Method for preparing electrocatalyst by utilizing cadmium-containing wastewater, electrocatalyst, working electrode containing electrocatalyst and application of working electrode

The preparation of electrocatalysts through electrochemical deposition and heat treatment has solved the problem of low recycling efficiency of cadmium-containing wastewater in the prior art, achieved efficient recycling and diversified utilization of cadmium elements, and demonstrated good CO selectivity in electrocatalytic reactions .

CN118880384APending Publication Date: 2024-11-01HUANENG CLEAN ENERGY RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411094259.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the process of recycling and utilization of cadmium-containing wastewater is complex, the process is long and the efficiency is low, and it has failed to effectively solve the problems of cadmium recycling and diversified utilization.

Method used

Electrocatalysts are prepared by pretreating cadmium-containing wastewater, electrochemical deposition and heat treatment, selective deposition and recovery of cadmium elements are achieved, and a working electrode of cadmium-containing electrocatalyst is prepared for electrocatalyzing carbon dioxide reduction reaction.

Benefits of technology

The process flow is simplified, the recovery efficiency of cadmium element and the stability of the electrocatalyst are improved, the specific recovery and diversified utilization of cadmium are achieved, and good CO selectivity is shown in the electrocatalytic reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880384A_ABST
    Figure CN118880384A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing an electrocatalyst by utilizing cadmium-containing wastewater, the electrocatalyst, a working electrode containing the electrocatalyst and application of the working electrode. The method comprises the steps of pretreatment of cadmium-containing wastewater, activation of a deposition substrate, electrochemical deposition, surface treatment and heat treatment to obtain the working electrode containing the electrocatalyst. According to the method, the pH of the cadmium-containing wastewater, the concentration of Cd < 2 + >, the voltage of electrochemical deposition and the heating temperature and atmosphere are particularly limited, the cadmium element can be recycled, the catalytic effect of the electrocatalyst is improved, and the method is relatively simple in preparation process, short in process, high in controllability, wide in application range, high in valuable metal recycling efficiency and suitable for industrial production. And the obtained electrocatalyst shows good CO selectivity in eCO2RR, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wastewater recovery and treatment, and in particular to a method for preparing an electrocatalyst by utilizing cadmium-containing wastewater, an electrocatalyst, an electrocatalyst-containing working electrode and applications thereof. Background Art

[0002] Cadmium (Cd) is a heavy metal that is commonly found in industrial wastewater. It has obvious biological toxicity, neurotoxicity and reproductive toxicity. It is easy to form complex pollution with other heavy metals in the environment, causing further harm to soil and water quality. Due to the biological and environmental hazards of cadmium, it is crucial to treat cadmium-containing wastewater. At present, there are many methods for treating cadmium ions, such as adsorbents, chemical precipitation, ion exchange, and membrane separation. However, the various methods differ in applicable scenarios and costs. For example, the chemical precipitation method is simple to operate, but the type and amount of precipitants must be strictly controlled during the process, and the sludge that may be generated must be treated; the ion exchange method has a high recovery purity, but the cost of ion exchange resin is high; the adsorption method has a low operating cost, but due to the capacity limitation of the adsorbent, the adsorbent needs to be replaced frequently, and there are certain difficulties in subsequent recovery; membrane separation technology is efficient and clean, but the membrane material is susceptible to pollution and clogging, and may even fail to work properly, and has not yet achieved full coupling with downstream utilization. Summary of the invention

[0003] The main purpose of the present invention is to provide a method for preparing an electrocatalyst using cadmium-containing wastewater, an electrocatalyst, an electrocatalyst-containing working electrode and its application, so as to solve the problems of complex process, long process and low efficiency in the prior art for recycling cadmium-containing wastewater.

[0004] In order to achieve the above object, according to one aspect of the present invention, a method for preparing electrocatalyst using cadmium-containing wastewater is provided, comprising the following steps: Step S1, pretreatment of cadmium-containing wastewater: adjusting the pH of the cadmium-containing wastewater to 2.5-7, Cd 2+ The concentration is 0.01 to 0.5 mol / L to obtain a pretreatment solution; step S2, electrocatalyst preparation: step S21, activating the deposition substrate, and then immersing it in the pretreatment solution to perform electrochemical deposition to obtain a deposition working electrode; step S22, sequentially performing surface treatment and heat treatment on the deposition working electrode to obtain an electrocatalyst-containing working electrode; the electrocatalyst-containing working electrode includes a deposition substrate and an electrocatalyst deposited on the surface of the deposition substrate; wherein the voltage of the electrochemical deposition is -0.45 to -0.69 V; the heat treatment includes a heating step, the heating temperature is 250 to 350°C, and the heating atmosphere includes a first inert gas.

[0005] Furthermore, step S1 further comprises the following steps: step S11, adjusting the pH of the cadmium-containing wastewater to 2-4 to obtain a first solution; step S12, filtering the first solution to obtain a second solution; step S13, adjusting the pH of the second solution to 2.5-7, Cd 2+ The concentration is 0.01 to 0.5 mol / L to obtain a pretreatment solution; preferably, step S11 also includes the step of purging the first solution with a second inert gas; and / or step S13 also includes the step of introducing a third inert gas into the pretreatment solution; more preferably, the first inert gas, the second inert gas, and the third inert gas are independently selected from nitrogen, helium or argon.

[0006] Further, in step S21, the deposition substrate includes one or more of activated carbon paper, carbon cloth, stainless steel mesh and titanium felt; and / or the activation includes the following steps: using the deposition substrate as the first working electrode, performing a first cyclic voltammetry scan; preferably, during the first cyclic voltammetry scan, using one or more of HClO4, H2SO4, H3PO4, H2C2O4, NaHSO4 and KHSO4 as the first electrolyte, and using platinum as the first counter electrode; preferably, the voltage of the first cyclic voltammetry scan is -0.2~1.0V, the scan rate is 2~20mV / s, and the number of cycles is 15~25.

[0007] Furthermore, in step S21, the electrochemical deposition time is 5 to 20 minutes and the temperature is 20 to 40°C.

[0008] Further, in step S22, the surface treatment includes the following steps: using the deposited working electrode as the second working electrode, using an alkaline aqueous solution and a tannic acid mixture as the second electrolyte, and using platinum as the second counter electrode to perform a second cyclic voltammetry scan; preferably, during the second cyclic voltammetry scan, the alkaline aqueous solution includes one or more of a KOH aqueous solution, a NaOH aqueous solution, a K2CO3 aqueous solution and a KHCO3 aqueous solution; more preferably, in the second electrolyte, the molar concentration of the alkaline aqueous solution is 0.1 to 1 M, and / or the concentration of tannic acid in the second electrolyte is 3 to 8 g / L; preferably, the voltage of the second cyclic voltammetry scan is 0 to -0.65 V, the scan rate is 2 to 20 mV / s, and the number of cycles is 2 to 10.

[0009] Furthermore, in step S23, the heating time is 10 to 20 minutes, and the heating rate is 5 to 20°C / min; and / or the heat treatment also includes an annealing step; preferably, the annealing temperature is 15 to 40°C, and the time is 10 to 20 minutes.

[0010] According to another aspect of the present invention, there is provided an electrocatalyst obtained according to the above-mentioned method for preparing an electrocatalyst using cadmium-containing wastewater.

[0011] Furthermore, the weight percentage of the cadmium-containing substance in the electrocatalyst is ≥85%; and / or the cadmium-containing substance includes cadmium element, cadmium hydroxide and cadmium oxide; preferably, by weight percentage, the cadmium-containing substance includes 65-75% of cadmium element, 15-25% of cadmium hydroxide and the remainder of cadmium oxide.

[0012] According to another aspect of the present invention, there is provided an electrocatalyst-containing working electrode, which is obtained according to the above-mentioned method for preparing an electrocatalyst using cadmium-containing wastewater.

[0013] Furthermore, the loading amount of the electrocatalyst in the electrocatalyst-containing working electrode is 0.2 to 7 mg / cm 2 .

[0014] According to another aspect of the present invention, an electrocatalytic system is provided, which is used for electrocatalytic reduction of carbon dioxide. In the electrocatalytic system, the electrocatalyst-containing working electrode is used as the third working electrode, and Ag / Ag + The electrode is used as a reference electrode, a platinum electrode is used as a third pair of electrodes, an ionic liquid-acetonitrile solution saturated with CO2 is used as a cathode solution, and HClO4 and / or H2SO4 is used as an anode solution.

[0015] Furthermore, the surface of the electrocatalyst-containing working electrode further comprises a perfluorosulfonic acid resin; preferably, the raw material of the perfluorosulfonic acid resin comprises a perfluorosulfonate ionomer, more preferably one or more of potassium perfluoro-1-octanesulfonate, potassium perfluoro-1-butanesulfonate, sodium perfluoro-1-pentanesulfonate, potassium perfluoro-1-hexanesulfonate and perfluorooctanesulfonic acid; and / or Ag / Ag + The electrode includes AgNO3 and / or tetrabutylammonium tetrafluoroborate-acetonitrile solution; and / or the ionic liquid includes 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium perchlorate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium dihydrogen phosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate and 1-hexyl-3-methylimidazolium tetrafluoroborate. One or more; and / or the reaction potential of the electrocatalytic system is -1.8 to -3.2 V (relative to Ag / Ag + Electrode); preferably, the CO product Faraday efficiency of the electrocatalytic system is ≥90%, and / or the CO generation rate is ≥0.2L / (cm 2 h).

[0016] By applying the technical solution of the present invention, cadmium-containing wastewater is used as raw material, and electric energy is used as the basis, and an electrocatalyst is prepared in situ by electrochemical means. On the one hand, the cadmium-containing wastewater is effectively utilized, and on the other hand, the electrocatalyst can be directly obtained to achieve specific recovery and multiple utilization of the cadmium element. Moreover, the preparation process of this method is relatively simple, the process is short, the controllability is strong, the application range is wide, the recovery efficiency of valuable metals is high, and the application prospects are broad. In addition, the method of the present invention effectively improves the stability of the electrocatalyst by heat treatment, and the obtained electrocatalyst shows good CO selectivity in eCO2RR. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 A schematic diagram of a process for producing an electrocatalyst using cadmium-containing wastewater according to Example 1 of the present invention is shown;

[0019] Figure 2 A schematic diagram of an electrolysis device used in a deposition process according to Example 1 of the present invention is shown;

[0020] Figure 3 A schematic diagram of an electrolysis device used in the electrochemical catalytic reduction of carbon dioxide according to Example 1 of the present invention is shown;

[0021] Figure 4 The performance test results of the electrocatalyst-containing working electrode for electrocatalyst reduction of carbon dioxide according to Example 1 of the present invention are shown; and

[0022] Figure 5 TEM images of the electrocatalyst-containing working electrodes according to Example 1 of the present invention and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0024] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged under appropriate circumstances to describe the embodiments of the present invention.

[0025] Terminology explanation:

[0026] eCO2RR: Electrocatalytic carbon dioxide reduction reaction, which uses electrochemical methods to convert carbon dioxide into useful compounds such as CO.

[0027] As described in the background of the present invention, the prior art has the problems of complex process, long process and low efficiency in recycling cadmium-containing wastewater. In order to solve the above problems, in a typical embodiment of the present invention, a method for preparing electrocatalyst using cadmium-containing wastewater is provided, comprising the following steps: Step S1, pretreatment of cadmium-containing wastewater: adjusting the pH of cadmium-containing wastewater to 2.5-7, Cd 2+ The concentration is 0.01 to 0.5 mol / L to obtain a pretreatment solution; step S2, electrocatalyst preparation: step S21, activating the deposition substrate, and then immersing it in the pretreatment solution to perform electrochemical deposition to obtain a deposition working electrode; step S22, sequentially performing surface treatment and heat treatment on the deposition working electrode to obtain an electrocatalyst-containing working electrode; the electrocatalyst-containing working electrode includes a deposition substrate and an electrocatalyst deposited on the surface of the deposition substrate; wherein the voltage of the electrochemical deposition is -0.45 to -0.69 V; the heat treatment includes a heating step, the heating temperature is 250 to 350°C, and the heating atmosphere includes a first inert gas.

[0028] In the method of the present invention, the pH of the cadmium-containing wastewater is first adjusted to 2.5-7 to dissolve out metal elements, such as oxides, hydroxides, sulfides, selenides, etc. of cadmium and zinc, reduce the content of impurity elements in the sediment layer, and adjust the Cd 2+ The concentration is 0.01-0.5 mol / L to enrich cadmium ions and pave the way for the recovery of cadmium elements in the subsequent electrochemical deposition step. It should be noted that the present invention specifically limits the amount of Cd in the pretreatment solution to 2+ The concentration is 0.01~0.5mol / L because Cd 2+ It is beneficial to increase the rate of subsequent electrochemical deposition, as well as to increase the thickness and uniformity of the deposited layer. It is also beneficial to obtain a stable crystal structure (such as crystals with crystal faces such as Cd (110), Cd (100), and Cd (111)) and a suitable grain size, thereby improving the structural stability and electrocatalytic performance of the electrocatalyst.

[0029] In addition, the deposition substrate is activated to increase the roughness of the substrate surface and increase the activity of the substrate surface, which is conducive to the adsorption and deposition of Cd on the substrate surface. 2+ , which is beneficial to improve the deposition rate, deposition quality and Cd 2+ It can also improve the recovery rate, improve the crystallinity and density of the deposited layer, remove oxides or other impurities on the surface of the deposited substrate, and increase the bonding strength between the deposited layer and the substrate, which is further beneficial to improving the stability of the electrocatalyst during use.

[0030] Then, the activated deposition substrate is immersed in the above-mentioned pretreatment solution to perform electrochemical deposition to obtain a deposition working electrode. The present invention particularly limits the voltage of the electrochemical deposition to -0.45 to -0.69 V. Within this potential range, the cadmium element in the cadmium-containing wastewater can be selectively deposited (such as: when treating electroplating (zinc) cadmium wastewater containing both cadmium and zinc, the deposition amount of the zinc element is negligible, and the cadmium element is selectively deposited), the deposition of other metal elements in the wastewater is reduced, the purity of cadmium in the deposition layer is improved, and the full recycling of the cadmium element is achieved, and the recovery efficiency of cadmium is high.

[0031] Next, the deposited working electrode is subjected to surface treatment. This process can effectively remove impurities and dirt on the electrode surface, making the electrode surface clean. It can also increase the active sites on the electrode surface, which helps to improve the electrochemical activity of the electrode, and further facilitates the adsorption and deposition of Cd ions on its surface. Then, the deposited working electrode is subjected to heat treatment. According to the laws of thermodynamics and kinetics, the crystal structure and organization of the electrode's effective components are effectively improved, which is conducive to improving the stability and conductivity of the electrode, so that the electrode can stably play its role in the process of electrocatalytic reduction of carbon dioxide.

[0032] It should be noted that the present invention specifically limits the heating temperature to 250-350°C, and the heated atmosphere includes a first inert gas. The inventor unexpectedly found during the experiment that within this temperature range, under the joint action of thermodynamics and kinetics, the crystal structure of the deposited layer can be significantly changed, and the various crystal interfaces in the crystal are significantly increased, which is beneficial to increase the surface active sites of the catalyst main structure and improve the working electrode reaction activity, thereby helping to improve the catalytic performance and structural stability of the catalyst layer. If the heating temperature is higher than 350°C, the catalyst layer will fall off and break, which is not conducive to the stability of the working electrode; if the heating temperature is lower than 250°C, the grain boundary transformation of the deposited layer will not be obvious, which is not conducive to improving the reaction activity. In addition, the inventor also found that heating under an inert atmosphere can effectively prevent the oxidation of cadmium, which is beneficial to improve the activity and stability of cadmium, and then to improve the catalytic performance and service life of the electrocatalyst.

[0033] In summary, the present invention uses cadmium-containing wastewater as raw material and electric energy as the basis to prepare electrocatalysts in situ by electrochemical means. On the one hand, cadmium-containing wastewater is effectively utilized, and on the other hand, electrocatalysts can be directly obtained to achieve specific recovery and multiple utilization of cadmium elements. Moreover, the preparation process of the method of the present invention is relatively simple, the process is short, the controllability is strong, the application range is wide, the recovery efficiency of valuable metals is high, and the application prospects are broad. Moreover, the method of the present invention is conducive to fully recovering cadmium elements, reducing the deposition of other metal elements, and increasing the content of cadmium-containing substances in the deposition layer by controlling the voltage of electrochemical deposition, which is further conducive to improving the catalytic effect of the electrocatalyst. In addition, the present invention is conducive to improving the catalytic performance and stability of the electrocatalyst by setting a heat treatment step and limiting the temperature and atmosphere of the heat treatment within a specific range.

[0034] In a preferred embodiment, the cadmium-containing wastewater includes Cd 2+ and Zn 2+ , the molar ratio of the two is (5-10): 1. Preferably, in the cadmium-containing wastewater, the metal cation components include Cd 2+ 、Zn 2+ ; Preferably, the anion components in the cadmium-containing wastewater include NO3 - , Cl - OH - 、SO4 2- 、CH3COO - , EDTA and CN - In a preferred embodiment, step S1 further comprises the following steps: step S11, adjusting the pH of the cadmium-containing wastewater to 2-4 to obtain a first solution; step S12, filtering the first solution to obtain a second solution; step S13, adjusting the pH of the second solution to 2.5-7, Cd 2+ The concentration is 0.01-0.5 mol / L to obtain a pretreatment solution. First, adjust the pH of the cadmium-containing wastewater to 2-4, which is more conducive to the dissolution of cadmium-containing substances and can significantly reduce the removal of CN - After filtering the first solution, adjust the pH to 2.5-7, Cd 2+ The concentration is 0.01 to 0.5 mol / L, which is more conducive to reducing energy consumption during the deposition process and reducing the impurity content in the deposition layer, thereby being able to more fully recycle the cadmium element, improve the catalytic effect of the electrocatalyst, and have a higher cadmium recovery efficiency.

[0035] In order to more effectively reduce the volatile substances (such as HCN) in the first solution, in a preferred embodiment, preferably, step S11 also includes the step of purging the first solution with a second inert gas. Under the above conditions, the energy consumption in the electrochemical process can be more effectively reduced, and the cadmium element can be more effectively separated and recovered, thereby improving the safety of the electrochemical process.

[0036] Conventional reagents can be used in the process of adjusting the pH of the solution. In order to reduce the introduced impurity elements, in a preferred embodiment, one or more of nitric acid, sulfuric acid and hydrochloric acid are used to adjust the pH of the cadmium-containing wastewater; preferably, one or more of nitric acid, potassium nitrate and hydrochloric acid are used to adjust the pH of the second solution. In a preferred embodiment, step S13 also includes the step of introducing a third inert gas into the pretreatment solution; more preferably, the first inert gas, the second inert gas, and the third inert gas are independently selected from nitrogen, helium or argon. Under the above conditions, the interference of gases such as O2 on cadmium deposition and recovery can be more effectively reduced.

[0037] In a preferred embodiment, in step S21, the deposition substrate includes one or more of activated carbon paper, carbon cloth, stainless steel mesh and titanium felt. The above-mentioned types of deposition substrates have better conductivity, are more conducive to the transmission of electrons, and increase the rate of electrochemical reactions. In order to more quickly and effectively achieve the cleaning and activation of the working electrode, in a preferred embodiment, the activation includes the following steps: using the deposition substrate as the first working electrode, performing a first cyclic voltammetric scan; preferably, during the first cyclic voltammetric scan, using one or more of HClO4, H2SO4, H3PO4, H2C2O4, NaHSO4 and KHSO4 as the first electrolyte, and platinum as the first counter electrode; preferably, the voltage of the first cyclic voltammetric scan is -0.2~1.0V (vs. standard hydrogen electrode), the scan rate is 2~20mV / s, and the number of cycles is 15~25.

[0038] In order to further improve the thickness and uniformity of the deposited layer, thereby being more conducive to improving the working efficiency and stability of the working electrode during the electrochemical deposition process, in a preferred embodiment, in step S21, the electrochemical deposition time is 5 to 20 minutes and the temperature is 20 to 40°C.

[0039] In order to further increase the active sites of the deposited layer, in a preferred embodiment, in step S22, the surface treatment includes the following steps: using the deposited working electrode as the second working electrode, using an alkaline aqueous solution and a mixture of tannic acid as the second electrolyte, and using platinum as the second counter electrode to perform a second cyclic voltammetric scan. Preferably, during the second cyclic voltammetric scan, the alkaline aqueous solution includes one or more of a KOH aqueous solution, a NaOH aqueous solution, a K2CO3 aqueous solution, and a KHCO3 aqueous solution; more preferably, in the second electrolyte, the molar concentration of the alkaline aqueous solution is 0.1 to 1M, and / or the mass concentration of tannic acid in the second electrolyte is 3 to 8 g / L. Under the above conditions, the alkaline aqueous solution and tannic acid can cooperate with each other to reconstruct the surface of the deposited layer according to the laws of thermodynamics and kinetics to produce Cd / Cd(OH) X In a preferred embodiment, the voltage of the second cyclic voltammetry scan is 0 to -0.65 V (vs. standard hydrogen electrode), the scan rate is 2 to 20 mV / s, and the number of cycles is 2 to 10. Under the above conditions, the thickness of the deposited layer is thicker and the recovery rate of cadmium is higher.

[0040] In a preferred embodiment, in step S23, the heating time is 10 to 20 minutes, and the rate is 5 to 20°C / min. Under the above conditions, the temperature difference between the surface temperature and the internal temperature of the deposited layer can be more effectively reduced, the thermal stress concentration can be effectively suppressed, the risk of cracking and deformation of the deposited layer can be reduced, and the side reactions between the elements can be reduced, which is more conducive to improving the quality and catalytic performance of the electrocatalyst. In a preferred embodiment, the heat treatment also includes an annealing step; preferably, the annealing medium is one or more of water, liquid nitrogen and liquid ammonia; the annealing temperature is 15 to 40°C and the time is 10 to 20 minutes. Under the above conditions, the structure of the catalyst can be made more stable through the quenching effect, which is more conducive to improving the reaction activity and stability of the catalyst.

[0041] In another typical embodiment of the present invention, an electrocatalyst is provided, which is obtained according to the above method of preparing an electrocatalyst using cadmium-containing wastewater. The raw material of the electrocatalyst of the present invention is cadmium-containing wastewater, which realizes the specific recovery and multiple utilization of cadmium elements, and the preparation process of the electrocatalyst is simple, with fewer processes and low costs, and has good catalytic performance for carbon dioxide.

[0042] In a preferred embodiment, the weight percentage of the cadmium-containing substance in the electrocatalyst is ≥ 85%; preferably, the cadmium-containing substance includes cadmium element, cadmium hydroxide and cadmium oxide; preferably, by weight percentage, the cadmium-containing substance includes 65-75% cadmium element, 15-25% cadmium hydroxide and the remainder cadmium oxide. Under the above conditions, the recovery rate of cadmium element is higher, the content of cadmium element in the electrocatalyst is higher, and the full recovery and utilization of cadmium is achieved.

[0043] In another typical embodiment of the present invention, there is also provided an electrocatalyst-containing working electrode, which is obtained according to the above-mentioned method of using cadmium-containing wastewater to prepare electrocatalysts. The raw materials of the electrocatalyst-containing working electrode of the present invention include cadmium-containing wastewater, which realizes the specific recovery and multiple utilization of cadmium elements, and the preparation process of the electrocatalyst-containing working electrode is simple, with fewer processes and low costs, and has good catalytic performance for carbon dioxide. In a preferred embodiment, in the electrocatalyst-containing working electrode, the loading amount of the electrocatalyst is 0.2 to 7 mg / cm 2 Under the above conditions, the loading amount of electrocatalyst in the electrocatalyst working electrode is higher.

[0044] In another typical embodiment of the present invention, an electrocatalytic system is provided, which is used for electrocatalytic reduction of carbon dioxide, using the electrocatalyst-containing working electrode as the third working electrode, and using Ag / Ag + The electrode is used as a reference electrode, the platinum electrode is used as a third pair of electrodes, the CO2-saturated ionic liquid-acetonitrile solution is used as a cathode solution, and HClO4 and / or H2SO4 are used as an anode solution. The raw material of the electrocatalytic system of the present invention comprises cadmium removal wastewater, which realizes the full recovery and utilization of cadmium elements, and the system has good catalytic activity for carbon dioxide and good electrocatalytic reduction effect.

[0045] In order to further improve and enhance the stability and durability of the electrocatalyst-containing working electrode of the present invention, in a preferred embodiment, the surface of the electrocatalyst-containing working electrode also includes a perfluorosulfonic acid resin; preferably, the raw material of the perfluorosulfonic acid resin includes a perfluorosulfonate ionomer, more preferably one or more of potassium perfluoro-1-octanesulfonate, potassium perfluoro-1-butanesulfonate, sodium perfluoro-1-pentanesulfonate, potassium perfluoro-1-hexanesulfonate and perfluorooctane sulfonic acid.

[0046] In a preferred embodiment, Ag / Ag +The electrode includes AgNO3 and / or tetrabutylammonium tetrafluoroborate-acetonitrile solution. In a preferred embodiment, the ionic liquid includes 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium perchlorate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium dihydrogen phosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate and 1-hexyl-3-methylimidazolium tetrafluoroborate. In a preferred embodiment, the reaction potential of the electrocatalytic system is -1.8 to -3.2 V (relative to Ag / Ag + Electrode), under this condition, the electrocatalytic system operates more stably and has a better catalytic effect on carbon dioxide. Preferably, the CO product Faraday efficiency of the electrocatalytic system is ≥90%, and / or the CO generation rate is ≥0.2L / (cm 2 h).

[0047] Typically but not limiting, the voltage of electrochemical deposition is a range consisting of any two values ​​of -0.45V, -0.5V, -0.55V, -0.6V, -0.65V, -0.69V, the time is 5min, 10min, 15min, 20min or a range consisting of any two values ​​thereof, and the temperature is 20°C, 30°C, 40°C or a range consisting of any two values ​​thereof.

[0048] Typically but not limiting, the heating temperature is 250°C, 300°C, 350°C or a range consisting of any two of them, the heating time is 10min, 15min, 20min or a range consisting of any two of them, and the heating rate is 5°C / min, 10°C / min, 15°C / min, 20°C / min or a range consisting of any two of them;

[0049] Typically but not limiting, the molar concentration of the alkaline aqueous solution is 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, 0.6M, 0.7M, 0.8M, 0.9M, 1M or a range consisting of any two of them; the concentration of tannic acid is 3g / L, 4g / L, 5g / L, 6g / L, 7g / L, 8g / L or a range consisting of any two of them;

[0050] Typically but not limiting, the weight percentage of the cadmium-containing substance in the electrocatalyst is 85%, 90%, 95%, 99%, 100% or a range consisting of any two of them; in the electrocatalyst-containing working electrode, the loading amount of the electrocatalyst is 0.2 mg / cm 2, 0.5mg / cm 2 , 1mg / cm 2 , 1.5mg / cm 2 , 2mg / cm 2 、3mg / cm 2 , 4mg / cm 2 , 5mg / cm 2 , 6mg / cm 2 , 7mg / cm 2 Or a range of values ​​consisting of any two of them.

[0051] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0052] Example 1

[0053] See the schematic diagram of the process of using cadmium-containing wastewater to produce electrocatalysts. Figure 1 .

[0054] Step S1, pretreatment of cadmium-containing wastewater:

[0055] Take 100mL of cadmium-containing wastewater (the main metal cation component in the wastewater is Cd 2+ 、Zn 2+ , anion is NO3 - , Cl - , OH - , SO4 2- , CH3COO - , EDTA, CN - etc., among which Cd 2+ and Zn 2+ The first solution was filtered for three times to obtain a second solution, and the pH of the solution was adjusted to 5 using a 3M nitric acid solution. The Cd content of the solution was tested using an inductively coupled plasma mass spectrometry method. 2+ concentration, Cd 2+ The solution was adjusted to 0.1 M to obtain a pretreatment solution, into which nitrogen was introduced for 20 minutes (with a flow rate of 15 sccm) until saturation.

[0056] Step S2, electrocatalyst preparation:

[0057] In the electrolytic cell 1, a porous activated carbon paper (area 10×10 cm 2) was used as the working electrode, and at an ambient temperature of 25°C, 1 M HClO4 solution was used as the electrolyte, platinum was used as the counter electrode, the potential range was -0.2~1.0 V (vs. RHE), and 20 cycles of cyclic voltammetry scanning were performed at a scan rate of 10 mV / s to activate the deposited substrate. The substrate was then rinsed with ultrapure water and acetone, respectively, and dried in a vacuum oven (80°C) to obtain an activated deposited substrate.

[0058] After sufficient drying, in the electrolytic cell 2, the above activated deposition substrate and pretreatment solution were used as the working electrode and electrolyte, respectively, at an ambient temperature of 25°C, with magnetic stirring (300 rpm), and a constant potential of -0.6 V (vs. RHE) was set for deposition for 15 minutes to obtain a deposition working electrode. The schematic diagram of the electrolytic device used in the deposition process is shown in Figure 2 .

[0059] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 0.5M KOH solution containing tannic acid at a concentration of 5 g / L, and a CV scan was performed in the range of 0 to -0.65 V (vs. RHE), with a scan rate of 10 mV / s and a number of cycles of 3. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone in turn, and dried in a vacuum drying oven (80° C.).

[0060] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 10°C / min to heat to 300°C. After maintaining for 15 minutes, cool to 25°C (20°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / carbon composite electrode, which is stored for later use.

[0061] Step S3, performance verification:

[0062] For the composite electrode, cut out 2×2 cm 2 The electrode was used as the eCO2RR working electrode, and 60 mL of 0.05 wt% Nafion solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. The cathode solution was a 0.5 M [Bmim]PF6-MeCN solution saturated with CO2, and the reference electrode was Ag / Ag + The electrode is (0.01M AgNO3+0.1MTBAP-MeCN solution), the counter electrode is a platinum electrode, and the anode solution is a 0.5M H2SO4 solution. At -1.8~-3.2V (relative to Ag / Ag + In the potential range of the electrode, starting from -0.9V, a constant potential test was performed at every -0.1V interval, and gas chromatography and nuclear magnetic resonance (hydrogen spectrum) were used to detect gas and liquid products respectively. The schematic diagram of the electrolysis device used in the electrochemical catalytic reduction of carbon dioxide is shown in Figure 3 .

[0063] The performance test results of the electrocatalyst-containing working electrode for electrocatalytic reduction of carbon dioxide are as follows: Figure 4 It can be seen that the working electrode has a good catalytic effect on CO2 conversion, and can maintain more than 90% of the CO product Faraday efficiency (FE co ), the Faraday efficiency reached 98.0% at -2.3V, and the highest CO generation rate in the test range could reach 0.227L / (cm 2 h). TEM image of the working electrode containing the electrocatalyst is shown in Figure 5 A. As can be seen from the figure, there are abundant grain boundaries on the catalyst surface, which produces abundant unsaturated sites, which have high activity in the catalytic reaction and significantly improve the catalytic effect of the working electrode.

[0064] Example 2

[0065] See the schematic diagram of the process of using cadmium-containing wastewater to produce electrocatalysts. Figure 1 .

[0066] Step S1, pretreatment of cadmium-containing wastewater:

[0067] Take 100mL of cadmium-containing wastewater (the main metal cation component in the wastewater is Cd 2+ 、Zn 2+ , anion is NO3 - , Cl - , OH - , SO4 2- , CH3COO - , EDTA, CN - etc., among which Cd 2+ and Zn 2+ The first solution was filtered for three times to obtain a second solution, and the pH of the solution was adjusted to 3 using a 3M hydrochloric acid solution. The Cd content of the solution was tested using an inductively coupled plasma mass spectrometry method. 2+ concentration, Cd 2+ The concentration was adjusted to 0.05 M to obtain a pretreatment solution, into which nitrogen gas was introduced for 30 minutes (with a flow rate of 15 sccm) until saturation.

[0068] Step S2, electrocatalyst preparation:

[0069] In electrolytic cell 1, titanium felt (area 5×5cm 2) as the working electrode, at an ambient temperature of 25°C, using 1M H2SO4 solution as the electrolyte, platinum as the counter electrode, the potential range is -0.2~1.0V (vs.RHE), and 20 cycles of cyclic voltammetry scanning are performed at a scan rate of 15mV / s to activate the deposited substrate. Subsequently, it is rinsed with ultrapure water and acetone, respectively, and dried in a vacuum oven (80°C) to obtain the activated deposited substrate.

[0070] After sufficient drying, in the electrolytic cell 2, the above activated deposition substrate and pretreatment solution were used as the working electrode and electrolyte, respectively, at an ambient temperature of 25°C, with magnetic stirring (250 rpm), and a constant potential of -0.6 V (vs. RHE) was set for deposition for 25 minutes to obtain a deposition working electrode. The schematic diagram of the electrolytic device used in the deposition process is shown in Figure 2 .

[0071] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 0.1M KOH solution with a concentration of 5 g / L tannic acid, and a CV scan was performed in the range of 0 to -0.65 V (vs. RHE), with a scan rate of 10 mV / s and a number of cycles of 3. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone in turn, and dried in a vacuum drying oven (80°C).

[0072] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 10°C / min to heat to 300°C. After maintaining for 15 minutes, cool to 25°C (20°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / titanium composite electrode, which is stored for later use.

[0073] Step S3, performance verification:

[0074] For the composite electrode, cut out 2×2 cm 2 The electrode was used as the eCO2RR working electrode, and 50 mL of 0.05 wt% Nafion solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. The cathode solution was a 0.5 M [Bmim]PF6-MeCN solution saturated with CO2, and the reference electrode was Ag / Ag + electrode (0.01M AgNO3+0.1MTBAP-MeCN solution), the counter electrode is a platinum electrode, the anode solution is a 0.5M H2SO4 solution, and the voltage range is -1.8~-3.2V (relative to Ag / Ag + Electrode). See the schematic diagram of the electrolysis device used in the electrochemical catalytic reduction of carbon dioxide. Figure 3 .

[0075] Example 3

[0076] Step S1, pretreatment of cadmium-containing wastewater:

[0077] Take 100mL of cadmium-containing wastewater (the main metal cation component in the wastewater is Cd 2+ 、Zn 2+ , anion is NO3 - , Cl - , OH - , SO4 2- , CH3COO - , EDTA, CN - etc., among which Cd 2+ and Zn 2+ The first solution was filtered for three times to obtain a second solution, and the pH of the solution was adjusted to 3 using a 3M hydrochloric acid solution. The Cd content of the solution was tested using an inductively coupled plasma mass spectrometry method. 2+ concentration, Cd 2+ The concentration was adjusted to 0.01 M to obtain a pretreatment solution, into which helium was introduced for 15 minutes (with a flow rate of 20 sccm) until saturation.

[0078] Step S2, electrocatalyst preparation:

[0079] In the electrolytic cell 1, a stainless steel mesh (area 10×10 cm 2 ) was used as the working electrode, and at an ambient temperature of 25°C, 1 M H3PO4 solution was used as the electrolyte, platinum was used as the counter electrode, the potential range was -0.2~1.0 V (vs. RHE), and 25 cycles of cyclic voltammetry were performed at a scan rate of 5 mV / s to activate the deposited substrate. The substrate was then rinsed with ultrapure water and acetone, respectively, and dried in a vacuum oven (80°C) to obtain the activated deposited substrate.

[0080] After sufficient drying, in electrolytic cell 2, the above-mentioned activated deposition substrate and pretreatment solution are used as the working electrode and electrolyte, respectively. At an ambient temperature of 20°C and magnetic stirring (200 rpm), a constant potential of -0.45 V (vs. RHE) is set and deposition is carried out for 20 minutes to obtain a deposited working electrode.

[0081] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 0.5M KOH solution containing tannic acid at a concentration of 5 g / L, and a CV scan was performed in the range of 0 to -0.7 V (vs. RHE), with a scan rate of 10 mV / s and a number of cycles of 3. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone in turn, and dried in a vacuum drying oven (80° C.).

[0082] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 10°C / min to heat to 250°C. After maintaining for 15 minutes, cool to 25°C (20°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / stainless steel composite electrode, which is stored for later use.

[0083] Step S3, performance verification:

[0084] For the composite electrode, cut out 2×2 cm 2 The electrode was used as the eCO2RR working electrode, and 60 mL of 0.05 wt% Nafion solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. The cathode solution was a 0.5 M [Bmim]PF6-MeCN solution saturated with CO2, and the reference electrode was Ag / Ag + The electrode was a platinum electrode (0.01M AgNO3+0.1MTBAP-MeCN solution), the counter electrode was a platinum electrode, the anode solution was a 0.5M H2SO4 solution, and the potential range was -1.8 to -3.2 V (relative to Ag / Ag + electrode).

[0085] Example 4

[0086] Step S1, pretreatment of cadmium-containing wastewater:

[0087] Take 100mL of cadmium-containing wastewater (the main metal cation component in the wastewater is Cd 2+ 、Zn 2+ , anion is NO3 - , Cl - , OH - , SO4 2- , CH3COO - , EDTA, CN - etc., among which Cd 2+ and Zn 2+ The first solution was filtered for three times to obtain a second solution, and the pH of the solution was adjusted to 7 using a 3M potassium nitrate solution. The Cd content of the solution was tested using an inductively coupled plasma mass spectrometry method. 2+ concentration, Cd 2+ The solution was adjusted to 0.5 M to obtain a pretreatment solution, into which argon gas was introduced for 25 minutes (with a flow rate of 10 sccm) until saturation.

[0088] Step S2, electrocatalyst preparation:

[0089] In electrolytic cell 1, a carbon cloth (area 10×10 cm 2 ) was used as the working electrode, and at an ambient temperature of 25°C, 1 M H2C2O4 solution was used as the electrolyte, platinum was used as the counter electrode, the potential range was -0.2~1.0 V (vs. RHE), and 15 cycles of cyclic voltammetry were performed at a scan rate of 15 mV / s to activate the deposited substrate. The substrate was then rinsed with ultrapure water and acetone, respectively, and dried in a vacuum oven (80°C) to obtain the activated deposited substrate.

[0090] After sufficient drying, in electrolytic cell 2, the above-mentioned activated deposition substrate and pretreatment solution are used as the working electrode and electrolyte respectively. At an ambient temperature of 40°C and magnetic stirring (400 rpm), a constant potential of -0.69 V (vs. RHE) is set and deposition is carried out for 5 minutes to obtain a deposited working electrode.

[0091] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 0.5M KOH solution containing tannic acid at a concentration of 5 g / L, and a CV scan was performed in the range of 0 to -0.7 V (vs. RHE), with a scan rate of 10 mV / s and a number of cycles of 3. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone in turn, and dried in a vacuum drying oven (80° C.).

[0092] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 10°C / min to heat to 350°C. After maintaining for 15 minutes, cool to 25°C (20°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / carbon composite electrode, which is stored for later use.

[0093] Step S3, performance verification:

[0094] For the composite electrode, cut out 2×2 cm 2 The electrode was used as the eCO2RR working electrode, and 60 mL of 0.05 wt% Nafion solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. The cathode solution was a 0.5 M [Bmim]PF6-MeCN solution saturated with CO2, and the reference electrode was Ag / Ag + The electrode was a platinum electrode (0.01M AgNO3+0.1MTBAP-MeCN solution), the counter electrode was a platinum electrode, the anode solution was a 0.5M H2SO4 solution, and the potential range was -1.8 to -3.2 V (relative to Ag / Ag + electrode).

[0095] Example 5

[0096] The only difference from Example 1 is:

[0097] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 1M NaOH solution containing 3 g / L tannic acid, and a CV scan was performed in the range of 0 to -0.65 V (vs. RHE), with a scan rate of 20 mV / s and a number of 2 cycles. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone in turn, and dried in a vacuum drying oven (80°C).

[0098] Example 6

[0099] The only difference from Example 1 is:

[0100] Then, the deposited working electrode was moved to the electrolytic cell 3, wherein the electrolyte was a 0.1M K2CO3 solution containing 8 g / L tannic acid, and CV scanning was performed in the range of 0 to -0.65 V (vs. RHE), with a scanning rate of 5 mV / s and 10 cycles. Then, the surface-treated working electrode was removed, and rinsed with nitrogen-saturated ultrapure water and nitrogen-saturated acetone, and dried in a vacuum drying oven (80°C).

[0101] Example 7

[0102] The only difference from Example 1 is:

[0103] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 5°C / min to heat to 250°C. After maintaining for 20 minutes, cool to 25°C (15°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / carbon composite electrode, which is stored for later use.

[0104] Example 8

[0105] The only difference from Example 1 is:

[0106] After drying, use a tubular furnace in a helium atmosphere and set the heating rate to 20°C / min to heat to 350°C. After maintaining for 10 minutes, cool to 25°C (25°C / min cooling rate) to obtain an electrocatalyst-containing working electrode: a cadmium / carbon composite electrode, which is stored for later use.

[0107] Example 9

[0108] The only difference from Example 1 is:

[0109] For the composite electrode, cut out 2×2 cm 2The electrode was used as the eCO2RR working electrode, and 60 mL of 0.05 wt% potassium perfluoro-1-octane sulfonate solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. The cathode solution was a 0.5 M 1-butyl-3-methylimidazolium tetrafluoroborate-acetonitrile solution saturated with CO2, and the reference electrode was Ag / Ag + The counter electrode is a platinum electrode, the anode solution is a 0.5M HClO4 solution, and the voltage range is -1.8 to -3.2 V (relative to Ag / Ag + electrode).

[0110] Example 10

[0111] The only difference from Example 1 is:

[0112] For the composite electrode, cut out 2×2 cm 2 The electrode was used as the eCO2RR working electrode, and 60 mL of 0.05 wt% potassium perfluoro-1-butanesulfonate solution was spin-coated on the surface. After being fully dried in a vacuum oven (80 ° C), it was loaded into the electrolytic cell 4. Among them, the cathode solution was a 0.5 M 1-butyl-3-methylimidazole bis (trifluoromethylsulfonyl) imide-acetonitrile solution saturated with CO2, and the reference electrode was Ag / Ag + The counter electrode is a platinum electrode, the anode solution is a 0.5M H2SO4 solution, and the voltage range is -1.8 to -3.2 V (relative to Ag / Ag + electrode).

[0113] Comparative Example 1

[0114] The only difference from Example 1 is:

[0115] In step S23, annealing is performed in an air atmosphere. The TEM image of the obtained electrocatalyst-containing working electrode is shown in Figure 5 B.

[0116] It can be seen that, compared with Example 1, the catalyst obtained by annealing in an air atmosphere has less obvious grain boundaries in its microstructure and significantly reduced active sites, which in turn reduces the catalytic activity.

[0117] Comparative Example 2

[0118] The only difference from Example 1 is:

[0119] In step S23, no surface treatment and no heat treatment are performed.

[0120] Compared with Example 1, it can be seen that without surface treatment and heat treatment, the surface stability of the catalyst layer is low and abundant grain boundaries are not formed, resulting in relatively low activity.

[0121] Comparative Example 3

[0122] The only difference from Example 1 is:

[0123] In step S23, 1M KClO4 is used as an electrolyte to perform surface treatment on the working electrode.

[0124] Compared with Example 1, it can be seen that the surface sites of the working electrode are not active enough, which makes it difficult for Cd to adhere during surface deposition. The external voltage of the cell needs to be further increased, resulting in increased energy consumption and decreased flatness of the catalyst layer.

[0125] Comparative Example 4

[0126] The only difference from Example 1 is:

[0127] In step S22, the voltage of the electrochemical deposition is -0.7 to 2.0V.

[0128] Compared with Example 1, it can be seen that under the deposition condition of lower voltage, Zn 2+ The presence of metal elements such as ions may cause the catalyst layer composition to become complex, or may have a negative impact on the catalytic effect of the working electrode.

[0129] Comparative Example 5

[0130] The only difference from Example 1 is:

[0131] In the electrocatalytic reduction system of carbon dioxide, an Ag / AgCl (KCl is used as a reference solution) electrode is used as a reference electrode.

[0132] Compared with Example 1, it can be seen that the voltage value of the reaction system drifted after 1 h of reaction, mainly because Ag / AgCl (KCl as a reference solution) had poor stability in the ionic liquid-MeCN system.

[0133] The components of the electrocatalysts prepared in the above examples and comparative examples, and the catalytic data of the electrocatalytic systems on carbon dioxide are shown in Table 1.

[0134] Test method:

[0135] Electrochemical test: The test was carried out at room temperature and pressure (25°C, 1 atm).

[0136] Table 1

[0137]

[0138]

[0139] From the above, it can be seen that the amount of catalyst layer deposition is related to the deposition time and the pH of the acidified solution; the hydroxide content in the catalyst layer is related to the scanning number of the tannic acid / KOH solution, and the oxide is related to the annealing atmosphere. Appropriate hydroxide will help improve the performance of the catalyst layer; too high or too low annealing temperature will have a negative impact on the catalytic effect; the activation solution of the deposition substrate has a certain impact on its subsequent deposition efficiency; the type of ionic liquid for CO2 reduction and the type of reference electrode will affect the catalytic effect of the working electrode. The use of Ag / AgCl electrode is more effective than Ag / AgCl electrode. + The reference electrode is even less effective.

[0140] Compared with the comparative example, each embodiment of the present invention uses cadmium-containing wastewater as raw material and electric energy as the basis to prepare an electrocatalyst in situ by electrochemical means. On the one hand, the cadmium-containing wastewater is effectively utilized, and on the other hand, the electrocatalyst can be directly obtained to achieve specific recovery and multiple utilization of the cadmium element. Moreover, the preparation process of the method is relatively simple, the process is short, the controllability is strong, the application range is wide, the recovery efficiency of valuable metals is high, and the application prospects are broad. In addition, the method of the present invention effectively improves the stability of the electrocatalyst by heat treatment, and the obtained electrocatalyst shows good CO selectivity in eCO2RR. In addition, it can be seen that when each process parameter is within the preferred range of the present invention, the electrocatalyst loading in the working electrode is higher, and the CO selectivity of the electrocatalyst is better.

[0141] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing electrocatalyst using cadmium-containing wastewater, characterized in that: The following steps are involved: Step S1, pretreatment of cadmium-containing wastewater: adjusting the pH of the cadmium-containing wastewater to 2.5-7, Cd 2+ The concentration is 0.01-0.5 mol / L to obtain a pretreatment solution; Step S2, electrocatalyst preparation: Step S21, activating the deposition substrate, and then immersing it in the pretreatment solution to perform electrochemical deposition to obtain a deposition working electrode; Step S22, performing surface treatment and heat treatment on the deposited working electrode in sequence to obtain an electrocatalyst-containing working electrode; the electrocatalyst-containing working electrode comprises the deposited substrate and the electrocatalyst deposited on the surface of the deposited substrate; Wherein, the voltage of the electrochemical deposition is -0.45 to -0.69 V; the heat treatment includes a heating step, the heating temperature is 250 to 350° C., and the heating atmosphere includes a first inert gas.

2. The method according to claim 1, characterized in that The step S1 further comprises the following steps: Step S11, adjusting the pH of the cadmium-containing wastewater to 2-4 to obtain a first solution; Step S12, filtering the first solution to obtain a second solution; Step S13, adjusting the pH of the second solution to 2.5-7, Cd 2+ The concentration is 0.01-0.5 mol / L to obtain the pretreatment solution; Preferably, the step S11 further comprises the step of purging the first solution with a second inert gas; and / or the step S13 further comprises the step of introducing a third inert gas into the pretreatment solution; More preferably, the first inert gas, the second inert gas, and the third inert gas are independently selected from nitrogen, helium, or argon.

3. The method according to claim 1 or 2, characterized in that: In the step S21, The deposition substrate comprises one or more of activated carbon paper, carbon cloth, stainless steel mesh and titanium felt; and / or The activation comprises the following steps: using the deposition substrate as a first working electrode, performing a first cyclic voltammetry scan; Preferably, during the first cyclic voltammetry scan, one or more of HClO4, H2SO4, H3PO4, H2C2O4, NaHSO4 and KHSO4 are used as the first electrolyte, and platinum is used as the first counter electrode; Preferably, the voltage of the first cyclic voltammetry scan is -0.2 to 1.0 V, the scan rate is 2 to 20 mV / s, and the number of cycles is 15 to 25.

4. The method according to any one of claims 1 to 3, characterized in that In the step S21, the electrochemical deposition time is 5 to 20 minutes and the temperature is 20 to 40°C.

5. The method according to any one of claims 1 to 4, characterized in that In the step S22, the surface treatment includes the following steps: using the deposited working electrode as a second working electrode, using a mixture of an alkaline aqueous solution and tannic acid as a second electrolyte, and using platinum as a second counter electrode to perform a second cyclic voltammetry scan; Preferably, during the second cyclic voltammetry scan, the alkaline aqueous solution includes one or more of a KOH aqueous solution, a NaOH aqueous solution, a K2CO3 aqueous solution and a KHCO3 aqueous solution; more preferably, in the second electrolyte, the molar concentration of the alkaline aqueous solution is 0.1 to 1 M, and / or the mass concentration of tannic acid in the second electrolyte is 3 to 8 g / L; Preferably, the voltage of the second cyclic voltammetry scan is 0 to -0.65 V, the scan rate is 2 to 20 mV / s, and the number of cycles is 2 to 10.

6. The method according to any one of claims 1 to 5, characterized in that In step S23, The heating time is 10 to 20 minutes, and the heating rate is 5 to 20°C / min; and / or The heat treatment further comprises an annealing step; preferably, the annealing temperature is 15 to 40° C. and the annealing time is 10 to 20 minutes.

7. An electrocatalyst, characterized in that Obtained according to the method for producing electrocatalyst using cadmium-containing wastewater according to any one of claims 1 to 6.

8. The electrocatalyst according to claim 7, characterized in that The weight percentage of cadmium-containing substances in the electrocatalyst is ≥ 85%; and / or The cadmium-containing substances include cadmium element, cadmium hydroxide and cadmium oxide; Preferably, in terms of weight percentage, the cadmium-containing substance comprises 65-75% of cadmium element, 15-25% of cadmium hydroxide and the remainder of cadmium oxide.

9. A working electrode containing an electrocatalyst, characterized in that: Obtained according to the method for producing electrocatalyst using cadmium-containing wastewater according to any one of claims 1 to 6.

10. The electrocatalyst-containing working electrode according to claim 9, characterized in that: In the electrocatalyst-containing working electrode, the loading amount of the electrocatalyst is 0.2 to 7 mg / cm 2 .

11. An electrocatalytic system, characterized in that: The electrocatalytic system is used for electrocatalytic reduction of carbon dioxide, In the electrocatalytic system, the electrocatalyst-containing working electrode according to claim 9 or 10 is used as the third working electrode, and Ag / Ag + The electrode is used as a reference electrode, a platinum electrode is used as a third pair of electrodes, an ionic liquid-acetonitrile solution saturated with CO2 is used as a cathode solution, and HClO4 and / or H2SO4 is used as an anode solution.

12. The electrocatalytic system according to claim 11, characterized in that The surface of the electrocatalyst-containing working electrode also includes a perfluorosulfonic acid resin; Preferably, the raw material of the perfluorosulfonic acid resin includes a perfluorosulfonate ionomer, more preferably one or more of potassium perfluoro-1-octanesulfonate, potassium perfluoro-1-butanesulfonate, sodium perfluoro-1-pentanesulfonate, potassium perfluoro-1-hexanesulfonate and perfluorooctanesulfonic acid; and / or The Ag / Ag + The electrode includes AgNO3 and / or tetrabutylammonium tetrafluoroborate-acetonitrile solution; and / or The ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium perchlorate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium dihydrogen phosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate and 1-hexyl-3-methylimidazolium tetrafluoroborate; and / or The reaction potential of the electrocatalytic system is -1.8 to -3.2 V (relative to Ag / Ag + electrodes); and / or The CO product Faraday efficiency of the electrocatalytic system is ≥90%, and / or the CO generation rate is ≥0.2 L / (cm 2 h).