Preparation method of detector-grade high-purity germanium single crystal
By using neck shrinkage, thin neck and multiple shoulder retraction techniques during the lifting process of high-purity germanium single crystal, the problems of instability in dislocation density control and the requirements of multiple detectors are solved, and stability and Improved adaptability can provide qualified products for a variety of detectors.
Patent Information
- Application Number
- CN202410768287.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively control the crystal dislocation density of high-purity germanium single crystals, resulting in unstable production process and it is difficult for one crystal to meet the needs of multiple detectors.
The method of shrinking the neck, thin neck and multiple shoulder retraction during the lifting process is adopted. The crystal dislocation density is first controlled, and then the dislocation hyperplasia is achieved by placing the shoulder and retraction to ensure the stability of the dislocation density and adapting to different Detector requirements.
Through this method, the 13N germanium qualified segment of different dislocation density levels can be obtained in one crystal, which can achieve the provision of qualified products of multiple detectors, and improve the stability and adaptability of production.
Smart Images

Figure CN118880440A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of crystal growth, and more specifically to a method for preparing detector-grade high-purity germanium single crystal. Background Art
[0002] The basic principle of single crystal growth using the Clausky method (hereinafter referred to as the CZ method) is to heat and melt the raw materials for crystal growth in a crucible, generate a certain degree of supercooling inside the melt, and generate a nucleation driving force. The seed crystal fixed at the lower end of the seed crystal rod is immersed in the melt from the upper surface. After one end of the seed crystal immersed in the melt is partially melted, the seed crystal rod is pulled upward at a certain speed. The heat generated at the solid-liquid interface during the crystallization process is transmitted through the seed crystal rod. The melt in contact with the seed crystal first obtains a certain degree of supercooling and begins the crystallization process. As the seed crystal rod is slowly pulled, continuous crystal growth can be achieved by controlling factors such as temperature and pulling speed. Crystals grown by the pulling method have high integrity, fast growth rate, and large crystal size. Crystals with a specific crystal orientation can be grown according to the crystal orientation of the seed crystal. Therefore, it is widely used in the field of single crystal growth.
[0003] High-purity germanium detectors play an increasingly important role in the high-tech field and are widely used in experimental research in nuclear physics, particle physics, and astrophysics. In terms of detecting particles, especially x-rays and gamma-rays, they have the advantages of good energy resolution, high detection efficiency, and strong stability, which are unmatched by other gamma-ray detectors. The net impurity concentration of this detector-grade high-purity germanium single crystal material must be less than 2E10 / cm 3 , the dislocation density must reach 500-10000 / cm 2 In order to obtain such high-purity, low-dislocation, high-purity germanium single crystals, it is necessary to use electronic-grade germanium (5N-6N) as the raw material, adopt a special zone melting purification method to obtain detector-grade germanium polycrystalline material, and then use a special single crystal pulling method to obtain a large volume of low-dislocation, high-purity germanium single crystal material.
[0004] The main sources of crystal dislocations are the downward extension of dislocations inside the seed crystal itself, dislocations caused by thermal shock during the crystallization process, and dislocations caused by thermal stress formed by uneven temperature distribution during the growth process. In order to reduce crystal dislocations, necking and thinning processes are usually set up, which use high pulling speeds to reduce the crystal diameter and maintain a certain length. Under such conditions, dislocations extend and slip along the slip plane, and then slip to the crystal surface and disappear.
[0005] In actual production, in order to pull out the dislocation density of 500-10000 / cm 2 The high-purity germanium crystal is affected by the number of dislocations in the seed crystal itself and the differences in operation during the crystallization process. There are differences in the neck diameter and the length of the thin neck during the pulling process, and crystals with zero dislocation or high dislocation are often pulled out. This dislocation control process is extremely unstable.
[0006] Different types of detectors have different requirements for product size, purity and dislocation. That is, within a certain range, the optimal detection performance of different types of detectors corresponds to their optimal size, purity requirements and dislocation requirements. One crystal usually cannot provide qualified products for multiple detectors. Summary of the invention
[0007] In view of the problems existing in the background technology, an object of the present disclosure is to provide a method for preparing detector-grade high-purity germanium single crystal, which is easy to control the crystal dislocation density.
[0008] Another object of the present disclosure is to provide a method for preparing detector-grade high-purity germanium single crystal, wherein one crystal can provide qualified products for a variety of detectors.
[0009] Therefore, a method for preparing detector-grade high-purity germanium single crystal includes a pulling process, wherein the pulling process includes seeding, necking, neck thinning, multiple shoulder release and shoulder retraction, and tailing.
[0010] The beneficial effects of the present disclosure are as follows.
[0011] In the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure, the dislocation density of the crystal is first controlled by shrinking the neck, and then the proliferation of dislocations is achieved through multiple shoulder releases and shoulder retractions, which makes it easy to control the dislocation density of the crystal, ensure the stability of the crystal dislocation density, and facilitate industrialization.
[0012] In the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure, by multiple shoulder release and shoulder collection, qualified 13N germanium segments with different dislocation density levels can be obtained in one crystal to meet the needs of preparing different detectors. That is, one crystal can provide qualified products for multiple detectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the pulling process of the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure.
[0014] Figure 2 It is a schematic diagram of the sampling and detection process of the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure, wherein A1, A2, A3, and A4 represent sampling positions, and B1, B2, and B3 represent product one, product two, and product three. DETAILED DESCRIPTION
[0015] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.
[0016] [Method for preparing detector-grade high-purity germanium single crystal]
[0017] Reference Figure 1 According to the disclosed method for preparing detector-grade high-purity germanium single crystal, the pulling process includes seeding, necking, neck thinning, multiple shoulder release and shoulder retraction, and tailing.
[0018] In the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure, the dislocation density of the crystal is first controlled by shrinking the neck, and then the proliferation of dislocations is achieved through multiple shoulder releases and shoulder retractions, which makes it easy to control the dislocation density of the crystal, ensure the stability of the crystal dislocation density, and facilitate industrialization.
[0019] In the method for preparing detector-grade high-purity germanium single crystal according to the present disclosure, by multiple shoulder release and shoulder collection, qualified 13N germanium segments with different dislocation density levels can be obtained in one crystal to meet the needs of preparing different detectors. That is, one crystal can provide qualified products for multiple detectors.
[0020] In one example, seeding is as follows: after the material is smelted, the crucible and crystal are turned on and stabilized for a period of time, the seed crystal is slowly inserted into the melt, the power is adjusted according to the melt interface, and after a certain width of aperture appears, wait for a specified time and start seeding: gradually increase the pulling speed to the seeding pulling speed, maintain this pulling speed for seeding, and control the crystal diameter to be stable at the specified diameter as the standard. Specifically, when seeding, the specified time is 10-20min; the seeding pulling speed is 20-30mm / h; maintain this pulling speed for seeding for 10-30min; the specified diameter is 5-10mm.
[0021] In one example, the necking is: manually increase the pulling speed until the pulling speed reaches the necking pulling speed, and control the crystal diameter to be stable at the specified neck diameter as the standard. Specifically, the manual increase of the pulling speed is to increase the pulling speed by 10-20mm / h at intervals of 10min; the necking pulling speed is 90-150mm / h; and the specified neck diameter is less than 3mm.
[0022] In one example, the thin neck is: the pulling speed is maintained at the thin neck pulling speed, the thin neck is pulled at this high pulling speed, and the pulling length in this stage is the thin neck length. Specifically, the thin neck pulling speed is 90-150mm / h; the thin neck length is 90-150mm.
[0023] In one example, multiple shoulder drops and shoulder pulls include:
[0024] After shoulder release, open the crucible lift, evenly reduce the pulling speed to 20-30mm / h, and the frequency of reducing the pulling speed is: evenly reduce the pulling speed by 20-40mm / h every 10min; control the power to evenly cool down, the cooling frequency is 60-100w / h, shoulder release for 2-3h, and the crystal diameter gradually grows to 80-85mm;
[0025] Shoulder 1, manually control the temperature to rise twice, 80-140w and 60-100w, 5-10min interval between the two times, then set the program temperature rise, the temperature rise frequency is 60-100w / h, the crystal diameter gradually decreases to 65-70mm;
[0026] Shoulder 2, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm;
[0027] Shoulder 2, manually control the temperature to 40-80w, then set the program temperature to rise, the temperature rise frequency is 60-100w / h, and the crystal diameter gradually decreases to 65-70mm;
[0028] Put shoulder three, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm;
[0029] Shoulder three, manually control the temperature to rise by 20-60w, then set the program to rise, the frequency of the temperature rise is 60-100w / h, and the crystal diameter gradually decreases to 65-70mm;
[0030] Put the shoulder four, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm. Specifically, the crucible lifting speed is 0.8-1mm / h.
[0031] In one example, the end is: reduce the crucible lifting speed, control the power to evenly cool down, and end until the melt in the quartz crucible is completely pulled out. Specifically, the cooling frequency is 100-200w / h, and the end is 2-3h.
[0032] In addition, the method for preparing detector-grade high-purity germanium single crystal may also include a sampling and testing process after the pulling process is completed. Figure 1 As shown, the sampling and testing process is: sampling at the position (A1) before the end of the first shoulder release (i.e., shoulder release 1), at the position of the minimum diameter between the first shoulder collection (i.e., shoulder collection 1) and the second shoulder release (i.e., shoulder release 2) (A2), at the position of the minimum diameter between the second shoulder collection (i.e., shoulder collection 2) and the third shoulder release (i.e., shoulder release 3) (A3), and so on (A4), to test the carrier density and dislocation density. The sampling position is at the position of the minimum crystal diameter, which reduces the loss of the crystal in the test process and improves the qualified rate.
[0033] In one example, the preparation method of detector-grade high-purity germanium single crystal according to the present disclosure also includes a preparation process. The preparation process includes: raw material grinding, grinding and cleaning the germanium ingot raw material; raw material corrosion, corroding and cleaning the germanium ingot raw material, and drying it with nitrogen; furnace loading, loading the germanium ingot raw material and high-purity seed crystal into the pulling furnace, sealing the pulling furnace and passing hydrogen to purge; material control heating power to increase the temperature and maintain a constant temperature, so that the germanium ingot raw material is completely melted.
[0034] Specifically, when the raw material is polished, prepare the carrier concentration ≤ 8E10 / cm 3 Use a scouring pad to polish the germanium ingot raw material, remove the uneven burrs on the surface of the raw material until the surface is smooth, and rinse it with pure water.
[0035] Specifically, when the raw material is corroded, the germanium ingot raw material is placed in a corrosive liquid of HNO3:HF=(2-3):1, and after being corroded until the surface is bright, it is taken out and rinsed with pure water for more than 20 minutes. When the conductivity of the rinse liquid is measured to be close to 0.1-0.15, 7N high-purity nitrogen is used to blow dry the germanium ingot raw material;
[0036] Specifically, when loading the furnace, the germanium ingot raw material is loaded into the crucible of the pulling furnace, the high-purity seed crystal is fixed on the seed crystal chuck under the seed crystal rod, the pulling furnace is sealed and evacuated to below 1 Pa and 9N hydrogen is introduced for purge for more than 3 hours.
[0037] Specifically, when the material is melted, the heating power is controlled to raise the temperature to 1000°C, and the temperature is kept constant so that all the raw materials of the germanium ingot are melted, and then the temperature is lowered to 940-970°C, and the temperature is kept constant for 30-60 minutes. In one example, the process for preparing high-purity germanium single crystal by the pulling method disclosed in the present invention also includes the step of heating the temperature to 1000°C within 2-4 hours.
[0038] In one example, the preparation method of detector-grade high-purity germanium single crystal according to the present disclosure also includes: cooling, closing the crystal lift and the crucible lift, cooling until it drops to room temperature, and completing the crystal pulling. Specifically, the cooling is divided into three stages: the first stage is to cool evenly at a cooling frequency of 300-400w / h for 1h; the second stage is to cool evenly at a cooling frequency of 500-600w / h for 2h; the third stage is to cool evenly at a cooling frequency of 800-1000w / h for 5-7h until it drops to room temperature.
[0039] [test]
[0040] Example 1
[0041] Example 1 adopts the following operation:
[0042] 1) Preparation process, the preparation process adopts the following steps:
[0043] Raw material polishing, prepare carrier concentration ≤8E10 / cm 3 Use a scouring pad to polish the germanium ingot raw material, remove the uneven burrs on the surface of the raw material until the surface is smooth, and rinse it with pure water;
[0044] Raw material corrosion: Place the germanium ingot raw material in a corrosion liquid of HNO3:HF=3:1 for corrosion, take it out after the surface is corroded to be bright, rinse with pure water for 30 minutes, and when the conductivity of the rinse liquid is close to 0.12, use 7N high-purity nitrogen to blow dry the germanium ingot raw material;
[0045] Load the germanium ingot into the crucible of the pulling furnace and set the net impurity carrier concentration to less than 2E11 / cm 3 The high-purity seed crystal is fixed on the seed crystal chuck under the seed crystal rod, and the sealed pulling furnace is evacuated to below 1Pa and purged with 9N hydrogen for 3 hours;
[0046] The material is melted, and the heating power is controlled to raise the temperature to 1000°C, and the temperature is kept constant so that all the germanium ingot raw materials are melted, and then the temperature is lowered to 950°C, and the temperature is kept constant for 45 minutes. Among them, the heating power is controlled to raise the temperature to 1000°C within 3 hours;
[0047] II) Pulling process, the pulling process adopts the following steps:
[0048] Seeding: After the material is melted, the crucible and crystal are turned on and stabilized for a period of time, the seed crystal is slowly inserted into the melt, the power is adjusted according to the melt interface, and after a certain width of aperture appears, wait for a specified time and start seeding: gradually increase the pulling speed to the seeding pulling speed, maintain this pulling speed for seeding, and control the crystal diameter to be stable at the specified diameter as the standard; during seeding, the specified time is 10-20min; the seeding pulling speed is 25mm / h; maintain this pulling speed for seeding for 15min; the specified diameter is 9mm;
[0049] Neck shrinkage: Manually increase the pulling speed, increase the pulling speed by 15mm / h evenly every 10min, until the pulling speed reaches the neck shrinkage pulling speed, control the crystal diameter to be stable at the specified neck diameter as the standard, the neck shrinkage pulling speed is 100mm / h; the specified neck diameter is 2.5mm;
[0050] Narrow neck: Keep the pulling speed at the narrow neck pulling speed, pull the narrow neck at this high pulling speed, the pulling length at this stage is the narrow neck length, the narrow neck pulling speed is 100mm / h; the narrow neck length is 100mm;
[0051] Repeatedly lowering and lowering the shoulders,
[0052] Put down the shoulder, start the crucible lifting, the crucible lifting speed is 0.9mm / h, and evenly reduce the pulling speed to 25mm / h. The frequency of reducing the pulling speed is: evenly reduce the pulling speed by 25mm / h every 10min;
[0053] Control the power to cool down evenly, the cooling frequency is 80w / h, and the shoulder is left for 2.5h. The crystal diameter gradually grows to 82mm.
[0054] Shoulder 1, manually control the temperature to rise twice, 100w and 80w respectively, with an interval of 6 minutes between the two times, and then set the program temperature rise, the temperature rise frequency is 80w / h, and the crystal diameter is gradually reduced to 68mm;
[0055] Shoulder 2, set program cooling, cooling frequency is 110w / h, the crystal diameter gradually grows to 82mm;
[0056] Shoulder 2, manually control the temperature to 60w, then set the program to heat up, the heating frequency is 80w / h, and the crystal diameter gradually decreases to 68mm;
[0057] Put shoulder three, set the program to cool down, the cooling frequency is 110w / h, and the crystal diameter gradually grows to 82mm;
[0058] Shoulder three, manually control the temperature to 40w, then set the program to heat up, the heating frequency is 80w / h, and the crystal diameter gradually decreases to 68mm;
[0059] Put the shoulder four, set the program to cool down, the cooling frequency is 110w / h, and the crystal diameter gradually grows to 82mm;
[0060] Towards the end, lower the crucible lifting speed to 0.5mm / h, control the power to evenly cool down, and finish until the molten material in the quartz crucible is completely pulled out; the cooling frequency is 150w / h, and the finishing time is 2.5h.
[0061] III) Cooling, turning off the crystal rotation and the crucible rotation, the cooling is divided into three stages: the first stage is to cool evenly at a cooling frequency of 350w / h for 1h; the second stage is to cool evenly at a cooling frequency of 550w / h for 2h; the third stage is to cool evenly at a cooling frequency of 900w / h for 6h until it reaches room temperature, completing the crystal pulling;
[0062] IV) Sampling and testing process: sampling is performed at the position (A1) before the end of the first shoulder release (i.e., shoulder release one), at the position of the minimum diameter between the first shoulder retraction (i.e., shoulder retraction one) and the second shoulder release (i.e., shoulder release two) (A2), at the position of the minimum diameter between the second shoulder retraction (i.e., shoulder retraction two) and the third shoulder release (i.e., shoulder release three) (A3), and at the position of the minimum diameter between the third shoulder retraction (i.e., shoulder retraction three) and the fourth shoulder release (i.e., shoulder release four) (A4), to detect the carrier density and dislocation density, as shown in Table 1.
[0063] Table 1 Test results of four sampling locations
[0064] A1 A2 A3 A4 PN type P-Type P-Type P-Type P-Type <![CDATA[Carrier concentration (1 / cm 3 )]]> 4.51E+10 1.26E+10 1.09E+10 9.42E+09 <![CDATA[Dislocation density (cm 2 )]]> 0 625 2392 4920
[0065] The carrier concentration and PN type are tested by HL9900 of Toho Technology, USA. The dislocation density is tested according to the test method of dislocation density of germanium single crystal in GB / T 5252-2020.
[0066] It can be seen that by shrinking the neck, the dislocation density of the crystal is first controlled to 0, and then the dislocation proliferation is achieved by continuously releasing and retracting the shoulder. This process can easily control the dislocation density of the crystal and ensure the stability of the crystal dislocation density. In addition, qualified 13N germanium segments with different dislocation density levels can be obtained in one crystal to meet the needs of different detector preparation. The test position is at the position with the smallest crystal diameter, which also reduces the loss of the crystal by the test process and improves the pass rate.
[0067] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.
Claims
1. A method for preparing a detector-grade high-purity germanium single crystal, comprising a pulling process, It is characterized in that The pulling process includes seeding, necking, neck thinning, multiple shoulder release and shoulder retraction, and tailing.
2. The method for preparing detector-grade high-purity germanium single crystal according to claim 1, It is characterized in that Seeding is as follows: after completing the material smelting, starting the crucible and crystal rotation and stabilizing for a period of time, slowly insert the seed crystal into the melt, adjust the power according to the melt interface, wait for a specified time after a certain width of aperture appears, and start seeding: gradually increase the pulling speed to the seeding pulling speed, maintain this pulling speed for seeding, and control the crystal diameter to be stable at the specified diameter as the standard.
3. The method for preparing detector-grade high-purity germanium single crystal according to claim 2, It is characterized in that During seeding, The prescribed time is 10-20 minutes; The seeding speed is 20-30 mm / h; Maintain this pulling speed for 10-30 minutes; The specified diameter is 5-10mm.
4. The method for preparing detector-grade high-purity germanium single crystal according to claim 1, It is characterized in that Neck shrinkage is as follows: manually increase the pulling speed until the pulling speed reaches the neck shrinkage pulling speed, and control the crystal diameter to be stable at the specified thin neck diameter as the standard.
5. The method for preparing detector-grade high-purity germanium single crystal according to claim 4, It is characterized in that Manually increase the pulling speed by evenly increasing the pulling speed by 10-20mm / h at intervals of 10min; The necking speed is 90-150mm / h; The diameter of the narrow neck is specified to be less than 3 mm.
6. The method for preparing detector-grade high-purity germanium single crystal according to claim 1, It is characterized in that The thin neck is: keep the pulling speed at the thin neck pulling speed, pull the thin neck at this high pulling speed, and the pulling length at this stage is the thin neck length.
7. The method for preparing detector-grade high-purity germanium single crystal according to claim 6, It is characterized in that The narrow neck pulling speed is 90-150mm / h; The length of the narrow neck is 90-150mm.
8. The method for preparing detector-grade high-purity germanium single crystal according to claim 1, It is characterized in that Multiple shoulder releases and retractions include: After shoulder release, open the crucible lift, evenly reduce the pulling speed to 20-30mm / h, and the frequency of reducing the pulling speed is: evenly reduce the pulling speed by 20-40mm / h at intervals of 10min; control the power to evenly cool down, the cooling frequency is 60-100w / h, shoulder release for 2-3h, and the crystal diameter gradually grows to 80-85mm; Shoulder 1, manually control the temperature to rise twice, 80-140w and 60-100w, 5-10min interval between the two times, then set the program temperature rise, the temperature rise frequency is 60-100w / h, the crystal diameter gradually decreases to 65-70mm; Shoulder 2, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm; Shoulder 2, manually control the temperature to 40-80w, then set the program temperature to rise, the temperature rise frequency is 60-100w / h, and the crystal diameter gradually decreases to 65-70mm; Put shoulder three, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm; Shoulder three, manually control the temperature to rise by 20-60w, then set the program to rise, the frequency of the temperature rise is 60-100w / h, and the crystal diameter gradually decreases to 65-70mm; Put the shoulder four, set the program to cool down, the cooling frequency is 100-120w / h, and the crystal diameter gradually grows to 80-85mm.
9. The method for preparing detector-grade high-purity germanium single crystal according to claim 1, It is characterized in that The finishing step is to lower the crucible lifting speed, control the power to evenly cool down the temperature, and finish until the dissolved material in the quartz crucible is completely pulled out.
10. The method for preparing detector-grade high-purity germanium single crystal according to claim 9, It is characterized in that The cooling frequency is 100-200w / h, and the final time is 2-3h.
Citation Information
Cited By
High-proportion 13N germanium single crystal and preparation method thereof
CN121065807A