AR coating product and preparation method thereof
By using argon ion source bombardment cleaning and nitrogen ion source bombardment repair during the AR coating preparation process, the adhesion and density between film layers are enhanced, solving the problem of poor wear resistance of AR protective film and achieving better wear resistance and performance.
Patent Information
- Application Number
- CN202411008221.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-01
AI Technical Summary
Existing AR screen protectors have poor abrasion resistance, causing the screen to become unsmooth after a period of use, which affects the user experience.
In the process of preparing AR coating, argon ion source bombardment cleaning and nitrogen ion source bombardment repair are used to enhance the adhesion and density between film layers. Multilayer silicon dioxide and refractive layers are sputtered, and AF solution is evaporated after nitrogen ion source bombardment repair on the outermost layer.
The wear resistance of the coating is improved, ensuring the effectiveness of AR coating products. The surface of the coating is more delicate and smooth, and the adhesion and density between the coating layers are enhanced.
Smart Images

Figure HDA0004964185230000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of film coating technology, and in particular relates to an AR coating product and a preparation method thereof. Background Art
[0002] AR protective film has the advantages of anti-condensation, high penetration and easy cleaning, and is widely used in the fields of front and rear windshields of automobiles, photovoltaic industry, range hoods, large advertising screens, etc. However, the existing AR protective film has poor wear resistance. For example, after using AR-coated electronic products for a period of time, the screen begins to become rough and the resistance becomes larger. This is due to the poor wear resistance of the product surface (AR protective film); what's more, as the protective film wears, some functions of the electronic product surface will gradually disappear, affecting the customer's experience. Therefore, how to improve the wear resistance of the protective film has become a technical difficulty for further promotion of the product. Summary of the invention
[0003] In view of this, the present invention provides an AR coating product and a preparation method thereof. The coating material prepared according to the preparation method provided by the present invention has higher density, thereby improving its wear resistance.
[0004] In order to solve the above technical problems, the present invention provides a method for preparing an AR coating product, comprising the following steps:
[0005] After cleaning the substrate with argon gas, a plurality of silicon dioxide layers and refractive layers are sputtered on any surface of the substrate to obtain a primary AR coating product; the number of silicon dioxide layers is one more than the number of refractive layers; after any film layer is sputtered, an argon ion source is bombarded and cleaned;
[0006] The surface of the silicon dioxide layer of the primary AR coating product is repaired by nitrogen ion source bombardment and then evaporated with AF liquid to obtain the AR coating product.
[0007] Preferably, the conditions for the argon ion source bombardment cleaning include: a vacuum degree of 5×10 -4 ~2×10 -3 Pa, current is 0.5-5A, argon flow rate is 100-500sccm, duty cycle is 20-80%, and cleaning time is 5-20min.
[0008] Preferably, the refractive layer includes a Nb2O5 refractive layer, a Si3N4 refractive layer, a TiO2 refractive layer, an Al2O3 refractive layer or a ZrO2 refractive layer.
[0009] Preferably, the conditions for the nitrogen ion source bombardment repair include: a current of 0.5 to 1.5 A, a nitrogen flow rate of 50 to 500 sccm, a duty cycle of 50%, and a repair time of 5 to 20 min.
[0010] Preferably, the argon cleaning is performed in a vacuum coating chamber, and the conditions for the argon cleaning include: a vacuum degree of 5×10 -4 ~2×10 -3 pa, current is 0.5-5A, argon flow rate is 50-500sccm, duty cycle is 20-80%, and cleaning time is 3-10min.
[0011] Preferably, before the argon cleaning, the method further comprises: cleaning the substrate with a neutral or alkaline detergent and then air-drying the substrate.
[0012] Preferably, the thickness of any silicon dioxide layer is independently 5 to 80 nm.
[0013] Preferably, the thickness of any refractive layer is independently 5 to 120 nm.
[0014] Preferably, the substrate comprises glass, polyethylene terephthalate material, polypropylene material or polystyrene material.
[0015] The present invention also provides an AR coating product prepared by the preparation method described in the above technical solution.
[0016] The present invention provides a method for preparing an AR coating product, comprising the following steps: cleaning a substrate with argon gas and then sputtering a plurality of silicon dioxide layers and refractive layers on any surface thereof to obtain a primary AR coating product; the number of silicon dioxide layers is one layer more than the number of refractive layers; after sputtering of any film layer is completed, argon ion source bombardment cleaning is performed; the surface of the silicon dioxide layer of the primary AR coating product is repaired by nitrogen ion source bombardment and then AF liquid is evaporated to obtain the AR coating product. In the coating process, the present invention performs argon ion source bombardment cleaning on the surface of each film layer, thereby enhancing the adhesion and density between each film layer and thus improving the wear resistance of the coating; the present invention performs nitrogen ion source bombardment repair on the surface of the silicon dioxide layer of the primary AR coating product, which can improve the fineness and flatness of the film surface and further improve the wear resistance of the coating, thereby ensuring the use effect of the AR coating product. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the structure of the AR coated glass prepared in Examples 1 and 2. DETAILED DESCRIPTION
[0018] The present invention provides a method for preparing an AR coating product, comprising the following steps:
[0019] After cleaning the substrate with argon gas, a plurality of silicon dioxide layers and refractive layers are sputtered on any surface of the substrate to obtain a primary AR coating product; the number of silicon dioxide layers is one more than the number of refractive layers; after any film layer is sputtered, an argon ion source is bombarded and cleaned;
[0020] The surface of the silicon dioxide layer of the primary AR coating product is repaired by nitrogen ion source bombardment and then evaporated with AF liquid to obtain the AR coating product.
[0021] The present invention cleans the substrate with argon gas and then sputters several layers of silicon dioxide layers and refractive layers on any surface thereof to obtain a primary AR coating product. In the present invention, the substrate preferably includes glass, polyethylene terephthalate material (PET), polypropylene material (PP) or polystyrene material (PS), and more preferably glass. In the present invention, the number of silicon dioxide layers is one more than the number of refractive layers. The present invention has no special requirements for the number of silicon dioxide layers, and can be designed according to the needs of AR coating products. In the present invention, the thickness of any silicon dioxide layer is preferably independently 5 to 80 nm, more preferably 10 to 50 nm, and further preferably 26 to 35 nm. In the present invention, the refractive layer preferably includes a Nb2O5 refractive layer, a Si3N4 refractive layer, a TiO2 refractive layer, an Al2O3 refractive layer or a ZrO2 refractive layer, and more preferably a Nb2O5 refractive layer. In the present invention, the thickness of any refractive layer is preferably independently 5 to 120 nm, more preferably 14.7 to 50 nm, and more preferably 20 to 30 nm. In the present invention, when the thickness of the silicon dioxide layer or the refractive layer is greater than 50 nm, the present invention preferably performs sputtering twice or multiple times, and performs an argon ion source bombardment cleaning after each sputtering, so that the effect of the argon ion source bombardment cleaning can be ensured to better improve the density of the film layer. In the present invention, when the sputtering is performed multiple times, the thickness of the silicon dioxide layer or the refractive layer formed by each sputtering is preferably less than or equal to 50 nm, and more preferably 40 nm.
[0022] In the present invention, the argon cleaning preferably also includes: cleaning the substrate with a neutral or alkaline detergent and then air-drying. In the present invention, the pH value of the detergent is preferably 7-9. The present invention uses a detergent to clean the substrate, which can remove floating dust and oil stains on the surface of the substrate, ensure the cleanliness of the substrate, and thus improve the bonding strength between the coating and the substrate. In the present invention, the air-drying is preferably ion air-drying. In the present invention, the cleaned substrate is air-dried and then coated with a protective film to prevent the surface of the substrate from being contaminated again. In the present invention, the protective film is preferably removed before argon cleaning.
[0023] In the present invention, the argon cleaning is preferably performed in a vacuum coating chamber, and the conditions for the argon cleaning preferably include: a vacuum degree of 5×10 -4 ~2×10 -3 pa, current is 0.5-5A, argon flow rate is 50-500sccm, duty cycle is 20-80%, cleaning time is 3-10min, more preferably: vacuum degree is 2×10 -3pa, current is 0.5-5A, argon flow rate is 200-300sccm, duty cycle is 40-50%, and cleaning time is 3-4min.
[0024] In the present invention, the sputtering is preferably magnetron sputtering, and the conditions of the magnetron sputtering are preferably: argon flow rate is 250-350sccm, oxygen flow rate is 150-200sccm, and power is 10-20kw; more preferably, the argon flow rate is 300sccm, the oxygen flow rate is 160sccm, and the power is 15kw.
[0025] In the present invention, after any film layer is sputtered, argon ion source bombardment cleaning is performed. In the present invention, the conditions for the argon ion source bombardment cleaning preferably include: a vacuum degree of 5×10 -4 ~2×10 -3 Pa, the current is 0.5-5A, the argon flow rate is 100-500sccm, the duty cycle is 20-80%, and the cleaning time is 5-20min; more preferably, the vacuum degree is 1×10 -3 ~2×10 -3 Pa, current is 1-3A, argon flow rate is 275-400sccm, duty cycle is 50-70%, and cleaning time is 10-15min. The present invention limits the argon flow rate to 100-500sccm to ensure that the gas ionization amount improves the surface bombardment effect. If the flow rate is too small, the amount of gas ions will also be small. On the one hand, the uniformity after bombardment will be poor, and on the other hand, the effect is not obvious in the same time. However, if the gas flow rate is greater than 500sccm, the vacuum degree will be destroyed to a certain extent, the number of ions will increase, and the ions will also affect each other, thereby affecting the ion bombardment effect. The present invention performs argon ion source bombardment cleaning on each film layer through plasma irradiation bombardment. On the one hand, it removes peroxide molecules on the surface of the film layer and improves the bonding force between the film layers. On the other hand, it improves the density of the film layer and improves the wear resistance.
[0026] After obtaining the primary AR coating product, the present invention performs nitrogen ion source bombardment repair on the surface of the silicon dioxide layer of the primary AR coating product and then evaporates AF liquid to obtain the AR coating product. In the present invention, the conditions for the nitrogen ion source bombardment repair preferably include: current of 0.5-1.5A, nitrogen flow of 50-500sccm, duty cycle of 50%, and repair time of 5-20min; more preferably: current of 1A, nitrogen flow of 150-300sccm, duty cycle of 50%, and repair time of 10-15min. The present invention can correct the surface flatness of the film layer through nitrogen ion source bombardment repair; the surface of the film layer is relatively rough after Ar ion source bombardment, and then it is repaired by N2 ion source bombardment, the surface of the film layer is more delicate and smooth, which is more conducive to the reaction with AF liquid, and the wear resistance will be better.
[0027] In the present invention, the evaporation preferably includes a first evaporation, a second evaporation, a third evaporation and a fourth evaporation performed in sequence. In the present invention, the vacuum degree of the first evaporation is preferably <0.001Pa, more preferably 0.0005Pa; the current ratio is preferably 15-18%, more preferably 17%; the time is preferably 30-120s, more preferably 60-100s. In the present invention, the vacuum degree of the second evaporation is preferably <0.001Pa, more preferably 0.0005Pa; the current ratio is preferably 17-20%, more preferably 18%; the time is preferably 60-120s, more preferably 90s. In the present invention, the vacuum degree of the third evaporation is preferably <0.001Pa, more preferably 0.0005Pa; the current ratio is preferably 18-21%, more preferably 19%; the time is preferably 90-150s, more preferably 120s. In the present invention, the vacuum degree of the fourth evaporation is preferably less than 0.001 Pa, more preferably 0.0005 Pa; the current ratio is preferably 20-25%, more preferably 22%; the time is preferably 90-150 s, more preferably 150 s.
[0028] In the present invention, after the evaporation, the step preferably further comprises: leaving the evaporation product to stand for 3 hours before washing. In the present invention, the washing detergent is preferably a weak alkaline detergent for removing oil stains on the surface of the product.
[0029] In the present invention, the silicon dioxide layer and the refractive layer are different from the traditional direct cumulative sputtering. The plasma irradiation bombardment method is used in the middle, which not only cleans the peroxide impurities on the surface of the film layer, but also enhances the compactness of the film layer, so that the bonding force between the film layers is better. The combination of the outermost SiO2 surface and the AF layer further improves its wear resistance. In addition, the impurities of the film layer are reduced and the compactness is stronger, the hardness of the film layer is relatively higher, and the wear resistance of the product is also improved.
[0030] The present invention also provides an AR coating product prepared by the preparation method described in the above technical solution.
[0031] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0032] Example 1
[0033] Step 1: Clean the glass. Use a weak alkaline detergent to clean the glass, then air dry it and apply protective film on both sides.
[0034] Step 2: Put the cleaned glass on the magnetron sputtering coating machine and fix it. Tear off the protective film on the coating surface. Use an ion air gun to sweep the glass surface to prevent dust from absorbing on the surface. Close the door.
[0035] Step 3: Argon cleaning, the main body vacuum is evacuated to 0.002Pa, Ar is introduced, the flow rate is 275sccm, the current is 1A, the duty cycle is 50%, and the cleaning is carried out for 3min.
[0036] Step 4: Magnetron sputtering of silicon dioxide layer, Ar flow rate 300sccm, O2 flow rate 160sccm, power 15kw, deposition thickness 10nm.
[0037] Step 5: The silicon dioxide layer is cleaned by bombardment with an argon ion source, the vacuum is evacuated to 0.001 Pa, and bombardment is performed using an anode layer ion source with an Ar flow rate of 275 sccm, a current of 1 A, a duty cycle of 50%, and a time of 5 min.
[0038] Step 6: Magnetron sputtering of niobium pentoxide layer, Ar flow rate 400sccm, O2 flow rate 60sccm, power 20kw, deposition thickness 14.7nm.
[0039] Step 7: The niobium pentoxide layer is cleaned by bombardment with an argon ion source, the vacuum is evacuated to 0.001 Pa, and the anode layer is bombarded with an ion source, with an Ar flow rate of 275 sccm, a current of 1 A, a duty cycle of 50%, and a time of 5 min.
[0040] Step 8: Magnetron sputtering of silicon dioxide layer, Ar flow rate 300sccm, O2 flow rate 160sccm, power 15kw, deposition thickness 26nm.
[0041] Step 9: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 10 min.
[0042] Step 10: magnetron sputtering the first part of the niobium pentoxide layer, Ar flow rate 400sccm, O2 flow rate 60sccm, power 20kw, deposition thickness 40nm.
[0043] Step 11: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 15 min.
[0044] Step 12: magnetron sputtering the second niobium pentoxide layer, with an Ar flow rate of 400 sccm, an O2 flow rate of 60 sccm, a power of 20 kW, and a deposition thickness of 40 nm.
[0045] Step 13: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 15 min.
[0046] Step 14: magnetron sputtering the third niobium pentoxide layer, with an Ar flow rate of 400 sccm, an O2 flow rate of 60 sccm, a power of 20 kW, and a deposition thickness of 36.6 nm.
[0047] Step 15: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 15 min.
[0048] Step 16: magnetron sputtering the first part of the silicon dioxide layer, with an Ar flow rate of 300 sccm, an O2 flow rate of 160 sccm, a power of 15 kW, and a deposition thickness of 40 nm.
[0049] Step 17: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 15 min.
[0050] Step 18: magnetron sputtering the second part of the silicon dioxide layer, with an Ar flow rate of 300 sccm, an O2 flow rate of 160 sccm, a power of 15 kW, and a deposition thickness of 40 nm.
[0051] Step 19: Bombardment and cleaning with argon ion source, vacuum pumped to 0.001 Pa, bombarded with anode layer ion source, introduced Ar, flow rate 275 sccm, current 1 A, duty cycle 50%, time 15 min.
[0052] Step 20: Nitrogen ion source bombardment repair, nitrogen flow rate 150sccm, current 1A, duty cycle 50%, time 10min.
[0053] Step 21: AF evaporation, the vacuum of the main body is evaporated to 0.0005pa, and the evaporation process begins. The evaporation process is divided into four parts: the first evaporation: the current accounts for 17%, the time is 1min; the second evaporation: the current accounts for 18%, the time is 1min30s; the third evaporation: the current accounts for 19%, the time is 2min, and the fourth evaporation: the current accounts for 22%, the time is 2min30s; after standing for 3h, use a weak alkaline detergent to clean the surface oil and obtain AR coated glass.
[0054] Example 2
[0055] The AR coated glass was prepared according to the method of Example 1, except that the time of the nitrogen ion source bombardment repair in step 20 was 20 minutes.
[0056] Comparative Example 1
[0057] Step 1: Clean the glass. Use a weak alkaline detergent to clean the glass, then air dry it and apply protective film on both sides.
[0058] Step 2: Put the cleaned glass on the magnetron sputtering coating machine and fix it. Tear off the protective film on the coating surface. Use an ion air gun to sweep the glass surface to prevent dust from absorbing on the surface. Close the door.
[0059] Step 3: Argon cleaning, the main body vacuum is evacuated to 0.002Pa, Ar is introduced, the flow rate is 275sccm, the current is 1A, the duty cycle is 50%, and the cleaning is carried out for 3min.
[0060] Step 4: Magnetron sputtering of silicon dioxide layer, Ar flow rate 300sccm, O2 flow rate 160sccm, power 15kw, deposition thickness 10nm.
[0061] Step 5: magnetron sputtering of niobium pentoxide layer, Ar flow rate 400sccm, O2 flow rate 60sccm, power 20kw, deposition thickness 14.7nm.
[0062] Step 6: Magnetron sputtering of silicon dioxide layer, Ar flow rate 300sccm, O2 flow rate 160sccm, power 15kw, deposition thickness 26nm.
[0063] Step 7: magnetron sputtering of niobium pentoxide layer, Ar flow rate 400sccm, O2 flow rate 60sccm, power 20kw, deposition thickness 116.6nm.
[0064] Step 8: Magnetron sputtering of silicon dioxide layer, with Ar flow rate of 300 sccm, O2 flow rate of 160 sccm, power of 15 kW, and deposition thickness of 80 nm.
[0065] Step 9: Argon ion source bombardment cleaning, introduce Ar, flow rate 275sccm, current 1A, duty cycle 50%, time 3min.
[0066] Step 10: AF evaporation, the vacuum of the main body is evaporated to 0.0005pa, and the evaporation process begins. The evaporation process is divided into four parts: the first evaporation: the current accounts for 17%, the time is 1min; the second evaporation: the current accounts for 18%, the time is 1min30s; the third evaporation: the current accounts for 19%, the time is 2min, and the fourth evaporation: the current accounts for 22%, the time is 2min30s; after standing for 3h, use a weak alkaline detergent to clean the surface oil and obtain AR coated glass.
[0067] Figure 1 Schematic diagram of the structure of the AR coated glass prepared in Examples 1 and 2.
[0068] The properties of the coated glass prepared in Examples 1 to 2 and Comparative Example 1 were tested in the following manner: using 0000# steel wool and a 10*10 grinding head, the water drop angle was tested after grinding 1000 times under the conditions of a load of 1000g, a stroke of 50mm, and a speed of 40 times / min. The results are listed in Table 1.
[0069] Table 1 Properties of coated glass prepared in Examples 1-2 and Comparative Example 1
[0070] Example Water drop angle (°) Example 1 102 Example 2 106 Comparative Example 1 87
[0071] It can be seen from Table 1 that the water drop angle of the AR coated product prepared by the preparation method provided by the present invention is 102-106°, which is much larger than the product of Comparative Example 1, indicating that the AR coated product prepared by the preparation method provided by the present invention has good wear resistance.
[0072] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing an AR coating product, characterized in that: The following steps are involved: After cleaning the substrate with argon gas, a plurality of silicon dioxide layers and refractive layers are sputtered on any surface of the substrate to obtain a primary AR coating product; the number of silicon dioxide layers is one more than the number of refractive layers; after any film layer is sputtered, an argon ion source is bombarded and cleaned; The surface of the silicon dioxide layer of the primary AR coating product is repaired by nitrogen ion source bombardment and then evaporated with AF liquid to obtain the AR coating product.
2. The method for preparing the AR coating product according to claim 1, characterized in that: The conditions for the argon ion source bombardment cleaning include: a vacuum degree of 5×10 -4 ~2×10 -3 Pa, current is 0.5-5A, argon flow rate is 100-500sccm, duty cycle is 20-80%, and cleaning time is 5-20min.
3. The method for preparing the AR coated product according to claim 1 or 2, characterized in that: The refractive layer includes a Nb2O5 refractive layer, a Si3N4 refractive layer, a TiO2 refractive layer, an Al2O3 refractive layer or a ZrO2 refractive layer.
4. The method for preparing the AR coating product according to claim 1, characterized in that: The conditions for the nitrogen ion source bombardment repair include: a current of 0.5 to 1.5 A, a nitrogen flow rate of 50 to 500 sccm, a duty cycle of 50%, and a repair time of 5 to 20 minutes.
5. The method for preparing an AR coating product according to claim 1, characterized in that: The argon cleaning is performed in a vacuum coating chamber, and the conditions of the argon cleaning include: a vacuum degree of 5×10 -4 ~2×10 -3 pa, current is 0.5-5A, argon flow rate is 50-500sccm, duty cycle is 20-80%, and cleaning time is 3-10min.
6. The method for preparing an AR coated product according to claim 1 or 5, characterized in that: Before the argon cleaning, the method further comprises: cleaning the substrate with a neutral or alkaline detergent and then air drying.
7. The method for preparing an AR coating product according to claim 1, characterized in that: The thickness of any silicon dioxide layer is independently 5 to 80 nm.
8. The method for preparing an AR coating product according to claim 1, characterized in that: The thickness of any refractive layer is independently 5 to 120 nm.
9. The method for preparing an AR coating product according to claim 1, characterized in that: The substrate includes glass, polyethylene terephthalate material, polypropylene material or polystyrene material.
10. An AR coated product prepared according to the preparation method according to any one of claims 1 to 9.