Optical waveguide and preparation method thereof
By wrapping the modulation layer in the optical waveguide and using the phase change material layer for modulation, the problem of insufficient stability of the optical waveguide during amorphous and crystalline switching is solved, and higher structural stability and light suitable for industrial production is achieved. Waveguide design.
Patent Information
- Application Number
- CN202411095187.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-12-29
AI Technical Summary
The existing optical waveguides are insufficient in stability when switching between amorphous and crystalline states of the modulation layer, and are difficult to apply in industrial production, and there are problems of structural instability and high manufacturing costs.
An optical waveguide structure is designed, wherein the modulation layer is encased in a closed cavity formed by a first isolation layer, a second isolation layer and a first protective layer, and a concave opening toward the protective layer is formed by a regional etching method. The groove is modulated using a phase change material layer, which improves the stability and integrity of the modulation layer and reduces damage to the phase change material.
It improves the structural stability of optical waveguides, reduces the service life of phase change materials, and makes them suitable for industrial production, achieving higher commercialization difficulty.
Smart Images

Figure CN118884609A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical waveguide, and in particular to an optical waveguide comprising a modulation layer and a preparation method thereof. Background Art
[0002] In photonic circuits, light can be controllably guided through an optical waveguide network through various optical switching devices and power shunting devices. Such devices usually operate by controlling the phase of light in a waveguide. For example, microring resonators and Mach-Zehnder Interferometers (MZIs) can achieve optical switching and power shunting functions by tuning the phase of a silicon-on-insulator (SOI) waveguide. In addition, directional couplers can temporarily couple different amounts of light between closely spaced waveguides by tuning their relative phases. Phase shift mechanisms are usually based on thermo-optical effects or free carrier dispersion effects. However, due to the weak perturbation of the refractive index, the waveguide length in such a device is relatively long for achieving the desired phase shift. For example, an MZI can achieve the desired π phase shift at approximately 500 μm. Microrings are small in size, but their operating bandwidth is limited by the resonance conditions. Another approach is to use a micro-electromechanical system (MEMS) switch in the photonic circuit, where each coupled waveguide can be mechanically moved to adjust the coupling efficiency. However, compared with traditional non-mechanical methods, this method has a slow switching speed (milliseconds), a non-compact structure, and relatively high manufacturing cost and complexity. Importantly, the above technology has problems of instability and short service life, that is, the state of the device controlling the optical phase needs to be maintained at a constant power consumption, and the life of the micro-electromechanical system is limited due to its own mechanical structure.
[0003] Phase-Change Materials (PCMs) are intrinsically nonvolatile and have been widely used in photonic applications, including photonic memory devices, rewritable optical disks, optical filters, displays, and optical switches. PCMs can be easily deposited on any substrate using standard methods and can switch back and forth between amorphous and crystalline states at high speed and with long-term stability. The refractive index changes dramatically when switching between the amorphous and crystalline states. Compact optical switches with Ge2Sb2Te5 (GST) and Ge2Sb2Se4Te1 (GSST) on top of waveguide couplers have been demonstrated to have high switching speeds (100ns) and low power consumption. Therefore, PCM-based photonic devices have several advantages over traditional photonic switching schemes and are expected to be used to develop large-scale nonvolatile reprogrammable photonic routing systems, such as field programmable coupler arrays.
[0004] Based on this, the prior art proposes a new optical waveguide. For example, the Chinese invention patent application with application number CN202180043314.8 sets a phase change material layer on the optical waveguide with low absorption loss in the amorphous state (i.e., the extinction coefficient is basically less than 0.1) and a large difference in optical coefficients between the crystalline state and the amorphous state, and the phase change material layer can switch between at least two stable solid states: amorphous state and crystalline state. However, the stability of the optical waveguide with this structure needs to be improved. Summary of the invention
[0005] The object of the present invention is to provide an optical waveguide to partially solve or alleviate the above-mentioned deficiencies in the prior art, wherein the stability of the modulation layer in the optical waveguide when switching between the amorphous state and the crystalline state is more reliable.
[0006] In order to solve the above-mentioned technical problems, the present invention specifically adopts the following technical solutions:
[0007] A first aspect of the present invention is to provide an optical waveguide, comprising: an optical waveguide layer, a modulation layer located on the optical waveguide layer, a first isolation layer arranged between the optical waveguide layer and the modulation layer, a first protective layer covering the modulation layer, and further comprising: a second isolation layer surrounding the first isolation layer and the modulation layer and having an inverted L-shaped cross section, and a second protective layer surrounding the first protective layer, the second isolation layer and the optical waveguide layer; wherein the modulation layer is wrapped in a closed cavity formed by the first protective layer, the first isolation layer and the second isolation layer, and the modulation layer is a phase change material layer or the modulation layer includes a phase change material layer.
[0008] In some embodiments of the present invention, the first isolation layer and the second isolation layer together form a second groove opening toward the first protective layer, and the height from the bottom of the second groove to the top opening is greater than or equal to the thickness of the modulation layer.
[0009] In some embodiments of the present invention, the second groove is formed by etching the second isolation layer with a T-shaped or concave cross-section that is pre-covered on the optical waveguide layer, and the second protective layer that covers the optical waveguide layer and the second isolation layer, through a regional etching method.
[0010] In some embodiments of the present invention, the phase change material layer is obtained by sputtering a phase change material on the first isolation layer through a sputtering process.
[0011] In some embodiments of the present invention, the first protective layer is deposited on the phase change material layer by a physical vapor deposition or chemical vapor deposition process.
[0012] In some embodiments of the present invention, the upper surface of the first protective layer is flush with the upper surface of the second protective layer.
[0013] In some embodiments of the present invention, the thickness of the first isolation layer is 1 nm to 100 nm.
[0014] In some embodiments of the present invention, the length of the first isolation layer extending along the length direction of the waveguide is 1 μm to 10 μm.
[0015] In some embodiments of the present invention, the thickness of the first protective layer is 0.1 μm to 3 μm.
[0016] In some embodiments of the present invention, the length of the first isolation layer extending along the length direction of the waveguide is 1 μm to 10 μm.
[0017] In some embodiments of the present invention, the thickness of the modulation layer is 1 nm to 1 μm.
[0018] In some embodiments of the present invention, the modulation layer extends along the length direction of the waveguide to a length of 1 μm to 10 μm.
[0019] In some embodiments of the present invention, the phase change material layer is made of a superlattice material; or, the phase change material layer is formed of a chalcogenide containing antimony or selenium, or the phase change material layer contains the chalcogenide, wherein the chalcogenide includes Sb2Se3 or SbSe, Sb2S3 or SbS, Ge2Sb2Se4Te; or, the phase change material of the phase change material layer includes a compound or alloy containing an element combination of germanium, antimony, selenium, and vanadium oxide, or a mixture of the compounds; the compounds include NbOx, GeTe, GeSb, GaSb, AgInSbTe, InSb, InSbTe, InSe, SbTe, TeGeSbS, AgSbSe, SbSe, GeSbMnSn, AgSbTe, AuSbTe and AlSb.
[0020] In some embodiments of the present invention, the optical waveguide layer includes a third region and a fourth region outside the third region, and the modulation layer is located above the fourth region. Herein, the third region refers to a region including a metal interconnection layer and a region including a channel connected to the metal interconnection layer; the fourth region refers to a region not including the metal interconnection layer and a region not including a channel connected to the metal interconnection layer.
[0021] In some embodiments of the present invention, the cross section of the optical waveguide layer is rectangular or convex.
[0022] In some embodiments of the present invention, the first protective layer and / or the second protective layer are made of any one or more of SO2, Al2O3, and ITO. The first protective layer and the second protective layer can be made of the same or different materials.
[0023] In some embodiments of the present invention, the first isolation layer and / or the second isolation layer are made of one or both of Si3N4 and TiN. Preferably, the first isolation layer and the second isolation layer are made of the same material.
[0024] A second aspect of the present invention is to provide a method for preparing the above optical waveguide, comprising the steps of:
[0025] S1021, integrating an optical waveguide layer on a substrate to form an optical waveguide platform;
[0026] S1023, forming a second stop layer of a third thickness and a second oxide layer of a second thickness on the outer surface of the optical waveguide layer exposed above the substrate by physical vapor deposition or chemical vapor deposition; wherein the second stop layer is located above the optical waveguide layer, and its cross section is a T-shaped or concave-shaped second stop layer, and the width of the vertical portion of the T-shaped second stop layer is greater than the width of the optical waveguide layer, or the width of the concave-shaped second stop layer is greater than the width of the optical waveguide layer;
[0027] S1025, performing a window opening process on the second stop layer and the second oxide layer by a regional etching method, so as to form a first stop layer with a fourth thickness on the optical waveguide layer, and a second stop layer surrounding the first stop layer and having an inverted L-shaped cross section; the fourth thickness is less than the third thickness;
[0028] S1027, using a first thin film deposition process to deposit a phase change material onto a surface of the first stop layer by a physical vapor deposition method, so as to form a phase change material layer of a preset thickness in a window formed by the first stop layer and the second stop layer around the first stop layer; the preset thickness is less than or equal to a difference between the third thickness and the fourth thickness;
[0029] S1033, using a second thin film deposition process to deposit an oxide layer of the same material as that in step S1013 onto the phase change material layer to cover it, thereby obtaining a first oxide layer of a sixth thickness.
[0030] Beneficial effects of the present invention: At present, the main method for preparing integrated optical devices based on phase change materials on mature and available commercial SOI substrates is: by using advanced magnetron sputtering or thermal evaporation processes, a variety of phase change materials are directly deposited on the upper surface of the optical waveguide layer (i.e., using an upward coupling method) or deposited on the upper surface and side walls of the waveguide (compared with the upward coupling method; the phase change material layer is also deposited on the side walls of the optical waveguide layer, which will cause unevenness, resulting in many uncertainties in the subsequent optical coupling and phase change material modulation process). The sputtering of phase change materials can be achieved by using a single target material or co-sputtering of multiple targets (the composition and doping can be adjusted). Magnetron sputtering technology is a technology that uses energetic particles to bombard the target surface in a vacuum, so that the bombarded particles are deposited on the substrate. After sputtering a layer of phase change material film on the surface using magnetron sputtering technology, a layer of oxide layer is sputtered for protection. Although this method can achieve heterogeneous integration of phase change materials and optical waveguides, there are still the following two problems:
[0031] On the one hand, the stability of the structure itself needs to be improved. 1. The oxide layer sputtered after the phase change material is very thin (10nm~30nm), and the oxide layer is sputtered immediately after the phase change material. It only covers the upper surface of the phase change material layer and cannot completely wrap the phase change material. Naturally, its protective effect is low. 2. After modulation (melting / recrystallization), the phase change material has fluidity after melting and will move a certain distance. It is precisely because there is only a thin oxide layer on its surface. Therefore, it is actually impossible to control the change area of the phase change material after modulation, so there may be problems of material separation or even volatilization, which leads to instability when the modulation layer in the structure switches between the amorphous and crystalline states.
[0032] On the other hand, it is difficult to achieve commercialization (for example, industrial production) and can only be used for scientific research. Because in industrial production, the chip generally also contains an oxide layer located on the surface of the optical waveguide and a metal interconnection layer embedded in the oxide layer. Limited by the existing front-end and back-end processes, phase change materials cannot be directly added to the chip manufacturing process, that is, the above-mentioned method of sputtering the phase change material layer directly on the waveguide layer cannot be directly applied to industrial production. Specifically, the existing chip manufacturing process is mainly divided into front-end process and back-end process. The front-end process includes wafer processing, oxidation process, photolithography, etching, deposition and doping / ion implantation, while the back-end process mainly forms the metal interconnection layer on the chip. Due to the many technical difficulties and complex operations of the front-end process, in order to avoid pollution, the phase change material is not allowed to be integrated on the waveguide in the front-end process. The dielectric layer and metallization in the back-end process require a higher operating temperature, which will affect the stability of the phase change material integration under this high temperature environment, so the phase change material is not allowed to be placed before the metallization. That is to say, the industrial production of optical waveguides with this structure is difficult.
[0033] Based on this, the present invention provides a new structure of optical waveguide, which has higher structural stability and is conducive to commercialization. Specifically, in order to avoid damage to the optical waveguide layer during the window opening process, a first isolation layer is set between the optical waveguide layer and the modulation layer, and in order to better wrap the modulation layer, the modulation layer is set in a cavity formed by the first isolation layer and the second isolation layer, and covered by the first protective layer, that is, the first isolation layer, the second isolation layer and the first protective layer define the movement space of the modulation layer during the switching of different states (for example, the first isolation layer and the second isolation layer form a wrapping layer that almost completely wraps the modulation layer, and is covered by the first protective layer to define the movement space of the modulation layer during the switching of different states), thereby ensuring the integrity and stability of the modulation layer, thereby reducing the irreversible damage of the phase change material and extending the service life of the phase change material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without paying creative labor.
[0035] Figure 1a is a schematic diagram of the cross-sectional structure of an optical waveguide according to an exemplary embodiment of the present invention;
[0036] Figure 1b for Figure 1a An exploded view of the optical waveguide shown;
[0037] Figure 1c is a schematic cross-sectional structure diagram of an optical waveguide according to another exemplary embodiment of the present invention;
[0038] Figure 1d for Figure 1c An exploded view of the optical waveguide shown;
[0039] Figure 1e is a schematic cross-sectional structure diagram of an optical waveguide of yet another exemplary embodiment of the present invention;
[0040] Figure 1f for Figure 1e An exploded view of the optical waveguide shown;
[0041] Figure 2a A flow chart of a method for preparing an optical waveguide according to an exemplary embodiment of the present invention;
[0042] Figure 2b To prepare the optical waveguide using the optical waveguide preparation method of the present invention Figure 1a Flowchart of the optical waveguide of the structure shown;
[0043] Figure 2c To prepare the optical waveguide using the optical waveguide preparation method of the present invention Figure 1c Flowchart of an optical waveguide of the structure shown;
[0044] Figures 3a to 3e 2 is a schematic diagram of preparing an optical waveguide using a strip waveguide layer as an example according to the method shown in FIG. 2 ;
[0045] Figure 3f to Figure 3j Taking a strip waveguide layer as an example, a schematic diagram of preparing an optical waveguide according to the method shown in FIG2 ;
[0046] Figure 4 This is a diagram of optical power cyclically modulated by an optical waveguide (i.e., a control group) prepared by using an existing integrated phase change material method;
[0047] Figure 5 To adopt Figures 3a to 3e Optical power diagram of cyclic modulation of the optical waveguide (i.e., the experimental group) obtained by the method shown.
[0048] Summary of reference numerals and symbols in the accompanying drawings: 01 substrate; 02 optical waveguide layer; 03 phase change material layer; 04 first stop layer; 05 first oxide layer; 06 second stop layer; 07 second oxide layer; 5 metal interconnection layer; 001 sealed cavity, 0011 first groove, 0012 second groove; H0 height of the phase change material layer extending along the Z-axis direction (or referred to as a preset thickness); H1, H3 height of the second stop layer extending along the Z-axis direction (or referred to as the first thickness, the third thickness) in different embodiments; H2 height of the second oxide layer extending along the Z-axis direction (or referred to as the second thickness) in different embodiments; H4 height of the first stop layer extending along the Z-axis direction (or referred to as the fourth thickness); H6 height of the first oxide layer extending along the Z-axis direction (or referred to as the sixth thickness); h1 height of the opening of the first groove; h2 height of the opening of the second groove (h2>h1). DETAILED DESCRIPTION
[0049] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0050] Herein, suffixes such as "module", "component" or "unit" used to represent elements are only used to facilitate the description of the present invention, and have no specific meanings by themselves. Therefore, "module", "component" or "unit" can be used mixedly.
[0051] In this document, the terms "upper", "lower", "inner", "outer", "front", "back", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0052] In this document, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] Herein, "and / or" includes any and all combinations of one or more of the listed related items. Herein, "plurality" means two or more, that is, it includes two, three, four, five, etc.
[0054] As used in this specification, the term "about" typically means + / - 5% of the stated value, more typically + / - 4% of the stated value, more typically + / - 3% of the stated value, more typically + / - 2% of the stated value, even more typically + / - 1% of the stated value, and even more typically + / - 0.5% of the stated value.
[0055] In this specification, some embodiments may be disclosed in a format of being within a certain range. It should be understood that such description of "being within a certain range" is only for convenience and brevity, and should not be interpreted as a rigid limitation on the disclosed range. Therefore, the description of the range should be considered to have specifically disclosed all possible sub-ranges and independent numerical values within this range. For example, the range The description of should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within this range, for example, 1, 2, 3, 4, 5, and 6. The above rules apply regardless of the breadth of the range.
[0056] Herein, "light" refers to electromagnetic radiation or electromagnetic waves with a wavelength in the ultraviolet (UV) to infrared (IR) range (eg, between 10 nm and 100 μm), which can propagate in free space and be guided by a waveguide.
[0057] In this context, "steady state" may mean substantially stable under standard temperature and pressure conditions specified by the National Institute of Standards and Technology (NIST).
[0058] As used herein, "optical waveguide layer" refers to any structure used to confine light in one or more dimensions within or adjacent to its surface, thereby guiding the light in a propagation direction parallel to its axis. The waveguide is formed by a series of layers / regions with different refractive indices, typically including an inner layer / region or a core layer / region. The inner layer / region or the core layer / region is made of a material with a higher refractive index than the surrounding (outer) layers / regions or cladding layers / regions. In this case, the waveguide confines light in two dimensions, for example, within a channel, in the thickness / growth direction and in the lateral / width direction perpendicular to the thickness / growth direction. The core layer / region and / or the cladding layer / region may be referred to as a guiding layer that actively confines and guides the light.
[0059] Herein, "modulation layer" refers to any entity that affects the properties of light, including transmission, refraction, absorption, etc. In some embodiments, the light modulation layer includes a phase change material layer made of a phase change material, or can be made of a phase change material.
[0060] The present invention proposes an optical waveguide with high stability and industrial production, which includes: an optical waveguide layer, and a modulation layer located on the optical waveguide layer, a first isolation layer is provided between the optical waveguide layer and the modulation layer to prevent the optical waveguide layer from being damaged during the window opening process, and the modulation layer is covered with a first protective layer. The modulation layer is made of a phase change material, or includes a phase change material layer (for ease of description, the phase change material layer is taken as the modulation layer in the subsequent embodiments as an example).
[0061] In the windowing process of current industrial production, it is difficult to directly and perfectly open above the optical waveguide layer, that is, to directly sputter or deposit the modulation layer on the optical waveguide layer without losing the waveguide layer at all during the windowing process. Therefore, each example in this article adopts a layer of isolation layer to protect the optical waveguide layer (such as the first stop layer) and wrap the modulation layer at the same time. For example, by pre-setting a stop layer and an oxide layer of a specified thickness on the optical waveguide layer (for example: a stop layer of the first thickness H1 or the third thickness H3, and an oxide layer of the second thickness H2), and then in the windowing process, by controlling the process parameters of the windowing process to control the etching depth on the stop layer, a stop layer of a specified thickness (for example, the fourth thickness H4) is retained on the optical waveguide layer, thereby avoiding certain damage to the optical waveguide and wrapping the modulation layer to ensure its stability.
[0062] Generally speaking, when coupling upward, a modulation layer is directly set on the upper surface of the optical waveguide layer, so that the modulation layer has the best range of the evanescent field of the light in the optical waveguide, and thus the optical signal power range that can be modulated is the best. However, as mentioned above, due to the limitations of the existing process, it is difficult to perfectly set the modulation layer directly without damaging the optical waveguide layer. Therefore, in order to avoid damage to the optical waveguide layer, an isolation layer is set on the optical waveguide layer for protection. However, at the same time, the setting of the isolation layer needs to consider the influence of the modulation layer on the evanescent field of the light in the optical waveguide. If the isolation layer is too thick, even if the modulation layer is in the same state and the same thickness, the evanescent field range that can be affected is smaller, and thus the optical signal power range that can be modulated is smaller; if the isolation layer is too thin, it is difficult to make it too thin due to the limitations of the existing windowing process. Therefore, the influence of the modulation layer on the evanescent field range of the light in the optical waveguide and the damage to the optical waveguide layer are comprehensively considered, and the thickness of the isolation layer is explored, so that the optical waveguide layer can be protected at the same time without greatly reducing the evanescent field range of the modulation layer on the light in the optical waveguide layer. For example, the specific thickness is determined by simulation according to actual needs. Preferably, the thickness H4 of the isolation layer between the optical waveguide layer and the modulation layer is 1 nm to 100 nm.
[0063] Of course, it is also possible to pre-set a desired thickness, such as an isolation layer of H4, on the optical waveguide layer, and then directly etch away the oxide layer in the subsequent windowing process, that is, stop etching when the isolation layer is seen during the etching process. Since the isolation layer has a certain thickness, even if a little bit is etched away, it will not affect the optical waveguide, but will reduce the thickness of the isolation layer and be beneficial to the effect of the modulation layer on the evanescent field of light in the optical waveguide layer. In particular, when it is impossible to directly make the thickness of the stop layer between the modulation layer and the optical waveguide layer thinner (for example, less than 1 nm) through etching parameters due to the limitations of the existing windowing process, by pre-depositing the isolation layer to a specified thickness (for example, the minimum value of the value range: 1 nm), the thickness of the isolation layer can be further reduced by etching the previously set oxide layer slightly over-etched.
[0064] In order to facilitate the description of the positional relationship between the various components of the optical waveguide, a three-dimensional coordinate system is constructed in this article with the length of the optical waveguide as the Y-axis, the height as the Z-axis, and the width as the X-axis, wherein the cross section refers to the cross-sectional plane obtained by cutting the corresponding area of the optical waveguide with a vertical plane (i.e., the XZ plane).
[0065] Example 1: See Figure 1a , is a schematic diagram of an optical waveguide structure of an exemplary embodiment of the present invention. Specifically, the optical waveguide structure includes: a silicon oxide substrate 01, an optical waveguide layer 02, and a phase change material layer 03 located on the optical waveguide layer 02. A first stop layer 04 (i.e., a first isolation layer) is provided between the optical waveguide layer 02 and the phase change material layer 03 (i.e., a modulation layer), and a first oxide layer 05 (i.e., a first protective layer) is covered on the phase change material layer 03. Preferably, the width of the first stop layer 04 (i.e., the length extending along the X-axis direction), the width of the optical waveguide layer 02 (i.e., the length extending along the X-axis direction), and the width of the phase change material layer 03 (i.e., the length extending along the X-axis direction) are the same.
[0066] See also Figure 1aOn the substrate 01, a second stop layer 06 is arranged around the first stop layer 04 and the first region of the phase change material layer 03 close to the first stop layer 04 (i.e., a portion of the sidewall region around the bottom where the phase change material layer 03 contacts the first stop layer 04), and a first thickness (i.e., a length extending along the Z-axis direction) H1 of the second stop layer 06 is greater than a fourth thickness H4 of the first stop layer 04, but less than the sum of the thicknesses of the phase change material layer 03 and the first isolation layer 04 (i.e., the sum of H0 and H4), so that the first stop layer and the second stop layer enclose a first region of the phase change material layer close to the optical waveguide layer on the side that wraps upward (i.e., the peripheral edge of the wrapping component extends upward from the bottom of the wrapped component along the peripheral sidewall height direction to form an enclosing sidewall). wrapping layer; and the second oxide layer 07 is arranged around the first oxide layer 05, the second region near the first oxide layer 05 (i.e., part of the side wall region around the top where the phase change material layer 03 contacts the first oxide layer 05), the second stop layer 06, and the optical waveguide layer 02 on the first oxide layer 05, so that the first oxide layer and the second oxide layer corresponding to the above-mentioned second region are enclosed to form a wrapping layer that wraps downward (i.e., the surrounding edge of the wrapping component extends downward from the top of the wrapped component along the height direction of its surrounding side wall to form an enclosing side wall) the second region of the phase change material layer away from the optical waveguide layer side, that is, the above-mentioned phase change material layer 03 is wrapped in the closed cavity 001 formed by the first oxide layer 05, the second oxide layer 07, the first stop layer 04, and the second stop layer 06.
[0067] In some embodiments, a stop layer (e.g., a second stop layer 06 having a first thickness H1 and a first width L1, where L1 is greater than the width L0 of the optical waveguide layer) and an oxide layer (e.g., a second oxide layer 07 having a second thickness H2) may be pre-set on the optical waveguide layer, see Figure 3b and Figure 3g ; In order to set the phase change material layer 03 on the optical waveguide layer 02, the oxide layer and the stop layer pre-covered on the optical waveguide layer 02 can be etched by a regional etching method to form a cavity with a top opening (or an open window), so as to prepare for the subsequent wrapping of the phase change material layer. For example, a regional etching method is used to open a window, and a stop layer with a fourth thickness H4 is retained directly above the optical waveguide layer, so that a first stop layer is formed between the bottom of the cavity or window and the optical waveguide layer. At the same time, a second stop layer with a second thickness H2 remains around the first stop layer. That is, when the phase change material is subsequently sputtered or deposited in the cavity or window, the first stop layer is the first isolation layer between the phase change material layer 03 and the optical waveguide layer 02. Specifically, by setting the etching parameters of the regional etching method, a stop layer with a fourth thickness H4 (for example, 1nm to 100nm) remains on the optical waveguide, thereby avoiding damage to the optical waveguide layer during the etching process or the window opening process, see. Figure 1b, Figure 3c and Figure 3h .
[0068] In some embodiments, after the above-mentioned cavity is opened on the oxide layer and the stop layer by a regional etching method, a phase change material layer of a specified thickness H0 (for example, 1nm~1um) can be set on the first stop layer by processes such as sputtering or deposition (physical vapor deposition or chemical vapor deposition), thereby obtaining a modulation layer. Of course, in order to protect the modulation layer, it is necessary to cover it with a sixth protective layer of thickness H6, for example, the first oxide layer 05. In order to ensure stability and avoid the situation where the oxide layer covering the phase change material layer is too thin and the change area of the phase change material after modulation cannot be controlled, preferably, the sixth thickness H6 of the first oxide layer is 0.1um~3um. More preferably, the first oxide layer is deposited on the phase change material layer by physical vapor deposition (PVD) or chemical vapor deposition (CVD).
[0069] Since the first stop layer 04 is obtained by regional etching on the original oxide layer and the stop layer, and the phase change material is sputtered or deposited on the first stop layer, when the first oxide layer 05 of the sixth thickness H6 is covered on the phase change material layer, the first oxide layer 05 (i.e., the oxide layer re-covered on the phase change material layer) and the second oxide layer 07 surrounding the first oxide layer 05 (i.e., the part of the oxide layer retained after the original oxide layer is etched) are enclosed to form a first groove 0011 with an opening facing the phase change material layer; and the first stop layer 04 and The second stop layer (i.e., the part of the stop layer retained after the original stop layer is etched) surrounding the first stop layer 04 encloses a second groove 0012 with an opening facing the phase change material layer 03, and the opening of the first groove 0011 and the opening of the second groove 0012 are arranged relative to each other, so that the first groove 0011 and the second groove 0012 enclose a closed cavity 001 as described above (i.e., the sum of the height h1 of the first groove notch and the height h2 of the second groove notch is the height of the sealed cavity, which is equal to or slightly greater than the thickness H0 of the phase change material layer). Preferably, the cross-sections of the first groove and the second groove are both rectangular, that is, the cross-section of the sealed cavity is rectangular.
[0070] In some embodiments, the upper surface of the first oxide layer 05 is flush with the upper surface of the second oxide layer 07. Of course, in other embodiments, the upper surface of the first oxide layer 05 is not flush with the upper surface of the second oxide layer; or, the first oxide layer covers part of the upper surface of the second oxide layer (preferably, the second oxide layer portion around the cavity top opening) or the entire upper surface.
[0071] In some embodiments, the optical waveguide layer is in a strip shape (ie, its cross section is rectangular). Of course, the optical waveguide layer may also be a ridge waveguide (ie, its cross section is convex).
[0072] In some embodiments, the substrate may also be an SOI substrate, as long as the substrate enables the optical waveguide layer to have an optical band gap of at least 1 eV.
[0073] Embodiment 2: In order to better protect and wrap the phase change material layer and reduce the process difficulty, the present invention also provides another exemplary structure of an optical waveguide, which includes the various components in the above-mentioned embodiment 1, except that the sealed cavity 001 in the exemplary optical waveguide is only formed by the first oxide layer 05 (i.e., the first protective layer) located on the top of the phase change material layer 03, the first stop layer 04 (i.e., the first isolation layer) located at the bottom of the phase change material layer 03 (i.e., the modulation layer), and the second stop layer 06 (i.e., the second isolation layer) surrounding the phase change material layer 03 and the first stop layer 04, see Figure 1c and Figure 1d ; and the second protective layer 07 surrounds the first oxide layer 05, the second stop layer 06 and the optical waveguide layer 02, forming an almost fully wrapped protection.
[0074] In some embodiments, the cross section of the second stop layer 06 surrounding the phase change material layer 03 and the first stop layer 04 is in an inverted L shape, and the upper surface of the second stop layer 06 is flush with or slightly higher than the upper surface of the phase change material layer.
[0075] In some embodiments, when preparing the optical waveguide of the exemplary structure, a second oxide layer 07 with a second thickness H2 and a second stop layer with a third thickness H3 may be pre-arranged on and around the optical waveguide layer, wherein the top of the second stop layer 06 extends a wing along the width direction of the optical waveguide, so that the cross section of the second stop layer 06 is T-shaped, and the first width L1 of the vertical portion thereof extending along the Z-axis direction is greater than the width L0 of the optical waveguide layer 02; then, the second oxide layer and the second stop layer are etched by a regional etching method to form a cavity with a top opening, specifically, by The etching parameters of the regional etching method are set to form a cavity for accommodating the phase change material layer, that is, the second groove 0012 formed in the second stop layer 06 (that is, the first stop layer serves as the bottom of the second groove, and the second stop layer serves as the sidewall of the second groove) serves as a cavity for accommodating the phase change material layer, and the height h2 from the bottom of the groove to the top opening is equal to or slightly greater than the preset thickness H0 of the sealed cavity / modulation layer, so that the periphery and bottom of the modulation layer are wrapped by the stop layer, thereby making the prepared optical waveguide more stable and less difficult to process.
[0076] In other embodiments, the cross section of the second stop layer pre-set on and around the optical waveguide layer is in a concave shape. Specifically, the concave shape includes the shape of the standard Chinese character "concave"; or the shape of the non-standard Chinese character "concave", but similar to the concave shape of the Chinese character (for example, its two side walls have a certain inclination, or the width of the side walls varies along the Z-axis direction, or the top edges of the two side walls extend a certain width of the protruding edge along the width direction of the optical waveguide). Accordingly, the third thickness H3 refers to the height from the top to the bottom of the side wall of the second stop layer with a concave cross section; and the thickness of the groove bottom is greater than or equal to the fourth thickness.
[0077] Embodiment 3: The optical waveguide of the above structure has strict requirements on the size of the window in the window opening process, and because the side walls of the cavity obtained by etching extend in the vertical direction (or are slightly inclined), when sputtering the phase change material, it may be deposited in other peripheral positions, and it is necessary to additionally remove this part of the phase change material or cover the phase change material deposited in the peripheral position with the same first protective layer, which not only makes the window opening process more difficult, but also makes the operation more complicated. Based on this, this article also provides another exemplary structure of the optical waveguide, which includes the various components in the above embodiment 1, except that in this example, the phase change material layer 03 is wrapped in a closed cavity 001 with a trumpet-shaped or bowl-shaped cross-section formed by the first protective layer 05, the second protective layer 07, the first isolation layer 04 and the second isolation layer 06.
[0078] In some embodiments, the first protective layer 05 and the second protective layer 06 surrounding the first protective layer 05 and the second region of the phase change material layer 03 away from the optical waveguide layer enclose a first groove with an inverted U-shaped cross section; the first isolation layer 04 and the second isolation layer 06 surrounding the first isolation layer and the first region of the phase change material layer 03 close to the optical waveguide layer enclose a second groove with a U-shaped cross section, and in the same cross section, the spacing between the oppositely arranged side walls of the first groove gradually decreases in the direction close to the optical waveguide layer (or in the vertical downward direction), while the spacing between the oppositely arranged side walls of the second groove gradually increases in the direction away from the optical waveguide layer (or in the vertical upward direction), and the opening of the first groove and the opening of the second groove are arranged opposite to each other, so that the side wall of the first groove and the side wall of the second groove are smoothly connected and enclosed to form a closed cavity.
[0079] In some embodiments, as described above, a stop layer and an oxide layer may be pre-set on the optical waveguide layer, and then a bowl-shaped or horn-shaped cavity with a top opening may be formed by etching using a regional etching method. On the one hand, since the top opening of the cavity is relatively large, the coverage area of the subsequent sputtering of the phase change material is expanded, and the inclined window sidewalls also make it easier for the phase change material to enter the window and deposit at the bottom of the window, reducing the difficulty of the sputtering process; on the other hand, since the top opening is relatively large and the surrounding sidewalls have a certain inclination or curvature, that is, non-vertical etching, the difficulty is lower than that of the etching process of the optical waveguide structure in Example 1 or Example 2.
[0080] Example 4: Optical waveguide preparation method. Figure 2a , is a flow chart of a method for preparing an optical waveguide according to an exemplary embodiment of the present invention. Specifically, the method comprises the steps of:
[0081] S101, integrating an optical waveguide layer on a substrate to form an optical waveguide platform.
[0082] In some embodiments, step S101 is performed using conventional pulsed laser deposition (PLD) technology, such as the process disclosed in Chinese patent CN1487636A, which will not be described in detail here. Figure 3a Taking a strip waveguide as an example, an optical waveguide layer 02 is integrated on a substrate 01 to form an optical chip with an optical waveguide platform.
[0083] In some embodiments, the substrate is a silicon nitride substrate or an SOI substrate; and the optical waveguide layer 02 has an optical bandgap of at least 1 eV. Preferably, the material of the optical waveguide layer is selected from: silicon, silicon nitride, gallium nitride, gallium arsenide, aluminum nitride, magnesium oxide and diamond (polycrystalline or single crystal).
[0084] S103, forming a stop layer and an oxide layer on the outer surface of the optical waveguide layer exposed above the substrate by physical vapor deposition or chemical vapor deposition, wherein the stop layer is located above the optical waveguide and has a width greater than that of the optical waveguide layer.
[0085] In some embodiments, the outer surface of the optical waveguide layer exposed on the substrate is covered with a stop layer and a thicker oxide layer in sequence. The function of the stop layer is to set an isolation layer above the waveguide layer for isolating the oxide layer dry etching process. When the oxide layer is dry-etched, the dry etching reaction will stop after etching the stop layer, thereby achieving the effect of etching the oxide layer without affecting the waveguide itself; at the same time, it also forms a wrapping effect on the modulation layer, improving the stability of the modulation layer when switching between the amorphous state and the crystalline state. The function of the thicker oxide layer is to protect the waveguide and the metal interconnection layer, and at the same time, it plays a role in insulating the silicon from the metal interconnection layer and between the metal interconnection layers.
[0086] In some embodiments, the material of the oxide layer is one of silicon oxide (SiO2), aluminum oxide (Al2O3) or ITO. Preferably, the material of the oxide layer is silicon oxide (SiO2). The material of the stop layer is one or more of silicon nitride (Si3N4) and titanium nitride (TiN). Preferably, the material of the stop layer is silicon nitride (Si3N4).
[0087] In some embodiments, the stop layer and the oxide layer are both formed by a basic coating process, which includes many types, including vacuum evaporation, ion beam sputtering, magnetron sputtering, chemical vapor deposition CVD, etc. The specific process parameters of this coating process are different in different silicon optical flow factories, which is a common prior art and will not be repeated here. It should be noted that when the oxide layer is deposited, a conventional physical vapor deposition (PVD) or chemical vapor deposition (CVD) process is used to deposit the metal interconnection layer 5 and embed it therein, and the metal interconnection layer 5 is connected to the optical waveguide layer by a through hole.
[0088] See also Figure 2b and Figure 3b Taking the strip waveguide as an example, a second stop layer 06 with a first thickness H1 and a second oxide layer 07 with a second thickness H2 are sequentially covered on the outer surface of the optical waveguide layer 02 exposed on the substrate 01 (i.e., S1013). In order to wrap the phase change material layer (for example, partially wrap and almost fully wrap), the width of the second stop layer is greater than the width of the optical waveguide layer, so that a subsequent window opening process can form a groove on the second stop layer. The bottom of the groove located between the phase change material layer and the optical waveguide layer is the first isolation layer, and the groove wall surrounding the first isolation layer is the second isolation layer.
[0089] See also Figure 2cIn other embodiments, in order to ensure that the phase change material layer is almost wrapped by the stop layer, for example, the upper surface of the phase change material layer is almost flush with the upper surface of the second stop layer, so that the second stop layer remains around the phase change material layer, the outer surface of the optical waveguide layer 02 exposed above the substrate 01 can be first covered with a second oxide layer 07 and a second stop layer with a T-shaped cross section (i.e., S1023), wherein the width L1 of the vertical portion of the T-shape is greater than the width L0 of the optical waveguide layer 02, thereby ensuring that in the subsequent etching process, when etching to the second stop layer, part of the stop layer can be retained around and at the bottom of the phase change material layer, wherein the portion located between the optical waveguide layer and the phase change material layer is the first stop layer (whose thickness is H4). Of course, in other embodiments, the outer surface of the optical waveguide layer 02 exposed on the substrate 01 is first covered with a second oxide layer 07 and a second stop layer with a concave cross-section, and the width of the concave shape is greater than the width of the optical waveguide layer 02, so as to ensure that in the subsequent etching process, when etching to the second stop layer, part of the stop layer can be retained around and at the bottom of the phase change material layer, wherein the part located between the optical waveguide layer and the phase change material layer is the first stop layer (whose thickness is H4).
[0090] S105, performing a window opening process of the stop layer and the oxide layer by a regional etching method, so that a stop layer remains on the optical waveguide layer.
[0091] In some embodiments, a window opening process of the stop layer and the oxide layer is performed by a regional etching method to expose a portion of the stop layer covered on the optical waveguide layer.
[0092] At present, the conventional regional etching window opening process is a combination of dry etching + wet etching or dry etching + dry etching. When dry etching is used for etching, the oxide layer of the window opening part is required, and the etching ends at the stop layer. Dry etching or wet etching is used to extend the stop layer of the window opening part to the top of the waveguide. The specific parameters vary among different silicon optical flow wafer factories, but mainly depend on the oxide layer process, stop layer process, dry etching process, and wet etching process. It is also a common existing technology and will not be repeated here.
[0093] In some embodiments, in S105, it should be noted that: the regional etching window opening process must avoid the metal interconnection layer 5 and the through hole, that is, the metal interconnection layer 5 and the through hole must not be exposed in the window and the metal interconnection layer and the through hole need to be at a certain distance from the area etched by the window opening process. The specific distance is determined according to the process level of different silicon photonic wafer factories.
[0094] As mentioned above, due to the limitations of the etching process in existing industrial production, it is difficult to directly and perfectly open the window process on the optical waveguide, that is, without causing any damage to the optical waveguide, there is no excess stop layer and / or oxide layer remaining on the optical waveguide layer. Therefore, in the present method, in step S103, a stop layer with a first thickness H1 or a third thickness H3 and an oxide layer with a second thickness H2 are pre-set on the optical waveguide layer 02, and then a window is opened on the oxide layer and the stop layer through a regional etching window opening process, and a stop layer with a fourth thickness H4 is retained on the optical waveguide layer 02, that is, in the window opening area, the stop layer on the optical waveguide layer is not completely etched away, but a groove is etched on the stop layer (see Figure 2b S1015 or Figure 2c (S1025).
[0095] On the other hand, as mentioned above, considering the influence of the stop layer on the phase change material layer and the evanescent field range of light in the optical waveguide layer, preferably, the fourth thickness H4 of the first stop layer is formed to be 1 nm to 100 nm.
[0096] In some embodiments, the area of the stop layer exposed in the window opening process is determined by the area of the phase change material to be plated. Preferably, the area of the stop layer exposed is the same as the area of the phase change material layer.
[0097] See also Figure 3c Taking the strip waveguide as an example, a window opening process of the stop layer and the oxide layer is performed by a regional etching method to expose a portion of the stop layer with a fourth thickness H4 (H4
[0098] To ensure that the area of the exposed stop layer is the same as the area of the phase change material layer, or the difference is not large, the control parameters of the etching process are very precise, that is, the processing difficulty is high, and the subsequent sputtering process requirements are also high. In view of this, when etching in step S105 or S1015, the window is not opened according to the above-mentioned 1:1 (or close to 1:1) area, but a bowl-shaped or trumpet-shaped cavity (or window) is etched, and then the phase change material is sputtered in it, and finally the first oxide layer 05 of the sixth thickness H6 is deposited, so as to obtain Figure 1e Optical waveguide with the structure shown.
[0099] S107, using a first thin film deposition process to deposit a phase change material onto the surface of the stop layer exposed in the window by a physical vapor deposition method to form a phase change material thin film.
[0100] In some embodiments, a first sputtering process is used to sputter the phase change material onto the upper surface of the stop layer exposed in the window to form a phase change material film (ie, the phase change material layer 03 ).
[0101] In some embodiments, the phase change material may be formed of or contain a chalcogenide containing antimony or selenium, such as antimony selenide (Sb2Se3 or SbSe), antimony sulfide (Sb2S3 or SbS), Ge2Sb2Se4Te (GSST); or, the phase change material may include or be composed of a compound or alloy of a combination of elements selected from GeSbTe, VOx; NbOx, GeTe, GeSb, GaSb, AgInSbTe, InSb, InSbTe, InSe, SbTe, TeGeSbS, AgSbSe, SbSe, GeSbMnSn, AgSbTe, AuSbTe and AlSb.
[0102] Of course, the phase change material may also include a mixture of the above compounds, or the phase change material may be a supercrystal.
[0103] In some embodiments, the first thin film deposition process is a magnetron sputtering process, and the specific process is as follows: after the optical chip in step S105 is placed in the vacuum chamber, the vacuum chamber is evacuated to a vacuum of 1×10 -6 After the vacuum reaches 3.5×10 Torr, argon gas is introduced and the vacuum is continued to be maintained to keep the process vacuum below 3.5×10 -3 Torr; turn on the magnetron sputtering RF power supply, control the power to 10-100W, and control the formed phase change material film to be between 1nm and 1μm.
[0104] See also Figure 3d Taking the strip waveguide as an example, the phase change material is directly sputtered in the cavity to obtain a phase change material layer with a thickness of 1nm to 1μm.
[0105] In some embodiments, a phase change material layer with a preset thickness H0 is deposited in the window, so that the sum of the preset thickness H0 and the fourth thickness H4 is greater than the first thickness H1, so that the groove etched on the stop layer wraps the bottom of the modulation layer and the first region close to the optical waveguide layer (see Figure 2b S1017, and Figure 1a , Figure 1b and Figure 1e , Figure 1f ), that is, the stop layer after etching forms a wrapping layer that wraps part of the modulation layer.
[0106] In some other embodiments, a phase change material layer with a preset thickness H0 is deposited in the window, so that the preset thickness H0 is less than or equal to the difference between the third thickness H3 and the fourth thickness H4, so that the groove etched on the stop layer wraps the bottom of the stop layer and all its side walls (see Figure 2c S1027, and Figure 1c and Figure 1d ), that is, the stop layer after etching forms a wrapping layer that almost completely wraps the modulation layer (except for the top surface of the modulation layer).
[0107] S109, using a second thin film deposition process to deposit an oxide layer of the same material as in step S103 onto the phase change material layer to achieve coverage, thereby achieving heterogeneous integration of the phase change material and the optical waveguide platform, thereby obtaining an optical waveguide.
[0108] In some embodiments, the second thin film deposition process deposits an oxide layer of the same material as in step S103 onto the phase change material layer to achieve coverage, thereby achieving heterogeneous integration of the phase change material and the optical waveguide platform to obtain an exemplary optical waveguide of the present invention. Preferably, the second thin film deposition process is a physical vapor deposition (PVD) or chemical vapor deposition (CVD) process.
[0109] In some embodiments, the specific process of depositing an oxide layer on the phase change material layer using physical vapor deposition (PVD) includes: after placing the optical chip after step S107 into a vacuum chamber, starting to evacuate the vacuum chamber, and after reaching a vacuum degree of 1×10-6Torr, introducing argon gas and continuing to evacuate the chamber to maintain the process vacuum degree below 3.5×10-3Torr, turning on the magnetron sputtering RF power supply, controlling the power at 10-200W, and controlling the thickness of the formed oxide layer film to be between 0.1 and 3μm.
[0110] In some other embodiments, the specific process of depositing an oxide layer on the phase change material layer by chemical vapor deposition (CVD) includes: placing the optical chip after step S107 into a vacuum chamber, and then evacuating the vacuum chamber to a vacuum of 1×10 -6 After the vacuum degree reaches 1000 Torr, heat the substrate to 150℃-350℃, introduce N2, SiH4, and N2O gases, maintain the deposition pressure at 0.2Torr-2.0Torr, turn on the RF power supply, control the power at 20W-150W, and control the thickness of the formed oxide layer film to be between 0.1μm and 3μm.
[0111] See also Figure 3e Taking the strip waveguide as an example, an oxide layer of the same material as in step S103 is deposited on the phase change material layer 03 through a second thin film deposition process to obtain a first oxide layer 05 with a thickness of H6, thereby realizing heterogeneous integration of the phase change material and the optical waveguide platform.
[0112] Example 5: Stability test. Generally, a voltage pulse can be used to cause a phase change material layer on a waveguide to undergo a reversible phase change between a crystalline state and an amorphous state, wherein when the phase change material layer is in a crystalline state, the optical power passing through the waveguide is low, while when the phase change material layer is in an amorphous state, the optical power passing through the waveguide is high. Therefore, the optical power passing through an optical waveguide containing a phase change material can be used to indicate the stability of the phase change material layer.
[0113] The optical waveguide prepared by the conventional integrated phase change material method is used as the control group, and the optical waveguide of the above-mentioned embodiment 1 in this article is used as the experimental group. The phase change material layer in the optical waveguides of the control group and the experimental group is subjected to cyclic modulation of melting and crystallization, and the optical powers of the two groups of optical waveguides in the cyclic modulation are respectively obtained to obtain respective cyclic modulation optical power diagrams, see Figure 4 (control group) and Figure 5 (Experimental group).
[0114] Specifically, during the cyclic modulation process, the phase change material layers in the two groups of optical waveguides are made of the same material and have the same thickness (both are 30 nm), with the same modulator modulation parameters; the pulse voltage for melting the phase change material layer (changing from crystalline to amorphous) is 9 V, with a duration of 200 ns; the pulse voltage for crystallization (changing from amorphous to crystalline) is 3 V, with a duration of 1 μs.
[0115] Control group: see Figure 4 Under the existing integrated phase change material method, the phase change material layer integrated on the optical waveguide is subjected to melt-crystallization cyclic modulation. After the phase change material layer is re-melted or re-crystallized, the optical power cannot be maintained at the same level, and its optical power fluctuates greatly during the cyclic modulation process (that is, during the cyclic modulation process, the optical powers in the two states deviate from their respective mean lines: the optical power mean line S1 in the crystalline state and the optical power mean line S2 in the amorphous state are farther away), indicating that the phase change material itself has undergone a change in properties during the modulation process, resulting in the inability to stably modulate the state of the phase change material.
[0116] Experimental group: see Figure 5 In the melting-crystallization cyclic modulation process of the phase change material layer in the optical waveguide shown in the above-mentioned embodiment 1, the optical power is kept at the same level after re-melting or re-crystallization, and the optical power fluctuation is very small during the cyclic modulation process (that is, during the cyclic modulation process, the optical powers in the two states almost coincide with their respective mean lines: the optical power mean line S3 in the crystalline state and the optical power mean line S4 in the amorphous state, or the deviation is very small), which shows that the phase change material is stable during the cyclic modulation process, and the state of the phase change material can be stably modulated under the existing structure.
[0117] The L-shape, T-shape, concave shape, etc. described in this article using text (such as Chinese or English, etc.) shape description words include the shapes of the text in various fonts, and also include structures with non-standard text shapes. For example, the top of the L-shape can have a protruding short side extending laterally (shorter than the bottom), and its general structure only needs to look like the corresponding text shape. Similarly, the various structures described in this article using geometric shapes include standard geometric shapes and non-standard geometric shapes (or similar or close shapes). For example, the rectangle in this article includes a standard rectangle in geometric shapes, and can also be a non-standard approximate rectangle. For example, due to process limitations and other factors, the side wall of the sealed cavity formed by the docking of the side wall of the first groove and the second groove has a slight tilt, or there is a slight deviation when the side wall of the first groove and the second groove are docked, but the overall structure is still close to a rectangle.
[0118] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0119] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for preparing an optical waveguide, characterized in that: Includes steps: S1021, integrating an optical waveguide layer on a substrate to form an optical waveguide platform; S1023, forming a second stop layer with a fourth thickness H4 and a second oxide layer with a second thickness H2 on the outer surface of the optical waveguide layer exposed on the substrate by physical vapor deposition or chemical vapor deposition; wherein the second stop layer is located above the optical waveguide layer, and its cross section is T-shaped or concave-shaped, and the width of the vertical part of the T-shaped second stop layer is greater than the width of the optical waveguide layer, or the width of the concave-shaped second stop layer is greater than the width of the optical waveguide layer; wherein the fourth thickness H4 is 1 nm to 100 nm; S1025, performing a window opening process on the second stop layer and the second oxide layer by a regional etching method, so that the second stop layer forms a first isolation layer having a thickness less than the fourth thickness H4 on the optical waveguide layer, and a second isolation layer surrounding the first isolation layer and having an inverted L-shaped cross section; S1027, using a first thin film deposition process to deposit a phase change material onto the surface of the first isolation layer by a physical vapor deposition method, so as to form a phase change material layer of a preset thickness in a window formed by the first isolation layer and the second isolation layer around it; the preset thickness is less than or equal to the difference between the fourth thickness H4 and the thickness of the first isolation layer; S1029, using a second thin film deposition process to deposit an oxide layer of the same material as that in step S1013 onto the phase change material layer to cover it, thereby obtaining a first protective layer of a sixth thickness.
2. A method for preparing an optical waveguide according to claim 1, characterized in that: The fourth thickness H4 is obtained in advance through simulation.
3. A method for preparing an optical waveguide according to claim 1, characterized in that: The first isolation layer extends along the length direction of the waveguide by a length of 1 μm to 10 μm.
4. A method for preparing an optical waveguide according to claim 1, characterized in that: The thickness of the phase change material layer is 1 nm to 1 μm; and / or the length of the phase change material layer extending along the length direction of the waveguide is 1 μm to 10 μm.
5. A method for preparing an optical waveguide according to any one of claims 1 to 4, characterized in that: The phase change material layer is made of super lattice material.
6. A method for preparing an optical waveguide according to any one of claims 1 to 4, characterized in that: The phase-change material layer is formed of a chalcogenide containing antimony or selenium, or the phase-change material layer contains the chalcogenide, wherein the chalcogenide includes Sb2Se3 or SbSe, Sb2S3 or SbS, Ge2Sb2Se4Te.
7. A method for preparing an optical waveguide according to any one of claims 1 to 4, characterized in that: The phase change material includes a compound or alloy containing an element combination of germanium, antimony, selenium, and vanadium oxide, or a mixture of the compounds; the compound includes NbOx, GeTe, GeSb, GaSb, AgInSbTe, InSb, InSbTe, InSe, SbTe, TeGeSbS, AgSbSe, SbSe, GeSbMnSn, AgSbTe, AuSbTe, and AlSb.
8. A method for preparing an optical waveguide according to any one of claims 1 to 4, characterized in that: The second stop layer is made of one or both of Si3N4 and TiN.
9. An optical waveguide prepared according to the method for preparing an optical waveguide according to any one of claims 1 to 8, characterized in that: include: an optical waveguide layer, a modulation layer located on the optical waveguide layer, a first isolation layer is arranged between the optical waveguide layer and the modulation layer, the modulation layer is covered with a first protective layer, and further comprises: a second isolation layer surrounding the first isolation layer and the modulation layer and having an inverted L-shaped cross section, and a second protective layer surrounding the first protective layer, the second isolation layer and the optical waveguide layer; wherein the modulation layer is wrapped in a closed cavity formed by the first protective layer, the first isolation layer and the second isolation layer, and the modulation layer is a phase change material layer or the modulation layer includes a phase change material layer; The thickness of the first isolation layer is less than a fourth thickness H4, and the fourth thickness is 1 nm to 100 nm.
10. The optical waveguide according to claim 9, characterized in that The first isolation layer and the second isolation layer are combined to form a second groove with an opening facing the first protective layer, and a height from a bottom of the second groove to a top opening is greater than or equal to a thickness of the modulation layer.
Citation Information
Patent Citations
Mid-infrared electro-optical modulator based on black phosphorus fluoride waveguide
CN105807454A
Preparation method of electro-optical crystal film, electro-optical crystal film and electro-optical modulator
CN111965857A
Preparation method of waveguide structure composite substrate, composite substrate and photoelectric crystal film
CN112379480A
Non-vertical indirect electric heating device compatible with silicon optical integration process
CN115308851A
Optical waveguide and optical device
CN115917408A