Preparation method of nano CoMoO4 / EG catalyst
By preparing nano CoMoO4 catalyst on expanded graphite, the problems of high cost and insufficient dispersion of precious metal catalysts are solved, and efficient electrocatalytic hydrogen evolution performance and stability are achieved, showing excellent application prospects in the field of electrocatalysis.
Patent Information
- Application Number
- CN202411055043.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-01
AI Technical Summary
The existing precious metal-based catalysts are expensive and scarce, and the dispersion of transition metal oxide catalysts in carbon material support is insufficient, which limits its wide application in the field of electrocatalytic hydrogen evolution.
The nanoCoMoO4/EG catalyst was prepared by hydrothermal method using expanded graphite (EG) as a support. The CoMoO4 nanoparticles were uniformly dispersed by using the high specific surface area and good conductivity of EG, and their size was reduced to fully expose the active site.
The hydrogen evolution current density and stability of the catalyst were significantly improved, and the nano-CoMoO4/EG showed excellent hydrogen evolution reaction activity under alkaline conditions and maintained good performance in long-term cyclic voltammetry tests.
Smart Images

Figure CN118880378A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electrocatalytic hydrogen evolution materials, and in particular relates to a nano CoMoO 4 / EG catalyst preparation method. Background Art
[0002] Traditional fossil fuels use carbon as energy. During use, they emit a large amount of carbon dioxide into the atmosphere, destroying the carbon cycle balance in nature and posing a serious threat to the ecological environment. Therefore, the use of carbon-free energy is a prerequisite for the future new energy economy. Hydrogen is the lightest and most abundant element known to date. Using hydrogen as an energy carrier has extremely high energy density and the widest source of raw materials, meeting the carbon-free requirement. At present, precious metal-based materials (Pt, Ir and Ru-based) are widely used as water electrolysis catalysts, but the high cost and scarcity hinder the widespread application of precious metals in the field of catalysis. Transition metals (Co, Ni, Fe, Cu, Mo, etc.) are inexpensive and have abundant reserves, which has attracted great attention from researchers.
[0003] (Small 17(2021):202101312) Singh et al. prepared a Fe-Co-Oxide / Co@NC-mNS catalyst with a heterogeneous structure through a MOF-derived synthesis method, introduced defects and in-situ topological transformation of the electrocatalyst, and produced a heterogeneous structure of mixed metal oxides (hydroxides), which showed excellent bifunctional properties in HER and OER. (Chem.Eng.J.446(2022):137045) Shreyanka et al. synthesized transition metal-based 3D metal organic framework (MOF) materials (M-BTC, M: Cu, Co, Ni) with various structures by pulsed laser ablation in dimethylformamide, and showed excellent bifunctional electrocatalyst capabilities. (J.Colloid Interface Sci.612(2022)413–423) Lei fixed metallic cobalt and crystalline Co-Mo oxide on graphite felt, which greatly promoted the production of hydrogen.
[0004] In order to improve the overall electron transfer efficiency of the catalytic process, mixing active substances with carbon materials to prepare composite catalysts has been proven to be a practical and useful method. (ACS Catal. 12 (2022) 1167–1179) Luo-inge carefully designed a HER catalyst with ultra-high current density by anchoring single atoms on carbon nanotubes, and finally achieved typical catalytic activity. (J. Power Sources 555 (2023), 232414) Wei et al. obtained HER electrocatalysts by attaching spindle-shaped cobalt-doped iron phosphide to three-dimensional graphene, and then showed impressive hydrogen evolution performance. So far, such research has been mostly limited to encapsulating metal catalysts in carbon materials such as carbon nanotubes, carbon nanofibers and graphene oxide, but due to their high cost and complex preparation process, it is difficult to achieve industrialization, so it is necessary to find suitable alternatives. Expanded graphite (EG) is a new porous carbon material with excellent electrical conductivity, high porosity, large specific surface area, low price and non-toxicity, which can be an ideal candidate for increasing electrocatalytic activity. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a nano CoMoO 4 Preparation method of CoMoO / EG catalyst 4 Uniformly dispersed on expanded graphite EG, the CoMoO is exposed to a greater extent by virtue of the high specific surface area of EG. 4 , giving full play to CoMoO 4 By reducing the CoMoO 4 size, so that its active sites are fully exposed, and it is combined with EG to solve the problems of insufficient catalyst dispersion and high cost.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A nano-CoMoO 4 The preparation method of the EG / EG catalyst comprises the following steps:
[0008] 1) Preparation of modified expanded graphite:
[0009] Take 0.02-0.06 g of expanded graphite and 50-60 mL of mixed acid solution and stir at room temperature for 20-24 hours; then wash thoroughly with water until the solution becomes neutral, and dry at 70-80° C. to obtain acidified expanded graphite;
[0010] 2) Prepare solution A:
[0011] Will Na 2 MoO 4 ·2H 2O, 1M HNO 3 and water in a mass ratio of (0.1-0.13):(1.4-1.6):1. After ultrasonication for 0.5-1h, 0.02-0.06g of acidified expanded graphite was added and stirred at room temperature for 0.5-1h to prepare solution A;
[0012] 3) Preparation of solution B:
[0013] Will Co(NO 3 ) 2 6H 2 O and water were prepared into solution B in a mass ratio of (0.1-0.12):1 by ultrasonication for 0.5-1h;
[0014] 4) Solution B was slowly dripped into solution A, the mass ratio of solution A to solution B was (2.1-2.4):1, pH was adjusted to 7-9 with aqueous ammonia, and then stirred for 4-6 hours, and then transferred to a polytetrafluoroethylene liner for hydrothermal reaction for 12-16 hours, and then washed with water / ethanol, and finally dried at 70-80°C to obtain nano-CoMoO 4 / EG.
[0015] The mixed acid solution is a solution of sulfuric acid and nitric acid in a volume ratio of (3-4):1, wherein the mass concentration of sulfuric acid is 95%-98%, and the mass concentration of nitric acid is 65%-68%.
[0016] The temperature of the hydrothermal reaction is 150-200°C.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention uses expanded graphite (EG) as a carbon carrier and adopts a simple hydrothermal method to prepare a composite material of carbon material loaded with transition metal oxides. By utilizing the worm-like shape and good conductivity of expanded graphite, CoMoO 4 Nanoparticles, reducing CoMoO 4 size, which helps to fully expose the active material nanoCoMoO 4 Active sites of nano-CoMoO 4 / EG catalyst is used in water electrolysis to catalyze hydrogen evolution reaction. Under alkaline conditions, the current density is 10mA / cm 2 The overpotential is 257 mV, much higher than that of CoMoO 4 / EG has a 364mV, showing excellent HER activity and good stability (still maintaining good catalytic performance after 5000 CV cycles). This shows that nano-CoMoO 4 / EG catalyst has considerable application prospects in electrocatalytic hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a preparation flow chart of expanded graphite (EG) catalyst.
[0020] Figure 2 It is nano CoMoO 4 Preparation flow chart of / EG catalyst.
[0021] Figure 3 It is nano CoMoO 4 Preparation flow chart of / EG catalyst.
[0022] Figure 4 EG, nano-CoMoO 4 / EG、CoMoO 4 Enlarged XRD pattern of the / EG catalyst.
[0023] Figure 5 EG, nano-CoMoO 4 / EG、CoMoO 4 XRD pattern of / EG catalyst.
[0024] Figure 6 It is nano CoMoO 4 / EG、CoMoO 4 XRD pattern of / EG catalyst.
[0025] Figure 7 It is nano CoMoO 4 Cathodic polarization curve of / EG catalyst.
[0026] Figure 8 It is nano CoMoO 4 Tafel slope plot of the / EG catalyst.
[0027] Fig. 9 It is nano CoMoO 4 Stability diagram of the / EG catalyst. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0029] A nano-CoMoO 4 The preparation method of the EG / EG catalyst comprises the following steps:
[0030] 1) Preparation of modified expanded graphite:
[0031] Take 0.02-0.06g of expanded graphite and 50-60mL of mixed acid solution and stir at room temperature for 20-24h; then wash thoroughly with water until the solution becomes neutral, and dry at 70-80°C to obtain acidified expanded graphite MEG; wherein the mixed acid solution is a concentrated sulfuric acid and concentrated nitric acid solution (concentrated sulfuric acid: 95%-98%, concentrated nitric acid: 65%-68%) in a volume ratio of (3-4):1.
[0032] 2) Prepare solution A:
[0033] Will Na 2 MoO 4 ·2H 2 O, 1M HNO 3 and water in a mass ratio of (0.1-0.13):(1.4-1.6):1. After ultrasonication for 0.5-1h, 0.02-0.06g of acidified expanded graphite was added and stirred at room temperature for 0.5-1h to prepare solution A;
[0034] 3) Preparation of solution B:
[0035] Will Co(NO 3 ) 2 6H 2 O and water were prepared into solution B in a mass ratio of (0.1-0.12):1 by ultrasonication for 0.5-1h;
[0036] 4) Solution A and solution B are in a mass ratio of (2.1-2.4):1, solution B is slowly dripped into solution A, pH is adjusted to 7-9 with ammonia water, stirred for 4-6 hours, and then transferred to a polytetrafluoroethylene liner for hydrothermal reaction at 150-200°C for 12-16 hours, then washed with water / ethanol, and finally dried at 70-80°C to obtain nano-CoMoO 4 / EG.
[0037] Control group: CoMoO 4 Preparation of EG:
[0038] Take 0.02-0.06g MEG and disperse it in a mixed solution (water: ethanol = 4:1-2:1), add Na 2 MoO 4 ·2H 2 O and Co(NO 3 ) 2 6H 2 O, ultrasonic treatment for 30-60 min to obtain a uniform dispersion, which was then evaporated to dryness at 80-110 °C and finally transferred to a muffle furnace for calcination at 350-400 °C for 2-2.5 h to obtain CoMoO 4 / EG.
[0039] Example 1
[0040] Nano-CoMoO 4 The preparation method of the EG / EG catalyst comprises the following steps:
[0041] 1) See Figure 1 First, 2g of natural flake graphite was dried in a vacuum oven at 80°C for 24 hours to remove moisture from the material. Subsequently, it was poured into a mixed acid solution (50mL) consisting of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 4:1 and stirred for 24 hours to form a graphite intercalation compound. The mixture was then filtered with deionized water until neutral, and finally the filter cake was dried in a vacuum oven at 80°C for 24 hours. After it was completely dried, it was rapidly expanded in a muffle furnace at 900°C for 60s to form expanded graphite (EG).
[0042] 2) See Figure 2 , take 0.05g of expanded graphite (EG) and stir it with 50mL of the mixed acid solution of sulfuric acid and nitric acid at room temperature for another 24h. Then, wash it thoroughly with water until the solution becomes neutral, and dry it at 80℃ to obtain acidified expanded graphite (MEG).
[0043] 3) See Figure 3 , prepare suspension A:
[0044] 2.5mmoL Na 2 MoO 4 ·2H 2 O, 5 mL of 1 M HNO 3 and 5 mL of deionized water to prepare a mixed solution, and then 0.05 g of MEG was added to prepare suspension A;
[0045] Prepare Solution B:
[0046] 2.5mmoLCo(NO 3 ) 2 6H 2 O and 5 ml of water to prepare solution B.
[0047] 4) All solution B was slowly dripped into solution A, and the pH was adjusted to 8 with ammonia water. The mixture was stirred for 4 h, and then transferred to a polytetrafluoroethylene liner for hydrothermal reaction. The mixture was heated at 200 °C for 14 h, and then washed and dried with water / ethanol and dried at 80 °C to obtain nano-CoMoO 4 / EG composite material.
[0048] CoMoO 4 Preparation of / EG catalyst:
[0049] Take 0.05g MEG and disperse it in 20ml mixed solution (water: ethanol = 4:1), add 2.5mmol Na 2 MoO 4 ·2H 2 O and Co(NO 3 ) 2 6H 2 O, and then ultrasonically treated for 30 min to obtain a uniform dispersion, which was then evaporated to dryness at 110 °C and finally transferred to a muffle furnace and calcined at 400 °C for 2 h to obtain CoMoO 4 / EG.
[0050] The electrocatalytic hydrogen evolution test process, including the preparation of catalyst ink, working electrode and electrolyte, is as follows:
[0051] Catalyst ink preparation: Weigh 1.5 mg of nano-CoMoO 4 The / EG catalyst was fully ground and placed in a 5 mL glass bottle. 170 uL of deionized water, 70 uL of isopropanol and 15 uL of 5% Nafion binder were respectively taken and dropped into the glass bottle using a pipette, and the mixed catalyst suspension was ultrasonically treated for more than 60 min to make it evenly dispersed.
[0052] Preparation of working electrode: Use a pipette to take 17 μL of catalyst suspension and drop it on the surface of the polished and ultrasonically cleaned glassy carbon electrode, and let it dry fully under natural conditions for use.
[0053] Use 1M KOH as the electrolyte and purge the electrolyte under nitrogen for 30 minutes before use.
[0054] Depend on Figure 4 It is known that nano-CoMoO 4 / EG、CoMoO 4 / EG and the standard card correspond perfectly, while the peak of pure expanded graphite (EG) does not correspond, only two peaks of the (002) and (100) planes of graphitized carbon, which shows that CoMoO 4 Successfully loaded onto expanded graphite, from Figure 5 Nano-CoMoO 4 / EG and CoMoO 4 The (002) and (100) peak intensities of CoMoO / EG are much weaker than those of EG matrix, which may be due to the 4 Nanoparticles coated on the EG surface and CoMoO 4 The spacer effect of the nanoparticles hinders the orderly stacking of EG nanosheets during the hydrothermal process.
[0055] Depend on Figure 6It can be seen that there are two peaks near 2θ = 24° and 43°, corresponding to the graphitized carbon Nano-CoMoO 4 / EG and CoMoO 4 / EG plane, nano-CoMoO 4 / EG also corresponds perfectly to the standard card, and CoMoO 4 Compared with / EG, nano-CoMoO 4 / EG is CoMoO at 17.7°, 34.5° and 36.6° 4 3 / 4H 2 O's peak.
[0056] Depend on Figure 7 It can be seen that it is generally used at a current density of 10 mA cm -2 The size of the corresponding overpotential value is used to evaluate the activity of the catalyst. Figure 7 , nano-CoMoO 4 / EG at a current density of 10 mA cm -2 The corresponding overpotential is 257 mV, which is much higher than that of CoMoO at the same current density. 4 / EG's 364mV indicates that nano-CoMoO 4 The catalytic effect of hydrogen evolution on the surface of the / EG electrode is better.
[0057] Depend on Figure 8 It can be seen that at the same current density, the smaller the Tafel slope, the faster the reaction kinetics, and the more favorable the reaction. Sample nano-CoMoO 4 The Tafel slope of / EG is 103mV decade -1 Slightly higher than CoMoO 4 / EG, which is much lower than that of EG, thus indicating that its kinetics have been well improved.
[0058] Fig. 9 The stability diagram of the sample catalyst prepared in Example 1 shows that after 5000 cyclic voltammetry tests, the material's transition point is slightly reduced, indicating that the material still has good catalytic activity and has excellent electrochemical cycle stability. -2 The long-term stability tested at the corresponding potential can also prove that it has good electrochemical stability.
[0059] The above electrochemical experimental results show that by loading nanostructured CoMoO on expanded graphite 4 Successfully improved CoMoO 4 The electrochemical performance of nano-CoMoO 4 / EG composite materials have certain applicability in the field of electrocatalysis.
[0060] Nano-CoMoO 4 Preparation method of catalyst:
[0061] 2.5mmoL Na 2 MoO 4 ·2H 2 O, 5 mL of 1 M HNO 3 and 5 mL of deionized water to prepare a mixed solution to obtain solution A. 2.5 mmol LCo(NO 3 ) 2 6H 2 O and 5 ml of water to prepare solution B. Then all solution B was slowly dripped into solution A, and the pH was adjusted to 8 with ammonia water. After stirring for 4 h, it was transferred to a polytetrafluoroethylene liner for hydrothermal reaction, heated at 200 ° C for 14 h, washed and dried with water / ethanol, and dried at 80 ° C to obtain nano CoMoO 4 catalyst.
[0062] CoMoO 4 / Preparation method of carbon black catalyst:
[0063] Take 0.05g carbon black and disperse it in 20ml mixed solution (water: ethanol = 4:1), add 2.5mmol Na 2 MoO 4 ·2H 2 O and 2.5mmol Co(NO 3 ) 2 6H 2 O, and then ultrasonically treated for 30 min to obtain a uniform dispersion, which was then evaporated to dryness at 110 °C and finally transferred to a muffle furnace and calcined at 400 °C for 2 h to obtain CoMoO 4 / Carbon black catalyst.
[0064] Table 1
[0065]
[0066] Table 1 summarizes the HER performance of catalysts prepared under different conditions. It is obvious from Table 1 that nano-CoMoO 4 / EG catalyst performance at a current density of 10 mA cm -2 When , the overpotential is far the lowest, indicating that the electrochemical performance is improved.
[0067] Example 2
[0068] Nano-CoMoO 4 The preparation method of the EG / EG catalyst comprises the following steps:
[0069] 1) See Figure 2 , take 0.05g of expanded graphite (EG) and stir it with 55mL of a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 3.4:1 at room temperature for another 24h. Then, wash it thoroughly with water until the solution becomes neutral, and dry it at 75°C to obtain acidified expanded graphite (MEG).
[0070] 2) See Figure 3 , prepare suspension A:
[0071] 2.5mmoL Na 2 MoO 4 ·2H 2 O, 5 mL of 1 M HNO 3 and 5 mL of deionized water to prepare a mixed solution, and then 0.04 g of MEG was added to prepare suspension A;
[0072] Prepare Solution B:
[0073] 2.5mmoLCo(NO 3 ) 2 6H 2 O and 5 ml of water to prepare solution B.
[0074] 4) All solution B was slowly dripped into solution A, and the pH was adjusted to 8 with ammonia water. The mixture was stirred for 4 h, and then transferred to a polytetrafluoroethylene liner for hydrothermal reaction. The mixture was heated at 180 °C for 14 h, and then washed and dried with water / ethanol, and dried at 80 °C to obtain nano-CoMoO 4 / EG composite material.
[0075] Nano-CoMoO 4 / EG at a current density of 10 mA cm -2 The corresponding overpotential is 246mV.
[0076] Example 3
[0077] Nano-CoMoO 4 The preparation method of the EG / EG catalyst comprises the following steps:
[0078] 1) See Figure 2 , take 0.05g of expanded graphite (EG) and stir it with 58mL of a mixed acid solution of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 3:1 at room temperature for another 24h. Then, wash it thoroughly with water until the solution becomes neutral, and dry it at 75°C to obtain acidified expanded graphite (MEG).
[0079] 2) See Figure 3 , prepare suspension A:
[0080] 2.5mmoL Na 2 MoO 4·2H 2 O, 5 mL of 1 M HNO 3 and 5 mL of deionized water to prepare a mixed solution, and then 0.03 g of MEG was added to prepare suspension A;
[0081] Prepare Solution B:
[0082] 2.5mmoLCo(NO 3 ) 2 6H 2 O and 5 ml of water to prepare solution B.
[0083] 4) All solution B was slowly dripped into solution A, and the pH was adjusted to 8 with ammonia water. The mixture was stirred for 4 h, and then transferred to a polytetrafluoroethylene liner for hydrothermal reaction. The mixture was heated at 180 °C for 14 h, and then washed and dried with water / ethanol, and dried at 80 °C to obtain nano-CoMoO 4 / EG composite material.
[0084] Nano-CoMoO 4 / EG at a current density of 10 mA cm -2 The corresponding overpotential is 251mV.
[0085] The present invention converts CoMoO 4 Uniformly dispersed on EG, the high specific surface area of EG can be used to expose CoMoO to a greater extent. 4 , giving full play to CoMoO 4 By reducing the CoMoO 4 The size of the catalyst fully exposes its active sites, and it is combined with expanded graphite, which has good electrical conductivity, is easy to make and inexpensive, to solve the problems of insufficient catalyst dispersion and high cost.
Claims
1. A method for preparing a nano CoMoO4 / EG catalyst, characterized in that: The following steps are involved: 1) Preparation of modified expanded graphite: Take 0.02-0.06 g of expanded graphite and 50-60 mL of mixed acid solution and stir at room temperature for 20-24 hours; then wash thoroughly with water until the solution becomes neutral, and dry at 70-80° C. to obtain acidified expanded graphite; 2) Prepare solution A: After ultrasonication for 0.5-1h, Na2MoO4·2H2O, 1M HNO3 and water in a mass ratio of (0.1-0.13):(1.4-1.6):1, 0.02-0.06g of acidified expanded graphite was added and stirred at room temperature for 0.5-1h to prepare solution A; 3) Preparation of solution B: Co(NO3)2·6H2O and water were prepared into solution B at a mass ratio of (0.1-0.12):1 by ultrasonication for 0.5-1h; 4) Slowly drip solution B into solution A, the mass ratio of solution A to solution B is (2.1-2.4):1, adjust the pH to 7-9 with ammonia water, stir for 4-6 hours, then transfer to a polytetrafluoroethylene liner for hydrothermal reaction for 12-16 hours, then wash with water / ethanol, and finally dry at 70-80°C to obtain nano CoMoO4 / EG.
2. The method for preparing a nano CoMoO4 / EG catalyst according to claim 1, characterized in that: The mixed acid solution is a solution of sulfuric acid and nitric acid in a volume ratio of (3-4):1, wherein the mass concentration of sulfuric acid is 95%-98%, and the mass concentration of nitric acid is 65%-68%.
3. The method for preparing a nano CoMoO4 / EG catalyst according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 150-200°C.