Stain-resistant decorative paper and preparation method thereof
By coating the surface of decorative paper with a stain-resistant coating composed of modified acrylic resin and other materials, a hydrophobic and oleophobic layer is formed, which solves the problem of decorative paper being easily contaminated, improves its stain resistance and service life, and makes it suitable for industrial production.
Patent Information
- Application Number
- CN202411151427.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing decorative paper is easily contaminated by sweat, grease, dust and other stains during use, resulting in poor appearance and user experience, inconvenient cleaning and reduced lifespan.
A stain-resistant coating is applied to the surface of the impregnated paper. The coating consists of modified acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano silica, and nano zinc oxide, forming a hydrophobic and oleophobic layer. The paper is then cured by baking and ultraviolet light to form a stain-resistant decorative paper.
It improves the stain resistance, abrasion resistance, and scratch resistance of decorative paper, extends its service life, and has a simple preparation method that is suitable for industrial production.
Smart Images

Figure BDA0005003769010000111 
Figure BDA0005003769010000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of decorative paper, and in particular to a stain-resistant decorative paper and a preparation method thereof. Background Art
[0002] With the progress of society and the improvement of people's living standards, decorative paper has been widely used in the fields of interior decoration, furniture, building materials, etc. to improve the aesthetics of the environment and the durability of objects. However, during the use of existing decorative paper, stains such as sweat, grease, and dust often adhere to the surface of the decorative paper, which has an adverse effect on the appearance and use experience of the product, is inconvenient to clean, and has an adverse effect on the service life of the product. Therefore, its stain resistance and durability need to be further improved. Summary of the invention
[0003] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a stain-resistant decorative paper and a preparation method thereof, wherein the stain-resistant decorative paper has good stain resistance, wear resistance and scratch resistance, and a long service life; the preparation method thereof has a simple process, is easy to operate, has high production efficiency, and is conducive to industrial production.
[0004] The purpose of the present invention is achieved through the following technical scheme: a kind of stain-resistant decorative paper, comprising an impregnated paper and a stain-resistant coating coated on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by curing the stain-resistant coating after being applied to the impregnated paper; the stain-resistant coating comprises the following raw materials in parts by weight: 40-50 parts of modified acrylic resin, 15-20 parts of epoxy acrylic resin, 10-15 parts of ethoxylated trimethylolpropane triacrylate, 5-9 parts of nano silicon dioxide, 4-8 parts of nano zinc oxide, 3-5 parts of polyoxyethylene ether, 2-4 parts of film-forming aid, 2-4 parts of photoinitiator, 5-10 parts of ethyl acetate, and 20-30 parts of water.
[0005] The anti-fouling coating of the present invention uses modified acrylic acid and epoxy acrylic resin as the main body, and adds ethoxylated trimethylolpropane triacrylate to provide unsaturated double bonds. The modified acrylic acid, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate and raw materials such as nano-silicon dioxide, nano-zinc oxide, and polyoxyethylene ether are well matched, which can give the coating anti-fouling, wear resistance and thermal stability, thereby improving the durability and usage experience of decorative paper.
[0006] Furthermore, the preparation method of each modified acrylic resin comprises the following steps:
[0007] A1. Take 30-40 parts of methyl methacrylate, 6-10 parts of isooctyl acrylate, 5-9 parts of ethyl isocyanate acrylate and 0.5-1 parts of initiator by weight and mix them evenly to obtain a mixture A; take 25-35 parts of butyl acetate, heat it to 75-80°C, and add the mixture A dropwise to the butyl acetate under nitrogen protection for 2-3 hours, then keep it warm for 6-8 hours, add 0.5-1 parts of initiator every 120-150 minutes during the heat preservation period, and cool it to room temperature after the reaction is completed to obtain a mixture A;
[0008] A2. Add 4-7 parts of perfluorooctyl trimethoxysilane, 3-6 parts of hexamethylcyclotrisiloxane and 3-6 parts of perfluorooctanol to mixture A, add a catalyst at a temperature of 75-85° C., and when the content of isocyanate in the reaction system reaches more than 98% of the theoretical value, add 3-6 parts of 1-2 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0009] The present invention prepares an acrylate copolymer by adopting the above method, and simultaneously grafts perfluorooctyltrimethoxysilane, hexamethylcyclotrisiloxane, perfluorooctanol and hydroxyethyl methacrylate on the acrylate copolymer to prepare a fluorosilicone-modified acrylic resin, which can give the coating excellent hydrophobic and oleophobic properties and improve the coating's anti-fouling, wear resistance and resistance to cold and hot cycles.
[0010] Furthermore, in the step A1, the initiator is at least one of azobisisobutyronitrile and azobisisoheptanenitrile.
[0011] Furthermore, in step A2, the catalyst is at least one of stannous octoate and dibutyltin dilaurate.
[0012] Furthermore, the film-forming aid is at least one of ethylene glycol tert-butyl ether, dipropylene glycol methyl ether and dipropylene glycol butyl ether.
[0013] Furthermore, the particle size of the nano silicon dioxide and nano zinc oxide is 30-80 nm.
[0014] Furthermore, the photoinitiator is at least one of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.
[0015] Furthermore, the preparation method of the anti-fouling coating comprises the following steps:
[0016] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 65-70° C. and stirring continuously, and keeping the temperature for 20-40 minutes to obtain a mixture B;
[0017] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 30-60 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0018] The present invention also provides a method for preparing the above-mentioned stain-resistant decorative paper, comprising the following steps:
[0019] (1) applying a stain-resistant coating to the surface of the impregnated paper;
[0020] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0021] Furthermore, in the step (2), the impregnated paper coated with the stain-resistant coating is baked at a temperature of 58-65° C. for 5-15 minutes, and then irradiated with ultraviolet light for 10-20 minutes to obtain the stain-resistant decorative paper.
[0022] The beneficial effects of the present invention are as follows: the stain-resistant decorative paper of the present invention forms a dense hydrophobic and oleophobic layer on the surface of the decorative paper by using a stain-resistant coating, so that the stain-resistant decorative paper has good stain resistance, wear resistance and scratch resistance, and a long service life; the preparation method is simple in process, easy to control, and has high production efficiency, which is conducive to industrial production. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of those skilled in the art, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In some embodiments of the present invention, a stain-resistant decorative paper comprises an impregnated paper and a stain-resistant coating coated on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by curing the stain-resistant coating after being applied to the impregnated paper; the stain-resistant coating comprises the following raw materials in parts by weight: 40-50 parts of modified acrylic resin, 15-20 parts of epoxy acrylic resin, 10-15 parts of ethoxylated trimethylolpropane triacrylate, 5-9 parts of nano silicon dioxide, 4-8 parts of nano zinc oxide, 3-5 parts of polyoxyethylene ether, 2-4 parts of film-forming aid, 2-4 parts of photoinitiator, 5-10 parts of ethyl acetate, and 20-30 parts of water. The epoxy acrylic resin is bisphenol A epoxy acrylic resin AgiSyn 1030.
[0025] In some embodiments of the present invention, the preparation method of each modified acrylic resin comprises the following steps:
[0026] A1. Take 30-40 parts of methyl methacrylate, 6-10 parts of isooctyl acrylate, 5-9 parts of ethyl isocyanate acrylate and 0.5-1 parts of initiator by weight and mix them evenly to obtain a mixture A; take 25-35 parts of butyl acetate, heat it to 75-80°C, and add the mixture A dropwise to the butyl acetate under nitrogen protection for 2-3 hours, then keep it warm for 6-8 hours, add 0.5-1 parts of initiator every 120-150 minutes during the heat preservation period, and cool it to room temperature after the reaction is completed to obtain a mixture A;
[0027] A2. Add 4-7 parts of perfluorooctyl trimethoxysilane, 3-6 parts of hexamethylcyclotrisiloxane and 3-6 parts of perfluorooctanol to mixture A, add a catalyst at a temperature of 75-85° C., and when the content of isocyanate in the reaction system reaches more than 98% of the theoretical value, add 3-6 parts of hydroxyethyl methacrylate and 1-2 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0028] In some embodiments of the present invention, in step A1, the initiator is at least one of azobisisobutyronitrile and azobisisoheptanenitrile.
[0029] In some embodiments of the present invention, in step A2, the catalyst is at least one of stannous octoate and dibutyltin dilaurate.
[0030] In some embodiments of the present invention, the film-forming aid is at least one of ethylene glycol tert-butyl ether, dipropylene glycol methyl ether and dipropylene glycol butyl ether.
[0031] In some embodiments of the present invention, the particle size of the nano silicon dioxide and nano zinc oxide is 30-80 nm.
[0032] In some embodiments of the present invention, the photoinitiator is at least one of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.
[0033] In some embodiments of the present invention, the method for preparing the anti-fouling coating comprises the following steps:
[0034] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 65-70° C. and stirring continuously, and keeping the temperature for 20-40 minutes to obtain a mixture B;
[0035] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 30-60 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0036] In some embodiments of the present invention, the method for preparing the above-mentioned stain-resistant decorative paper comprises the following steps:
[0037] (1) Apply the anti-fouling coating to the surface of the impregnated paper, with a coating amount of 30-60g / m 2 ;
[0038] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0039] Furthermore, in the step (2), the impregnated paper coated with the stain-resistant coating is baked at a temperature of 58-65° C. for 5-15 minutes, and then irradiated with ultraviolet light for 10-20 minutes to obtain the stain-resistant decorative paper.
[0040] Example 1
[0041] In this embodiment, a stain-resistant decorative paper includes impregnated paper and a stain-resistant coating coated on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by curing the stain-resistant coating after being applied to the impregnated paper; the stain-resistant coating includes the following raw materials in parts by weight: 45 parts of modified acrylic resin, 18 parts of epoxy acrylic resin, 12 parts of ethoxylated trimethylolpropane triacrylate, 6 parts of nano silicon dioxide, 6 parts of nano zinc oxide, 4 parts of polyoxyethylene ether, 3 parts of film-forming aid, 3 parts of photoinitiator, 7 parts of ethyl acetate, and 25 parts of water. The epoxy acrylic resin adopts bisphenol A type epoxy acrylic resin AgiSyn 1030. The impregnated paper adopts the impregnated paper in the prior art, which is obtained by impregnating digital printing paper in the polyurethane impregnating glue in the prior art.
[0042] Furthermore, the preparation method of each modified acrylic resin comprises the following steps:
[0043] A1. By weight, 35 parts of methyl methacrylate, 8 parts of isooctyl acrylate, 7 parts of ethyl isocyanate acrylate and 0.7 parts of initiator were mixed evenly to obtain a mixture A; 30 parts of butyl acetate were taken, the temperature was raised to 78°C, and under nitrogen protection, the mixture A was added dropwise to the butyl acetate for 2.5 hours, and then kept warm for 7 hours. During the insulation period, 0.6 parts of initiator were added every 120 minutes. After the reaction was completed, the temperature was lowered to room temperature to obtain a mixture A;
[0044] A2. Add 6 parts of perfluorooctyl trimethoxysilane, 4 parts of hexamethylcyclotrisiloxane and 4 parts of perfluorooctanol to mixture A, add a catalyst at 80° C., and when the isocyanate content in the reaction system reaches more than 98% of the theoretical value, add 5 parts of hydroxyethyl methacrylate and 1.5 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0045] Furthermore, in the step A1, the initiator is azobisisobutyronitrile.
[0046] Furthermore, in step A2, the catalyst is composed of stannous octoate and dibutyltin dilaurate in a weight ratio of 1:1.
[0047] Furthermore, the film-forming aid is composed of ethylene glycol tert-butyl ether and dipropylene glycol methyl ether in a weight ratio of 2:1.
[0048] Furthermore, the particle size of the nano silicon dioxide and nano zinc oxide is 30-80 nm.
[0049] Furthermore, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone.
[0050] Furthermore, the preparation method of the anti-fouling coating comprises the following steps:
[0051] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 67° C. and stirring continuously, and keeping the temperature for 300 min to obtain mixture B;
[0052] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 40 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0053] The method for preparing the above-mentioned stain-resistant decorative paper comprises the following steps:
[0054] (1) Apply the anti-fouling coating to the surface of the impregnated paper at a coating amount of 50 g / m 2 ;
[0055] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0056] Furthermore, in step (2), the impregnated paper coated with the anti-fouling coating is baked at 60°C for 10 minutes, and then irradiated with ultraviolet light for 10 minutes, with an ultraviolet energy of 900 mJ / cm 2 Obtain stain-resistant decorative paper.
[0057] Example 2
[0058] In the present embodiment, a stain-resistant decorative paper includes an impregnated paper and a stain-resistant coating wrapped on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by applying the stain-resistant coating to the impregnated paper and then curing; the stain-resistant coating includes the following raw materials in parts by weight: 40 parts of modified acrylic resin, 15 parts of epoxy acrylic resin, 15 parts of ethoxylated trimethylolpropane triacrylate, 5 parts of nano-silicon dioxide, 4 parts of nano-zinc oxide, 3 parts of polyoxyethylene ether, 4 parts of film-forming aid, 2 parts of photoinitiator, 5 parts of ethyl acetate, and 20 parts of water.
[0059] Furthermore, the preparation method of each modified acrylic resin comprises the following steps:
[0060] A1. By weight, 40 parts of methyl methacrylate, 6 parts of isooctyl acrylate, 5 parts of ethyl isocyanate acrylate and 0.5 parts of initiator were mixed evenly to obtain a mixture A; 25 parts of butyl acetate were taken, the temperature was raised to 75°C, and under nitrogen protection, the mixture A was added dropwise to the butyl acetate for 2 hours, and then kept warm for 6 hours. During the insulation period, 0.5 parts of initiator were added every 120 minutes. After the reaction was completed, the temperature was lowered to room temperature to obtain a mixture A;
[0061] A2. Add 4 parts of perfluorooctyl trimethoxysilane, 3 parts of hexamethylcyclotrisiloxane and 3 parts of perfluorooctanol to mixture A, add a catalyst at 75° C., and when the isocyanate content in the reaction system reaches more than 98% of the theoretical value, add 3 parts of hydroxyethyl methacrylate and 1 part of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0062] Furthermore, in the step A1, the initiator is azobisisobutyronitrile.
[0063] Furthermore, in step A2, the catalyst is at least one of dibutyltin dilaurate.
[0064] Furthermore, the film-forming aid is composed of ethylene glycol tert-butyl ether and dipropylene glycol butyl ether in a weight ratio of 1:1.
[0065] Furthermore, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropane.
[0066] Furthermore, the preparation method of the anti-fouling coating comprises the following steps:
[0067] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 65° C. and stirring continuously, and keeping the temperature for 40 minutes to obtain a mixture B;
[0068] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 30 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0069] The method for preparing the above-mentioned stain-resistant decorative paper comprises the following steps:
[0070] (1) Apply the anti-fouling coating to the surface of the impregnated paper at a coating amount of 50 g / m 2 ;
[0071] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0072] Furthermore, in the step (2), the impregnated paper coated with the stain-resistant coating is placed at a temperature of 58° C. for 5-15 minutes and then irradiated with ultraviolet light for 20 minutes to obtain stain-resistant decorative paper.
[0073] The rest of the content of this embodiment is the same as that of Embodiment 1.
[0074] Example 3
[0075] In the present embodiment, a stain-resistant decorative paper includes an impregnated paper and a stain-resistant coating wrapped on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by applying the stain-resistant coating to the impregnated paper and then curing; the stain-resistant coating includes the following raw materials in parts by weight: 50 parts of modified acrylic resin, 20 parts of epoxy acrylic resin, 10-15 parts of ethoxylated trimethylolpropane triacrylate, 8 parts of nano-silicon dioxide, 6 parts of nano-zinc oxide, 3-5 parts of polyoxyethylene ether, 2-4 parts of film-forming aid, 2-4 parts of photoinitiator, 5-10 parts of ethyl acetate, and 20-30 parts of water.
[0076] Furthermore, the preparation method of each modified acrylic resin comprises the following steps:
[0077] A1. By weight, 40 parts of methyl methacrylate, 10 parts of isooctyl acrylate, 9 parts of ethyl isocyanate acrylate and 1 part of initiator were mixed evenly to obtain a mixture A; 35 parts of butyl acetate were taken, the temperature was raised to 80°C, and under nitrogen protection, the mixture A was added dropwise to the butyl acetate for 3 hours, and then kept warm for 8 hours. During the warming period, 1 part of initiator was added every 150 minutes. After the reaction was completed, the temperature was lowered to room temperature to obtain a mixture A;
[0078] A2. Add 7 parts of perfluorooctyl trimethoxysilane, 5 parts of hexamethylcyclotrisiloxane and 4 parts of perfluorooctanol to mixture A, add a catalyst at 80° C., and when the content of isocyanate in the reaction system reaches more than 98% of the theoretical value, add 6 parts of hydroxyethyl methacrylate and 2 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0079] Furthermore, in step A1, the initiator is at least one of diisoheptyl azo.
[0080] Furthermore, in step A2, the catalysts are stannous octoate and dibutyltin dilaurate.
[0081] Furthermore, the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.
[0082] Furthermore, the preparation method of the anti-fouling coating comprises the following steps:
[0083] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 70° C. and stirring continuously, and keeping the temperature for 40 minutes to obtain a mixture B;
[0084] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 60 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0085] The method for preparing the above-mentioned stain-resistant decorative paper comprises the following steps:
[0086] (1) Apply the anti-fouling coating to the surface of the impregnated paper at a coating amount of 50 g / m 2 ;
[0087] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0088] Furthermore, in the step (2), the impregnated paper coated with the stain-resistant coating is baked at 65° C. for 5 minutes, and then irradiated with ultraviolet light for 15 minutes to obtain stain-resistant decorative paper.
[0089] The rest of the content of this embodiment is the same as that of Embodiment 1.
[0090] Example 4
[0091] In the present embodiment, a stain-resistant decorative paper includes an impregnated paper and a stain-resistant coating wrapped on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by applying the stain-resistant coating to the impregnated paper and then curing; the stain-resistant coating includes the following raw materials in parts by weight: 45 parts of modified acrylic resin, 16 parts of epoxy acrylic resin, 12 parts of ethoxylated trimethylolpropane triacrylate, 6 parts of nano-silicon dioxide, 5 parts of nano-zinc oxide, 4 parts of polyoxyethylene ether, 3 parts of film-forming aid, 3 parts of photoinitiator, 6 parts of ethyl acetate, and 25 parts of water.
[0092] Furthermore, the preparation method of each modified acrylic resin comprises the following steps:
[0093] A1. By weight, 35 parts of methyl methacrylate, 8 parts of isooctyl acrylate, 8 parts of ethyl isocyanate acrylate and 0.8 parts of initiator were mixed evenly to obtain a mixture A; 28 parts of butyl acetate were taken, the temperature was raised to 75°C, and under nitrogen protection, the mixture A was added dropwise to the butyl acetate for 3 hours, and then kept warm for 6 hours. During the insulation period, 0.6 parts of initiator were added every 120 minutes. After the reaction was completed, the temperature was lowered to room temperature to obtain a mixture A;
[0094] A2. Add 6 parts of perfluorooctyl trimethoxysilane, 4 parts of hexamethylcyclotrisiloxane and 5 parts of perfluorooctanol to mixture A, add a catalyst at 80° C., and when the isocyanate content in the reaction system reaches more than 98% of the theoretical value, add 4 parts of hydroxyethyl methacrylate and 2 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
[0095] Furthermore, the preparation method of the anti-fouling coating comprises the following steps:
[0096] B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water are mixed in proportion, heated to 70° C. and stirred continuously, and kept warm for 25 minutes to obtain a mixture B;
[0097] B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 50 minutes, and cool to room temperature to obtain a stain-resistant coating.
[0098] The method for preparing the above-mentioned stain-resistant decorative paper comprises the following steps:
[0099] (1) Apply the anti-fouling coating to the surface of the impregnated paper at a coating amount of 50 g / m 2 ;
[0100] (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
[0101] Furthermore, in the step (2), the impregnated paper coated with the stain-resistant coating is baked at 60° C. for 10 minutes, and then irradiated with ultraviolet light for 10 minutes to obtain stain-resistant decorative paper.
[0102] The rest of the content of this embodiment is the same as that of Embodiment 1.
[0103] Comparative Example 1
[0104] The difference between this comparative example and Example 1 is that this comparative example uses an equal amount of JONCRYL HRC 1661 acrylic emulsion to replace the modified acrylic resin in Example 1.
[0105] Comparative Example 2
[0106] The difference between this comparative example and Example 1 is that this comparative example does not contain ethoxylated trimethylolpropane triacrylate.
[0107] The decorative papers of Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, and the anti-fouling performance and anti-fingerprint effect were evaluated by using an oil-resistance pen and hydrophobicity and oleophobicity.
[0108] Oil-resistant pen test: Take two points several centimeters apart in the middle of the decorative paper surface, draw a straight line between the two points with an oil-resistant pen, and repeatedly wipe the straight line with a dust-free cloth until the handwriting cannot be wiped clean. Record the number of times as N, and the number of oil-resistant pen times is N-1. The more times the oil-resistant pen is drawn, the better the oil resistance of the surface.
[0109] Hydrophobicity and oleophobicity test: The static contact angle of water droplets and oil droplets on the coating is tested using a JC2000C1 contact angle meter. The larger the θ of the water droplet or oil droplet, the better the hydrophobicity and oleophobicity of the anti-fingerprint coating. The test liquids are water and oleic acid, and the droplet size is 5μL, in degrees. The test conditions are room temperature 25℃ and relative humidity 65%RH.
[0110] Take the decorative paper of Example 1-4 and Comparative Example 1-2, and heat press one side of the decorative paper onto the artificial board for 3 minutes under the conditions of pressure of 5 MPa and temperature of 160°C. The artificial board is a fiberboard, and the density of the artificial board is 0.68-0.72 g / cm 3 According to GB / T28995-2012, the appearance quality of the stain-resistant decorative paper was observed. It can be seen that the surface stain-resistant coating of Examples 1-4 and Comparative Examples 1-2 has no damage, stains, gaps, etc., and the product appearance quality meets the standard of GB / T 28995-2012. According to GBT17657-2022, the surface wear resistance, surface scratch resistance (≥1.5N surface has no scratches greater than 90%) and surface cold and hot cycle resistance of the veneer artificial board were measured respectively. The test results are shown in the following table:
[0111]
[0112]
[0113] The stain-resistant decorative paper of the present invention has good stain resistance, wear resistance and scratch resistance, and the surface has good resistance to cold and heat cycles and excellent comprehensive performance.
[0114] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A stain-resistant decorative paper, characterized in that: The invention comprises an impregnated paper and a stain-resistant coating coated on the outer surface of the impregnated paper, wherein the stain-resistant coating is formed by coating the stain-resistant coating on the impregnated paper and then curing the coating; the stain-resistant coating comprises the following raw materials in parts by weight: 40-50 parts of modified acrylic resin, 15-20 parts of bisphenol A epoxy acrylate, 10-15 parts of ethoxylated trimethylolpropane triacrylate, 5-9 parts of nano silicon dioxide, 4-8 parts of nano zinc oxide, 3-5 parts of polyoxyethylene ether, 2-4 parts of film-forming aid, 2-4 parts of photoinitiator, 5-10 parts of ethyl acetate and 20-30 parts of water.
2. The stain-resistant decorative paper according to claim 1, characterized in that: The preparation method of each modified acrylic resin comprises the following steps: A1. Take 30-40 parts of methyl methacrylate, 6-10 parts of isooctyl acrylate, 5-9 parts of ethyl isocyanate acrylate and 0.5-1 parts of initiator by weight and mix them evenly to obtain a mixture A; take 25-35 parts of butyl acetate, heat it to 75-80°C, and add the mixture A dropwise to the butyl acetate under nitrogen protection for 2-3 hours, then keep it warm for 6-8 hours, add 0.5-1 parts of initiator every 120-150 minutes during the heat preservation period, and cool it to room temperature after the reaction is completed to obtain a mixture A; A2. Add 4-7 parts of perfluorooctyl trimethoxysilane, 3-6 parts of hexamethylcyclotrisiloxane and 3-6 parts of perfluorooctanol to mixture A, add a catalyst at a temperature of 75-85° C., and when the content of isocyanate in the reaction system reaches more than 98% of the theoretical value, add 3-6 parts of hydroxyethyl methacrylate and 1-2 parts of hydroquinone monomethyl ether to obtain a modified acrylic resin.
3. The stain-resistant decorative paper according to claim 2, characterized in that: In the step A1, the initiator is at least one of azobisisobutyronitrile and azobisisoheptanenitrile.
4. The stain-resistant decorative paper according to claim 2, characterized in that: In the step A2, the catalyst is at least one of stannous octoate and dibutyltin dilaurate.
5. The stain-resistant decorative paper according to claim 1, characterized in that: The film-forming aid is at least one of ethylene glycol tert-butyl ether, dipropylene glycol methyl ether and dipropylene glycol butyl ether.
6. The stain-resistant decorative paper according to claim 1, characterized in that: The particle sizes of the nano silicon dioxide and nano zinc oxide are 30-80nm.
7. The stain-resistant decorative paper according to claim 1, characterized in that: The photoinitiator is at least one of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl acetone and 2,4,6-trimethylbenzoyl-diphenyl phosphine oxide.
8. The stain-resistant decorative paper according to claim 1, characterized in that: The preparation method of the anti-fouling coating comprises the following steps: B1, modifying acrylic resin, epoxy acrylic resin, ethoxylated trimethylolpropane triacrylate, nano-silicon dioxide, nano-zinc oxide, polyoxyethylene ether and water in proportion, heating to 65-70° C. and stirring continuously, and keeping the temperature for 20-40 minutes to obtain a mixture B; B2. Add film-forming aid, photoinitiator and ethyl acetate to mixture B, stir for 30-60 minutes, and cool to room temperature to obtain a stain-resistant coating.
9. A method for preparing the stain-resistant decorative paper according to any one of claims 1 to 8, characterized in that: The steps include: (1) applying a stain-resistant coating to the surface of the impregnated paper; (2) The impregnated paper coated with the stain-resistant coating is baked, and then cured by ultraviolet light to obtain stain-resistant decorative paper.
10. The method for preparing the stain-resistant decorative paper according to claim 1, characterized in that: In the step (2), the impregnated paper coated with the stain-resistant coating is baked at 60-65° C. for 5-15 minutes, and then irradiated with ultraviolet light for 10-20 minutes to obtain the stain-resistant decorative paper.
Citation Information
Patent Citations
Hydrophobic decorative paper and preparation method thereof
CN112127207A
Composition and preparation method of 172nm excimer UV skin-feel stain-resistant floor coating
CN115433481A
Formaldehyde-free printing decorative paper, preparation method thereof and veneer artificial board
CN117888402A
Coating composition and coating layer forming method
JP2022079377A
Scratch-resistant Clear paint composition containg Nano silica particles
KR1020120032263A