Annealing method of indium antimonide wafer

The liquid phase annealing is carried out through the recoagulation method of mixed solution of ethanol and tellurium tetrachloride, which solves the problem of indium antimonide crystal doping integrated, improves the uniformity and use effect of the InSb detector, reduces chip damage, and simplifies Equipment requirements.

CN118880469AActive Publication Date: 2024-11-01GUANGDONG JINGZHI OPTOELECTRONICS TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410959237.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The uneven fringe problem caused by the inhomogeneity of doping in indium antimonide crystals during growth affects the effectiveness of the InSb detector, and the commonly used gas-phase annealing method will lead to wafer damage and high equipment costs.

Method used

The liquid phase annealing is performed by a mixed solution of ethanol and tellurium tetrachloride. By gradually diffusing the Te element to improve doping uniformity, and avoiding the loss of Te through the coagulation device, the dual functions of annealing and doping are achieved.

Benefits of technology

The doping uniformity of indium antimonide wafers is improved, the uneven stripe problem of InSb detectors is solved, the damage to the wafer is reduced, and the equipment needs are simplified, ensuring the effectiveness of the InSb detectors is used.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880469A_ABST
    Figure CN118880469A_ABST
Patent Text Reader

Abstract

The annealing method of the indium antimonide wafer comprises the following steps: S1, growing an undoped Te InSb crystal with the carrier concentration of less than 2E14 / cm < 3 > by using a Czochralski method; s2, slicing the InSb crystal to serve as an InSb wafer; s3, grinding and polishing the InSb wafer; s4, the mixed solution of ethyl alcohol and tellurium tetrachloride is added into the flask through a ground opening of the flask, the mass fraction of tellurium tetrachloride in the mixed solution is 1-5%, and the other ground opening of the flask is used for installing a back condensation device; s5, putting the ground and polished InSb wafer into the mixed solution of the flask through one grinding opening, and completely immersing the InSb wafer into the mixed solution; s6, mounting the recondensation device on the corresponding ground opening of the flask, and blocking the other ground opening of the flask; and S7, raising the temperature of the mixed solution in the flask to 60-70 DEG C, and annealing for 10-20 hours by adopting a recondensation mode to finish annealing. Therefore, the doping uniformity of the indium antimonide wafer is improved, and the problem of non-uniform stripes of the manufactured InSb detector is fundamentally solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of indium antimonide crystals, and more particularly to an annealing method for indium antimonide wafers. Background Art

[0002] InSb is a narrow-bandgap III-V semiconductor material with a bandgap width of 0.232eV at 77K. It has intrinsic absorption in the 3-5μm band and has extremely high electron mobility. It is currently one of the best materials for medium-wave infrared detectors. The melting point of inSb is 525℃. Compared with other III-V compounds, it is easy to purify and grow single crystals, so it is often the object of choice in theoretical research on III-V compound solids.

[0003] When growing N-type indium antimonide crystals, it is generally necessary to dope Te (tellurium) elements. However, because the segregation coefficient of the Te element is less than 1, as the crystal grows, the concentration of the Te element in the crystal becomes higher and higher. Moreover, due to the existence of the facet effect, the amount of Te element doping in the facet area and the non-facet area is different, resulting in uneven radial electrical parameters of the crystal. In response to the problem of axial doping unevenness, the "Progress in Research on Indium Antimonide Single Crystal Materials" (Zhe Weilin et al., Laser and Infrared, Vol. 54, No. 2, February 2024, pp. 235-241) adjusted the growth rate and rotation speed of the crystal throughout the process, and reduced the axial Te element unevenness of the crystal by controlling the effective segregation coefficient of the Te element, thereby improving the uniformity of the electrical parameters of the crystal in the axial direction. In response to the problem of radial doping unevenness, the size of the facet area is controlled as much as possible by stably controlling the solid-liquid interface of crystal growth, thereby improving the uniformity of the electrical parameters of the crystal in the radial direction. However, despite this, uneven vertical stripes can still be seen in the signal response diagram of the InSb detector. The presence of these stripes indicates that there is still a large unevenness in the wafer, which seriously affects the use effect of the detector prepared with this material.

[0004] Annealing is a commonly used method to improve the electrical uniformity of materials. In the commonly used gas phase annealing / vacuum annealing process, Te atoms in InSb migrate in the crystal by diffusion at high temperature, but InSb will also decompose at high temperature, causing damage to the wafer surface, and easily generating thermal stress, causing dislocation proliferation. In addition, due to the need to ensure a sufficiently low oxygen content and use the gas phase as the annealing medium, large-sized single crystals require a larger vacuum chamber to control single crystal defects, which increases equipment cost and process complexity.

[0005] Therefore, it is necessary to provide further improvements on the doping uniformity of the indium antimonide wafer, so as to ensure the use effect of the manufactured InSb detector. Summary of the invention

[0006] In view of the problems existing in the background technology, an object of the present disclosure is to provide an annealing method of an InSb wafer, which can improve the doping uniformity of the InSb wafer.

[0007] Another object of the present disclosure is to provide an annealing method for an InSb wafer, which can fundamentally solve the problem of uneven stripes of InSb detectors made of InSb wafers, thereby ensuring the use effect of InSb detectors made of InSb wafers.

[0008] Another object of the present disclosure is to provide an annealing method for an indium antimonide wafer, which can reduce damage to the InSb wafer.

[0009] Another object of the present disclosure is to provide an annealing method for an indium antimonide wafer, which requires simple equipment.

[0010] Thus, an annealing method for an indium antimonide wafer comprises the steps of: S1, growing an undoped Te wafer having a carrier concentration of 2E14 / cm by a Czochralski method; 3 The following InSb crystals; S2, slicing the InSb crystals as InSb wafers; S3, grinding and polishing the InSb wafers; S4, adding a mixed solution of ethanol and tellurium tetrachloride into the flask through a ground mouth of the flask, the mass fraction of tellurium tetrachloride in the mixed solution is 1-5%, and the other ground mouth of the flask is used to install a condensation device; S5, placing the ground and polished InSb wafer into the mixed solution of the flask through one of the ground mouths and completely immersing it in the mixed solution; S6, installing the condensation device on the corresponding ground mouth of the flask, and sealing the other ground mouth of the flask; S7, heating the mixed solution in the flask to 60-70°C, annealing for 10-20h by condensation, and completing annealing.

[0011] The beneficial effects of the present disclosure are as follows.

[0012] In the annealing method of the indium antimonide wafer according to the present disclosure, the undoped Te is grown by the pulling method in step S1 with a carrier concentration of 2E14 / cm 3 The following InSb crystal, after the InSb wafer is made in step S2 to step S3, is subjected to liquid phase annealing in a mixed solution consisting of ethanol and tellurium tetrachloride in a recondensation manner through steps S4 to step S7, and Te in the mixed solution gradually diffuses into the interior of the InSb wafer to achieve the purpose of uniform doping, that is, to improve the doping uniformity of the InSb wafer, thereby fundamentally solving the problem of uneven stripes of the InSb detector made of the InSb wafer, thereby ensuring the use effect of the InSb detector made of the InSb wafer.

[0013] Compared with the doping method of growing InSb crystals by the pulling method in the background art, in the annealing method of indium antimonide wafer according to the present invention, through steps S1 to S7, the doping of Te is adjusted to the annealing process, that is, the annealing process has the dual functions of doping and annealing, making the uniformity of Te doping more simple and effective.

[0014] In the annealing method of indium antimonide wafer according to the present disclosure, in steps S4 to S7, the use of a condensation device avoids the loss of Te caused by the volatilization of ethanol and ensures the accuracy of doping.

[0015] In the annealing method of the indium antimonide wafer according to the present disclosure, through steps S4 to S7, the carrier concentration of the annealed InSb wafer can be made to be 4E14 / cm 3 -1.4E15 / cm 3 Within the range of , the use effect of InSb detectors made of InSb wafers is guaranteed.

[0016] In the annealing method of indium antimonide wafers according to the present disclosure, the use of a liquid phase mixed solution as the annealing medium makes the defect reaction process (i.e., doping and redistribution of existing impurities inside) more gentle and moderate, reduces damage to the InSb wafer, and requires relatively simple equipment. Because the liquid phase mixed solution has no definite shape and good fluidity, liquid phase annealing is not limited by the size of the InSb wafer, as long as it can flow and cover the InSb wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a schematic diagram of an exemplary Czochralski growth apparatus involved in the annealing method of an indium antimonide wafer according to the present disclosure.

[0018] Figure 2 Schematic diagram of an exemplary flask with a condensation device involved in the annealing method of indium antimonide wafer according to the present disclosure.

[0019] Figure 3 This is a carrier concentration distribution diagram of a slice at the head of the InSb crystal rod grown by the Czochralski method in Example 1.

[0020] Figure 4 This is a carrier concentration distribution diagram of a slice at the tail of the InSb crystal rod grown by the Czochralski method in Example 1.

[0021] Figure 5 This is a carrier concentration distribution diagram of the InSb wafer of Example 1 after annealing.

[0022] Figure 6 This is a signal response diagram of the InSb detector after the annealed InSb wafer in Example 1 is used to make an InSb infrared focal plane detector.

[0023] Figure 7 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 1 after annealing.

[0024] Figure 8 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 2 after annealing.

[0025] Fig. 9 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 3 after annealing.

[0026] Fig.10 This is a carrier concentration distribution diagram of the InSb wafer made from the InSb crystal rod grown by the Czochralski method in Example 4.

[0027] Fig.11 This is a signal response diagram of the InSb detector after the InSb infrared focal plane detector is manufactured from the InSb wafer of Comparative Example 4. DETAILED DESCRIPTION

[0028] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.

[0029] [Annealing method of indium antimonide wafer]

[0030] Reference Figure 1 and Figure 2 According to the present disclosure, the annealing method of indium antimonide wafer comprises the steps of:

[0031] S1, undoped Te grown by Czochralski method with a carrier concentration of 2E14 / cm 3 The following InSb crystals;

[0032] S2, slicing the InSb crystal into InSb wafers;

[0033] S3, grinding and polishing the InSb wafer;

[0034] S4, adding a mixed solution of ethanol and tellurium tetrachloride into the flask through a ground mouth of the flask, wherein the mass fraction of tellurium tetrachloride in the mixed solution is 1-5%, and another ground mouth of the flask is used to install a condensation device;

[0035] S5, placing the ground and polished InSb wafer into the mixed solution in the flask through one of the ground openings and completely immersing the wafer in the mixed solution;

[0036] S6, installing the condensation device on the corresponding ground mouth of the flask, and sealing the other ground mouth of the flask;

[0037] S7, raising the temperature of the mixed solution in the flask to 60-70°C, and annealing for 10-20 hours by condensation to complete annealing.

[0038] In the annealing method of the indium antimonide wafer according to the present disclosure, the undoped Te is grown by the pulling method in step S1 with a carrier concentration of 2E14 / cm 3 The following InSb crystal, after the InSb wafer is made in step S2 to step S3, is subjected to liquid phase annealing in a mixed solution consisting of ethanol and tellurium tetrachloride in a recondensation manner through steps S4 to step S7, and Te in the mixed solution gradually diffuses into the interior of the InSb wafer to achieve the purpose of uniform doping, that is, to improve the doping uniformity of the InSb wafer, thereby fundamentally solving the problem of uneven stripes of the InSb detector made of the InSb wafer, thereby ensuring the use effect of the InSb detector made of the InSb wafer.

[0039] Compared with the doping method of growing InSb crystals by the pulling method in the background art, in the annealing method of indium antimonide wafer according to the present invention, through steps S1 to S7, the doping of Te is adjusted to the annealing process, that is, the annealing process has the dual functions of doping and annealing, making the uniformity of Te doping more simple and effective.

[0040] In the annealing method of indium antimonide wafer according to the present disclosure, in steps S4 to S7, the use of a condensation device avoids the loss of Te caused by the volatilization of ethanol and ensures the accuracy of doping.

[0041] In the annealing method of the indium antimonide wafer according to the present disclosure, through steps S4 to S7, the carrier concentration of the annealed InSb wafer can be made to be 4E14 / cm 3 -1.4E15 / cm 3 Within the range of , the use effect of InSb detectors made of InSb wafers is guaranteed.

[0042] In the annealing method of indium antimonide wafers according to the present disclosure, the use of a liquid phase mixed solution as the annealing medium makes the defect reaction process (i.e., doping and redistribution of existing impurities inside) more gentle and moderate, reduces damage to the InSb wafer, and requires relatively simple equipment. Because the liquid phase mixed solution has no definite shape and good fluidity, liquid phase annealing is not limited by the size of the InSb wafer, as long as it can flow and cover the InSb wafer.

[0043] In one example, refer to Figure 1 In step S1, the Czochralski method adopts the following sub-steps:

[0044] S11, the zone-melted purified 7.5N InSb polycrystalline material is cleaned with aqua regia and then

[0045] Rinse with water for more than 3 times, and dry in a vacuum oven for later use;

[0046] S12, loading the dried InSb polycrystalline material into the quartz crucible;

[0047] S13, evacuate the CZ crystal growth device, remove gas, and check for leaks, so that the CZ crystal growth device reaches a vacuum, and the vacuum pressure is below 10Pa (monitored by a pressure gauge (not shown)). The vacuum pump is used to evacuate the CZ crystal growth device and fill nitrogen into the CZ crystal growth device alternately 2-3 times. The vacuum interface is set at the bottom of the CZ crystal growth device. Nitrogen (purity 7N) is used to remove gas, and nitrogen is filled into the CZ crystal growth device.

[0048] The gas inlet is arranged at the top of the Czochralski crystal growth device;

[0049] S14, after sub-step S13 is completed, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, and then the vacuum port and the gas inlet are closed;

[0050] S15, opening the gas inlet again, filling the CZC crystal growth apparatus with a nitrogen-hydrogen mixed gas so that the pressure in the CZC crystal growth apparatus reaches 0.1 MPa (monitored by a pressure gauge), and then closing the gas inlet;

[0051] S16, start heating the quartz crucible to heat up and melt the InSb polycrystalline material in the quartz crucible, wherein the heater includes a graphite heater, a graphite double-layer insulation cover and carbon felt, the graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover, and the heater for heating the quartz crucible is a Czochralski crystal production method.

[0052] The only heating device in a long device;

[0053] S17, when the InSb polycrystalline material is completely melted to form a melt-pulling crystal growth device, the pressure in the device rises to 0.15 MPa (monitored by a pressure gauge), and the temperature of the quartz crucible is maintained unchanged, wherein:

[0054] Observe and confirm the formation of melt through an observation window (not shown, disposed on the top cover);

[0055] S18, after sub-step S17, the crystal pulling rod drives the seed crystal to move downward into the quartz crucible and immerse it from the surface of the melt, and then the crystal pulling rod is pulled upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the crystal pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 1rpm, the rotation speed of the crystal pulling rod is 3rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant.

[0056] Set to 5mm / h;

[0057] S19, after the crystal growth is completed, stop heating, cool down, replace the gas in the Czochralski crystal growth equipment with nitrogen through the vacuum pump through the vacuum interface and the gas inlet, open the Czochralski crystal growth equipment, and cut the crystal rod from the pulling rod.

[0058] It is noted that before the vacuum pump in sub-steps S15 to S19 is turned on, the atmosphere in the Czochralski crystal growth apparatus is a closed nitrogen-hydrogen mixed gas.

[0059] In one example, in step S2, the InSb crystal is sliced ​​using diamond single wire sawing.

[0060] In one example, in step S3, a double-sided grinder is used for grinding and polishing.

[0061] In one example, in step S3, grinding and polishing uses a polishing liquid prepared by mixing SiO2 sol at room temperature and pure water in a volume ratio of 1:1, and the grinding and polishing time is 30 seconds.

[0062] In one example, in step S4, the ethanol is ethanol with a mass fraction of 99%.

[0063] In step S5, the inner diameter of the corresponding ground opening for placing the InSb wafer is sufficient to accommodate the InSb wafer.

[0064] In one example, in step S7, the temperature is raised by using a water bath. Figure 2 As shown, the flask is placed in a water bath, and a heating device is used to heat the water in the water bath to achieve water bath temperature increase. The heating device can be an electric heating device.

[0065] In one example, in step S7, the condensation method is to install a condensation device at the corresponding ground mouth and introduce circulating cooling water through two interfaces to achieve the condensation of the mixed solution volatilized during the heating process and drop it back into the mixed solution.

[0066] [test]

[0067] Example 1

[0068] Example 1 adopts the following steps:

[0069] S1, undoped Te grown by Czochralski method with a carrier concentration of 2E14 / cm 3 For the following InSb crystal, the Czochralski method uses the following sub-steps:

[0070] S11, the zone-melted purified 7.5N InSb polycrystalline material is cleaned with aqua regia and then

[0071] Rinse with water for more than 3 times, and dry in a vacuum oven for later use;

[0072] S12, loading the dried InSb polycrystalline material into the quartz crucible;

[0073] S13, evacuate the CZ crystal growth device, remove gas, and check for leaks, so that the CZ crystal growth device reaches a vacuum, and the vacuum pressure is below 10Pa (monitored by a pressure gauge (not shown)). The vacuum pump is used to evacuate the CZ crystal growth device and fill nitrogen into the CZ crystal growth device alternately 2-3 times. The vacuum interface is set at the bottom of the CZ crystal growth device. Nitrogen (purity 7N) is used to remove gas, and nitrogen is filled into the CZ crystal growth device.

[0074] The gas inlet is arranged at the top of the Czochralski crystal growth device;

[0075] S14, after sub-step S13 is completed, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, and then the vacuum port and the gas inlet are closed;

[0076] S15, opening the gas inlet again, filling the CZC crystal growth apparatus with a nitrogen-hydrogen mixed gas so that the pressure in the CZC crystal growth apparatus reaches 0.1 MPa (monitored by a pressure gauge), and then closing the gas inlet;

[0077] S16, start heating the quartz crucible to heat up and melt the InSb polycrystalline material in the quartz crucible, wherein the heater includes a graphite heater, a graphite double-layer insulation cover and carbon felt, the graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover, and the heater for heating the quartz crucible is a Czochralski crystal production method.

[0078] The only heating device in a long device;

[0079] S17, when the InSb polycrystalline material is completely melted to form a melt-pulling crystal growth device, the pressure in the device rises to 0.15 MPa (monitored by a pressure gauge), and the temperature of the quartz crucible is maintained unchanged, wherein:

[0080] Observe and confirm the formation of melt through an observation window (not shown, disposed on the top cover);

[0081] S18, after sub-step S17, the crystal pulling rod drives the seed crystal to move downward into the quartz crucible and immerse it from the surface of the melt, and then the crystal pulling rod is pulled upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the crystal pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 1rpm, the rotation speed of the crystal pulling rod is 3rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant.

[0082] Set to 5mm / h;

[0083] S19, after the crystal growth is completed, the heating is stopped, the temperature is lowered, and the gas in the Czochralski crystal growth equipment is replaced with nitrogen through the vacuum pump interface and the gas inlet.

[0084] Czochralski crystal growth equipment, which cuts the crystal rod from the pulling rod;

[0085] S2, slicing the InSb crystal into InSb wafers using diamond single wire sawing;

[0086] S3, grinding and polishing the InSb wafer using a double-sided grinder, using a polishing liquid prepared by mixing SiO2 sol at room temperature and pure water in a volume ratio of 1:1, and the grinding and polishing time is 30 seconds;

[0087] S4, adding a mixed solution of ethanol and tellurium tetrachloride into the flask through a ground mouth of the flask, wherein the ethanol has a mass fraction of 99%, and the mass fraction of tellurium tetrachloride in the mixed solution is 3%, and another ground mouth of the flask is used to install a condensation device;

[0088] S5, placing the ground and polished InSb wafer into the mixed solution in the flask through one of the ground openings and completely immersing the wafer in the mixed solution;

[0089] S6, installing the condensation device on the corresponding ground mouth of the flask, and sealing the other ground mouth of the flask;

[0090] S7, placing the flask in a water bath, heating the water in the water bath by an electric heating device, raising the temperature of the mixed solution in the flask to 65°C, introducing circulating cooling water through two interfaces of the condensation device installed at the corresponding ground mouth, annealing for 15 hours by condensation method, and completing annealing.

[0091] Comparative Example 1

[0092] Except that in step S4, the mass fraction of tellurium tetrachloride in the mixed solution is 6%, the rest is the same as in Example 1.

[0093] Comparative Example 2

[0094] Except that the mixed solution in the flask is heated to 75° C. in step S7 , the rest is the same as in Example 1.

[0095] Comparative Example 3

[0096] Except for annealing for 25 hours in step S7, the rest is the same as in Example 1.

[0097] Comparative Example 4

[0098] Comparative Example 4 adopts the following steps:

[0099] Sa, InSb crystals are grown by the Czochralski method, which uses the following sub-steps:

[0100] Sa1, the zone-melt purified 7.5N InSb polycrystalline material was cleaned with aqua regia and then

[0101] Rinse with water for more than 3 times, and dry in a vacuum oven for later use;

[0102] Sa2, load the mixed and dried InSb polycrystalline material and Te powder into the quartz crucible

[0103] In the crucible, the mass ratio of Te powder to InSb polycrystalline material is 1 mg:10 kg;

[0104] Sa3, evacuate the CZ crystal growth equipment, remove gas, and check for leaks, so that the CZ crystal growth equipment reaches a vacuum, and the vacuum pressure is below 10Pa (monitored by a pressure gauge (not shown)). The vacuum pump is used to evacuate the CZ crystal growth equipment and fill nitrogen into the CZ crystal growth equipment alternately 2-3 times. The vacuum interface for evacuation is set at the bottom of the CZ crystal growth equipment. Nitrogen (purity 7N) is used to remove gas, and nitrogen is filled into the CZ crystal growth equipment.

[0105] The gas inlet is arranged at the top of the Czochralski crystal growth device;

[0106] Sa4, after the completion of sub-step Sa3, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, and then the vacuum interface and the gas inlet are closed;

[0107] Sa5, open the gas inlet again, fill the CZC crystal growth apparatus with a nitrogen-hydrogen mixture gas so that the pressure in the CZC crystal growth apparatus reaches 0.1 MPa (monitored by a pressure gauge), and then close the gas inlet;

[0108] Sa6, start heating the quartz crucible, heat up and melt the InSb polycrystalline material and Te powder in the quartz crucible, wherein the heater includes a graphite heater, a graphite double-layer insulation cover and carbon felt, the graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover, and the heater for heating the quartz crucible is provided

[0109] The only heating device in the Rafa crystal growth equipment;

[0110] Sa7, when the pressure in the Czochralski crystal growth apparatus rises to 0.15 MPa (monitored by a pressure gauge) after the InSb polycrystalline material and the Te powder are completely melted to form a melt, the temperature of the quartz crucible is maintained unchanged, wherein the formation of the melt is confirmed by observing through an observation window (not shown, disposed on the top cover);

[0111] Sa8, after sub-step Sa7, the pulling rod drives the seed crystal to move downward into the quartz crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds, the crucible rotation speed is 1rpm, the pulling rod rotation speed is 3rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant.

[0112] Set to 5mm / h;

[0113] Sa9, after the crystal growth is completed, stop heating, cool down, and replace the gas in the Czochralski crystal growth equipment with nitrogen through the vacuum pump interface and the gas inlet again.

[0114] Czochralski crystal growth equipment, which cuts the crystal rod from the pulling rod;

[0115] Sb, the InSb crystal is sliced ​​into InSb wafers using diamond single wire sawing.

[0116] That is, in Comparative Example 4, steps S3 to S7 of Example 1 are not adopted, and Te doping is directly performed in the InSb crystal grown by the Czochralski method.

[0117] Figure 3 This is a carrier concentration distribution diagram of a slice at the head of the InSb crystal rod grown by the Czochralski method in Example 1. Figure 4 This is a carrier concentration distribution diagram of a slice at the tail of the InSb crystal rod grown by the Czochralski method in Example 1. The carrier concentration distribution was plotted after detection by HL9900 of Toho Technology Company, USA.

[0118] from Figure 3 and Figure 4 It can be seen that the carrier distribution in the head slice and the tail slice of the InSb crystal rod is lower than 2E14 / cm 3 This reflects that the carriers of the InSb crystal in the middle part between the head and the tail of the InSb crystal rod are also lower than 2E14 / cm 3 , meeting the requirements of step S1 of Example 1.

[0119] Figure 5 This is a carrier concentration distribution diagram of the InSb wafer of Example 1 after annealing. Figure 6This is a signal response diagram of the InSb detector after the annealed InSb wafer in Example 1 is used to make an InSb infrared focal plane detector. Fig.10 This is a carrier concentration distribution diagram of the InSb wafer made from the InSb crystal rod grown by the Czochralski method in Example 4. Fig.11 This is a signal response diagram of the InSb detector after the InSb infrared focal plane detector is manufactured from the InSb wafer of comparative example 4. The signal response diagram of the InSb detector is a level diagram of the Dewar test of the manufactured InSb infrared focal plane detector.

[0120] from Figure 5 and Fig.10 By comparison, Fig.10 The carrier concentration distribution of Comparative Example 4 is obviously unevenly distributed with a small upper portion and a large lower portion. Figure 5 The carrier concentration distribution of Example 1 is uniform. The carrier concentration non-uniformity is defined as (maximum value - minimum value) / average value. Fig.10 The carrier concentration non-uniformity of Comparative Example 4 is 73.82%. Figure 5 The carrier concentration non-uniformity of Example 1 is 4.46%. That is, compared with Comparative Example 4, Example 1 achieves the purpose of uniform doping, that is, improves the doping uniformity of the indium antimonide wafer.

[0121] from Figure 6 and Fig.11 By comparison, Fig.11 The InSb wafer of Comparative Example 4 has arc-shaped stripes in the InSb detector signal response diagram after the InSb infrared focal plane detector is manufactured. Figure 6 There are no stripes in the InSb detector signal response diagram after the InSb infrared focal plane detector is manufactured from the annealed InSb wafer of Example 1, that is, Example 1 ensures the use effect of the InSb detector manufactured from the indium antimonide wafer.

[0122] Figure 7 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 1 after annealing. Figure 7 The tellurium tetrachloride content of Comparative Example 1 is too high, and the minimum value of the distributed carrier concentration is 2.10E15 / cm 3 , which is greater than the required 1.4E15 / cm 3 ,also, Figure 7 The carrier concentration non-uniformity of Comparative Example 1 is 14.41%. Therefore, the annealed InSb wafer of Comparative Example 1 cannot be used for making InSb detectors.

[0123] Figure 8 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 2 after annealing. Figure 8The annealing temperature of Comparative Example 2 is too high, and the minimum value of the distributed carrier concentration is 1.75E15 / cm 3 , which is greater than the required 1.4E15 / cm 3 ,also, Figure 8 The carrier concentration non-uniformity of Comparative Example 2 is 12.45%. Therefore, the annealed InSb wafer of Comparative Example 2 cannot be used for making InSb detectors.

[0124] Fig. 9 This is a carrier concentration distribution diagram of the InSb wafer of comparative example 3 after annealing. Fig. 9 The annealing time of comparative example 3 is too long, and the minimum value of the distributed carrier concentration is 1.46E15 / cm 3 , which is greater than the required 1.4E15 / cm 3 ,also, Fig. 9 The carrier concentration non-uniformity of Comparative Example 3 is 11.58%. Therefore, the annealed InSb wafer of Comparative Example 3 cannot be used for making InSb detectors.

[0125] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.

Claims

1. A method for annealing an indium antimonide wafer, characterized in that: Includes steps: S1, undoped Te grown by Czochralski method with a carrier concentration of 2E14 / cm 3 The following InSb crystals; S2, slicing the InSb crystal into InSb wafers; S3, grinding and polishing the InSb wafer; S4, adding a mixed solution of ethanol and tellurium tetrachloride into the flask through a ground mouth of the flask, wherein the mass fraction of tellurium tetrachloride in the mixed solution is 1-5%, and another ground mouth of the flask is used to install a condensation device; S5, placing the ground and polished InSb wafer into the mixed solution in the flask through one of the ground openings and completely immersing the wafer in the mixed solution; S6, installing the condensation device on the corresponding ground mouth of the flask, and sealing the other ground mouth of the flask; S7, raising the temperature of the mixed solution in the flask to 60-70°C, and annealing for 10-20 hours by condensation to complete annealing.

2. The annealing method of indium antimonide wafer according to claim 1, characterized in that: In step S1, the Czochralski method adopts the following sub-steps: S11, crushing the 7.5NInSb polycrystalline material purified by zone melting, cleaning it with aqua regia, rinsing it with deionized water for more than 3 times, and drying it in a vacuum oven for later use; S12, loading the dried InSb polycrystalline material into the quartz crucible; S13, evacuating, degassing, and leak checking the CZC crystal growth device to achieve a vacuum in the CZC crystal growth device, wherein the vacuum pressure is below 10Pa, evacuating and degassing the CZC crystal growth device and filling nitrogen into the CZC crystal growth device are performed alternately 2-3 times by using a vacuum pump, wherein a vacuum evacuation interface is provided at the bottom of the CZC crystal growth device, and nitrogen is used for degassing, and a nitrogen filling gas inlet is provided at the top of the CZC crystal growth device; S14, after sub-step S13 is completed, the top cover and the middle tube are locked by corresponding screws, and the middle tube and the base are locked by corresponding screws, and then the vacuum port and the gas inlet are closed; S15, opening the gas inlet again, filling the CZC crystal growth apparatus with a nitrogen-hydrogen mixed gas so that the pressure in the CZC crystal growth apparatus reaches 0.1 MPa, and then closing the gas inlet; S16, start heating the quartz crucible to heat up and melt the InSb polycrystalline material in the quartz crucible. The heater includes a graphite heater, a graphite double-layer insulation cover and carbon felt. The graphite heater is arranged around the crucible, the graphite double-layer insulation cover is arranged around the graphite heater, and the carbon felt is filled between the inner layer and the outer layer of the graphite double-layer insulation cover. The heater for heating the quartz crucible is the only heating device in the Czochralski crystal growth equipment. S17, when the InSb polycrystalline material is completely melted to form a melt, the pressure in the Czochralski crystal growth device rises to 0.15 MPa, and the temperature of the quartz crucible is maintained unchanged, wherein the formation of the melt is confirmed by observation through an observation window; S18, after sub-step S17, the pulling rod drives the seed crystal to move downward into the quartz crucible and immerse into the melt from the surface, and then the pulling rod pulls the crystal upward to grow the crystal to form a crystal rod. During the crystal growth process, the quartz crucible and the pulling rod maintain opposite rotation speeds, the rotation speed of the crucible is 1 rpm, the rotation speed of the pulling rod is 3 rpm, the seed crystal is an indium antimonide single crystal with a purity of 7.5N, and the pulling speed is constant at 5 mm / h; S19, after the crystal growth is completed, stop heating, cool down, replace the gas in the Czochralski crystal growth equipment with nitrogen through the vacuum pump through the vacuum interface and the gas inlet, open the Czochralski crystal growth equipment, and cut the crystal rod from the pulling rod.

3. The annealing method of indium antimonide wafer according to claim 1, characterized in that: In step S2, the InSb crystal is sliced ​​using diamond single wire sawing.

4. The annealing method of indium antimonide wafer according to claim 1, characterized in that: In step S3, a double-sided grinder is used for grinding and polishing.

5. The annealing method of indium antimonide wafer according to claim 4, characterized in that: In step S3, the grinding and polishing uses a polishing liquid prepared by mixing SiO2 sol at room temperature and pure water in a volume ratio of 1:1, and the grinding and polishing time is 30 seconds.

6. The annealing method of indium antimonide wafer according to claim 1, characterized in that: In step S7, the temperature is raised using a water bath.

Citation Information

Patent Citations

  • Low Te doped InSb wafer and preparation thereof

    CN116791210A