Magnesium-lithium alloy perovskite-like NaMgF3 coating, preparation method and application
The preparation of perovskite NaMgF3 coating of magnesium lithium alloy, combined with microarc oxidation and chemical conversion technology, formed NaMgF3 composite coating, which solved the problem of poor corrosion resistance of magnesium lithium alloy, and achieved uniformization of the surface of magnesium lithium alloy and Improved corrosion resistance and is suitable for long-term protection in the aerospace field.
Patent Information
- Application Number
- CN202410918737.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The corrosion resistance of magnesium lithium alloys in corrosive environments is poor, resulting in a decrease in mechanical properties. The existing protection methods are mostly harmless and have insufficient long-term effectiveness, and their biphasic structure leads to uneven coating preparation.
The preparation method of the perovskite NaMgF3 coating of magnesium lithium alloy is adopted to form a porous microarc oxide layer by combining microarc oxidation and chemical conversion, and chemical conversion is carried out in a solution containing caffeic acid and sodium fluoride to form a spherical accumulation. NaMgF3 composite coating, coordinated to enhance corrosion resistance.
The surface of magnesium lithium alloy is uniformized and porous, which significantly improves corrosion resistance and protective effect. It is suitable for aerospace and provides good long-term protection.
Smart Images

Figure CN118880413A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal surface treatment, in particular to the technical field of lithium-magnesium alloy surface treatment, and specifically relates to a magnesium-lithium alloy perovskite NaMgF3 coating, a preparation method and an application thereof. Background Art
[0002] As the lightest metal structural material, magnesium-lithium alloy has unique physical and mechanical properties such as high specific strength, high dimensional stability, high specific stiffness, good processing performance, excellent magnetic shielding and impact resistance, and has become a promising candidate material in many fields such as aviation, automobile industry, satellite and consumer electronics industry. However, the corrosion resistance of magnesium-lithium alloy in corrosive environment is very poor, on the one hand because magnesium and lithium have high chemical reactivity, on the other hand because of the unique dual-phase structure of magnesium-lithium alloy. When the lithium content is between 5.7 and 10.3wt%, magnesium-lithium alloy usually exhibits a dual-phase structure of hexagonal α-Mg phase and body-centered cubic β-Li phase. The potential difference between the two phases aggravates the micro-galvanic corrosion inside the alloy, resulting in aggravated local corrosion. This uncontrollable rapid corrosion in the actual service process leads to a significant decrease in the mechanical properties of magnesium-lithium alloy, which has become the main obstacle to its further development.
[0003] At present, perovskite-like coatings have been applied to AZ magnesium alloys, and are mostly used to improve the corrosion resistance of magnesium alloys. The existing magnesium-lithium alloy protection methods mainly include chemical conversion and anodic oxidation. Chemical conversion mainly includes chromic acid, phytic acid, phosphoric acid, stannic acid and rare earth conversion. Compared with chemical conversion film, anodized film has better wear resistance and corrosion resistance, and its bonding strength, electrical insulation and heat shock resistance are also very good.
[0004] There are many methods to protect magnesium-lithium alloys, but there is no method that is both environmentally friendly and can effectively protect magnesium-lithium alloys for a long time. Phosphates pollute the environment, the surface of stannic acid conversion films has fine lines, which is not conducive to long-term corrosion protection, the quality of phytic acid conversion films is difficult to control, the adhesion of single rare earth conversion is poor, the anodized film has a porous structure that needs to be sealed, and due to the special dual-phase structure of magnesium-lithium alloys, ordinary coating preparation has the problem of unevenness. Summary of the invention
[0005] In view of this, on the one hand, some embodiments disclose a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, comprising the steps of:
[0006] S1. The magnesium-lithium alloy substrate is subjected to micro-arc oxidation in a first solution to form a micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate; wherein the first solution is an aqueous solution comprising Na3PO4·12H2O, NaOH and C3H8O3, wherein the concentration of Na3PO4·12H2O is 0.1 to 1.0 M, the concentration of NaOH is 0.03 to 0.1 M, and the concentration of C3H8O3 is 0.01 to 0.1 M;
[0007] S2. The micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate reacts in the second solution to generate a spherically accumulated perovskite-type composite metal fluoride NaMgF3 coating on the surface of the micro-arc oxidation layer; wherein the second solution is an aqueous solution containing NaF and CA, the concentration of NaF is 0.05 to 0.2 M, and the concentration of CA is 0.01 to 0.05 M; the pH value of the second solution is 6.8 to 7.2.
[0008] Furthermore, in some embodiments of the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating, step S1 also includes a pretreatment process of the magnesium-lithium alloy substrate.
[0009] In some embodiments of the method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, the magnesium-lithium alloy in step S1 is LAZ931 alloy, LZ91 alloy or LAZ832 alloy.
[0010] In some embodiments of the method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, the second solution also includes metal ions Ce, Cr, Eu or Yb.
[0011] Some embodiments disclose a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating. In step S1, a magnesium-lithium alloy substrate is used as an anode, a stainless steel plate is used as a cathode, and a first solution is used as an electrolyte to form an anodizing system, wherein the distance between the anode and the cathode is 2 to 6 cm, the voltage is 250 to 300 V, the frequency is 400 to 2000 Hz, and the micro-arc oxidation time is 5 to 10 min.
[0012] In the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating disclosed in some embodiments, the reaction of step S2 is carried out in a drying oven, the temperature is set at 25-80°C, and the pressure is atmospheric pressure.
[0013] In some embodiments of the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating, NaOH is used to adjust the pH of the second solution to 6.8-7.2.
[0014] On the other hand, some embodiments disclose a magnesium-lithium alloy perovskite NaMgF3 coating, which is obtained by a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating.
[0015] On the other hand, some embodiments disclose the application of magnesium-lithium alloy perovskite NaMgF3 coating, which is used to prepare anti-corrosion coating on the surface of magnesium-lithium alloy.
[0016] The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating disclosed in the embodiment of the present invention organically combines the anodic oxidation and chemical conversion processes to form a porous micro-arc oxidation coating on the surface of the magnesium-lithium alloy, so as to make the alloy surface uniform and porous. The micro-arc oxidation coating is then chemically converted in a conversion solution containing CA and NaF to form a composite coating in which micro-arc oxidation and NaMgF3 are synergistically adapted to each other. The composite coating has good application prospects in the field of magnesium-lithium alloy protection for aerospace. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The infrared spectra of the micro-arc oxidation coating in Example 1 and the coating after further chemical conversion treatment;
[0018] Figure 2 is the SEM morphology of the NaMgF3 coating in Example 1;
[0019] Figure 3 1 is the hydrogen evolution curve of the bare substrate and the coating under different parameters in Example 1;
[0020] Figure 4 This is the SEM morphology of the NaMgF3 coating in Example 2;
[0021] Figure 5 This is the SEM morphology of the coating after adding Ce(NO3)3 to the conversion solution in Example 3. DETAILED DESCRIPTION
[0022] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.
[0023] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.
[0024] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0025] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0026] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.
[0027] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.
[0028] In some embodiments, the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating comprises the steps of:
[0029] S1. The magnesium-lithium alloy substrate is subjected to micro-arc oxidation in a first solution to form a micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate; wherein the first solution is an aqueous solution comprising Na3PO4·12H2O, NaOH and C3H8O3, wherein the concentration of Na3PO4·12H2O is 0.1 to 1.0 M, the concentration of NaOH is 0.03 to 0.1 M, and the concentration of C3H8O3 is 0.01 to 0.1 M;
[0030] S2. The micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate undergoes a chemical conversion reaction in the second solution, and a spherical NaMgF3 coating is generated on the surface of the micro-arc oxidation layer; wherein the second solution is an aqueous solution containing NaF and CA, the concentration of NaF is 0.05-0.2M, and the concentration of CA is 0.01-0.05M; the pH value of the second solution is 6.8-7.2. Generally, when the sample with the micro-arc oxidation layer is immersed in the second solution for a chemical conversion reaction, caffeic acid first accelerates the corrosion of the magnesium-lithium alloy substrate and forms a Mg(CA) complex with the precipitated magnesium ions, which provides more nucleation sites for the growth of NaMgF3. On the other hand, the formation of the Mg(CA) complex also regulates the Mg in the solution. 2+ With F + When Mg 2+ With F - When the ratio of NaMgF3 is less than 0.81, NaMgF3 begins to form; in addition, NaMgF3 is a perovskite-type composite metal fluoride with a typical perovskite-type structure. + and F - Together they form a cubic close-packed structure, Na + There are 12 F-coordinates around it, Mg 2+ Occupying all the octahedral voids formed by F-, this structure provides sufficient space for the incorporation of active particles such as Ce.
[0031] Generally, the micro-arc oxidation coating formed by micro-arc oxidation has a porous structure, which can control the Mg 2+ The release rate of Mg 2+ On the other hand, the porous structure provides an effective storage chamber for the conversion solution in the subsequent chemical conversion process. 2+ It dissolves preferentially in porous areas, so perovskite-type composite metal fluoride NaMgF3 is usually generated preferentially in porous areas, which plays a good sealing role in the micropores of the micro-arc oxidation layer; on the other hand, the porous structure surface of the micro-arc oxidation coating is relatively rough, and there are more nucleation sites than the bare substrate, which is more conducive to the growth of perovskite-type composite metal fluoride NaMgF3.
[0032] In the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating disclosed in some embodiments, step S1 also includes a pretreatment process of the magnesium-lithium alloy substrate.
[0033] In some embodiments of the method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, the magnesium-lithium alloy in step S1 is LAZ931 alloy, LZ91 alloy or LAZ832 alloy.
[0034] In some embodiments of the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating, the pretreatment process of the magnesium-lithium alloy substrate in step S1 includes surface grinding and cleaning.
[0035] Some embodiments disclose a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, wherein the second solution is an aqueous solution containing NaF, CA and metal ions Ce, Cr, Eu or Yb, wherein the concentration of NaF is 0.05-0.2M, the concentration of CA is 0.01-0.05M, the metal ions Ce, Cr, Eu or Yb exist in the form of inorganic salts, such as nitrates, and the concentration of metal ions Ce, Cr, Eu or Yb is 0.01-0.2M; the pH value of the second solution is 6.8-7.2.
[0036] Some embodiments disclose a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating. In step S1, a magnesium-lithium alloy substrate is used as an anode, a stainless steel plate is used as a cathode, and a first solution is used as an electrolyte to form an anodizing system, wherein the distance between the anode and the cathode is 2 to 6 cm, the voltage is 250 to 300 V, the frequency is 400 to 2000 Hz, and the micro-arc oxidation time is 5 to 10 min.
[0037] In the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating disclosed in some embodiments, the reaction of step S2 is carried out in a drying oven, the temperature is set at 25-80°C, and the pressure is atmospheric pressure.
[0038] In some embodiments of the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating, NaOH is used to adjust the pH of the second solution to 6.8-7.2.
[0039] On the other hand, some embodiments disclose a magnesium-lithium alloy perovskite NaMgF3 coating, which is obtained by a method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating.
[0040] On the other hand, some embodiments disclose the application of magnesium-lithium alloy perovskite NaMgF3 coating, which is used to prepare anti-corrosion coating on the surface of magnesium-lithium alloy.
[0041] Some embodiments disclose the application of a perovskite-like NaMgF3 coating on a magnesium-lithium alloy, which is applied to form a perovskite-like NaMgF3 coating on the surface of a magnesium-lithium alloy.
[0042] The chemical stability and corrosion resistance of the perovskite-type composite metal fluoride NaMgF3 make it suitable as an external protective coating for aircraft, especially for aircraft applications that require reducing weight while improving durability.
[0043] The technical details are further illustrated below in conjunction with embodiments.
[0044] Example 1
[0045] In Example 1, the preparation method of the magnesium-lithium alloy perovskite NaMgF3 coating comprises the following steps:
[0046] (1) The rolled LAZ931 plate with a size of 10*10*3 mm was polished with SiC sandpaper #100, #200, #400, #600 and #800 in sequence, and the polished sample was polished. After polishing, it was ultrasonically cleaned in anhydrous ethanol for 5 minutes to remove oil stains, etc., and then taken out and dried with cold air for use;
[0047] (2) dissolving sodium phosphate Na3PO4, sodium hydroxide NaOH and glycerol C3H8O3 in deionized water to prepare a first solution, wherein the concentration of Na3PO4·12H2O is 0.3 M, the concentration of NaOH is 0.05 M, and the concentration of C3H8O3 is 0.08 M; dissolving caffeic acid CA and sodium fluoride NaF in deionized water to prepare a second solution, wherein the concentration of CA is 0.01 M, and the concentration of NaF is 0.2 M, and adjusting the pH of the second solution to 7 with the diluted NaOH solution;
[0048] (3) Using the LAZ931 plate treated in step (1) as the anode and the stainless steel plate as the cathode, the cathode and the anode are completely immersed in the first solution at the same time, with a distance of 2 cm between the anode and the cathode, and micro-arc oxidation is performed at a constant voltage of 300 V and a pulse frequency of 2000 Hz for 5 minutes, taking out the LAZ931 plate treated with micro-arc oxidation, rinsing it with deionized water, and drying it for later use;
[0049] (4) completely immersing the LAZ931 plate treated with micro-arc oxidation obtained in step (3) into 40 ml of the second solution, and then placing it in a vacuum drying oven and keeping it warm at 80° C. for 6 hours under atmospheric pressure;
[0050] (5) The LAZ931 sheet obtained in step (4) is taken out from the vacuum drying oven, rinsed with deionized water and dried naturally, thereby obtaining a perovskite-like NaMgF3 coating on the surface of the LAZ931 sheet.
[0051] In Example 1, the sample with the micro-arc oxidation layer obtained in step (3) and the sample obtained by chemical conversion treatment in step (4) were subjected to infrared spectroscopy test. The results are as follows: Figure 1 As shown, caffeic acid functional groups and NaMgF3 substances were detected in the coating after chemical conversion treatment, indicating that caffeic acid was involved in the formation process of NaMgF3 coating.
[0052] After being treated with the conversion solution containing caffeic acid and NaF in step (4), the surface morphology of the LAZ931 sheet sample is as follows: Figure 2As shown in the figure, the surface is densely packed with spherical NaMgF3 substances, and the microporous structure of the previous micro-arc oxidation layer is almost invisible, indicating that the spherical NaMgF3 substances have a good sealing effect on the micropores of the micro-arc oxidation coating;
[0053] The hydrogen evolution performance of three coatings, namely, LAZ931 bare substrate, MAO micro-arc oxidation layer, and MAO+NaMgF3 coating on the surface of the micro-arc oxidation layer, was tested. The results are as follows: Figure 3 As shown; Figure 3 The hydrogen evolution curves of LAZ931 bare substrate and two coatings, MAO and MAO+NaMgF3, were measured after being immersed in 3.5% NaCl for 5 days. Figure 3 It can be seen that the amount of hydrogen evolution of the MAO+NaMgF3 coating is the smallest. Compared with the bare substrate, the amount of hydrogen evolution does not change much within 5 days, indicating that the MAO+NaMgF3 coating enhances the corrosion resistance of the magnesium-lithium alloy and can provide good protection for the magnesium-lithium alloy.
[0054] Example 2
[0055] In Example 2, the method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating comprises the following steps:
[0056] (1) The rolled LAZ832 plate with a size of 10*10*3 mm was polished with SiC sandpaper #100, #200, #400, #600 and #800 in sequence, and the polished sample was polished. After polishing, it was ultrasonically cleaned in anhydrous ethanol for 5 minutes to remove oil stains, etc., and then taken out and dried with cold air for use;
[0057] (2) dissolving sodium phosphate Na3PO4, sodium hydroxide NaOH and glycerol C3H8O3 in deionized water to prepare a first solution, wherein the concentration of Na3PO4·12H2O is 0.2 M, the concentration of NaOH is 0.03 M, and the concentration of C3H8O3 is 0.05 M; dissolving caffeic acid CA and sodium fluoride NaF in deionized water to prepare a second solution, wherein the concentration of CA is 0.033 M, and the concentration of NaF is 0.1 M, and adjusting the pH of the second solution to 7 with the diluted NaOH solution;
[0058] (3) Using the LAZ832 plate treated in step (1) as the anode and the stainless steel plate as the cathode, the cathode and the anode are completely immersed in the first solution at the same time, with a distance of 3 cm between the anode and the cathode, and micro-arc oxidation is performed for 7 minutes at a constant voltage of 270 V and a pulse frequency of 1200 Hz. The LAZ832 plate treated with micro-arc oxidation is taken out, rinsed with deionized water, and dried for later use;
[0059] (4) The LAZ832 plate obtained in step (3) and treated with micro-arc oxidation was completely immersed in 30 ml of the second solution, and then placed in a vacuum drying oven and kept warm at 60° C. for 8 h under atmospheric pressure;
[0060] (5) The LAZ832 sheet obtained in step (4) is taken out from the vacuum drying oven, rinsed with deionized water and then dried naturally to obtain a perovskite-like NaMgF3 coating on the surface of the LAZ832 sheet.
[0061] Example 3
[0062] In Example 3, the preparation method of the magnesium-lithium alloy perovskite NaMgF3 coating comprises the following steps:
[0063] (1) The rolled LAZ931 plate with a size of 10*10*3 mm was polished with SiC sandpaper #100, #200, #400, #600 and #800 in sequence, and the polished sample was polished. After polishing, it was ultrasonically cleaned in anhydrous ethanol for 5 minutes to remove oil stains, etc., and then taken out and dried with cold air for use;
[0064] (2) dissolving sodium phosphate Na3PO4, sodium hydroxide NaOH and glycerol C3H8O3 in deionized water to prepare a first solution, wherein the concentration of Na3PO4·12H2O is 0.4M, the concentration of NaOH is 0.05M, and the concentration of C3H8O3 is 0.06M; dissolving caffeic acid CA, sodium fluoride NaF and cerium nitrate Ce(NO3)3 in deionized water to prepare a second solution, wherein the concentration of CA is 0.05M, the concentration of NaF is 0.05M, and the concentration of Ce(NO3)3 is 0.01M; adjusting the pH of the second solution to 7 with the diluted NaOH solution;
[0065] (3) Using the LAZ931 plate treated in step (1) as the anode and the stainless steel plate as the cathode, the cathode and the anode are completely immersed in the first solution at the same time, with a distance of 4 cm between the anode and the cathode, and micro-arc oxidation is performed for 10 min at a constant voltage of 250 V and a pulse frequency of 400 Hz. The LAZ931 plate treated with micro-arc oxidation is taken out, rinsed with deionized water, and dried for later use;
[0066] (4) The LAZ931 plate obtained in step (3) and treated with micro-arc oxidation was completely immersed in 50 ml of the second solution, and then placed in a vacuum drying oven and kept warm at 40° C. for 12 h under atmospheric pressure;
[0067] (5) The LAZ931 sheet obtained in step (4) is taken out from the vacuum drying oven, rinsed with deionized water and dried naturally, thereby obtaining a perovskite-like NaMgF3 coating on the surface of the LAZ931 sheet.
[0068] The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating disclosed in the embodiment of the present invention organically combines the anodic oxidation and chemical conversion processes to form a porous micro-arc oxidation coating on the surface of the magnesium-lithium alloy, so as to make the alloy surface uniform and porous. The micro-arc oxidation coating is then chemically converted in a conversion solution containing CA and NaF to form a composite coating in which micro-arc oxidation and NaMgF3 are synergistically adapted to each other. The composite coating has good application prospects in the field of magnesium-lithium alloy protection for aerospace.
[0069] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a magnesium-lithium alloy perovskite NaMgF3 coating, characterized in that: Includes steps: S1. The magnesium-lithium alloy substrate is subjected to micro-arc oxidation in a first solution to form a micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate; wherein the first solution is an aqueous solution comprising Na3PO4·12H2O, NaOH and C3H8O3, wherein the concentration of Na3PO4·12H2O is 0.1 to 1.0 M, the concentration of NaOH is 0.03 to 0.1 M, and the concentration of C3H8O3 is 0.01 to 0.1 M; S2. The micro-arc oxidation layer on the surface of the magnesium-lithium alloy substrate reacts in the second solution to generate a spherically accumulated perovskite-type composite metal fluoride NaMgF3 coating on the surface of the micro-arc oxidation layer; wherein the second solution is an aqueous solution containing NaF and CA, the concentration of NaF is 0.05 to 0.2 M, and the concentration of CA is 0.01 to 0.05 M; the pH value of the second solution is 6.8 to 7.
2.
2. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: Step S1 also includes a pretreatment process of the magnesium-lithium alloy substrate.
3. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: The magnesium-lithium alloy in step S1 is LAZ931 alloy, LZ91 alloy, or LAZ832 alloy.
4. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: The second solution also includes metal ions Ce, Cr, Eu or Yb.
5. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: In step S1, an anodic oxidation system is formed with a magnesium-lithium alloy substrate as an anode, a stainless steel plate as a cathode, and a first solution as an electrolyte, wherein the distance between the anode and the cathode is 2 to 6 cm, the voltage is 250 to 300 V, the frequency is 400 to 2000 Hz, and the micro-arc oxidation time is 5 to 10 min.
6. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: The reaction in step S2 is carried out in a drying oven with the temperature set at 25-80° C. and the pressure set at atmospheric pressure.
7. The method for preparing the magnesium-lithium alloy perovskite NaMgF3 coating according to claim 1, characterized in that: The pH of the second solution was adjusted to 6.8-7.2 using NaOH.
8. Magnesium-lithium alloy perovskite NaMgF3 coating, characterized in that: The coating is obtained by the preparation method of the magnesium-lithium alloy perovskite NaMgF3 coating according to any one of claims 1 to 7.
9. Application of magnesium-lithium alloy perovskite NaMgF3 coating, characterized in that: The magnesium-lithium alloy perovskite NaMgF3 coating described in claim 8 is used to prepare an anti-corrosion coating on the surface of a magnesium-lithium alloy.