Cobalt-doped nickel diselenide coated cobalt hydroxide composite material and preparation and application thereof

By cobalt-doped nickel diselenide-coated cobalt hydroxide nanocomposites, the problems of low catalyst activity and poor stability in alkaline electrolytic hydrogen production technology are solved, and efficient and low-cost full water-removal catalytic performance is achieved. Suitable for industrial applications.

CN118880381APending Publication Date: 2024-11-01PEKING UNIV

Patent Information

Application Number
CN202410912036.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing alkaline electrolytic hydrogen production technology, the catalyst has low activity and poor stability, the preparation process is complex and costly, and cannot meet industrial needs.

Method used

CoxNi1-xSe2@Co(OH)2, a nanocomposite material coated with cobalt diselenide, was adopted to grow cobalt hydroxide nanoarrays by hydrothermal method and prepared by radiation reduction method to form a nanorod-like structure and regulate Electronic structure to improve catalytic activity and stability.

Benefits of technology

High catalytic performance and electrochemical stability are achieved, energy consumption and cost of preparation are reduced, and are better than commercial precious metal catalysts, and can achieve high current density full water-removing reaction at lower operating voltages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880381A_ABST
    Figure CN118880381A_ABST
Patent Text Reader

Abstract

The invention discloses a cobalt-doped nickel diselenide coated cobalt hydroxide composite material as well as preparation and application thereof, and belongs to the technical field of new materials and electrochemistry. The material is a CoxNi (1-x) Se2 (at) Co (OH) 2 self-supporting composite material loaded on a conductive substrate, x is more than or equal to 0.1 and less than or equal to 0.9, and the mass loading rate of CoxNi (1-x) Se2 (at) Co (OH) 2 on the conductive substrate is 2-60%. The preparation method comprises the following steps: firstly, growing a cobalt hydroxide nano array on a conductive substrate by a hydrothermal method, and then preparing cobalt-doped nickel diselenide on the surface of the cobalt hydroxide nano array from a nickel precursor and sodium selenite by a radiation reduction method. The material is applied to electrochemical hydrogen evolution and oxygen evolution reactions as a full-electrolysis water catalyst, and compared with an existing commercial catalyst, the material has great advantages in the aspects of catalytic activity and stability. And moreover, the condition for synthesizing the transition metal selenide by using a radiation method is mild and controllable, the energy consumption is low, the environmental pollution is small, a strong reducing substance is not used in the preparation process, and the preparation process is safer and more convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new materials and electrochemical technology, and in particular to a cobalt-doped nickel diselenide-coated cobalt hydroxide composite material and a preparation method and application thereof. Background Art

[0002] Alkaline water electrolysis hydrogen production technology is a green, environmentally friendly and sustainable hydrogen production process. Different from the traditional acidic water electrolysis technology, alkaline water electrolysis hydrogen production can effectively reduce the serious corrosion problem of the highly acidic working environment on the electrodes, diaphragms and electrolyzers in the water electrolysis system, and reduce the maintenance and operation costs of water electrolysis hydrogen production. However, the production of hydrogen under alkaline conditions is limited by the low OH content in the solution. - The ion conduction rate is high, and there are problems such as high water decomposition energy barrier and slow reaction kinetics. At present, the performance of commercial platinum carbon Pt / C catalysts in alkaline water electrolysis for hydrogen production cannot meet the needs of large-scale industrial alkaline water electrolysis. At the same time, the oxygen evolution reaction occurring on the anode side of alkaline water electrolysis has a large overpotential, which further increases the working voltage of water electrolysis for hydrogen production, which makes the alkaline water electrolysis hydrogen production process face huge challenges. Therefore, the development of new oxygen evolution reaction electrocatalysts is also crucial to reduce the energy consumption of alkaline water electrolysis hydrogen production process. In addition, conventional powder catalyst materials are often not used directly, and they need to be prepared as membrane electrodes before they can be assembled into water electrolyzers. The complex preparation process of membrane electrodes increases the cost of water electrolyzers, and the organic additives used to prepare membrane materials will destroy the catalyst structure and reduce its catalytic activity to a certain extent. At the same time, the service life of membrane electrodes in alkaline water electrolyzers is short, making it impossible to operate stably for a long time under industrial-scale production conditions. At present, transition metal selenides have received widespread attention in the field of full water splitting as electrocatalysts that can replace precious metals. Compared with other non-precious metal catalysts, it has the advantages of abundant resources, low price, strong composition and structural design, and high conductivity near metals. The 3s and 3p orbitals of selenium in transition metal selenides are close to the 3d orbitals of transition metals in energy, which can effectively cause orbital overlap and hybridization, which is beneficial to adjust its adsorption energy for intermediates in the water decomposition process. However, the limited catalytic active sites of transition metal selenides themselves cannot fully exert their performance in the field of electrocatalytic water splitting.

[0003] To this end, researchers are mainly committed to developing new transition metal selenide full hydrolysis catalysts in order to obtain high catalytic performance while improving the stability of the material structure and reducing the cost of use and maintenance. Fan et al. (Fan H., et al., Nano Research 2024, 17, 1199–1208) prepared chromium-doped nickel diselenide full water splitting catalyst Cr supported on carbon cloth by hydrothermal and high-temperature calcination. 0.05 Ni 0.95Se2. The catalyst promoted the reconstruction process of oxygen evolution reaction due to Cr doping, regulated the adsorption energy of intermediates in hydrogen evolution reaction, accelerated the water decomposition kinetics, and achieved 10mA cm -2 The total water splitting current density only requires an operating voltage of 1.59V. However, the stability of the catalyst needs to be improved, and the preparation method of selenide involves a high-temperature process and high energy consumption. Fang Caihong et al. prepared a nanorod-shaped nickel selenide / cobalt molybdenum oxide composite material Ni3Se2 / Co2Mo3O8 by room temperature selenization and high temperature annealing, which can achieve 100mA cm at an operating voltage of 1.60V. -2 The current density of the complete water splitting reaction (CN117448874A). However, this work still has problems such as complex material composition, unclear structure-activity relationship and catalytic stability. Li Hengyi et al. developed a graphene-loaded selenide nanoparticle electrolysis catalyst, which can evenly grow nickel diselenide and cobalt diselenide on the surface of graphene oxide to achieve low-cost electrocatalytic hydrogen evolution reaction (CN117230472A). However, this strategy did not greatly change the electronic structure and intrinsic catalytic activity of selenide, and the material itself had poor electrocatalytic hydrogen evolution activity. Zhang et al. (Zhang, C., et al., Journal of Alloys and Compounds 2020, 818, 152833) used Ni-Fe metal foam as a template to grow three-dimensional porous Fe-doped NiSe2 nanofolds on its surface, which can achieve 10mA cm at an operating voltage of 1.58V. -2 However, the material has a low specific surface area and insufficient exposure of active sites, which is not conducive to mass transfer kinetics under high current density, and its catalytic performance is far from meeting the requirements of industrial production. Summary of the invention

[0004] The purpose of the present invention is to develop a transition metal selenide-based complete water splitting electrocatalyst with excellent catalytic performance, high stability and low cost, so as to solve the problems of low activity, poor stability, complex preparation process and high cost of current non-precious metal catalysts.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect of the present invention, a Co supported on a conductive substrate is provided. x Ni 1-x Se2@Co(OH)2 self-supporting composite material, in which Co x Ni 1-x Se2@Co(OH)2 is a nanocomposite material of cobalt-doped nickel diselenide coated with cobalt hydroxide, 0.1≤x≤0.9, and Co x Ni 1-xThe mass loading rate of Se2@Co(OH)2 on the conductive substrate is 2%-60%.

[0007] Preferably, in the above Co x Ni 1-x In the Se2@Co(OH)2 nanocomposite material, the Co(OH)2 is a nano-needle structure.

[0008] Furthermore, the above-mentioned Co x Ni 1-x In the Se2@Co(OH)2 nanocomposite material, the Co x Ni 1-x Se2 has a nano-spherical structure.

[0009] Furthermore, the above-mentioned Co x Ni 1-x In Se2@Co(OH)2 nanocomposite materials, 0.2≤x≤0.5 is preferred.

[0010] Furthermore, the above-mentioned Co x Ni 1-x The Se2@Co(OH)2 self-supporting composite material was prepared by a two-step method: first, a cobalt hydroxide nanoarray was grown on a conductive substrate by a hydrothermal method, and then cobalt-doped nickel diselenide was prepared on the surface of the cobalt hydroxide nanoarray by a nickel precursor and sodium selenosulfite by a radiation reduction method. Cobalt hydroxide serves as a template to provide a cobalt precursor, which is doped into nickel diselenide under a radiation reduction atmosphere, forming Ni-Se-Co bonds in the lattice, promoting the charge redistribution of nickel selenide and regulating its inherent electronic structure.

[0011] Furthermore, the conductive substrate is, for example, nickel foam, copper foam, titanium foam, carbon cloth, carbon paper, stainless steel mesh, titanium mesh, etc.

[0012] In a second aspect of the present invention, there is provided the Co x Ni 1-x A method for preparing a Se2@Co(OH)2 self-supporting composite material comprises the following steps:

[0013] 1) placing a conductive substrate in an aqueous solution containing a cobalt precursor, urea and ammonium fluoride, heating to hydrothermally grow cobalt hydroxide, and taking out after the reaction is completed, washing, and vacuum drying;

[0014] 2) Place the conductive substrate after the above reaction in a solution containing both a nickel precursor and sodium selenosulfite, add a free radical scavenger, seal it in an inert atmosphere, and use γ rays or electron beams to perform radiation reduction reaction. Take out the reacted material, wash it, and vacuum dry it to obtain Co supported on the conductive substrate. x Ni 1-xSe2@Co(OH)2 self-supporting composite materials.

[0015] The above step 1) is to grow a cobalt hydroxide nanoneedle array on the surface of a conductive substrate, and the required hydrothermal conditions are a hydrothermal temperature of 90 to 150° C. and a heating time of 4 to 24 hours. Generally, the hydrothermal reaction of step 1) is carried out in a hydrothermal kettle lined with polytetrafluoroethylene, and the material is washed with water and ethanol several times after the reaction is completed.

[0016] In the above step 1), the cobalt precursor may be selected from one or more of cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt citrate and cobalt acetate.

[0017] In the above step 2), the nickel precursor may be selected from one or more of nickel acetate, nickel sulfate, nickel chloride, nickel citrate, and nickel nitrate.

[0018] In the above step 2), the free radical scavenger is an alcohol organic solvent, which can be selected from one or more of methanol, ethanol, n-propanol, isopropanol, tert-butanol, ethylene glycol, and glycerol.

[0019] In the above step 2), the inert atmosphere can be nitrogen, argon or a mixture thereof, and the ventilation time is 5 to 60 minutes.

[0020] In the above step 2), one solution is to place the sample in an irradiation tube and 60 The gamma rays generated by Co carry out the radiation reduction reaction. Preferably, the gamma ray irradiation is carried out at room temperature, with a dose rate of 10 to 200 Gy / min and an absorbed dose of 10 to 200 kGy.

[0021] In the above step 2), if electron beam irradiation is selected, the sample is injected into a plastic bag and sealed with an inert gas, and a radiation reduction reaction is performed at room temperature using an electron accelerator irradiation device. The energy of the electron accelerator is preferably 0.2 to 10 MeV, the dose rate of the electron beam irradiation is 5 to 20 kGy / pass, and the absorbed dose is 10 to 200 kGy.

[0022] The material after the reduction reaction in step 2) is washed with water or ethanol once or multiple times, and then vacuum dried.

[0023] In some embodiments of the present invention, the concentration of the cobalt precursor in the aqueous solution in step 1) is 1 to 80 mmol / L, preferably 1 to 40 mmol / L, and more preferably 5 to 20 mmol / L.

[0024] In some embodiments of the present invention, the concentration of urea in the aqueous solution in step 1) is 0.1-10 mmol / L, preferably 0.2-5 mmol / L, and more preferably 0.5-5 mmol / L.

[0025] In some embodiments of the present invention, the concentration of ammonium fluoride in the aqueous solution in step 1) is 0.05-20 mmol / L, preferably 0.1-10 mmol / L, and more preferably 0.3-8 mmol / L.

[0026] In some embodiments of the present invention, the concentration of the nickel precursor in step 2) is 1 to 100 mmol / L, preferably 3 to 50 mmol / L, and more preferably 5 to 30 mmol / L.

[0027] In some embodiments of the present invention, the concentration of sodium selenosulfite in step 2) is 1 to 100 mmol / L, preferably 5 to 80 mmol / L, and more preferably 5 to 60 mmol / L.

[0028] In some embodiments of the present invention, the concentration of the free radical scavenger in step 2) is 1 to 80 mL / L, preferably 5 to 50 mL / L, and more preferably 5 to 20 mL / L.

[0029] In a third aspect of the present invention, the Co x Ni 1-x Application of Se2@Co(OH)2 self-supporting composite materials as full water electrolysis catalyst in electrochemical hydrogen and oxygen evolution reactions.

[0030] Furthermore, the present invention provides a self-supporting electrode, comprising a substrate electrode fixture and the Co x Ni 1-x Se2@Co(OH)2 self-supporting composite material. The substrate electrode fixture is an inert electrode fixture, preferably a platinum fixture, a titanium fixture, a copper fixture, a stainless steel fixture, or a carbon fixture; x Ni 1-x The Se2@Co(OH)2 self-supporting composite material was fixedly mounted between the two clamping plates of the electrode fixture.

[0031] The present invention provides a water electrolysis hydrogen production device, which includes the self-supporting electrode as described above. It should be noted that, for the water electrolysis hydrogen production device provided by the present invention, except that the electrode adopts the self-supporting electrode provided by the present invention, other components required for the water electrolysis hydrogen production device, such as a peristaltic pump, a temperature controller, a bipolar plate, a gas diffusion layer, an ion exchange membrane and an electrolyte, can all be implemented by using relevant technical solutions in the prior art, and the present invention is not limited here.

[0032] The present invention provides an electric equipment product, which includes the water electrolysis hydrogen production device as described above. It should be noted that the other parts of the equipment product except the aforementioned device can be implemented by using relevant technical solutions in the prior art, and the present invention is not limited here. The electric equipment product is preferably a hydrogen generator or an oxygen generator.

[0033] Compared with the prior art, the present invention has the following technical advantages:

[0034] (1) The present invention uses cobalt hydroxide nanoneedle arrays grown on the surface of a conductive substrate as a template and synthesizes Co by radiation reduction method. x Ni 1-x Se2@Co(OH)2 self-supporting composite material. The composite material has a nanorod array structure, which is beneficial to improve the utilization rate of catalytic active sites, and at the same time helps bubbles to detach from the catalyst surface, enhances the electrocatalytic mass transfer kinetics, and gives the catalyst excellent electrochemical stability. Cobalt hydroxide serves as a morphological template and provides cobalt ions, which helps the subsequent growth of cobalt-doped nickel diselenide on its surface. Co prepared by radiation method x Ni 1-x Se2 optimizes the charge distribution of the material through the bonding form of Ni-Se-Co and adjusts the inherent electronic structure, making it have a more suitable hydrogen / oxygen intermediate adsorption energy and a lower free energy barrier for water decomposition.

[0035] (2) Co synthesized by the present invention x Ni 1-x Se2@Co(OH)2 composite material has excellent catalytic performance in water splitting, and has greater advantages in catalytic activity and stability compared with the commercial precious metal catalyst assembled full electrolytic water splitting device RuO2 / / Pt / C.

[0036] (3) Compared with the traditional solvothermal method and high temperature calcination method, the radiation method is used to synthesize the transition metal selenide catalyst Co x Ni 1-x The Se2@Co(OH)2 preparation conditions are mild and controllable, with low energy consumption and little environmental pollution. The use of strong reducing substances is avoided during the preparation process, making the preparation process safer and more convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 . Schematic diagram of the process of preparing a cobalt-doped nickel diselenide-coated cobalt hydroxide composite material according to an embodiment of the present invention.

[0038] Figure 2A Example 1 Preparation of Co x Ni 1-x Scanning electron microscopy (SEM) image of Se2@Co(OH)2 composite material.

[0039] Figure 2B Example 1 Preparation of Co x Ni 1-x Transmission electron microscopy (TEM) image of Se2@Co(OH)2 composite material.

[0040] Figure 3A Example 1 Preparation of Co x Ni 1-x X-ray photoelectron spectroscopy (XPS) diagram of Se2@Co(OH)2 composite material.

[0041] Figure 3B Example 1 Preparation of Co x Ni 1-x XPS high-resolution image of Co in Se2@Co(OH)2 composite material.

[0042] Figure 3C Example 1 Preparation of Co x Ni 1-x XPS high-resolution image of Ni in Se2@Co(OH)2 composite material.

[0043] Figure 3D Example 1 Preparation of Co x Ni 1-x XPS high-resolution image of Se in Se2@Co(OH)2 composite material.

[0044] Figure 4A .Co x Ni 1-x Polarization curves of hydrogen evolution catalyzed by Se2@Co(OH)2 catalyst and 20% Pt / C in an alkaline three-electrode system.

[0045] Figure 4B .Co x Ni 1-x η values ​​of Se2@Co(OH)2 catalyst and 20% Pt / C at different catalytic hydrogen evolution current densities in an alkaline three-electrode system.

[0046] Figure 5A .Co x Ni 1-x Polarization curves of catalytic oxygen evolution over Se2@Co(OH)2 catalyst and RuO2 in an alkaline three-electrode system.

[0047] Figure 5B .Co x Ni 1-x η values ​​of Se2@Co(OH)2 catalyst and RuO2 at different catalytic oxygen evolution current densities in an alkaline three-electrode system.

[0048] Fig. 6A .Cox Ni 1-x Polarization curves of complete water splitting of Se2@Co(OH)2 catalyst and RuO2 / / Pt / C electrodes.

[0049] Figure 6B .Co x Ni 1-x Chronopotentiometry curves of Se2@Co(OH)2 catalyst and RuO2 / / Pt / C for water splitting. DETAILED DESCRIPTION

[0050] The present invention is further described in detail below by way of examples, but the scope of the present invention is not limited in any way.

[0051] Example 1

[0052] 300 mg of cobalt nitrate, 150 mg of ammonium fluoride and 600 mg of urea were added to 40 mL of deionized water and stirred to form a uniform solution. The nickel foam cut to a suitable size was added and placed in a stainless steel hydrothermal kettle and heated at 120°C in a blast oven for 6 hours. The nickel foam material loaded with cobalt hydroxide after the reaction was taken out, rinsed with deionized water and ethanol three times respectively, and dried in a vacuum oven at 60°C for 24 hours.

[0053] Add 150 mg nickel acetate, 8 mL 0.25 M sodium selenosulfite solution, and 5 mL isopropanol to 22 mL deionized water to prepare a precursor solution with a total volume of 35 mL. Place the nickel foam material loaded with cobalt hydroxide in the precursor solution, pass N2 to remove air from the system, and seal it for use. 60 Co radioactive source was used for γ-ray irradiation, with a dose rate of 30 Gy / min and an absorbed dose of 50 kGy. After the irradiation reaction, the nickel foam was taken out, rinsed with deionized water and ethanol three times respectively, and dried in a vacuum oven at 60 °C for 24 hours to obtain Co x Ni 1-x Se2@Co(OH)2 self-supporting material, x=0.3.

[0054] The Co x Ni 1-x The SEM, TEM and XPS images of Se2@Co(OH)2 self-supporting materials are shown in Figure 2A , Figure 2B and Figures 3A to 3D As shown, cobalt-doped nickel diselenide grows uniformly on the surface of cobalt hydroxide in the form of 100-300 nm nanospheres. Figures 3A to 3D It shows that cobalt-doped nickel diselenide material was successfully synthesized by radiation reduction method, and the cobalt element was doped into the nickel diselenide lattice in the form of Co-Se-Ni.

[0055] Directly x Ni1-x Se2@Co(OH)2 self-supporting material is used to test the electrocatalytic water splitting performance of alkaline three-electrode system. x Ni 1-x Se2@Co(OH)2 was used as the working electrode, graphite rod as the counter electrode, and mercury / mercury oxide electrode (1M KOH) as the reference electrode. A three-electrode test system was assembled in 1M KOH solution, and the room temperature alkaline water splitting catalytic performance test was carried out in an argon-saturated atmosphere.

[0056] The Co was tested using the above method x Ni 1-x The electrocatalytic hydrogen evolution performance of Se2@Co(OH)2 as a catalyst assembled in an alkaline three-electrode system is shown in Figure 2. Figure 4A , Figure 4B As shown, its η 10 (i.e., the current density is 10 mA cm -2 The overpotential under (hereinafter the same) is as low as 87mV, η 100 As low as 185mV, comparable to commercial 20% Pt / C catalyst. Figure 5A , Figure 5B As shown, its η 10 As low as 231mV, η 100 As low as 307mV, better than commercial RuO2 catalyst.

[0057] The Co mounted on the electrode fixture x Ni 1-x Se2@Co(OH)2 material was used as both positive and negative electrodes and assembled into a two-electrode water splitting device in 1M KOH solution to test its catalytic performance and long-term working stability. Fig. 6A , 6B As shown. x Ni 1-x Se2@Co(OH)2 can achieve 10 mA cm at operating voltages of 1.51 V and 1.67 V, respectively. -2 With 100mA cm -2 The working current is much better than that of the commercial catalyst-assembled RuO2 / / Pt / C water splitting device (RuO2 is the positive electrode catalyst and Pt / C is the negative electrode catalyst). x Ni 1-x Se2@Co(OH)2 can generate a high current at 300 mA cm -2 It can run stably for 480 hours at a high current density without obvious performance degradation, while the commercial catalyst has a rapid voltage increase within 50 hours.

[0058] Example 2

[0059] The amount of nickel acetate in Example 1 was changed to 50 mg, and the other preparation conditions were the same as in Example 1. The change in the amount of nickel acetate affected the cobalt doping amount and thus affected the electrocatalytic performance of the material. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.8. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 180mV, η 100 is 283mV; oxygen evolution reaction η 10 is 286mV, η 100 It is 356mV.

[0060] Example 3

[0061] The amount of nickel acetate in Example 1 was changed to 100 mg, and the other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.5. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 167mV, η 100 is 275mV; oxygen evolution reaction η 10 is 274mV, η 100 It is 336mV.

[0062] Example 4

[0063] The amount of nickel acetate in Example 1 was changed to 200 mg, and the other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.2. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 assembled in the three-electrode system is slightly lower than that of Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 123mV, η 100 is 213mV; oxygen evolution reaction η 10 is 275mV, η 100 It is 332mV.

[0064] Example 5

[0065] The amount of nickel acetate in Example 1 was changed to 300 mg, and the other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.1. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 assembled in the three-electrode system is slightly lower than that of Example 1. The hydrogen evolution reaction η in the three-electrode system10 is 145mV, η 100 is 228mV; oxygen evolution reaction η 10 is 281mV, η 100 It is 342mV.

[0066] Example 6

[0067] The dose rate of radiation synthesis in Example 1 was changed to 50 Gy / min, and the other preparation conditions were the same as in Example 1. The dose rate change affected the morphology and structure of the nickel diselenide material and thus affected the electrocatalytic performance of the material. x Ni 1-x Se2@Co(OH)2, x = 0.3. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 112mV, η 100 is 195mV; oxygen evolution reaction η 10 is 248mV, η 100 It is 359mV.

[0068] Example 7

[0069] The dose rate of radiation synthesis in Example 1 was changed to 70 Gy / min, and other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.3. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 131mV, η 100 is 207mV; oxygen evolution reaction η 10 is 252mV, η 100 It is 348mV.

[0070] Example 8

[0071] The dose rate of radiation synthesis in Example 1 was changed to 100 Gy / min, and other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.3. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 135mV, η 100 is 211mV; oxygen evolution reaction η 10 is 257mV, η 100 It is 357mV.

[0072] Example 9

[0073] The dose rate of radiation synthesis in Example 1 was changed to 200 Gy / min, and other preparation conditions were the same as in Example 1. The composite material composition is Co x Ni 1-x Se2@Co(OH)2, x = 0.3. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 155mV, η 100 is 228mV; oxygen evolution reaction η 10 is 262mV, η 100 It is 363mV.

[0074] Example 10

[0075] The gamma irradiation in Example 1 was changed to electron beam irradiation, the absorbed dose was 50 kGy, the dose rate was 10 kGy / pass, and the other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.2. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 assembled in the three-electrode system is slightly lower than that of Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 162mV, η 100 is 241mV; oxygen evolution reaction η 10 is 258mV, η 100 It is 346mV.

[0076] Embodiment 11

[0077] The γ-irradiation absorbed dose in Example 1 was changed to 30 kGy, and the other preparation conditions were the same as in Example 1. The composite material composition is Co x Ni 1-x Se2@Co(OH)2, x = 0.7. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 172mV, η 100 is 283mV; oxygen evolution reaction η 10 is 266mV, η 100 It is 382mV.

[0078] Example 12

[0079] The γ-irradiation absorbed dose in Example 1 was changed to 70 kGy, and the other preparation conditions were the same as in Example 1. The composite material composition was Co x Ni 1-x Se2@Co(OH)2, x = 0.3. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system10 is 162mV, η 100 is 251mV; oxygen evolution reaction η 10 is 263mV, η 100 It is 342mV.

[0080] Example 13

[0081] The γ-irradiation absorbed dose in Example 1 was changed to 100 kGy, and the other preparation conditions were the same as in Example 1. The composite material composition is Co x Ni 1-x Se2@Co(OH)2, x = 0.4. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 157mV, η 100 is 263mV; oxygen evolution reaction η 10 is 259mV, η 100 It is 374mV.

[0082] Embodiment 14

[0083] The nickel precursor in Example 1 is nickel citrate, and other preparation conditions are the same as in Example 1. The composite material composition is Co x Ni 1-x Se2@Co(OH)2, x = 0.6. The catalytic performance of the overall water splitting of the Se2@Co(OH)2 in the three-electrode system is slightly lower than that in Example 1. The hydrogen evolution reaction η in the three-electrode system 10 is 157mV, η 100 is 263mV; oxygen evolution reaction η 10 is 259mV, η 100 It is 374mV.

[0084] Embodiment 15

[0085] The nickel precursor in Example 1 is nickel sulfate, and the other preparation conditions are the same as in Example 1. The composite material composition is Co x Ni 1-x Se2@Co(OH)2, x = 0.3. Hydrogen evolution reaction η in a three-electrode system 10 is 121mV, η 100 is 194mV; oxygen evolution reaction η 10 is 243mV, η 100 It is 328mV.

[0086] Comparative Example 1

[0087] The substrate material synthesized by radiation in Example 1 was changed to nickel foam metal (NF) without cobalt hydroxide, and the other preparation conditions were the same as in Example 1. The material composition was NiSe2, and the overall water splitting catalytic performance assembled in the three-electrode system was significantly reduced compared with that in Example 1 (see FIG. 4A to FIG. 5B ), the hydrogen evolution reaction η in the three-electrode system 10 is 126mV, η 100 is 226mV; oxygen evolution reaction η 10 is 254mV, η 100 The value is 392 mV. This highlights the important role of cobalt hydroxide array template in the synthesis and catalytic performance of cobalt-doped nickel selenide materials.

[0088] Comparative Example 2

[0089] The electrochemical performance of the nickel foam metal containing cobalt hydroxide in Example 1 was tested. The material composition is Co(OH)2, and the overall water splitting catalytic performance assembled in the three-electrode system is significantly reduced compared with Example 1 (see FIG. 4A to FIG. 5B ), the hydrogen evolution reaction η in the three-electrode system 10 is 183mV, η 100 is 314mV; oxygen evolution reaction η 10 is 330mV, η 100 It is 484mV.

[0090] Comparative Example 3

[0091] The electrochemical performance of the nickel foam metal in Example 1 was tested. The overall water splitting catalytic performance assembled in the three-electrode system was significantly reduced compared with that in Example 1 (see FIG. 4A to FIG. 5B ), the hydrogen evolution reaction η in the three-electrode system 10 is 211mV, η 100 is 371mV; oxygen evolution reaction η 10 is 361mV, η 100 is 480mV.

[0092] The above is only a partial embodiment of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. For ordinary technicians in this field, various forms of changes and improvements can still be made to the technical solutions in the embodiments based on the above description. It is not necessary and impossible to list all implementation methods here. Any modification, change, replacement, etc. made on the basis of the technical content disclosed by the present invention are equivalent to equivalent implementation cases and should be included in the protection scope of the present invention.

Claims

1. A kind of Co x Ni 1-x Se 2 @Co(OH) 2 The self-supporting composite material is a nanocomposite material of cobalt hydroxide coated with cobalt doped nickel diselenide supported on a conductive substrate, 0.1≤x≤0.9, and Co x Ni 1-x Se 2 @Co(OH) 2 The mass loading rate of the nanocomposite material on the conductive substrate is 2%-60%.

2. The Co according to claim 1 x Ni 1-x Se 2 @Co(OH) 2 Self-supporting composite materials, It is characterized in that In Co x Ni 1- x Se 2 @Co(OH) 2 In nanocomposites, Co(OH) 2 The nano-needle structure, Co x Ni 1-x Se 2 It is a nano-spherical structure.

3. The Co according to claim 1 x Ni 1-x Se 2 @Co(OH) 2 Self-supporting composite materials, It is characterized in that 0.2≤x≤0.5。 4. The Co according to claim 1 x Ni 1-x Se 2 @Co(OH) 2 Self-supporting composite materials, It is characterized in that The Co x Ni 1- x Se 2 @Co(OH) 2 The self-supporting composite material is prepared by a two-step method: first, cobalt hydroxide nanoarrays are grown on a conductive substrate by a hydrothermal method, and then cobalt-doped nickel diselenide is prepared on the surface of the cobalt hydroxide nanoarrays by a radiation reduction method using a nickel precursor and sodium selenosulfite.

5. The Co according to claim 1 x Ni 1-x Se 2 @Co(OH) 2 Self-supporting composite materials, It is characterized in that The conductive substrate is foamed nickel, foamed copper, foamed titanium, carbon cloth, carbon paper, stainless steel mesh or titanium mesh.

6. The Co according to any one of claims 1 to 5 x Ni 1-x Se 2 @Co(OH) 2 Method for preparing a self-supporting composite material, The following steps are involved: 1) placing a conductive substrate in an aqueous solution containing a cobalt precursor, urea and ammonium fluoride, heating to hydrothermally grow cobalt hydroxide, and after the reaction is completed, taking out the material, cleaning it, and vacuum drying it; 2) placing the material obtained in step 1) in a solution containing a nickel precursor and sodium selenosulfite, adding a free radical scavenger, and then sealing under an inert atmosphere, and performing a radiation reduction reaction using gamma rays or electron beams; taking out the reacted material, washing it, and vacuum drying it.

7. The preparation method according to claim 6, It is characterized in that The hydrothermal reaction temperature of step 1) is 90-150° C.; step 2) adopts gamma ray irradiation with a dose rate of 10-200 Gy / min and an absorbed dose of 10-200 kGy; or adopts electron beam irradiation with a dose rate of 5-20 kGy / pass and an absorbed dose of 10-200 kGy.

8. The preparation method according to claim 6, It is characterized in that The cobalt precursor in step 1) is selected from one or more of cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt citrate, and cobalt acetate; the nickel precursor in step 2) is selected from one or more of nickel acetate, nickel sulfate, nickel chloride, nickel citrate, and nickel nitrate; and the free radical scavenger is an alcohol organic solvent.

9. The preparation method according to claim 6, It is characterized in that In step 1), the concentration of the cobalt precursor in the aqueous solution is 1-80 mmol / L, the concentration of urea in the aqueous solution is 0.1-10 mmol / L, and the concentration of ammonium fluoride in the aqueous solution is 0.05-20 mmol / L; in step 2), the concentration of the nickel precursor is 1-100 mmol / L, the concentration of sodium selenosulfite is 1-100 mmol / L, and the concentration of the free radical scavenger is 1-80 mL / L.

10. The Co according to any one of claims 1 to 5 x Ni 1-x Se 2 @Co(OH) 2 Application of self-supporting composite materials as catalysts for electrochemical hydrogen and oxygen evolution reactions.

11. A self-supporting electrode, comprising a base electrode fixture and the Co according to any one of claims 1 to 5 x Ni 1-x Se 2 @Co(OH) 2 Self-supporting composite materials.

12. A device for producing hydrogen by electrolysis of water, It is characterized in that The water electrolysis hydrogen production device comprises the self-supporting electrode according to claim 11.

Citation Information

Patent Citations

  • Graphene-loaded selenide nanoparticle electrolyzed water catalyst electrode and preparation method thereof

    CN117230472A

  • Nickel selenide / cobalt molybdenum oxide composite material, preparation method and application of nickel selenide / cobalt molybdenum oxide composite material in hydrogen evolution, oxygen evolution and full water splitting reaction

    CN117448874A

Cited By

  • Selenide heterojunction catalyst for coupling hydrogen evolution, method and application of selenide heterojunction catalyst in electro-catalysis of 5-hydroxymethylfurfural

    CN119465270A