Manufacturing method of crystal for adjusting spectrum
Through the combination of quantum dot crystals and single crystals, the problem that the light source cannot adjust the spectral band is solved, the eyes are protected, the damage to the eyes by invisible light is reduced, and the safety of the light source is improved.
Patent Information
- Application Number
- CN202410783260.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing light sources such as LED lights and mobile phones cannot adjust the spectral band when used, resulting in invisible band light causing damage to the eyes and affecting vision and health.
The combination of quantum dot crystals and single crystals is used to form metal ion colloidal particles through ultrasonic cleaning, drying, dissolution, reduction and stabilizer treatment, forming nanocrystals, and sintered on the substrate surface to generate crystals with spectral adjustment capabilities.
Controllable adjustment of the spectral band is achieved, which reduces damage to the eyes, protects eye health, and improves the safety of the light source.
Smart Images

Figure CN118880459A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical crystals, and in particular to a method for manufacturing a crystal for adjusting a spectrum. Background Art
[0002] The spectrum is a pattern in which the dispersed monochromatic lights are arranged in sequence according to their wavelengths after the complex lights are split by the dispersion system. The full name is the optical spectrum. The largest part of the spectrum, the visible spectrum, is the part of the electromagnetic spectrum visible to the human eye. The electromagnetic radiation in this wavelength range is called visible light. The spectrum does not include all the colors that the human brain can distinguish, such as brown and pink. With the introduction of various artificial light sources into our lives, some wavelengths of light in the spectrum are difficult to be seen by the naked eye, but are harmful to the human eye, such as short-wave blue light and short-wave red light. These wavelengths are not directly seen by the human eye. If the human eye is affected by these wavelengths for a long time, it is easy to cause eye damage and affect the health of the human eye.
[0003] Some current electronic products or lighting sources, such as LED lights or tablets and mobile phones, will generate invisible bands of light. These bands of light are very harmful to the human eyes. Long-term use can easily cause symptoms such as myopia, hyperopia, astigmatism and eye fatigue, causing eye damage and affecting vision. When these current light sources are used, it is impossible to adjust the spectral bands of the light sources, which causes visible light and invisible light to enter the human eye at the same time, and the human body has no perception. Over time, eye fatigue and damage will occur, affecting eye vision. Summary of the invention
[0004] The object of the present invention is to provide a crystal manufacturing method for adjusting spectrum to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a crystal for adjusting a spectrum, comprising the following steps:
[0006] S1. Prepare the substrate, place the substrate into an ultrasonic cleaning device for cleaning, then remove the cleaned substrate from the ultrasonic cleaning device, and place the cleaned substrate into a drying device for drying;
[0007] S2. Then prepare at least one of the metallic silver, copper, cadmium and zinc raw materials, prepare a solvent and a reaction vessel, add the solvent to the reaction vessel, and then add the metal raw material to the solvent in the reaction vessel to form metal ions;
[0008] S3. preparing an active agent, then adding water to the dissolved metal ion material to form a metal ion solution, and then adding the active agent to the metal ion solution to form metal ion colloidal particles;
[0009] S4. preparing a reducing agent, adding the reducing agent to the mixed solution containing the metal ion colloidal particles, reducing the metal ions in the metal ion colloidal particles to metal atoms under the catalytic action of the reducing agent, and then forming nanocrystals through the continued catalysis of the active agent;
[0010] S5. Prepare a stabilizer, add the stabilizer after adding the reducing agent to the mixed solution of the metal ion colloidal particles, the stabilizer will form a chemical bond protective film on the surface of the nanocrystals to prevent oxygen and light from entering the nanocrystals;
[0011] S6. Attach the formed nanocrystals to the surface of the substrate, and then sinter the substrate and the nanocrystals so that the nanocrystals are fixed to the surface of the substrate, and then the nanocrystals grow on the surface of the substrate to form quantum dot crystals.
[0012] In a further embodiment, the substrate is a single crystal silicon crystal, and the ultrasonic cleaning time of the substrate is 10 minutes to 15 minutes. The single crystal silicon crystal has good light regulation ability, and combined with the quantum dot nanocrystals, it can achieve spectrum regulation, so that the light source can limit its spectral range, reduce the damage to the eyes caused by invisible light in a larger range of bands, and ensure the health of the eyes.
[0013] In a further embodiment, the drying equipment uses inert gas blowing and drying, and the inert gas is at least one of helium, argon and xenon. The substrate drying time is 20 minutes to 30 minutes. The inert gas can improve the drying efficiency of the substrate, and at the same time prevent the cleaned substrate from being damaged by oxidation due to oxygen, thereby ensuring the integrity of the precipitation.
[0014] In a further embodiment, the dissolving agent is at least one of hydrochloric acid and nitric acid, and the reaction container is a round-bottom flask.
[0015] In a further embodiment, the active agent is a surfactant, and the active agent is at least one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the sodium dodecyl sulfate and sodium dodecylbenzene sulfonate are both solid powders, which are dissolved and mixed into a solvent by adding clean water before adding.
[0016] In a further embodiment, the reducing agent is at least one of hydrogen, sodium hydride, lithium aluminum hydride and sodium borohydride, and the metal ions are reduced by the reducing agent to form nanocrystals with the active agent crystallization.
[0017] In a further embodiment, the stabilizer is at least one of propylacetic acid and mercaptopropionic acid. The stabilizer provides protection during the synthesis of quantum dot nanocrystals to ensure that the nanocrystals will not be affected by the external environment, which would cause the quality of the nanocrystals to deteriorate.
[0018] In a further embodiment, the sintering temperature of the substrate and the nanocrystals is 250° C.-280° C., and the sintering time of the substrate and the nanocrystals is 1 h-1.5 h. The synthesis of the crystals and the substrate is made more efficient and stable by high temperature.
[0019] In a further embodiment, after sintering the substrate and the nanocrystals, an inert gas is sprayed onto the surface of the generated crystal. The inert gas is at least one of helium, argon and xenon. By spraying the inert gas onto the surface of the synthesized crystal, the crystal is isolated from contact with oxygen, thereby preventing the problem of high-temperature oxidation.
[0020] In a further embodiment, the sintering of the substrate and the nanocrystals is carried out under a pressure environment of 0.05-0.1 MPa. During the sintering process of the crystals, the sintering effect and quality can be stabilized by adjusting the pressure.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention uses quantum dot crystals in combination with single crystals to form a spectrum adjustment crystal that can adjust the spectrum band. This crystal is applied to the light source to achieve controllable spectrum band adjustment, reduce the light band that causes damage to human eyes, prevent damage to the eyes caused by light of different bands, and protect the health of the eyes;
[0023] 2. The present invention adopts quantum dot material technology to make spectrum-adjusting crystals. Quantum dots are a kind of nanomaterial whose properties depend on their size and shape. They are usually synthesized on a sub-second time scale through difficult-to-control ion metathesis reactions. They are a kind of luminescent material with practical value and are commonly used in light-emitting diodes, liquid crystal displays, lasers, scintillators and various lighting equipment. The material exhibits good photoluminescence properties, including a nearly uniform photoluminescence quantum yield and a photoluminescence peak value that is adjustable within the spectral range, thereby achieving a good light source adjustment effect for the spectral band seen by the human eye, reducing the damage to the human eye caused by more invisible light in the light source spectrum, and ensuring eye health;
[0024] 3. The present invention utilizes a single crystal substrate with high crystal integrity and light transmittance, as well as low input loss, and grows nano-quantum dot crystals on its surface to form a crystal with spectrum adjustment function, which can better provide spectral band adjustment and light transmission for the light source, so that the spectrum of the light source can be constrained within a certain band, reducing the presence of invisible light that is harmful to the eyes in larger bands, thereby improving the safety of the light source spectrum and protecting the user's eye health. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1It is a schematic diagram of the framework of the crystal production method of the present invention. DETAILED DESCRIPTION
[0026] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] See also Figure 1 This embodiment provides a method for making a crystal for adjusting a spectrum, comprising the following steps:
[0029] S1. Prepare a substrate, place the substrate in an ultrasonic cleaning device for cleaning, then take the cleaned substrate out of the ultrasonic cleaning device, place the cleaned substrate in a drying device for drying, clean and dry the substrate so that the surface of the substrate is clean, and the subsequent substrate and nanocrystals are combined to generate a crystal for adjusting the spectrum, so that the adhesion is stronger, and more impurities are prevented from appearing in the crystal, which affects the light source adjustment effect of the crystal;
[0030] S2. Then prepare at least one of the metallic silver, copper, cadmium and zinc raw materials, prepare a solvent and a reaction vessel, add the solvent to the reaction vessel, and then add the metal raw material to the solvent in the reaction vessel to form metal ions;
[0031] S3. preparing an active agent, then adding water to the dissolved metal ion material to form a metal ion solution, and then adding the active agent to the metal ion solution to form metal ion colloidal particles;
[0032] S4. preparing a reducing agent, adding the reducing agent to the mixed solution containing the metal ion colloidal particles, reducing the metal ions in the metal ion colloidal particles to metal atoms under the catalytic action of the reducing agent, and then forming nanocrystals through the continued catalysis of the active agent;
[0033] S5. Prepare a stabilizer. After adding the reducing agent to the mixed solution of metal ion colloidal particles, add the stabilizer. The stabilizer will form a chemical bond protective film on the surface of the nanocrystals to prevent oxygen and light from entering the nanocrystals. The stabilizer can form an anti-oxidation and anti-glare protective layer during the nanocrystal generation process, which can effectively reduce the impact of external factors on the nanocrystals and ensure the production quality of the nanocrystals.
[0034] S6. Attach the formed nanocrystals to the surface of the substrate, and then sinter the substrate and the nanocrystals so that the nanocrystals are fixed to the surface of the substrate, and then the nanocrystals grow on the surface of the substrate to form quantum dot crystals.
[0035] Quantum dots, also known as "semiconductor nanocrystals", are nano-scale semiconductors. By applying a certain electric field or light pressure to this nano-semiconductor material, they will emit light of a specific frequency, and the frequency of the emitted light will change with the size of the semiconductor. Therefore, by adjusting the size of the nano-semiconductor, the color of the light it emits can be controlled. Since this nano-semiconductor has the property of limiting electrons and electron holes, this property is similar to atoms or molecules in nature, it is called quantum dots. Quantum dot display is considered to be the next generation of display technology after organic light-emitting display, with the advantages of high color purity, wide color gamut, easy to realize large-screen flexible display, and low device cost. Nanocrystals made of quantum dots can adjust the range of the spectrum, effectively preventing the spectral range of the light source from being too large and causing damage to the eyes.
[0036] Because the quantum dots may have poor stability in the nanocrystals after the production process, if there are defects in the production of nanocrystals, multi-base ligand modification is used to stabilize the quantum dots. Multi-base ligand modification can be completed by cucurbituril. Multi-base ligands have a large number of binding sites. When they are used to modify quantum dots, they can significantly improve the stability of quantum dots in complex environments. At the same time, multi-base ligand encapsulation modification technology can also increase the synthesis rate of quantum dots. The conventional quantum dot synthesis rate is about 30%. The synthesis rate of quantum dots modified with multi-base ligands in aqueous phase is greatly improved. For example, the quantum yield of CdSe / CdS modified with dextran in aqueous phase can reach 46%; citrate and polycysteine modified The quantum yield of quantum dots reaches 52%; the quantum yield of CdSe / CdS modified with stearylamine polymer or water-soluble resin stone in aqueous phase can reach 56%. Polymer modification is also suitable for the preparation of high-quality alloy quantum dots. However, its disadvantages are also obvious. The surface of quantum dots modified with multi-base ligands is wrapped by a large number of multi-base ligands, which leads to a decrease in the luminescence intensity of quantum dots. At the same time, due to the low activation energy of the chemical reaction of multi-base ligands and the reaction is easily affected by the external environment concentration, temperature and pH value, etc., so controlling the reaction conditions is the key factor in determining the synthesis yield of quantum dots. Therefore, multi-base ligand modification is used to further stabilize the production of nanocrystals made of quantum dots and improve the quality of nanocrystals.
[0037] Example 2
[0038] See also Figure 1A method for making a crystal for adjusting a spectrum comprises the following steps: preparing a substrate, placing the substrate in an ultrasonic cleaning device for cleaning, then taking the cleaned substrate out of the ultrasonic cleaning device, and placing the cleaned substrate in a drying device for drying; then preparing at least one of metal silver, copper, cadmium and zinc raw materials, then preparing a solvent and a reaction container, adding the solvent to the reaction container, and then adding the metal raw material to the solvent in the reaction container to form metal ions; preparing an active agent, then adding clean water to the dissolved metal ion material to form a metal ion solution, and then adding the active agent to the metal ion solution to form metal ion colloidal particles; preparing A reducing agent is added to a mixed solution containing metal ion colloidal particles. Under the catalytic action of the reducing agent, the metal ions in the metal ion colloidal particles are reduced to metal atoms. At this time, nanocrystals are formed through the continued catalysis of the activator; a stabilizer is prepared. After the reducing agent is added to the mixed solution of the metal ion colloidal particles, the stabilizer will form a chemical bond protective film on the surface of the nanocrystals to prevent oxygen and light from entering the nanocrystals; the formed nanocrystals are attached to the surface of the substrate, and then the substrate and the nanocrystals are sintered to fix the nanocrystals to the surface of the substrate, and then the nanocrystals grow on the surface of the substrate to form quantum dot crystals.
[0039] Quantum dot crystals can be excited by wavelength excitation light in the spectrum, and the fluorescence peak can be regulated by changing the physical size. In this way, the same excitation light can be used to simultaneously excite multiple quantum dots, thereby emitting fluorescence of different wavelengths for multivariate fluorescence detection. On the contrary, the fluorescence of multiple dyes often requires multiple lasers to be excited, which not only increases the cost of the experiment, but also makes the analysis system more complicated. In addition, due to this optical property, a more suitable excitation wavelength can be selected from its continuous excitation spectrum, so as to minimize the spontaneous fluorescence of biological samples, improve resolution and sensitivity, make various display devices and lighting equipment more colorful, and be able to limit the spectral band to a certain range, thereby achieving the effect of eye protection, reducing the damage to the eyes caused by different wavelengths, and ensuring the health of the user's eyes.
[0040] The substrate is a single crystal silicon crystal, and the ultrasonic cleaning time of the substrate is 10 minutes to 15 minutes.
[0041] The drying equipment uses inert gas blowing for drying. The inert gas is at least one of helium, argon and xenon. The substrate drying time is 20 minutes to 30 minutes. During the drying process of the substrate, the inert gas is used for drying. Filling with inert gas can effectively protect the product quality and avoid oxidation, corrosion or other chemical reactions of the sample during the processing. Especially for products that are easily oxidized, corrosive and volatile, filling with inert gas can better maintain their stability. Filling with inert gas can also increase the drying speed of the drying equipment, because inside the drying equipment, in addition to the product, a large number of gas molecules will occupy the remaining space, causing the drying speed to slow down. Filling with inert gas can occupy these spaces, so that the drying speed is increased, thereby shortening the processing time and improving the efficiency of substrate processing.
[0042] The dissolving agent is at least one of hydrochloric acid and nitric acid, and the reaction container is a round-bottom flask. The dissolving agent can dissolve the metal raw material, neutralize the pH value of the metal raw material, and form metal ions.
[0043] The active agent is a surfactant, which is at least one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate. Both sodium dodecyl sulfate and sodium dodecylbenzene sulfonate are solid powders, which are dissolved and mixed into a solvent by adding clean water before adding.
[0044] The reducing agent is at least one of hydrogen, sodium hydride, lithium aluminum hydride and sodium borohydride. The reducing agent can reduce metal ions to metal atoms, and then form nanocrystals under the action of a surfactant.
[0045] The stabilizer is at least one of propylacetic acid and mercaptopropionic acid. During the crystallization process of the quantum dot nanocrystals, the stabilizer will wrap a protective film on the outside of the quantum dot nanocrystals, which can prevent the nanocrystals from being affected by oxygen and strong light during the crystallization process, and prevent problems such as oxidation and strong light damage, thereby ensuring the production stability and quality of the nanocrystals.
[0046] The sintering temperature of the substrate and the nanocrystals is 250°C-280°C, and the sintering time of the substrate and the nanocrystals is 1h-1.5h. Through high-temperature flame sintering, the substrate and the nanocrystals can be fully synthesized, making the crystal structure generated by the substrate and the nanocrystals more stable. When used in the subsequent light source production, the crystals can be used more stably.
[0047] After the substrate and nanocrystals are sintered, an inert gas is sprayed onto the surface of the generated crystal. The inert gas is at least one of helium, argon and xenon. After the substrate and nanocrystals are sintered, in order to prevent the problem of high-temperature oxidation of the crystal surface after sintering, by spraying inert gas onto the surface of the generated crystal, the surface oxidation of the crystal can be effectively reduced before cooling, thereby ensuring the integrity of the crystal.
[0048] The sintering of the substrate and the nanocrystals is carried out under a pressure environment of 0.05-0.1MPa. The substrate and the nanocrystals are sintered under a pressure of 0.05-0.1MPa. This sintering pressure can effectively improve the generation efficiency of quantum dot crystals, increase the yield of quantum dot crystals, and ensure that the combined crystals of the substrate and nanocrystals after sintering are more stable.
[0049] The method for making a crystal with an adjustable spectrum specifically comprises the following steps: firstly preparing a substrate, a metal raw material, an activator, a reducing agent, a stabilizer and a solvent material, and then preparing an ultrasonic cleaning device, a drying device, a reaction vessel and a sintering device, and a device and equipment for making a crystal. When making a crystal, firstly placing the substrate in an ultrasonic cleaning device for cleaning, using an acetone solution or clean water for cleaning, and taking out the substrate after cleaning in the ultrasonic cleaning device, placing the cleaned substrate in a drying device, starting the drying device for blowing and drying the substrate, and using an inert gas to dry the substrate. The inert gas can effectively reduce the involvement of oxygen and prevent the problem of surface oxidation of the substrate. The dried substrate is taken out for use, and then the production of quantum dot crystals is started. Firstly, a metal raw material is taken, and the metal raw material is added to a reaction vessel, and then the activator prepared in advance is added to the reaction vessel containing the metal raw material, and a solvent for mixing is added at the same time. The solvent can be selected from at least one of clean water, methanol and ethanol. Then, the activator catalyzes the generation of a certain amount of colloidal particles in the mixed liquid of the metal material and the solvent, and then a reducing agent and a stabilizer are added to the reaction vessel. The reducing agent can reduce the metal in the mixed liquid. The material is reduced to metal atoms, and the active agent continues to catalyze, so that crystals are formed on the outside of the colloidal particles. The crystals are gradually catalyzed to form nanocrystals. In the process of forming crystals, the stabilizer will generate a protective layer on the surface of the crystals. This protective layer can isolate the crystals from external oxygen and reduce direct exposure to strong light. After waiting for the crystallization in the mixed liquid to be completed, nanocrystals of quantum dots are obtained. The nanocrystals are then spread on the surface of the substrate, and then the substrate and nanocrystals are placed in a sintering device. The sintering device is turned on, and the nanocrystals are attached to the outside of the substrate by high temperature to produce a complete crystal that adjusts the spectrum. During the sintering process, the protective layer produced by the stabilizer will fall off and melt, so that the obtained crystals can have better light adjustment capabilities. The crystals produced are made of nanomaterials. Quantum dots are a type of semiconductor nanocrystal material, and their size is usually between a few nanometers and tens of nanometers. Due to the quantum confinement effect, quantum dots exhibit different photoelectric properties from traditional bulk materials, especially their adjustable luminescence wavelength and high luminescence efficiency, which can effectively limit the spectral range of the light source, achieve band adjustment of the spectrum, reduce damage to the human eye due to a larger spectral range, and ensure the health of the user's eyes.
[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for making a crystal for adjusting a spectrum, It is characterized in that The following steps are involved: S1. Prepare the substrate, place the substrate into an ultrasonic cleaning device for cleaning, then remove the cleaned substrate from the ultrasonic cleaning device, and place the cleaned substrate into a drying device for drying; S2. Then prepare at least one of the metallic silver, copper, cadmium and zinc raw materials, prepare a solvent and a reaction vessel, add the solvent to the reaction vessel, and then add the metal raw material to the solvent in the reaction vessel to form metal ions; S3. preparing an active agent, then adding water to the dissolved metal ion material to form a metal ion solution, and then adding the active agent to the metal ion solution to form metal ion colloidal particles; S4. preparing a reducing agent, adding the reducing agent to the mixed solution containing the metal ion colloidal particles, reducing the metal ions in the metal ion colloidal particles to metal atoms under the catalytic action of the reducing agent, and then forming nanocrystals through the continued catalysis of the active agent; S5. Prepare a stabilizer, add the stabilizer after adding the reducing agent to the mixed solution of the metal ion colloidal particles, the stabilizer will form a chemical bond protective film on the surface of the nanocrystals to prevent oxygen and light from entering the nanocrystals; S6. Attach the formed nanocrystals to the surface of the substrate, and then sinter the substrate and the nanocrystals so that the nanocrystals are fixed to the surface of the substrate, and then the nanocrystals grow on the surface of the substrate to form quantum dot crystals.
2. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The substrate is a single crystal silicon crystal, and the ultrasonic cleaning time of the substrate is 10 minutes to 15 minutes.
3. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The drying equipment uses inert gas blowing for drying, the inert gas is at least one of helium, argon and xenon, and the substrate drying time is 20 minutes to 30 minutes.
4. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The dissolving agent is at least one of hydrochloric acid and nitric acid, and the reaction container is a round-bottom flask.
5. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The active agent is a surfactant, and the active agent is at least one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate. Both sodium dodecyl sulfate and sodium dodecylbenzene sulfonate are solid powders, and are dissolved and mixed into a solvent by adding clean water before adding.
6. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The reducing agent is at least one of hydrogen, sodium hydride, lithium aluminum hydride and sodium borohydride.
7. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The stabilizer is at least one of propylacetic acid and mercaptopropionic acid.
8. A method for making a crystal for adjusting a spectrum according to claim 1, Features: The sintering temperature of the substrate and the nanocrystals is 250° C.-280° C., and the sintering time of the substrate and the nanocrystals is 1 h-1.5 h.
9. A method for making a crystal for adjusting a spectrum according to claim 1, Features: After the substrate and the nanocrystals are sintered, an inert gas is sprayed onto the surface of the generated crystals, wherein the inert gas is at least one of helium, argon and xenon.