Antibacterial conductive non-woven fabric and preparation method and application thereof

Through the synergistic effect of modified graphene and quaternary ammonium salts and other components, the problems of poor conductivity and mechanical properties of antibacterial conductive non-woven fabrics are solved, and high efficiency, broad-spectrum antibacterial effect and excellent conductivity and mechanical properties are achieved, and the company has expanded the Its application scope.

CN118880607APending Publication Date: 2024-11-01JIANGSU GEM ADVANCED FIBER MATERIALS RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410966475.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The poor conductivity, poor mechanical properties and single functionality of existing antibacterial conductive nonwovens limit their application scope.

Method used

By covalently grafting the graphene oxide and the hydrophilic acrylic monomer, hydrophilic modified graphene is prepared and mixed with quaternary ammonium salt, dispersant, and water-soluble binder to form a modified slurry The fiber web was impregnated and dried and heat-shaped to prepare an antibacterial conductive non-woven fabric with excellent conductivity, antibacterial and mechanical properties.

Benefits of technology

It improves the conductivity and antibacterial properties of non-woven fabrics, enhances the conductivity and mechanical properties of the fiber network, and makes it suitable for medical bed sheets, surgical gowns and other fields. At the same time, the method is green, environmentally friendly, simple and easy to use, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880607A_ABST
    Figure CN118880607A_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial conductive non-woven fabric and a preparation method and application thereof, and belongs to the technical field of non-woven fabric materials. The preparation method provided by the invention comprises the following steps: performing covalent bond grafting modification on graphene oxide and a hydrophilic acrylic monomer, performing reduction through a reducing agent to obtain hydrophilic modified graphene, mixing the hydrophilic modified graphene, quaternary ammonium salt, a dispersing agent, a water-soluble adhesive and deionized water to obtain modified slurry, and performing spray drying on the modified slurry. The antibacterial conductive non-woven fabric is obtained by modifying a fiber web with the modified fiber web, taking out, drying and performing heat setting, and the non-woven fabric can be endowed with excellent high-efficiency and broad-spectrum antibacterial property, mechanical property and conductive property; meanwhile, the preparation method is green, environment-friendly, simple and easy to implement, suitable for industrial production, good in economic benefit and widely applied to preparation of medical bed sheets, surgical gowns, isolation gowns and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of non-woven fabric materials, and in particular relates to an antibacterial conductive non-woven fabric and a preparation method and application thereof. Background Art

[0002] Nonwoven fabrics, also known as non-woven fabrics, are made of directional or random fibers. They are a new generation of environmentally friendly materials with the advantages of being breathable, flexible, lightweight, easy to decompose, colorful, low-priced, and recyclable. They are widely used in smart wearables, artificial intelligence, aerospace, and other fields. At present, various functional materials are usually introduced into nonwoven fabrics to prepare functional nonwoven fabrics. However, due to the uneven dispersion of various functional materials, they are easy to stack, resulting in poor corresponding functionality. Therefore, it is necessary to develop nonwoven fabrics with excellent comprehensive performance to expand the scope of application.

[0003] The prior art with application publication number CN 114149576 A discloses a process for preparing a non-woven fabric with excellent conductive properties, wherein both sides of a non-woven fabric base fabric are modified by a mixed solution of carbon fiber powder and pure acrylic foam binder, and then dried and rolled to form a non-woven fabric with excellent conductive properties.

[0004] However, the above-mentioned conductive non-woven fabric has the following problems: first, the carbon fiber powder is unevenly dispersed in the mixed solution and is easy to stack, resulting in poor conductivity; second, the surface of the non-woven fabric is treated with a mixed solution, which makes the fabric brittle and has poor mechanical properties; third, the obtained non-woven fabric has a single functionality, which limits its application. Summary of the invention

[0005] The present application discloses an antibacterial conductive nonwoven fabric and a preparation method and application thereof, aiming to solve the technical problems of poor conductivity, poor mechanical properties and single functionality limiting application existing in the preparation technology of the existing antibacterial conductive nonwoven fabric.

[0006] In order to achieve the above purpose, the technical solution of this application is:

[0007] The first aspect of the present application provides a method for preparing an antibacterial conductive non-woven fabric, the method comprising:

[0008] After adding graphene oxide to an organic solvent and ultrasonically dispersing it, adding ammonium persulfate and a hydrophilic acrylic monomer, reacting at a temperature of 50-80° C. to obtain a reaction system, adding a reducing agent to the reaction system, reducing it at a temperature of 80-100° C., separating and collecting, and obtaining hydrophilic modified graphene;

[0009] The hydrophilic modified graphene, the quaternary ammonium salt, the dispersant, the water-soluble binder and the deionized water are mixed to obtain a modified slurry;

[0010] The fiber web is immersed in the modified slurry, taken out, dried, and heat-set to obtain an antibacterial conductive non-woven fabric.

[0011] In combination with the first aspect, preferably, the organic solvent is one or more of N,N-dimethylformamide, dimethyl sulfoxide, dimethylformamide, and ethanol;

[0012] And / or, the ratio of graphene oxide to organic solvent is 0.1-1 g: 200 ml.

[0013] In combination with the first aspect, preferably, the hydrophilic acrylic monomer is one or more of acrylic acid, acrylic ester, hydroxyethyl methacrylate, methyl methacrylate, and hydroxyethyl acrylate.

[0014] In combination with the first aspect, preferably, the reducing agent is one or more of vitamin C, chitosan and glucose.

[0015] In combination with the first aspect, preferably, the dispersant is one of polyvinylpyrrolidone, polyethylene glycol, and sodium polyacrylate;

[0016] And / or, the quaternary ammonium salt is one or more of benzalkonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, and glycidyl dodecyl quaternary ammonium salt.

[0017] In combination with the first aspect, preferably, the water-soluble adhesive is one or more of polyacrylate, sodium carboxymethyl cellulose, and tamarind gum;

[0018] And / or, 8-10 parts of the hydrophilic modified graphene, 0.5-1 parts of the quaternary ammonium salt, 0.5-1 parts of the dispersant, 8-10 parts of the water-soluble adhesive, and 60-80 parts of deionized water;

[0019] And / or, the modified slurry has a viscosity of 1000-2000 mPa.s.

[0020] In combination with the first aspect, preferably, the fiber web is made of one or more of viscose fiber, polylactic acid fiber, and polyester fiber with a length of 38-51 mm;

[0021] And / or, the fiber web has a grammage of 30-40 g / m 2 .

[0022] In combination with the first aspect, preferably, the fiber web is immersed in the modified slurry for reaction, and after being taken out, it is dried and heat-oriented. The drying temperature is 120-170°C and the drying time is 1-3 minutes; the heat setting temperature is 120-150°C and the setting time is 1 minute.

[0023] The second aspect of the present application provides an antibacterial conductive non-woven fabric made by the preparation method described in the first aspect.

[0024] The third aspect of the present application provides the use of the antibacterial conductive non-woven fabric described in the second aspect in the preparation of medical bed sheets, surgical gowns, isolation gowns, etc.

[0025] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:

[0026] The preparation method provided by the present application comprises the following steps: covalently grafting graphene oxide with a hydrophilic acrylic monomer, reducing the graphene to obtain a hydrophilic modified graphene, mixing the graphene oxide with a quaternary ammonium salt, a dispersant, and a water-soluble adhesive to prepare a modified slurry, and modifying the fiber web with the modified slurry to prepare an antibacterial conductive non-woven fabric. On the one hand, the hydrophilic modified graphene greatly improves the dispersion performance in the aqueous phase, and the addition of a dispersant can greatly improve the uniform and stable dispersion of the modified slurry, so that the prepared non-woven fabric has excellent conductivity and antistatic effect; on the other hand, the quaternary ammonium The synergistic antibacterial effects of salt and hydrophilic modified graphene with physical and chemical sterilization can give the non-woven fabric excellent antibacterial properties and achieve high-efficiency and broad-spectrum antibacterial effects; thirdly, the modified pulp can be dispersed vertically and horizontally in the entire fiber network and firmly combined with the fibers, thereby achieving high conductivity of the fiber network, further giving the non-woven fabric excellent conductivity, and at the same time enabling the fiber network to form a non-woven fabric with excellent mechanical properties and soft feel; at the same time, the preparation method provided in the present application is green and environmentally friendly, simple and easy to operate, suitable for industrial production, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 This is a physical picture of the A1-antibacterial conductive non-woven fabric prepared in the example of the present application. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0030] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0031] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0032] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0033] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0034] It should be noted that all raw materials and reagents in the examples of the present application are purchased on the market or prepared according to conventional methods well known to those skilled in the art. For example, N,N-dimethylformamide, dimethyl sulfoxide, dimethylformamide, ethanol, vitamin C, graphene oxide, polyvinylpyrrolidone, polyethylene glycol, sodium polyacrylate, etc. are all purchased on the market or prepared according to conventional methods well known to those skilled in the art.

[0035] In a first aspect, an embodiment of the present application provides a method for preparing an antibacterial conductive non-woven fabric, the method comprising:

[0036] After adding graphene oxide to an organic solvent and ultrasonically dispersing it, adding ammonium persulfate and a hydrophilic acrylic monomer, reacting at a temperature of 50-80° C. to obtain a reaction system, adding a reducing agent to the reaction system, reducing it at a temperature of 80-100° C., separating and collecting, and obtaining hydrophilic modified graphene;

[0037] The hydrophilic modified graphene, the quaternary ammonium salt, the dispersant, the water-soluble binder and the deionized water are mixed to obtain a modified slurry;

[0038] The fiber web is immersed in the modified slurry, taken out, dried, and heat-set to obtain an antibacterial conductive non-woven fabric.

[0039] Among them, on the one hand, the hydrophilic modified graphene greatly improves the dispersion performance in the aqueous phase. At the same time, the addition of a dispersant can greatly improve the uniform and stable dispersion of the modified slurry, so that the prepared non-woven fabric has excellent conductivity and antistatic effect; on the other hand, through the synergistic antibacterial effect of quaternary ammonium salt and hydrophilic modified graphene with physical sterilization and chemical sterilization, the non-woven fabric can be given excellent antibacterial properties, achieving high-efficiency and broad-spectrum antibacterial effects; thirdly, the modified slurry can be dispersed vertically and horizontally in the entire fiber network, firmly combined with the fibers, thereby achieving high conductivity of the fiber network, further giving the non-woven fabric excellent conductivity, and at the same time, the fiber network can be formed into a non-woven fabric with excellent mechanical properties and soft feel; at the same time, the preparation method provided by the present application is green and environmentally friendly, simple and easy to operate, suitable for industrial production, and has good economic benefits.

[0040] It should be noted that graphene oxide contains a large number of oxygen-containing groups (-OH, C=O, C=O and other oxygen-containing groups) on the surface of the carbon atom layered skeleton. -OH and C=O are distributed at the edges of graphene oxide sheets, and C=O and other oxygen-containing groups are distributed between graphene oxide sheets. The presence of these functional groups increases the distance between graphene oxide sheets, allowing the solvent to better enter the sheets, improving the dispersibility of graphene oxide. At the same time, hydrophilic modified graphene can optimize the antistatic properties of non-woven fabrics on the one hand, and has strong antibacterial properties on the other.

[0041] In the embodiment of the present application, the organic solvent is preferably one or more of N,N-dimethylformamide, dimethyl sulfoxide, dimethylformamide, and ethanol; the ratio of graphene oxide to organic solvent is preferably 0.1-1g:200ml. Among them, because graphene oxide has a special large π bond conjugated electronic structure, there is a large van der Waals force between its layers, and its sheets are very easy to re-aggregate and stack. These polar organic solvents can disperse graphene oxide and form a uniform and stable solution.

[0042] In the embodiment of the present application, the hydrophilic acrylic monomer is preferably one or more of acrylic acid, acrylic acid ester, hydroxyethyl methacrylate, methyl methacrylate, and hydroxyethyl acrylate; the reaction temperature is preferably 50-80°C, for example, 50°C, 60°C, 65°C, 70°C, 80°C, or any temperature within the range. The hydrophilic acrylic monomer is covalently grafted with graphene by ultrasonically dispersing graphene oxide and an organic solvent, using ammonium persulfate as an initiator, and reacting the functionalized groups in the acrylic monomer with the abundant oxygen-containing groups (carboxyl, hydroxyl, epoxy, etc.) on the surface of graphene oxide, and performing corresponding functionalization modification.

[0043] In the embodiment of the present application, the reducing agent is preferably one or more of vitamin C, chitosan, and glucose. Among them, by adding the dienol structure in the reducing agent to reduce the hydrophilic acrylic modified graphene, the functional groups in the graphene are reduced, which not only improves the electronic properties of graphene oxide, but also realizes the dispersion uniformity and stability of graphene in the aqueous phase, thereby improving the compatibility with the modified slurry. At the same time, these reducing agents are safe, green, environmentally friendly, and suitable for large-scale production.

[0044] In the embodiment of the present application, the dispersant is preferably one of polyvinylpyrrolidone, polyethylene glycol, and sodium polyacrylate; the quaternary ammonium salt is preferably one or more of benzalkonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, and epoxypropyl dodecyl quaternary ammonium salt. Among them, by selecting these dispersants, the modified hydrophilic modified graphene, the quaternary ammonium salt and the water-soluble adhesive can be dispersed in the modified slurry; by selecting these quaternary ammonium salts, the hydrophilic modified graphene can play a synergistic antibacterial role, greatly improving the antibacterial properties of the non-woven fabric, and achieving a high-efficiency and broad-spectrum antibacterial effect.

[0045] In the embodiment of the present application, the water-soluble adhesive is preferably one or more of polyacrylate, sodium carboxymethyl cellulose, and tamarind gum; the hydrophilic modified graphene is 8-10 parts, the quaternary ammonium salt is 0.5-1 parts, the dispersant is 0.5-1 parts, the water-soluble adhesive is 8-10 parts, and the deionized water is 60-80 parts; the viscosity of the modified slurry is preferably 1000-2000mPa.s. Among them, by selecting these water-soluble adhesives, the modified slurry can be safely and stably adhered to the fiber net, which is suitable for industrial production; by controlling the content of each component of the modified slurry, the viscosity of the modified slurry can be controlled, and the modified slurry can be penetrated into the interior of the fiber net, which can make the adhesion and bonding between fibers better, thereby improving the comprehensive performance of the prepared non-woven fabric.

[0046] In the embodiment of the present application, the fiber mesh is preferably made of one or more of viscose fiber, polylactic acid fiber, and polyester fiber with a length of 38-51 mm; the weight of the fiber mesh is preferably 30-40 g / m2 , for example 30g / m 2 , 35g / m 2 , 40g / m 2 Among them, by using these short fibers with a length of 38-51 mm, opening, mixing and combing to form a three-dimensional randomly arranged fiber web, and by controlling the gram weight of the fiber web, the slurry can be evenly and stably dispersed inside the fiber web, thereby giving the non-woven fabric excellent conductivity, antibacterial and mechanical properties.

[0047] In the embodiment of the present application, the fiber web is immersed in the modified slurry, and after being taken out and dried and heat-set, the drying temperature is preferably 120-170°C, for example, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or any temperature in the range; the drying time is preferably 1-3min, for example, 1min, 2min, 3min or any time in the range; the heat-setting temperature is preferably 120-150°C, for example, 120°C, 130°C, 140°C, 150°C or any temperature in the range; the setting time is preferably 1min. Among them, by controlling the drying temperature and time of the fiber web in the modified slurry, the temperature and time of heat setting, the modified slurry can be uniformly and stably fixed to the inside of the fiber web, so that the prepared non-woven fabric has stable performance and forms a non-woven fabric with excellent appearance quality.

[0048] It should be noted that when the fiber web is immersed in the modified slurry for reaction, the amount of the modified slurry applied to the fiber web is represented by the fiber web liquid carrying rate (the fiber web liquid carrying rate is a characterization of the amount of liquid carried by the fiber web after squeezing, and the calculation formula is:

[0049] Liquid carrying rate = (weight of fiber web after squeezing - weight of fiber web before squeezing) / weight of fiber web before squeezing * 100%. The liquid carrying rate of fiber web is 200%-300%, which is controlled by the pressure of the roller or the magnetic force of the magnetic rod.

[0050] In the second aspect, the present application provides an antibacterial conductive nonwoven fabric prepared by the preparation method described in the first aspect. Based on the above preparation method, the prepared antibacterial conductive nonwoven fabric has excellent antibacterial properties, electrical conductivity, antistatic effect, soft skin-friendly properties and mechanical properties, with a longitudinal breaking strength of 67-103N, a transverse breaking strength of 8-29N, and a maximum electrical resistance of 6.26×10 5 Ω / cm, it has a highly efficient and stable antibacterial effect on Escherichia coli, Staphylococcus aureus and Candida albicans, with an inhibition rate of ≥93.2%.

[0051] In the third aspect, the embodiment of the present application provides the use of the antibacterial conductive non-woven fabric described in the second aspect in the preparation of medical bed sheets, surgical gowns, isolation gowns, etc. Among them, based on the above antibacterial conductive non-woven fabric has excellent antibacterial properties, conductivity, antistatic effect, soft skin-friendly and mechanical properties, so that it has excellent product competitiveness in the preparation of medical bed sheets, surgical gowns, isolation gowns.

[0052] The technical solution of the present application will be further described below in conjunction with specific embodiments.

[0053] Example 1

[0054] This embodiment provides a method for preparing an A1-antibacterial conductive nonwoven fabric, which specifically includes:

[0055] S101: 10 g of graphene oxide and 20 L of N,N-dimethylformamide were added to a reactor, and dispersed evenly under ultrasonic action at a pressure of 5 MPa and a power of 30 W for 4 hours, and then 1% by mass of ammonium persulfate and 3% by mass of acrylic acid were added, and the reaction was carried out at a constant temperature of 65° C. for 5 hours, and a reaction system of hydrophilic graphene oxide was obtained through covalent bond grafting modification; 2 g of vitamin C was added to the reaction system of hydrophilic graphene oxide at 95° C., and the reaction was reduced at a constant temperature for 2.5 hours to obtain hydrophilic modified graphene;

[0056] S102: 10 g of hydrophilic modified graphene, 1 g of benzalkonium chloride, 1 g of polyvinylpyrrolidone, 10 g of polyacrylate and 78 g of deionized water were mixed to obtain a modified slurry (the slurry viscosity was 2000 mPa.s);

[0057] S103: 50% viscose fiber + 50% polylactic acid fiber is carded into a fiber web, the fiber web weight is 30g / m 2 The fiber web is subjected to a two-immersion and two-pressing process, and after being taken out, it is dried and heat-set to obtain the A1-antibacterial conductive non-woven fabric.

[0058] In order to verify the morphology and structure of the antibacterial conductive nonwoven fabric prepared in the embodiment of the present application, Figure 1 This is a physical picture of the A1-antibacterial conductive non-woven fabric prepared in Example 1 of the present application. It can be seen from the figure that the modified slurry is evenly and stably distributed on the non-woven fabric, thereby giving the non-woven fabric excellent antibacterial properties, conductive properties and mechanical properties.

[0059] Example 2

[0060] The component ratio, preparation operation and process parameters of the A2-antibacterial conductive non-woven fabric prepared in the embodiment of the present application are basically the same as those in Example 1, the difference being that in this embodiment, the fiber web is subjected to a dipping and pressing process to obtain the A2-antibacterial conductive non-woven fabric.

[0061] Example 3

[0062] The present application embodiment provides a method for preparing A3-antibacterial conductive non-woven fabric, which specifically includes:

[0063] S301: 10g of graphene oxide and 2L of N,N-dimethylformamide are added to a reactor, and dispersed uniformly under ultrasonic action at a pressure of 5MPa and a power of 30W for 4 hours, and then 1% by mass of ammonium persulfate and 3% by mass of acrylic acid are added, and the reaction is carried out at a constant temperature of 65°C for 5 hours, and a reaction system of hydrophilic graphene oxide is obtained by covalent bond grafting modification; 2g of vitamin C is added to the reaction system of hydrophilic graphene oxide at 95°C, and the reaction is reduced at a constant temperature for 2.5 hours to obtain hydrophilic modified graphene;

[0064] S302: 8 g of hydrophilic modified graphene, 0.5 g of benzalkonium chloride, 0.5 g of polyvinylpyrrolidone, 8 g of tamarind gum and 80 g of deionized water were mixed to obtain a modified slurry (slurry viscosity was 1000 mPa.s);

[0065] S303: 20% viscose fiber + 80% polyester fiber is carded into a fiber web with a weight of 40g / m 2 The fiber web was screen printed by a rotary screen printing process, taken out, dried, and heat-set to obtain an A3-antibacterial conductive nonwoven fabric.

[0066] Example 4

[0067] The component ratio, preparation operation and process parameters of the A4-antibacterial conductive non-woven fabric prepared in the embodiment of the present application are basically the same as those in Example 3, except that in this embodiment, the A4-antibacterial conductive non-woven fabric is obtained by flat screen printing of the fiber web using a screen printing method.

[0068] Example 5

[0069] This embodiment provides a method for preparing A5-antibacterial conductive non-woven fabric, which specifically includes:

[0070] S501: 10g of graphene oxide and 20L of N,N-dimethylformamide are added to a reactor, and dispersed uniformly under ultrasonic action at a pressure of 5MPa and a power of 30W for 4h, and then 1% by mass of ammonium persulfate and 3% by mass of acrylic acid are added, and the reaction is carried out at a constant temperature of 65°C for 5h, and the reaction system of hydrophilic graphene oxide is obtained by covalent bond grafting modification; 2g of vitamin C is added to the reaction system of hydrophilic graphene oxide at 95°C, and the reaction is carried out at a constant temperature of 2.5h to obtain hydrophilic modified graphene;

[0071] S502: 9 g of hydrophilic modified graphene, 0.8 g of benzalkonium chloride, 0.5 g of polyvinylpyrrolidone, 8 g of sodium carboxymethyl cellulose and 80 g of deionized water are mixed to obtain a modified slurry (slurry viscosity is 1500 mPa.s);

[0072] S503: 100% viscose fiber is carded into a fiber web with a weight of 35g / m 2 The fiber web was screen printed by a rotary screen printing process, taken out, dried, and heat-set to obtain an A5-antibacterial conductive non-woven fabric.

[0073] Example 6

[0074] The component ratio, preparation operation and process parameters of the A6-antibacterial conductive non-woven fabric prepared in the embodiment of the present application are basically the same as those in Example 4, the difference being that in this embodiment, the A6-antibacterial conductive non-woven fabric is obtained by using a screen printing method and a flat screen printing process on the fiber web.

[0075] At the same time, in order to verify the comprehensive performance of the antibacterial conductive non-woven fabric prepared in the above embodiments, the present application provides the following comparative examples for detailed description.

[0076] Comparative Example 1

[0077] This comparative example provides a method for preparing B1-nonwoven fabric, which specifically includes:

[0078] S701: 10 g of graphene oxide, 1 g of benzalkonium chloride, 1 g of polyvinylpyrrolidone, 10 g of polyacrylate and 78 g of deionized water are mixed to obtain a modified slurry;

[0079] S702: 50% viscose fiber + 50% polylactic acid fiber is carded into a fiber web, the fiber web weight is 30g / m 2 The fiber web is subjected to a two-immersion and two-pressing process, and after being taken out, it is dried and heat-set to obtain a B1-nonwoven fabric.

[0080] Comparative Example 2

[0081] This comparative example provides a method for preparing a B2-nonwoven fabric, which specifically includes:

[0082] S801: 10g of graphene oxide and 20L of N,N-dimethylformamide were added to a reactor, and dispersed evenly under ultrasonic action at a pressure of 5MPa and a power of 30W for 4h, and then 1% by mass of ammonium persulfate and 3% by mass of acrylic acid were added, and the reaction was carried out at a constant temperature of 65°C for 5h, and the reaction system of hydrophilic graphene oxide was obtained through covalent bond grafting modification; 2g of vitamin C was added to the reaction system of hydrophilic graphene oxide at 95°C, and the reaction was carried out at a constant temperature of 2.5h to obtain hydrophilic modified graphene;

[0083] S802: 10 g of hydrophilic modified graphene, 1 g of polyvinylpyrrolidone, 10 g of polyacrylate and 78 g of deionized water are mixed to obtain a modified slurry;

[0084] S803: 50% viscose fiber + 50% polylactic acid fiber is carded into a fiber web with a weight of 30g / m 2 The fiber web is subjected to a two-immersion and two-pressing process, and after being taken out, it is dried and heat-set to obtain a B2-nonwoven fabric.

[0085] Comparative Example 3

[0086] This comparative example provides a method for preparing a B3-nonwoven fabric, which specifically includes:

[0087] S901: 1 g of benzalkonium chloride, 1 g of polyvinylpyrrolidone, 10 g of polyacrylate and 78 g of deionized water are mixed to obtain a modified slurry;

[0088] S902: 50% viscose fiber + 50% polylactic acid fiber is carded into a fiber web with a weight of 30g / m 2 The fiber web is subjected to a two-immersion and two-pressing process, and after being taken out, it is dried and heat-set to obtain a B3-nonwoven fabric.

[0089] The samples 1-6 prepared in the examples of the present application and the comparative examples 1-3 were tested for conductivity, mechanical properties, and antibacterial properties, and the test results are shown in Table 1 and Table 2:

[0090] Conductivity: The conductivity of the antibacterial conductive non-woven fabric was tested using a JK 2516 DC resistance tester at a temperature of 20°C and a relative humidity of 65%, specific resistance, Ω / cm;

[0091] Mechanical properties: Referring to GB / T 24218.3-2010 "Test methods for textile nonwovens Part 3: Determination of breaking strength and elongation at break (strip method)", the longitudinal and transverse breaking strength of the antibacterial conductive nonwoven fabric was tested using the Mesdan.SpA2516 electronic fabric strength tester;

[0092] Antibacterial property: refer to GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method".

[0093] Table 1 Test results of conductivity and antibacterial properties of samples prepared in Examples and Comparative Examples

[0094]

[0095]

[0096] Table 2 Test results of mechanical properties of samples prepared in Examples and Comparative Examples

[0097]

[0098] According to Table 1 and Table 2, the difference between Comparative Example 1 of the present application and Example 1 is that the graphene oxide is not modified, so that the dispersibility of its modified slurry is poor, thereby reducing the conductivity and antibacterial properties of the non-woven fabric, the breaking strength is low, and the elongation at break is reduced; the difference between Comparative Example 2 of the present application and Example 1 is that no quaternary ammonium salt is added, so that the antibacterial property of the prepared B2- non-woven fabric is poor, and the breaking strength and elongation at break of the non-woven fabric are basically unaffected; the difference between Comparative Example 3 of the present application and Example 1 is that no graphene oxide is added, there is no conductive material in the modified slurry, the conductivity and antibacterial properties of the non-woven fabric are poor, and because no graphene oxide is added, the bonding force between the adhesive and the fiber web is strong, and the breaking strength and elongation at break of the non-woven fabric are relatively high. Therefore, the preparation method provided in the present application modifies the graphene oxide, mixes it with a quaternary ammonium salt, a dispersant, a water-soluble adhesive and deionized water to form a modified slurry, modifies the fiber web, takes it out, and then dries and heat-orients it to obtain an antibacterial conductive non-woven fabric, which can greatly improve the conductivity, antibacterial properties and mechanical properties of the non-woven fabric, and has broad application prospects.

[0099] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0100] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions recorded in the aforementioned embodiments may still be modified, or some or all of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the present application.

Claims

1. A method for preparing an antibacterial conductive nonwoven fabric, characterized in that: The method comprises: After adding graphene oxide to an organic solvent and ultrasonically dispersing it, adding ammonium persulfate and a hydrophilic acrylic monomer, reacting at a temperature of 50-80° C. to obtain a reaction system, adding a reducing agent to the reaction system, reducing it at a temperature of 80-100° C., separating and collecting, and obtaining hydrophilic modified graphene; The hydrophilic modified graphene, the quaternary ammonium salt, the dispersant, the water-soluble binder and the deionized water are mixed to obtain a modified slurry; The fiber web is immersed in the modified slurry, taken out, dried, and heat-set to obtain an antibacterial conductive non-woven fabric.

2. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The organic solvent is one or more of N,N-dimethylformamide, dimethyl sulfoxide, dimethylformamide, and ethanol; And / or, the ratio of graphene oxide to organic solvent is 0.1-1 g: 200 ml.

3. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The hydrophilic acrylic monomer is one or more of acrylic acid, acrylic ester, hydroxyethyl methacrylate, methyl methacrylate, and hydroxyethyl acrylate.

4. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The reducing agent is one or more of vitamin C, chitosan and glucose.

5. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The dispersant is one of polyvinylpyrrolidone, polyethylene glycol, and sodium polyacrylate; And / or, the quaternary ammonium salt is one or more of benzalkonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, and glycidyl dodecyl quaternary ammonium salt.

6. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The water-soluble adhesive is one or more of polyacrylate, sodium carboxymethyl cellulose, and tamarind gum; And / or, 8-10 parts of the hydrophilic modified graphene, 0.5-1 parts of the quaternary ammonium salt, 0.5-1 parts of the dispersant, 8-10 parts of the water-soluble adhesive, and 60-80 parts of deionized water; And / or, the modified slurry has a viscosity of 1000-2000 mPa.s.

7. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The fiber web is made of one or more of viscose fiber, polylactic acid fiber, and polyester fiber with a length of 38-51 mm; And / or, the fiber web has a grammage of 30-40 g / m 2 .

8. The method for preparing the antibacterial conductive nonwoven fabric according to claim 1, characterized in that: The fiber web is immersed in the modified slurry for reaction, and then taken out and dried and heat-oriented. The drying temperature is 120-170°C and the drying time is 1-3 minutes; the heat-setting temperature is 120-150°C and the setting time is 1 minute.

9. An antibacterial conductive nonwoven fabric made according to any one of the preparation methods of claims 1-8.

10. Use of the antibacterial conductive non-woven fabric according to claim 9 in the preparation of medical bed sheets, surgical gowns, isolation gowns, etc.

Citation Information

Cited By

  • Antistatic epoxy resin composite coating and preparation method thereof

    CN119371875A