Automatic production equipment and preparation method of titanium-based ruthenium iridium coating anode material

Through automated production equipment and processes, the health hazards and corrosion risks caused by manual operation in the production of titanium-based ruthenium iridium coated anode materials are solved, and efficient and safe production of anode materials is achieved, meeting the automatic control needs of product length and improving the Productivity.

CN118880299APending Publication Date: 2024-11-01FUJIAN ZHONGCABLE WIRE & CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909402.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

There is manual brushing and baking operation in the production of existing titanium-based ruthenium iridium coated anode materials, which leads to human health hazards and corrosion resistance risks of anode products, and the production length is limited, which cannot meet the needs of use.

Method used

An automated production equipment for titanium-based ruthenium iridium coated anode material was designed, including active wire laying frames, sandblasting machines, heated pickling tanks, dryers, automatic brushing machines, pipe sintering furnaces, etc., through the automated process The titanium wire is processed, brushed and sintered, and the PLC controller is used to realize automatic disconnection and disk cutting, reducing manual operation and precious metal usage.

Benefits of technology

It effectively reduces the harm of chemical materials to the human body, reduces the corrosion risk of anode products, improves work efficiency, meets the automatic control needs of product length, reduces the amount of precious metals, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880299A_ABST
    Figure CN118880299A_ABST
Patent Text Reader

Abstract

The invention discloses automatic production equipment and a preparation method of a titanium-based ruthenium iridium coating anode material. The automatic production equipment for the titanium-based ruthenium iridium coating anode material comprises an active pay-off rack, a small tension wire storage rack matched with the active pay-off rack, a sand blasting machine, a heating pickling tank, a water-free air dryer I, a water washing tank, a water-free air dryer II, a drying machine, a parallel wire guide wheel, a tractor front end, an automatic brushing device, a peristaltic pump loaded with a saturated solution and an oven, the device comprises a pipeline type sintering furnace, a tractor rear end, a meter counter, a take-up stand, a control cabinet with a PLC (Programmable Logic Controller), an automatic coiling machine and an air compressor. The whole process of preparing the titanium-based ruthenium iridium coating anode material is completed in an automatic production mode, manual brushing operation is not needed, therefore, harm of chemical materials to the human body can be effectively reduced, in addition, the length of the product can be automatically controlled according to production requirements, subsequent independent connection is not needed, and the production cost is reduced. Therefore, the corrosion risk of the anode product is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium-based ruthenium-iridium coating anode materials, and in particular to automated production equipment and a preparation method for titanium-based ruthenium-iridium coating anode materials. Background Art

[0002] At present, most of the manufacturers of ruthenium-iridium coated anode materials on the market use ruthenium (Ru), iridium (Ir), tantalum (Ta), and platinum (Pt) as the main metal materials. If the anode products of the electrode materials are to be prepared, in addition to the saturated salt solutions of the above metals, concentrated hydrochloric acid, tetrabutyl titanate, n-butanol, and isopropanol need to be added to obtain a mixed solution, and the anode products of the electrode materials can only be obtained by high-temperature sintering (oxidation-reduction reaction). In the prior art, most of them are manually brushed and baked, and each repetition time takes 15-20 minutes, and it needs to be repeated 10-15 times. The last sintering (oxidation-reduction reaction, not less than 60 minutes) can obtain qualified anode products of the electrode materials. The acid ester and alcohol products of the chemical industry themselves are very irritating to the human respiratory tract. If an inorganic mixed solvent is prepared and sintered at a high temperature, it needs to be manually operated repeatedly. If the human body is exposed to this environment for a long time and inhaled through the human respiratory tract, it will cause coma and poisoning to varying degrees in mild cases, and other organ failure in severe cases.

[0003] In addition, speaking of anode products in the field of electro-osmosis moisture-proofing of electrode materials, the longest length of products currently produced by domestic manufacturers can only be 157 meters, which requires 2-3 people to coordinate and complete. According to the field of electro-osmosis moisture-proofing, the normally matched electrode material anode products for most villa basements are about 278 meters. Then a disadvantage is that there will be a joint in the middle, which increases the risk of corrosion resistance of the anode product and cannot meet the use requirements. Based on the above situation, we have proposed an automated production equipment and preparation method for titanium-based ruthenium-iridium coated anode materials. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes an automated production equipment and preparation method for titanium-based ruthenium-iridium coating anode materials.

[0005] The present invention proposes an automated production equipment for titanium-based ruthenium-iridium coating anode materials, comprising an active pay-off frame, a small tension wire storage frame matched with the active pay-off frame, a sandblaster, a heated pickling tank, a first waterless air dryer, a water washing tank, a second waterless air dryer, a drying machine, a parallel wire wheel, a front end of a traction machine, an automatic brush coating device, a peristaltic pump loaded with a saturated solution, an oven, a pipeline sintering furnace, a rear end of a traction machine, a meter counter, a take-up frame, a control cabinet with a PLC controller, an automatic coiling machine and an air compressor, wherein the above equipment is arranged in sequence from left to right;

[0006] The two ends of the heated pickling tank are respectively provided with a sponge water retaining end and a water return port, and the two ends inside the heated pickling tank need to be installed with corrosion-resistant ceramic bearings and corrosion-resistant polytetrafluoroethylene wire wheels;

[0007] The parallel wire wheel can be placed as a turning point of the equipment according to the actual production site;

[0008] The front end of the traction machine is provided with a first wire wheel with a diameter of 600 mm and a groove depth of 20 mm, and the first wire wheel is used to guide the titanium wire;

[0009] The automatic brush coating device is provided with a processing material trough, the base size of the processing material trough is 20cm*35cm, the middle material trough is 2cm wide, filled with alcohol cotton, and 10 tooth strips are reserved at the front and rear ends of the processing material trough for fixing the thickness of the automatic brush coating;

[0010] The rear end of the traction machine is equipped with a reducer, a one-way bearing and a second wire wheel, the diameter of the second wire wheel is 600mm, and the groove depth is 20mm;

[0011] The take-up frame is provided with a 600mm-800mm wheel-type wire drum.

[0012] Preferably, the active pay-off stand is used for actively paying out the titanium wire, and the small tension wire storage stand is used for storing the titanium wire, and is used in conjunction with the active pay-off stand.

[0013] Preferably, the sandblasting machine uses an air compressor to spray out the silicon carbide inside the sandblasting machine to treat the surface of the titanium metal material.

[0014] Preferably, the heated pickling tank is filled with a pickling solution obtained by mixing oxalic acid with water, and the concentration of the pickling solution is 16.78 wt %.

[0015] The present invention also proposes an automated preparation method for a titanium-based ruthenium-iridium coating anode material, comprising the following steps:

[0016] S1: Through the cooperation of a small tension wire storage rack and an active wire pay-off rack, the titanium wire stored on the small tension wire storage rack can be paid out;

[0017] S2: During the wire laying process, when the titanium wire moves to the workstation of the sandblasting machine, the air compressor is used to spray silicon carbide in the sandblasting machine to treat the surface of the titanium wire passing through;

[0018] S3: heating the pickling solution in the heated pickling tank to 70°-100°, and after the treated titanium wire enters the heated pickling tank, immersing it in the pickling solution. The anti-corrosion ceramic bearing and the anti-corrosion polytetrafluoroethylene wire wheel in the heated pickling tank cooperate to allow the titanium wire to be fully immersed in the pickling solution for 40-50 minutes.

[0019] S4: The soaked titanium wire is removed from the heated pickling tank, and a waterless air dryer blows the soaked titanium wire dry. The blown-dry titanium wire enters the water washing tank, and the surface of the titanium wire is rinsed clean with deionized water.

[0020] S5: the rinsed titanium wire moves to the position of the waterless air dryer 2, the waterless air dryer 2 blows the deionized water on the surface of the titanium wire dry, and the dried titanium wire enters the drying machine with a temperature of 100°-150°, the drying machine dries the surface of the titanium wire for 1-15 minutes;

[0021] S6: The dried titanium wire is pulled into the processing material tank of the automatic brush coating device through the cooperation of the parallel wire wheel and the front end of the traction machine. The peristaltic pump loaded with saturated solution adjusts the discharge speed of the peristaltic pump according to the thickness of the required product, and the peristaltic pump sprays the saturated solution to brush the surface of the titanium wire;

[0022] S7: the titanium wire coated with the saturated solution is placed in an oven at a temperature of 380°-440° for baking for 5-10 minutes;

[0023] S8: The dried titanium wire enters into a tubular sintering furnace at a temperature of 380°-470° for sintering for 7-25 minutes;

[0024] S9: The sintered titanium wire is pulled through the rear end of the traction machine and pulled onto the meter. The meter measures the titanium wire passing through. At the same time, the measured titanium wire is wound and reeled by the take-up frame in cooperation with the wheel-type wire reel, and the wound and reeled titanium wire is reeled in cooperation with the automatic reeling machine.

[0025] S10: With the setting of the control cabinet with PLC controller, it can automatically cut off the line and stop after winding to the required length, thus completing the preparation of titanium-based ruthenium-iridium coated anode material.

[0026] Preferably, in S6, the saturated solution is a mixture of ruthenium trichloride (Ru), chloroiridic acid (Ir), tantalum chloride (Ta), tetrabutyl titanate, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid, and the preparation process of the saturated solution is as follows:

[0027] S601: soaking ruthenium trichloride in an n-butanol solution to prepare a first saturated salt solution;

[0028] S602: soaking tantalum chloride in isopropanol to obtain a second saturated salt solution;

[0029] S603: After the first saturated salt solution in S601 is completely dissolved, it is added to the second saturated salt solution in S602 to further obtain a third saturated salt solution;

[0030] S604: adding anhydrous ethanol and hydrochloric acid to the third saturated salt solution in S603 in sequence to obtain a fourth saturated salt solution;

[0031] S605: After the fourth saturated salt solution in S604 is fully stirred, tetrabutyl titanate is added to obtain a fifth saturated salt solution, and a saturated solution is obtained.

[0032] Preferably, in S601, the volume ratio of ruthenium trichloride, n-butanol solution and the first saturated salt solution is: 1: (2.2-7.3): (27:36), in S602, the volume ratio of tantalum chloride and isopropanol is: (0.5-0.6): (13:18), in S603, the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol and isopropanol in the third saturated salt solution is: 1: (0.5-0.6): (28-40): (15:20), in S604, the volume ratio of ruthenium trichloride in the fourth saturated salt solution is: 1: (0.5-0.6): (28-40): (15:20), The volume ratio of ruthenium, tantalum chloride, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid is 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5). In S605, the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol, isopropanol, anhydrous ethanol, hydrochloric acid and tetrabutyl titanate in the fifth saturated salt solution is 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5): (17-25).

[0033] Preferably, in S605, in the fifth saturated salt solution, the theoretical weight of ruthenium content is 4.6-5.5 times, the theoretical weight of tantalum content is 0.3-0.45 times, the theoretical weight of iridium content is 0.6-0.7 times, and the theoretical ratio of precious metal content is (2-7): (11-15).

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention completes the entire process of preparing the titanium-based ruthenium-iridium coated anode material by an automated production method, and does not require human brushing operations, thereby effectively reducing the harm of chemical materials to the human body. In addition, the length of the product can be automatically controlled according to production needs, and does not require subsequent separate connection, thereby reducing the risk of corrosion of the anode product and will not affect the service life of the product. While improving work efficiency, it reduces labor costs. In addition, the automated operation method saves the amount of precious metal mixed solution and meets usage requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The present invention provides a flow chart for preparing an automated production equipment for titanium-based ruthenium-iridium coating anode materials. DETAILED DESCRIPTION

[0037] The present invention will be further explained below in conjunction with specific embodiments.

[0038] Embodiment 1

[0039] Reference Figure 1 This embodiment proposes an automated production equipment for titanium-based ruthenium-iridium coated anode materials, including an active pay-off frame, a small tension wire storage frame matched with the active pay-off frame, a sandblaster, a heated pickling tank, a waterless air dryer 1, a water washing tank, a waterless air dryer 2, a drying machine, a parallel wire wheel, a front end of a traction machine, an automatic brush applicator, a peristaltic pump loaded with a saturated solution, an oven, a pipeline sintering furnace, a rear end of a traction machine, a meter, a take-up frame, a control cabinet with a PLC controller, an automatic coiling machine and an air compressor. The above equipment is arranged from left to right in sequence, wherein the active pay-off frame is used for actively paying off the titanium wire, the small tension wire storage frame is used for storing the titanium wire, and it is used in conjunction with the active pay-off frame, and the sandblaster sprays out the silicon carbide in the sandblaster through the air compressor to treat the surface of the titanium material;

[0040] The two ends of the heated pickling tank are respectively provided with a sponge water retaining end and a water return port, and the two ends of the heated pickling tank need to be installed with corrosion-resistant ceramic bearings and corrosion-resistant polytetrafluoroethylene wire wheels, wherein the heated pickling tank is filled with a pickling solution obtained by mixing oxalic acid with water, and the concentration of the pickling solution is 16.78wt%;

[0041] The parallel wire wheel can be placed as a turning point of the equipment according to the actual production site;

[0042] A first wire wheel with a diameter of 600 mm and a groove depth of 20 mm is provided at the front end of the traction machine, and the first wire wheel is used to guide the titanium wire;

[0043] The automatic brush coating machine is equipped with a processing trough. The base size of the processing trough is 20cm*35cm, the width of the middle trough is 2cm, and it is filled with alcohol cotton. 10 tooth strips are reserved at the front and rear ends of the processing trough to fix the thickness of the automatic brush coating.

[0044] The rear end of the traction machine is equipped with a reducer, a one-way bearing and a second wire pulley. The diameter of the second wire pulley is 600mm and the groove depth is 20mm.

[0045] The take-up frame is equipped with a 600mm-800mm wheel-type wire drum.

[0046] Embodiment 2

[0047] Reference Figure 1 This embodiment proposes an automated preparation method for a titanium-based ruthenium-iridium coating anode material, comprising the following steps:

[0048] S1: Through the cooperation of a small tension wire storage rack and an active wire pay-off rack, the titanium wire stored on the small tension wire storage rack can be paid out;

[0049] S2: During the wire laying process, when the titanium wire moves to the workstation of the sandblasting machine, the air compressor is used to spray silicon carbide in the sandblasting machine to treat the surface of the titanium wire passing through;

[0050] S3: heating the pickling solution in the heated pickling tank to 70°-100°, and after the treated titanium wire enters the heated pickling tank, immersing it in the pickling solution. The anti-corrosion ceramic bearing and the anti-corrosion polytetrafluoroethylene wire wheel in the heated pickling tank cooperate to allow the titanium wire to be fully immersed in the pickling solution for 40-50 minutes.

[0051] S4: The soaked titanium wire is removed from the heated pickling tank, and a waterless air dryer blows the soaked titanium wire dry. The blown-dry titanium wire enters the water washing tank, and the surface of the titanium wire is rinsed clean with deionized water.

[0052] S5: The rinsed titanium wire moves to the position of the waterless air dryer 2, and the waterless air dryer 2 blows the deionized water on the surface of the titanium wire dry. The dried titanium wire enters the drying machine with a temperature of 100°-150°, and the drying machine dries the surface of the titanium wire for 1-15 minutes. Because the titanium material will appear uneven after being polished by the sandblasting machine and the pickling tank etching, the waterless air dryer can only remove most of the water molecules on the surface, so the dryer needs to be dried again;

[0053] S6: The dried titanium wire is pulled into the processing material tank of the automatic brush coating device by cooperating with the parallel wire wheel and the front end of the traction machine. The peristaltic pump loaded with the saturated solution adjusts the discharge speed of the peristaltic pump according to the thickness of the required product, and the peristaltic pump sprays the saturated solution to brush the surface of the titanium wire; wherein the saturated solution is a mixture of ruthenium trichloride (Ru), chloroiridic acid (Ir), tantalum chloride (Ta), tetrabutyl titanate, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid, and the preparation process of the saturated solution is as follows:

[0054] S601: soaking ruthenium trichloride in a n-butanol solution to prepare a first saturated salt solution, wherein the volume ratio of ruthenium trichloride, the n-butanol solution and the first saturated salt solution is: 1:(2.2-7.3):(27:36);

[0055] S602: soaking tantalum chloride in isopropanol to obtain a second saturated salt solution, wherein the volume ratio of tantalum chloride to isopropanol is (0.5-0.6):(13:18);

[0056] S603: After the first saturated salt solution in S601 is completely dissolved, it is added into the second saturated salt solution in S602 to further obtain a third saturated salt solution, wherein the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol and isopropanol in the third saturated salt solution is: 1: (0.5-0.6): (28-40): (15:20);

[0057] S604: adding anhydrous ethanol and hydrochloric acid to the third saturated salt solution of S603 in sequence to obtain a fourth saturated salt solution, wherein the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid in the fourth saturated salt solution is 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5);

[0058] S605: After the fourth saturated salt solution in S604 is fully stirred, tetrabutyl titanate is added to obtain a fifth saturated salt solution, and a saturated solution is obtained, wherein the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol, isopropanol, anhydrous ethanol, hydrochloric acid and tetrabutyl titanate in the fifth saturated salt solution is: 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5): (17-25), and in the fifth saturated salt solution, the theoretical weight of ruthenium content is 4.6-5.5 times, the theoretical weight of tantalum content is 0.3-0.45 times, the theoretical weight of iridium content is 0.6-0.7 times, and the theoretical ratio of precious metal content is (2-7): (11-15);

[0059] S7: the titanium wire coated with the saturated solution is placed in an oven at a temperature of 380°-440° for baking for 5-10 minutes;

[0060] S8: The dried titanium wire enters into a tubular sintering furnace at a temperature of 380°-470° for sintering for 7-25 minutes;

[0061] S9: The sintered titanium wire is pulled through the rear end of the traction machine. The rear end of the traction machine is convenient for the use of multiple cycles of brushing the titanium wire. When the titanium wire is pulled onto the meter, the meter measures the titanium wire passing through, and reduces the loss by measuring the distance.

[0062] At the same time, the measured titanium wire is wound and reeled through the take-up frame and the wheel reel. The wheel reel can be customized according to the required number of meters of the product, and the wound and reeled titanium wire is reeled with the automatic reeling machine;

[0063] S10: With the setting of the control cabinet with PLC controller, it can automatically cut off the line and stop after winding to the required length, thus completing the preparation of titanium-based ruthenium-iridium coated anode material.

[0064] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An automated production equipment for titanium-based ruthenium-iridium coating anode materials, characterized in that: It includes an active pay-off rack, a small tension wire storage rack matched with the active pay-off rack, a sandblaster, a heated pickling tank, a waterless air dryer 1, a water washing tank, a waterless air dryer 2, a drying machine, a parallel wire wheel, a front end of a traction machine, an automatic brush applicator, a peristaltic pump loaded with a saturated solution, an oven, a pipeline sintering furnace, a rear end of a traction machine, a meter counter, a take-up rack, a control cabinet with a PLC controller, an automatic coiling machine and an air compressor. The above equipment is arranged in order from left to right; The two ends of the heated pickling tank are respectively provided with a sponge water retaining end and a water return port, and the two ends inside the heated pickling tank need to be installed with corrosion-resistant ceramic bearings and corrosion-resistant polytetrafluoroethylene wire wheels; The parallel wire wheel can be placed as a turning point of the equipment according to the actual production site; The front end of the traction machine is provided with a first wire wheel with a diameter of 600 mm and a groove depth of 20 mm, and the first wire wheel is used to guide the titanium wire; The automatic brush coating device is provided with a processing trough, the base size of the processing trough is 20cm*35cm, the width of the middle trough is 2cm, filled with alcohol cotton, and 10 tooth strips are reserved at the front and rear ends of the processing trough; The rear end of the traction machine is equipped with a reducer, a one-way bearing and a second wire wheel, the diameter of the second wire wheel is 600mm, and the groove depth is 20mm; The take-up frame is provided with a 600mm-800mm wheel-type wire drum.

2. The automated production equipment for titanium-based ruthenium-iridium coating anode materials according to claim 1, characterized in that: The active pay-off rack is used for actively paying out the titanium wire, and the small tension wire storage rack is used for storing the titanium wire, and is used in conjunction with the active pay-off rack.

3. The automated production equipment for titanium-based ruthenium-iridium coating anode materials according to claim 1, characterized in that: The sandblasting machine uses an air compressor to spray out the silicon carbide in the sandblasting machine to process the surface of the titanium metal material.

4. The automated production equipment for titanium-based ruthenium-iridium coating anode materials according to claim 1, characterized in that: The heated pickling tank is filled with a pickling solution obtained by mixing oxalic acid with water, and the concentration of the pickling solution is 16.78 wt %.

5. An automated preparation method for titanium-based ruthenium-iridium coating anode material, characterized in that: The following steps are involved: S1: Through the cooperation of a small tension wire storage rack and an active wire pay-off rack, the titanium wire stored on the small tension wire storage rack can be paid out; S2: During the wire laying process, when the titanium wire moves to the workstation of the sandblasting machine, the air compressor is used to spray silicon carbide in the sandblasting machine to treat the surface of the titanium wire passing through; S3: heating the pickling solution in the heated pickling tank to 70°-100°, and after the treated titanium wire enters the heated pickling tank, immersing it in the pickling solution. The anti-corrosion ceramic bearing and the anti-corrosion polytetrafluoroethylene wire wheel in the heated pickling tank cooperate to allow the titanium wire to be fully immersed in the pickling solution for 40-50 minutes. S4: The soaked titanium wire is removed from the heated pickling tank, and a waterless air dryer blows the soaked titanium wire dry. The blown-dry titanium wire enters the water washing tank, and the surface of the titanium wire is rinsed clean with deionized water. S5: the rinsed titanium wire moves to the position of the waterless air dryer 2, the waterless air dryer 2 blows the deionized water on the surface of the titanium wire dry, and the dried titanium wire enters the drying machine with a temperature of 100°-150°, the drying machine dries the surface of the titanium wire for 1-15 minutes; S6: The dried titanium wire is pulled into the processing material tank of the automatic brush coating device through the cooperation of the parallel wire wheel and the front end of the traction machine. The peristaltic pump loaded with saturated solution adjusts the discharge speed of the peristaltic pump according to the thickness of the required product, and the peristaltic pump sprays the saturated solution to brush the surface of the titanium wire; S7: the titanium wire coated with the saturated solution is placed in an oven at a temperature of 380°-440° for baking for 5-10 minutes; S8: The dried titanium wire enters into a tubular sintering furnace at a temperature of 380°-470° for sintering for 7-25 minutes; S9: The sintered titanium wire is pulled through the rear end of the traction machine and pulled onto the meter. The meter measures the titanium wire passing through. At the same time, the measured titanium wire is wound and reeled by the take-up frame in cooperation with the wheel-type wire reel, and the wound and reeled titanium wire is reeled in cooperation with the automatic reeling machine. S10: With the setting of the control cabinet with PLC controller, it can automatically cut off the line and stop after winding to the required length, thus completing the preparation of titanium-based ruthenium-iridium coated anode material.

6. The automated preparation method of a titanium-based ruthenium-iridium coating anode material according to claim 5, characterized in that: In S6, the saturated solution is a mixture of ruthenium trichloride (Ru), chloroiridic acid (Ir), tantalum chloride (Ta), tetrabutyl titanate, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid, and the preparation process of the saturated solution is as follows: S601: soaking ruthenium trichloride in an n-butanol solution to prepare a first saturated salt solution; S602: soaking tantalum chloride in isopropanol to obtain a second saturated salt solution; S603: After the first saturated salt solution in S601 is completely dissolved, it is added to the second saturated salt solution in S602 to further obtain a third saturated salt solution; S604: adding anhydrous ethanol and hydrochloric acid to the third saturated salt solution in S603 in sequence to obtain a fourth saturated salt solution; S605: After the fourth saturated salt solution in S604 is fully stirred, tetrabutyl titanate is added to obtain a fifth saturated salt solution, and a saturated solution is obtained.

7. The automated preparation method of a titanium-based ruthenium-iridium coating anode material according to claim 6, characterized in that: In S601, the volume ratio of ruthenium trichloride, n-butanol solution and the first saturated salt solution is: 1: (2.2-7.3): (27:36), in S602, the volume ratio of tantalum chloride and isopropanol is: (0.5-0.6): (13:18), in S603, the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol and isopropanol in the third saturated salt solution is: 1: (0.5-0.6): (28-40): (15:20), in S604, the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol and isopropanol in the fourth saturated salt solution is: 1: (0.5-0.6): (28-40): (15:20), The volume ratio of tantalum chloride, n-butanol, isopropanol, anhydrous ethanol and hydrochloric acid is 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5). In S605, the volume ratio of ruthenium trichloride, tantalum chloride, n-butanol, isopropanol, anhydrous ethanol, hydrochloric acid and tetrabutyl titanate in the fifth saturated salt solution is 1: (0.5-0.6): (28-40): (15-20): (3.5-4.8): (1.7-3.5): (17-25).

8. The automated preparation method of a titanium-based ruthenium-iridium coating anode material according to claim 6, characterized in that: In the fifth saturated salt solution in S605, the theoretical weight of ruthenium content is 4.6-5.5 times, the theoretical weight of tantalum content is 0.3-0.45 times, the theoretical weight of iridium content is 0.6-0.7 times, and the theoretical ratio of precious metal content is (2-7): (11-15).