transferred to forging. In order to ensure that the excellent structure of the outer layer of the roller blank is retained as much as possible when the BD roller is forged, the blank is forged by the near-net-shape forging method according to the hole-shaped finished product drawing. During forging, the machining allowance of the diameter and length of each hole must be considered and a certain amount of trimming must be reserved to prevent the final machining size from being affected due to mutual interference during hole processing, which may cause the product to be scrapped. The blank hole shape is similar to the finished product shape, ensuring that the single-side machining allowance of the blank in the hole position in the diameter direction is ≤25mm;
[0044] The near-net-shape forging process is as follows: design the forging drawing of the forging hole type according to the finished hole type. Since the finished diameter of the forged blank is small, a certain diameter allowance needs to be reserved as the initial diameter of the blank for forging when forging the finished product. The diameter allowance is ≤50mm, which is twice the single-side machining allowance in the diameter direction. This can effectively prevent the insufficient machining allowance at the end of the workpiece after engraving and drawing. Then, the blank length required for each forging hole type is calculated according to a specific algorithm, and the corresponding blank position is engraved one by one according to the calculation result, and then each hole type is forged using a special forging tool;
[0045] The near-net-shape forging method forging a blank specifically includes the following steps:
[0046] Step S601: designing a forging drawing of the forging pass according to the finished pass and classifying and designing the machining allowance of the pass: classifying and designing the machining allowance of the pass diameter and length according to the design requirements of the roll, such as the roll diameter, the total length of the roll and the shape of the finished corners;
[0047] Step S602: Designing the margin for the BD roller pass: When designing the BD roller pass, a certain margin needs to be reserved to ensure sufficient material removal to achieve the required finished product size and shape. The length margin is 35-40mm on one side, and the diameter margin is 15-25mm on one side. If the depth of the finished product pass is ≥100mm, the length margin and diameter margin can be increased by 10-15% to ensure the strength and dimensional accuracy of the finished product.
[0048] Step S603: Design the spacing distance between the BD roller pass profiles and the length of the groove side of the roller body edge: Design the spacing distance between the BD roller pass profiles to be ≥300 mm, and the length of the groove side of the roller body edge to be ≥220 mm;
[0049] Step S604: Determine the corresponding length of the blank at the hole position before the engraving card table and perform hole forging on the blank: In order to ensure that the hole can be forged correctly, first calculate the blank length required for engraving according to the principle of conservation of blank volume and weight, and then engrave at both ends of the corresponding position to determine the blank length. Preferably, the blank length required for engraving is ≥100mm, and finally the engraved blank is forged through the card table to form a hole concave file;
[0050] Step S7: Rough machining the blank according to the hole type finished product drawing and the heat treatment reserve principle: before the performance heat treatment, rough machining is performed according to the hole type finished product drawing and the heat treatment reserve principle required by the user, the processing amount after the heat treatment is reduced, and the excellent structure of the hardened layer is retained to the maximum extent. The blank at the rough machining hole position has a single-side reserve of 5-10mm in the diameter direction; the blank with the forged hole type can shorten the processing time and save the processing cost during rough machining, and more uniform and dense metal materials are retained at the corresponding position, which is very beneficial for obtaining a better hardened layer structure in the subsequent heat treatment, and effectively avoids the removal of a large amount of outer layer structure at the hole type due to machining. After the heat treatment, the hardness and structure at the bottom and side of the hole groove are greatly different, which affects the later use and service of the roller, thereby better improving the service life of the roller;
[0051] Step S8: Performance heat treatment: adopt differential temperature quenching + tempering, the quenching temperature is 850-1000℃, and the tempering temperature is 500-600℃, to ensure the high strength of the roller body and the high toughness of the roller neck after quenching, and obtain a uniform and consistent structure;
[0052] Step S9: After the heat treatment is completed, the forging is subjected to performance testing.
[0053] Example 1
[0054] The high-strength long roll BD roll provided in this embodiment is made of high-alloy pure steel, and its chemical composition is as follows: C: 0.55%, Si: 0.20%, Mn: 0.81%, Cr: 0.70%, Ni: 1.69%, Mo: 0.30%, W: 0.11%, Cu: 0.20%, [H]: 1.2ppm, [O]: 10ppm, [N]: 63ppm, P: 0.015, S: 0.005%, and the remainder is Fe and unavoidable impurities.
[0055] The preparation method of the high-strength long roll BD roll comprises the following steps:
[0056] Step S1: Select the furnace charge, use scrap steel, pig iron and alloy materials: do not allow non-pure furnace charge to enter the furnace, the residual elements of scrap steel, pig iron and alloy materials must meet the requirements of the chemical composition of the finished product, especially control the harmful elements P, Sn and Sb that affect the performance;
[0057] Step S2: Oxidation furnace smelting: The molten steel is initially smelted by electric arc furnace oxidation method; the end point before tapping is guaranteed to be 0.007%;
[0058] Step S3: LF refining: After the molten steel is smelted, it is transferred to the LF refining furnace. The LF refining furnace should be cleaned before use, without residual steel and slag. Slag should be strictly prevented during the whole process of steel tapping. White slag is operated during the whole process of LF refining. Alloy materials and micro-alloy materials are added in batches according to the target composition requirements, the refining time is extended, the slag making batches are increased, the purity of the molten steel is improved, and the harmful elements are ensured to meet the process requirements;
[0059] At the end of refining, ferrotungsten is added in batches according to the alloy amount of 0.2kg / t molten steel added at a time. According to the diameter of the refining ladle, ferrotungsten is added at no less than 5 locations to ensure uniform distribution of the alloy material. Ferrotungsten is added in 5 times in total.
[0060] Step S4: VD vacuum degassing: After LF refining is completed, VD vacuum degassing operation is performed in a VD vacuum degassing furnace after heating;
[0061] Step S5: heating after VD vacuum degassing, and then casting using a large-taper steel ingot mold hanging ladle;
[0062] Step S6: After the steel ingot is demoulded, it is hot-transferred to forging. In order to maximize the retention of the excellent structure of the outer layer of the roll blank when the BD roll is forged, the blank is forged by a near-net-shape forging method. The blank hole shape is similar to the finished product shape, and the blank single-side machining allowance at the hole position is ensured to be 15 mm.
[0063] Step S7: Rough machining according to the hole type finished product drawing and the principle of heat treatment allowance: Before the performance heat treatment, rough machining is performed according to the hole type finished product drawing and the principle of heat treatment allowance required by the user, reducing the amount of machining after heat treatment, maximizing the retention of the excellent structure of the hardened layer, and the rough machining single-side allowance is 5-10mm;
[0064] Step S8: Performance heat treatment: adopt differential temperature quenching + tempering, the quenching temperature is 860℃, and the tempering temperature is 590℃, to ensure the high strength of the roller body and the high toughness of the roller neck after quenching, and obtain a uniform and consistent structure;
[0065] Step S9: After the heat treatment is completed, the forging is subjected to performance testing.
[0066] The product was ultrasonically tested according to the JB / T3733-2017 flaw detection standard. The test results were qualified and met the user's requirements. The hardness of the roller body after quenching and tempering was 43-45HSD, which met the user's requirement of 40-50HSD.
[0067] Example 2
[0068] The high-strength long roll BD roll provided in this embodiment is different from that in embodiment 1 in that:
[0069] The chemical composition of the high-strength long roll BD roll is as follows: C: 0.52%, Si: 0.48%, Mn: 0.76%, Cr: 2.9%, Ni: 0.23%, Mo: 0.75%, W: 0.38%, Cu: 0.15%, [H]: 1.5ppm, [O]: 15ppm, [N]: 58ppm, P: 0.013, S: 0.007%, the remainder is Fe and unavoidable impurities; tungsten iron is added in batches at the end of refining according to the alloy amount of 0.7kg / t molten steel added in a single time; the quenching temperature is 990℃ and the tempering temperature is 520℃.
[0070] The product was ultrasonically tested according to the JB / T3733-2017 flaw detection standard, and the test results were qualified and met the user's requirements. The hardness of the roller body after quenching and tempering is 55-57HSD, which meets the user's requirement of 53-60HSD.
[0071] Comparative Example 1
[0072] The difference between this comparative example and Example 1 is that:
[0073] In step S3, at the end of refining, ferroniobium is added in batches according to the alloy amount of 0.1 kg / t molten steel added at a time, and ferroniobium is added at no less than 5 positions according to the diameter of the refining ladle to ensure uniform distribution of the alloy material. Ferroniobium is added in 5 times in total.
[0074] Comparative Example 2
[0075] The difference between this comparative example and Example 1 is that:
[0076] In step S6, the steel ingot is hot-transferred to forging after demoulding, and forged into a flat roll shape according to a conventional forging process. After forging, the single-side machining allowance of the blank is 25 mm.
[0077] Comparative Example 3
[0078] The difference between this comparative example and Example 1 is that:
[0079] A BD roller is provided, which is made of conventional alloy forged steel and has the following chemical composition: C: 0.58%, Si: 0.25%, Mn: 0.81%, Cr: 0.93%, Mo: 0.23%, Cu: 0.18%, [H]: 1.1ppm, [O]: 11ppm, [N]: 75ppm, P: 0.013%, S: 0.004%, and the remainder is Fe and unavoidable impurities.
[0080] The products of Example 1 and Example 2 and Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for mechanical properties, basic properties and ultrasonic flaw detection. The test results are shown in Table 1.
[0081] Table 1 Comparison results of product performance testing in the embodiment:
[0082]
[0083] It can be seen that the tensile strength and cross-sectional shrinkage rate of the roll neck of the BD roller forged according to the preparation method of the present invention are greatly improved, and the impact energy is 1.5 times and 2.4 times that of the BD roller produced by the conventional process, respectively. The strength and toughness are significantly improved, so that the BD roller can better withstand loads and resist crack propagation during use, thereby extending its service life. The BD roller forged by the near-net-shape forging process has a working layer hardness drop of less than half of that of the conventional BD roller, and has higher mechanical properties, which improves the overall performance of the BD roller while extending its service life.
[0084] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application are within the scope of protection of the present invention.
Claims
1. A high-strength long roll BD roll, characterized in that: The chemical composition of the high-strength long roll BD roll is as follows: C: 0.4-0.7%, Si: 0.2-0.6%, Mn: 0.5-1.0%, Cr: 0.5-3.5%, Ni: 0.2-1.7%, Mo: 0.1-0.8%, W: 0.1-0.4%, Cu: ≤0.3%, [H]: ≤2ppm, [O]: ≤15ppm, [N]: ≤70ppm, P and S are both ≤0.025%, and the balance is Fe and unavoidable impurities.
2. A method for preparing a high-strength long roll BD roll, characterized in that: Forging the high-strength long roll BD roll described in claim 1 comprises the following steps: Step S1: Selecting furnace materials, using scrap steel, pig iron and alloy materials; Step S2: using an arc furnace oxidation method to perform primary smelting of molten steel, and ensuring that P≤0.01% is the end point before steel tapping; Step S3: The molten steel after primary refining is transferred to the LF refining furnace. The whole LF refining process is white slag operation. The alloy material and micro-alloy material are added in batches according to the chemical composition of the high-strength long roll BD roll; Step S4: After LF refining is completed, VD vacuum degassing operation is performed in a VD vacuum degassing furnace after heating; Step S5: heating after VD vacuum degassing, and then casting using a large-taper steel ingot mold hanging ladle; Step S6: After the steel ingot is demoulded, it is hot-transferred to forging, and the blank is forged by using the near-net-shape forging method according to the hole shape finished product drawing, and the single-side machining allowance of the blank in the diameter direction at the hole shape position is ≤25mm; Step S7: Rough machining the blank according to the hole pattern finished product drawing and the heat treatment allowance principle, and the blank at the rough machining hole position is made to have a single side allowance of 5-10 mm in the diameter direction; Step S8: Performance heat treatment: using differential temperature quenching + tempering, the quenching temperature is 850-1000°C, and the tempering temperature is 500-600°C; Step S9: After the heat treatment is completed, the forging is subjected to performance testing.
3. The method for preparing a high-strength long roll BD roll according to claim 2, characterized in that: In step S3, at the end of LF refining, W element is added in batches at different positions evenly distributed on the surface of molten steel, with a single addition amount not exceeding 0.10 kg / t molten steel, and the W content is between 0.1-0.4%.
4. The method for preparing a high-strength long roll BD roll according to claim 3, characterized in that: The near-net-shape forging method in step S6 comprises the following steps: Step S601: designing a forging drawing of the forging pass according to the finished pass and classifying and designing the machining allowance of the pass: classifying and designing the machining allowance of the pass diameter and length according to the roll body diameter, the total length of the roll and the shape of the finished corner; Step S602: Designing the margin reserve of the BD roller pass; Step S603: designing the spacing distance of the BD roller pass profile and the length of the groove side of the roller body edge; Step S604: Determine the corresponding length of the blank at the hole position before the imprinting station and perform hole forging on the blank.
5. The method for preparing a high-strength long roll BD roll according to claim 4, characterized in that: In step S602, the length margin of the BD roller pass is designed to be 35-40 mm on one side, and the diameter margin is 15-25 mm on one side. When the depth of the finished pass is ≥100 mm, the length margin and the diameter margin are both increased by 10-15%.
6. The method for preparing a high-strength long roll BD roll according to claim 5, characterized in that: In step S603, the spacing distance between the BD roller pass profiles is designed to be ≥300 mm, and the length of the groove side of the roller body edge is ≥220 mm.
7. The method for preparing a high-strength long roll BD roll according to claim 6, characterized in that: In step S604, the blank length required for engraving is first calculated based on the principle of conservation of blank volume and weight, and then the blank length is determined by engraving at both ends of the corresponding position. Finally, the engraved blank is forged through a card table to form a hole-shaped concave file.
8. The method for preparing a high-strength long roll BD roll according to claim 7, characterized in that: The blank length required for engraving is ≥100mm.