Ceramic composite wave-absorbing coating with high temperature resistance as well as preparation method and application of ceramic composite wave-absorbing coating
Through ceramic composite wave absorbing coating, air spraying technology and high-temperature resistant inorganic binders, the problems of existing wave absorbing coating failure and corrosion resistance at high temperatures are solved, and efficient stealth in aerospace and other fields are achieved and durability improvement.
Patent Information
- Application Number
- CN202410941517.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
The existing absorbent coating fails in high temperature environments and has poor corrosion resistance, which cannot meet the needs of high temperature and complex environments in aerospace and other fields.
Using ceramic composite wave absorbing coating, including radar bonding layer and radar wave absorbing layer, prepared by air spraying technology, Al2O3 powder, Sm0.9Sr0.1Al0.5Co0.5O3 powder and aluminum dihydrogen phosphate adhesive are used to combine with resistance High temperature inorganic binder forms a stable ceramic composite coating.
Excellent electromagnetic wave absorption performance above 600°C is achieved, adhesion, high-temperature oxidation resistance, thermal shock and corrosion resistance are improved, and the durability of the coating is enhanced.
Smart Images

Figure CN118880217A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of absorbing materials, and in particular relates to a high-temperature resistant ceramic composite absorbing coating and a preparation method and application thereof. Background Art
[0002] Absorbing materials refer to a type of material that can absorb electromagnetic wave energy projected onto its surface, or convert electromagnetic wave energy into heat or other forms of energy through electromagnetic loss of the material. It is mainly divided into structural absorbing materials and coated absorbing materials. Compared with the shortcomings of structural absorbing materials (such as radar wave layer materials, absorbing interlayer materials, high-temperature stealth composite materials, etc.) with complex design and application, coated absorbing materials have become the mainstream development trend of absorbing materials due to their advantages of not changing the appearance and structure of the substrate and easy application and maintenance.
[0003] Among them, the coating type absorbing material refers to a functional coating that is coated on the surface of the substrate through a certain structural design to make it have the ability to absorb waves. Its main performance depends on the absorber material used. The widely used absorbing coatings are mainly magnetic loss materials, mainly including ferrite materials, carbonyl iron powder materials, etc. The characteristics of this type of coating are good absorbing performance at room temperature or low temperature, but when the temperature exceeds the Curie point of the material, it will partially or even completely lose its absorbing performance, that is, it cannot play the stealth function in a high temperature environment; at the same time, because most of the existing coatings contain metal powders such as iron powder, copper powder or aluminum powder, they cannot solve the corrosion resistance problem.
[0004] As we all know, radar-absorbing coating is an important means to achieve radar stealth. However, in recent years, with the continuous breakthroughs in science and technology in my country, the fields of aviation and aerospace technology have achieved rapid development. The most typical example is that the flight speeds of various aircraft are getting faster and faster, and there are many high-temperature parts directly exposed to radar waves, such as the nose cone, wings, and tail nozzles of high-speed aircraft. In order to improve their survivability, the stealth of these parts urgently needs high-temperature resistant (above 600°C) radar-absorbing coatings. Moreover, high-temperature radar-absorbing coatings must withstand severe thermal shock during rapid temperature rise and fall during service, accompanied by the erosion of high-speed airflow and strong mechanical vibration. In addition, they may sometimes face humid and acid rain environments. The above harsh service environment requires that the radar-absorbing coating not only has excellent high-temperature radar-absorbing performance, but also has good thermal shock resistance, high adhesion, and strong corrosion and oxidation resistance, thereby improving the durability of the coating.
[0005] In view of this, this invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a high-temperature resistant ceramic composite absorbing coating and a preparation method and application thereof, so as to solve the problems that the existing absorbing coating has poor mechanical properties and unsatisfactory absorbing effect under various complex environments such as high temperature, vibration, acid rain, etc. The ceramic composite absorbing coating provided by the present invention is mainly prepared by air spraying technology, the preparation method is stable and controllable, and the prepared ceramic composite absorbing coating still has the advantages of excellent high-temperature absorbing performance, adhesion performance, high-temperature oxidation resistance, thermal shock performance and corrosion resistance under various complex environments.
[0007] The purpose of the present invention is to be solved by the following technical solutions:
[0008] On the one hand, the present invention provides a ceramic composite absorbing coating with high temperature resistance, comprising a radar bonding layer and a radar absorbing layer sequentially arranged on the surface of a metal substrate from the inside to the outside;
[0009] Wherein, the radar absorbing layer includes Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder, and the Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The mass ratio between O3 powder and aluminum dihydrogen phosphate binder is 1:(1-2):(2.5-3.5).
[0010] Furthermore, the radar bonding layer is a NiCoCrAlY bonding layer, and the radar bonding layer is prepared by plasma spraying technology, and its thickness is 85μm to 115μm.
[0011] Furthermore, the radar absorbing layer is prepared by air spraying technology and has a thickness of 1.3 mm to 1.4 mm.
[0012] On the other hand, the present invention provides a method for preparing the above-mentioned ceramic composite radar absorbing coating, characterized in that it specifically comprises the following steps:
[0013] Step 1: Substrate pretreatment: sandblasting the metal substrate to remove oxides and impurities on the surface of the metal substrate;
[0014] Step 2: preparing a radar bonding layer: using plasma spraying technology to prepare a radar bonding layer on a metal substrate after sandblasting;
[0015] Step 3: Prepare radar absorbing coating: weigh Al2O3 powder, Sm 0.9 Sr 0.1Al 0.5 Co 0.5 The O3 powder and the aluminum dihydrogen phosphate binder are mixed evenly to obtain the radar absorbing coating;
[0016] Step 4: Prepare a ceramic composite absorbing coating: Use air spraying technology to evenly spray the radar absorbing coating obtained in step 3 on the radar bonding layer prepared in step 2, and after curing and heat treatment, a high-temperature resistant ceramic composite absorbing coating is formed.
[0017] Furthermore, in step 1, the roughness of the surface of the metal substrate after sandblasting should be 5 μm to 15 μm, and the flatness of the surface of the metal substrate after sandblasting should be ≤1.0 mm.
[0018] Furthermore, the Al2O3 powder is of analytical grade, and the particle size of the Al2O3 powder is ≤5 μm;
[0019] The Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high temperature solid phase sintering method, and its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder, and the mass ratio between the raw materials is: Sm2O3 powder: SrCO3 powder: Al2O3 powder: Co3O4 powder = 10: 1: 1.5 ~ 2: 2 ~ 2.5;
[0020] The solid content of the aluminum dihydrogen phosphate binder is 20wt% to 30wt%.
[0021] Furthermore, the Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 When mixing O3 powder and aluminum dihydrogen phosphate binder, first use a spatula to stir and mix manually until there is no precipitation, and then use a homogenizer to further mix until the mixture is uniform;
[0022] The process parameters of the homogenizer during mixing are set as follows: the rotation speed is set to 1500r / min to 2000r / min, and the mixing time is set to 3min to 5min.
[0023] Furthermore, in step 4, when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the set thickness, and then heat treatment is performed;
[0024] Wherein, during the air spraying, the weight gain of a single spraying is 10g to 20g;
[0025] The heat treatment system is: heating the cured metal substrate from room temperature to 340° C. to 360° C. and keeping the temperature for 25 min to 35 min, and finally air cooling to room temperature.
[0026] In a third aspect, the present invention provides an aircraft, comprising a metal substrate and a ceramic composite absorbing coating as described above formed on the surface of the metal substrate or a ceramic composite absorbing coating prepared by the preparation method as described above.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The ceramic composite absorbing coating provided by the present invention mainly consists of a radar bonding layer and a radar absorbing layer. The radar bonding layer is used to match the thermal expansion coefficient between the substrate and the radar absorbing layer to improve the thermal shock resistance. The radar absorbing layer directly gives the coating radar stealth performance. The radar bonding layer is a NiCoCrAlY bonding layer, and the radar absorbing layer is composed of Al2O3 powder and Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder are used, and when the coating of the radar absorbing layer finally forms a ceramic composite absorbing coating on the metal substrate, it is carried out by air spraying and curing alternately and repeatedly, which is not only convenient for preparation, but also easy to control the thickness of the coating. The ceramic composite absorbing coating finally prepared has excellent high-temperature absorbing performance, adhesion performance, high-temperature oxidation resistance, thermal shock performance and corrosion resistance. At the same time, the present invention also has the following advantages:
[0029] First, the raw materials used in the present invention can be directly obtained from the market or obtained through simple processing, and the preparation process is safe and controllable, which is conducive to large-scale industrial production and application;
[0030] Second, the wave absorbing agent used in the present invention is a ceramic wave absorbing agent, which is not easy to undergo phase change or decomposition at a high temperature of 900°C, so that the finally formed wave absorbing coating still maintains excellent electromagnetic wave absorbing performance even at above 600°C. Therefore, the ceramic composite wave absorbing coating of the present invention has a good application value in the field of high-temperature wave absorbing;
[0031] Third, the present invention uses a high temperature resistant inorganic binder to further enhance the bonding force between the final ceramic composite radar absorbing coating and the metal substrate, thereby improving the durability of the ceramic composite radar absorbing coating.
[0032] In summary, the ceramic composite absorbing coating provided by the present invention can not only be used in the fields of aerospace, military and defense, but can also reduce the reflection of radar waves, improve the stealth performance of aircraft, ships and equipment, and reduce the probability of being detected and identified. It can also be applied to laboratories, astronomical observations, radio measurements and scientific research fields to reduce electromagnetic interference and stray signals and improve the accuracy and precision of experiments and measurements. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0035] Figure 1 is a flow chart of the method for preparing the ceramic composite radar absorbing coating of the present invention;
[0036] Figure 2 It is a reflectivity curve diagram of the ceramic composite absorbing coating prepared in Example 2 of the present invention at different temperatures. DETAILED DESCRIPTION
[0037] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples consistent with some aspects of the present invention as detailed in the appended claims.
[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0039] The present invention provides a high temperature resistant ceramic composite absorbing coating, comprising a radar bonding layer and a radar absorbing layer which are sequentially arranged on the surface of a metal substrate from the inside to the outside. The radar bonding layer is a NiCoCrAlY bonding layer, which is prepared on the metal substrate by plasma spraying technology and has a thickness of (100±15) μm; the radar absorbing layer comprises Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder, and Al2O3 powder, Sm 0.9 Sr 0.1Al 0.5 Co 0.5 The mass ratio of O3 powder to aluminum dihydrogen phosphate binder is 1:(1-2):(2.5-3.5). During the specific forming process, the three powders need to be mixed into a coating first, and then the coating is applied to the radar bonding layer through air spraying technology and formed into a radar absorbing layer after curing and heat treatment. The thickness of the coating is 1.3mm-1.4mm.
[0040] See also Figure 1 The present invention also provides a method for preparing the above ceramic composite radar absorbing coating, which specifically comprises the following steps:
[0041] Step 1: Substrate pretreatment: sandblasting the metal substrate to remove oxides and impurities on the surface of the metal substrate;
[0042] Specifically, the roughness of the surface of the metal substrate after sandblasting should be 5 μm to 15 μm, and the flatness of the surface of the metal substrate after sandblasting should be ≤1.0 mm.
[0043] Step 2: preparing a radar bonding layer: using plasma spraying technology to prepare a radar bonding layer on a metal substrate after sandblasting;
[0044] Specifically, the radar bonding layer of the present invention is a NiCoCrAlY bonding layer, and its thickness is 85 μm to 115 μm.
[0045] Step 3: Prepare radar absorbing coating: weigh Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The O3 powder and the aluminum dihydrogen phosphate binder are mixed evenly to obtain the radar absorbing coating;
[0046] Specifically, the Al2O3 powder of the present invention is analytically pure, and the particle size of the Al2O3 powder is ≤5 μm; Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high-temperature solid-phase sintering method. Its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder, and the mass ratio between the raw materials is: Sm2O3 powder: SrCO3 powder: Al2O3 powder: Co3O4 powder = 10:1: 1.5~2:2~2.5; the solid content of aluminum dihydrogen phosphate binder is 20wt%~30wt%.
[0047] Furthermore, Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co0.5 When mixing O3 powder and aluminum dihydrogen phosphate binder, first stir and mix manually with a spatula until there is no precipitation, and then use a homogenizer to further mix until the mixture is uniform; wherein, the process parameters of the homogenizer during mixing are set as follows: the speed is set to 1500r / min~2000r / min, and the mixing time is set to 3min~5min.
[0048] Step 4: Prepare a ceramic composite absorbing coating: Use air spraying technology to evenly spray the radar absorbing coating obtained in step 3 on the radar bonding layer prepared in step 2, and after curing and heat treatment, a high-temperature resistant ceramic composite absorbing coating is formed.
[0049] Specifically, during curing, the curing equipment used is a resistance furnace or a high-temperature oven with a temperature difference of ≤15°C. The specific curing process is as follows:
[0050] First, cure at room temperature for ≥10 minutes until the surface is dry; then use the curing equipment to heat from room temperature to 75℃~85℃ for the first time and keep it warm for 8min~12min. After the first insulation, heat it for the second time to 140℃~160℃ and keep it warm for 8min~12min. After the second insulation, heat it for the third time to 290℃~310℃ and keep it warm for 4min~6min. Finally, after the curing equipment cools down to ≤100℃, take out the metal substrate and cool it down to room temperature naturally.
[0051] It should be noted that when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the set thickness, and then heat treatment is carried out; among them, when air spraying, generally a single spraying increases the weight by 10g to 20g per square meter; the heat treatment system is: the cured metal substrate is heated from room temperature to 340℃ to 360℃ and kept warm for 25min to 35min, and finally air-cooled to room temperature.
[0052] In order to further verify the efficacy of the ceramic composite radar absorbing coating of the present invention, the inventors conducted the following specific experiments:
[0053] Example 1
[0054] The ceramic composite radar absorbing coating provided by the embodiment of the present invention comprises a radar bonding layer and a radar radar absorbing layer which are sequentially arranged on the surface of a metal substrate from the inside to the outside.
[0055] The radar bonding layer is a NiCoCrAlY bonding layer, which is prepared by plasma spraying technology and has a thickness of 110μm. The radar absorbing layer is prepared by air spraying technology, including Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5O3 powder and aluminum dihydrogen phosphate binder, and Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The mass ratio of O3 powder and aluminum dihydrogen phosphate binder is 1:1:2.5, and the thickness is 1.33 mm.
[0056] The specific preparation process of the ceramic composite radar absorbing coating mentioned in the embodiment of the present invention is as follows:
[0057] 1) Substrate pretreatment: Select a metal substrate with a specification of φ25.4mm*5mm and perform sandblasting on the metal substrate to remove oxides and impurities on the surface of the metal substrate;
[0058] 2) Preparing a radar bonding layer: using plasma spraying technology to spray a radar bonding layer on a metal substrate after sandblasting;
[0059] 3) Preparation of radar absorbing coating: Al2O3 powder and Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder are mixed evenly to obtain a radar absorbing layer coating;
[0060] 4) Preparation of ceramic composite absorbing coating: The radar absorbing coating obtained in step 3) is evenly sprayed on the radar bonding layer prepared in step 2) by air spraying technology, and after curing and heat treatment, a high temperature resistant ceramic composite absorbing coating is formed.
[0061] Wherein, in step 1), the roughness of the surface of the metal substrate after sandblasting is 10 μm, and the flatness of the surface of the metal substrate after sandblasting is ≤1.0 mm.
[0062] In step 2), the thickness of the radar bonding layer is 100 μm.
[0063] In step 3), the Al2O3 powder is analytically pure and has a particle size of ≤5 μm; Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high-temperature solid-phase sintering method. Its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder in a mass ratio of 10:1:1.5:2; the solid content of dihydrogen aluminum phosphate binder is 20wt%.
[0064] Furthermore, Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5When mixing O3 powder and aluminum dihydrogen phosphate binder, first use a spatula to manually stir and mix until there is no precipitation, and then use a homogenizer to further mix the paint until the paint is mixed evenly; the process parameters of the homogenizer when mixing the paint are set as follows: the speed is set to 1500r / min, and the mixing time is set to 5min.
[0065] In step 4), during curing, the curing equipment used is a resistance furnace or a high temperature oven with a temperature difference of ≤15°C. The specific curing process is as follows:
[0066] First, cure at room temperature for 18 minutes until the surface is dry; then use the curing equipment to heat from room temperature to 75°C for the first time and keep it warm for 12 minutes. After the first insulation, heat it for the second time, heat it to 160°C for the second time and keep it warm for 8 minutes. After the second insulation, heat it for the third time, heat it to 290°C for the third time and keep it warm for 6 minutes. Finally, after the curing equipment cools down to 45°C, take out the metal substrate and cool it down to room temperature naturally.
[0067] Furthermore, when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the target thickness, and then heat treatment is performed. In the case of air spraying, the weight gain of a single spraying is 15g; the heat treatment system is: the cured metal substrate is heated from room temperature to 350°C and kept warm for 30 minutes, and finally air-cooled to room temperature.
[0068] Results test:
[0069] Six samples of the three batches of ceramic composite absorbing coatings (ceramic-alloy system) prepared in Example 1 of the present invention were randomly selected from each batch and marked for adhesion performance testing. The test was conducted using a pull-off method. The test equipment was a tensile testing machine. The test results are shown in Table 1 below:
[0070] Table 1
[0071] Sample 1# 2# 3# 4# 5# 6# average value One batch 15.25 16.25 15.20 13.89 15.02 13.69 14.88 Second batch 14.50 13.21 14.89 15.22 15.26 14.10 14.53 Three batches 12.56 12.58 13.85 15.67 15.48 14.42 14.09
[0072] The results in Table 1 show that the ceramic composite absorbing coating prepared by the present invention has excellent adhesion performance and batch stability, and the adhesion is ≥10MPa.
[0073] Example 2
[0074] The ceramic composite radar absorbing coating provided by the embodiment of the present invention comprises a radar bonding layer and a radar radar absorbing layer which are sequentially arranged on the surface of a metal substrate from the inside to the outside.
[0075] The radar bonding layer is a NiCoCrAlY bonding layer, which is prepared by plasma spraying technology and has a thickness of 115 μm. The radar absorbing layer is prepared by air spraying technology, including Al2O3 powder, Sm 0.9 Sr0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder, and Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The mass ratio of O3 powder and aluminum dihydrogen phosphate binder is 1:2:3.5, and the thickness is 1.4 mm.
[0076] The specific preparation process of the ceramic composite radar absorbing coating mentioned in the embodiment of the present invention is as follows:
[0077] 1) Substrate pretreatment: Select a metal substrate with a specification of φ180mm*80mm*5mm and perform sandblasting on the metal substrate to remove oxides and impurities on the surface of the metal substrate;
[0078] 2) Preparing a radar bonding layer: using plasma spraying technology to spray a radar bonding layer on a metal substrate after sandblasting;
[0079] 3) Preparation of radar absorbing coating: Al2O3 powder and Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder are mixed evenly to obtain a radar absorbing layer coating;
[0080] 4) Preparation of ceramic composite absorbing coating: The radar absorbing coating obtained in step 3) is evenly sprayed on the radar bonding layer prepared in step 2) by air spraying technology, and after curing and heat treatment, a high temperature resistant ceramic composite absorbing coating is formed.
[0081] Wherein, in step 1), the roughness of the surface of the metal substrate after sandblasting is 15 μm, and the flatness of the surface of the metal substrate after sandblasting is ≤1.0 mm.
[0082] In step 2), the thickness of the radar adhesive layer is 85 μm.
[0083] In step 3), the Al2O3 powder is analytically pure and has a particle size of ≤5 μm; Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high-temperature solid-phase sintering method. Its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder in a mass ratio of 10:1:2:2.5; the solid content of dihydrogen aluminum phosphate binder is 25wt%.
[0084] Furthermore, Al2O3 powder, Sm 0.9 Sr0.1 Al 0.5 Co 0.5 When mixing O3 powder and aluminum dihydrogen phosphate binder, first use a spatula to manually stir and mix until there is no precipitation, and then use a homogenizer to further mix the paint until the paint is evenly mixed; the process parameters of the homogenizer when mixing the paint are set as follows: the speed is set to 2000r / min, and the mixing time is set to 3min.
[0085] In step 4), during curing, the curing equipment used is a resistance furnace or a high temperature oven with a temperature difference of ≤15°C. The specific curing process is as follows:
[0086] First, cure at room temperature for 15 minutes until the surface is dry; then use the curing equipment to heat from room temperature to 80℃ for the first time and keep it warm for 10 minutes. After the first insulation, heat it for the second time, heat it to 150℃ for the second time and keep it warm for 10 minutes. After the second insulation, heat it for the third time, heat it to 300℃ for the third time and keep it warm for 5 minutes. Finally, after the curing equipment cools down to 20℃, take out the metal substrate and cool it down to room temperature naturally.
[0087] Furthermore, when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the target thickness, and then heat treatment is performed. In the case of air spraying, the weight gain of a single spraying is 10g; the heat treatment system is: the cured metal substrate is heated from room temperature to 340°C and kept warm for 35 minutes, and finally air-cooled to room temperature.
[0088] Results test:
[0089] The ceramic composite absorbing coating (ceramic-alloy system) prepared in Example 2 of the present invention was tested for reflection loss. The testing equipment was a vector network analyzer and the testing method was the bow method test. The test results are shown in FIG. Figure 2 shown. Figure 2 1 is the reflectivity curve of the ceramic composite absorbing coating at room temperature, 2 is the reflectivity curve of the ceramic composite absorbing coating at 600° C., and 3 is the reflectivity curve of the ceramic composite absorbing coating at 900° C. That is, the results show that the ceramic composite absorbing coating provided by the present invention has excellent reflectivity performance at high temperatures.
[0090] Example 3
[0091] The ceramic composite radar absorbing coating provided by the embodiment of the present invention comprises a radar bonding layer and a radar radar absorbing layer which are sequentially arranged on the surface of a metal substrate from the inside to the outside.
[0092] The radar bonding layer is a NiCoCrAlY bonding layer, which is prepared by plasma spraying technology and has a thickness of 85μm. The radar absorbing layer is prepared by air spraying technology, including Al2O3 powder, Sm0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder, and Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The mass ratio of O3 powder and aluminum dihydrogen phosphate binder is 1:1.5:3, and the thickness is 1.3 mm.
[0093] The specific preparation process of the ceramic composite radar absorbing coating mentioned in the embodiment of the present invention is as follows:
[0094] 1) Substrate pretreatment: Select a metal substrate with a specification of φ25.4mm*5mm and perform sandblasting on the metal substrate to remove oxides and impurities on the surface of the metal substrate;
[0095] 2) Preparing a radar bonding layer: using plasma spraying technology to spray a radar bonding layer on a metal substrate after sandblasting;
[0096] 3) Preparation of radar absorbing coating: Al2O3 powder and Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder are mixed evenly to obtain a radar absorbing layer coating;
[0097] 4) Preparation of ceramic composite absorbing coating: The radar absorbing coating obtained in step 3) is evenly sprayed on the radar bonding layer prepared in step 2) by air spraying technology, and after curing and heat treatment, a high temperature resistant ceramic composite absorbing coating is formed.
[0098] Wherein, in step 1), the roughness of the surface of the metal substrate after sandblasting is 5 μm, and the flatness of the surface of the metal substrate after sandblasting is ≤1.0 mm.
[0099] In step 2), the thickness of the radar adhesive layer is 115 μm.
[0100] In step 3), the Al2O3 powder is analytically pure and has a particle size of ≤5 μm; Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high-temperature solid-phase sintering method. Its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder in a mass ratio of 10:1:1.8:2.3; the solid content of dihydrogen aluminum phosphate binder is 30wt%.
[0101] Furthermore, Al2O3 powder, Sm0.9 Sr 0.1 Al 0.5 Co 0.5 When mixing O3 powder and aluminum dihydrogen phosphate binder, first use a spatula to manually stir and mix until there is no precipitation, and then use a homogenizer to further mix the paint until the paint is evenly mixed; the process parameters of the homogenizer when mixing the paint are set as follows: the speed is set to 1800r / min, and the mixing time is set to 4min.
[0102] In step 4), during curing, the curing equipment used is a resistance furnace or a high temperature oven with a temperature difference of ≤15°C. The specific curing process is as follows:
[0103] First, cure at room temperature for 16 minutes until the surface is dry; then use the curing equipment to heat from room temperature to 85℃ for the first time and keep it warm for 8 minutes. After the first insulation, heat it for the second time to 140℃ and keep it warm for 12 minutes. After the second insulation, heat it for the third time to 310℃ and keep it warm for 4 minutes. Finally, after the curing equipment cools down to 30℃, take out the metal substrate and cool it down to room temperature naturally.
[0104] Furthermore, when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the target thickness, and then heat treatment is performed. In the case of air spraying, the weight gain of a single spraying is 20g; the heat treatment system is: the cured metal substrate is heated from room temperature to 360°C and kept warm for 25 minutes, and finally air-cooled to room temperature.
[0105] Results test:
[0106] One of the three batches of ceramic composite absorbing coatings (ceramic-alloy system) prepared in Example 3 of the present invention was randomly selected from each batch and marked for high temperature oxidation resistance test. The test was conducted according to HB 5258-2000 standard. The test environment temperature was (600±10)°C. The test results are shown in Table 1 below:
[0107] Table 2
[0108]
[0109] The results in Table 2 show that the ceramic composite absorbing coating prepared in the embodiment of the present invention has excellent high-temperature oxidation resistance, and the oxidation resistance evaluation result is completely oxidation resistance level.
[0110] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0111] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A high temperature resistant ceramic composite radar absorbing coating, characterized in that: It includes a radar bonding layer and a radar absorbing layer which are sequentially arranged on the surface of the metal substrate from the inside to the outside; Wherein, the radar absorbing layer includes Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder and aluminum dihydrogen phosphate binder, and the Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The mass ratio between O3 powder and aluminum dihydrogen phosphate binder is 1:(1-2):(2.5-3.5).
2. The high temperature resistant ceramic composite radar absorbing coating according to claim 1, characterized in that: The radar bonding layer is a NiCoCrAlY bonding layer, and the radar bonding layer is prepared by plasma spraying technology, and the thickness thereof is 85 μm to 115 μm.
3. The high temperature resistant ceramic composite radar absorbing coating according to claim 1, characterized in that: The radar absorbing layer is prepared by air spraying technology and has a thickness of 1.3 mm to 1.4 mm.
4. A method for preparing a high temperature resistant ceramic composite radar absorbing coating according to any one of claims 1 to 3, characterized in that: The specific steps include: Step 1: Substrate pretreatment: sandblasting the metal substrate to remove oxides and impurities on the surface of the metal substrate; Step 2: preparing a radar bonding layer: using plasma spraying technology to prepare a radar bonding layer on a metal substrate after sandblasting; Step 3: Prepare radar absorbing coating: weigh Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 The O3 powder and the aluminum dihydrogen phosphate binder are mixed evenly to obtain the radar absorbing coating; Step 4: Prepare a ceramic composite absorbing coating: Use air spraying technology to evenly spray the radar absorbing coating obtained in step 3 on the radar bonding layer prepared in step 2, and after curing and heat treatment, a high-temperature resistant ceramic composite absorbing coating is formed.
5. The preparation method according to claim 4, characterized in that: In step 1, the roughness of the surface of the metal substrate after sandblasting should be 5 μm to 15 μm, and the flatness of the surface of the metal substrate after sandblasting should be ≤1.0 mm.
6. The preparation method according to claim 4, characterized in that: In step 3, the Al2O3 powder is of analytical grade and has a particle size of ≤5 μm; The Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 O3 powder is prepared by high temperature solid phase sintering method, and its raw materials are Sm2O3 powder, SrCO3 powder, Al2O3 powder and Co3O4 powder, and the mass ratio between the raw materials is: Sm2O3 powder: SrCO3 powder: Al2O3 powder: Co3O4 powder = 10: 1: 1.5 ~ 2: 2 ~ 2.5; The solid content of the aluminum dihydrogen phosphate binder is 20wt% to 30wt%.
7. The preparation method according to claim 4, characterized in that: The Al2O3 powder, Sm 0.9 Sr 0.1 Al 0.5 Co 0.5 When mixing O3 powder and aluminum dihydrogen phosphate binder, first use a spatula to stir and mix manually until there is no precipitation, and then use a homogenizer to further mix until the mixture is uniform; The process parameters of the homogenizer during mixing are set as follows: the rotation speed is set to 1500r / min to 2000r / min, and the mixing time is set to 3min to 5min.
8. The preparation method according to claim 4, characterized in that: In step 4, during the curing, the curing equipment used is a resistance furnace or a high temperature oven with a temperature difference of ≤15°C. The specific curing process is: First cure at room temperature for ≥10min until the surface is dry; Then use the curing equipment to heat up from room temperature to 75℃~85℃ for the first time and keep it warm for 8min~12min. After the first heat preservation is completed, heat up for the second time to 140℃~160℃ and keep it warm for 8min~12min. After the second heat preservation is completed, heat up for the third time to 290℃~310℃ and keep it warm for 4min~6min. Finally, after the curing equipment is cooled to ≤100°C, the metal substrate is taken out and cooled naturally to room temperature.
9. The preparation method according to claim 4, characterized in that: In step 4, when preparing the ceramic composite absorbing coating, air spraying and curing are repeated alternately until the thickness of the ceramic composite absorbing coating meets the set thickness, and then heat treatment is performed; Wherein, during the air spraying, the weight gain of a single spraying is 10g to 20g; The heat treatment system is: heating the cured metal substrate from room temperature to 340° C. to 360° C. and keeping the temperature for 25 min to 35 min, and finally air cooling to room temperature.
10. An aircraft, characterized in that: The invention comprises a metal substrate and a ceramic composite microwave absorbing coating as claimed in any one of claims 1 to 3 or a ceramic composite microwave absorbing coating prepared by the preparation method as claimed in any one of claims 4 to 9 formed on the surface of the metal substrate.