Method for etching back photoresist

By forming a dense isolation layer in the photoresist back-etching process and using hydrogen to remove the photoresist layer, the problems of abnormal photolithography line width and incomplete removal of silicon nitride layer in the photoresist etching process are solved, and more stable lithography process.

CN119008530APending Publication Date: 2024-11-22CHONGQING XINLIAN MICROELECTRONICS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411078027.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the photoresist etching process, the problem of abnormal photolithography line width and the inability of phosphoric acid to completely remove the silicon nitride layer, which affects the stability and accuracy in the subsequent process.

Method used

The N-well and PMOS devices are formed on the substrate, covering the protective layer and isolation layer, making the top surface height of the PMOS and NMOS devices the same through the photoresist back-etching process, and using hydrogen to remove light when the photoresist layer is remade Resist layer avoids oxidation thickening and incomplete cleaning problems caused by ashing process.

Benefits of technology

The stable lithography line width and complete silicon nitride layer removal are achieved, which reduces the impact of photoresist reproduction on the surface condition of the protective layer and improves the stability of subsequent lithography processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008530A_ABST
    Figure CN119008530A_ABST
Patent Text Reader

Abstract

According to the photoresist back-etching method provided by the invention, the isolation layer is formed on the protection layer before the photoresist layer is formed and is used for isolating the protection layer from the photoresist layer, so that a poisoning effect generated by silicon nitride and photoresist is avoided, and short-second oxygen treatment is not needed to improve the poisoning effect of the photoresist. Meanwhile, the isolating layer provided by the invention is high in density and stable in process, and a more stable photoetching line width can be obtained in a subsequent photoetching process. Furthermore, when the photoresist layer needs to be remanufactured, plasma taking hydrogen as a main part is adopted to remove the photoresist layer, so that the surface oxidation amount is reduced, and the problems that the photoresist is removed by adopting an ashing process, so that the protection layer is oxidized and thickened again, the subsequent photoetching line width is abnormal, the protection layer cannot be completely removed by phosphoric acid, and the production efficiency is improved are solved. The isolation layer formed on the protection layer can reduce the influence of photoresist remaking on the surface condition of the protection layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to a photoresist back-etching method. Background Art

[0002] The photoresist etch back process (PREB) is mainly used to solve the problem of excessive N / P loading (NMOS area and PMOS area loading) caused by making germanium silicon trenches in p-MOS devices in processes below 40nm. The photoresist etch back process includes: forming a layer of silicon nitride film after forming the second sidewall of the NMOS device and the PMOS device. Because photoresist is to be applied later, in order to avoid the poisoning effect of the silicon nitride film and the photoresist, an oxidation treatment (O 2 Treatment) forms a silicon oxide film layer on the surface of the silicon nitride film. However, the density of the formed silicon oxide film layer is poor, and the process is unstable. If photoresist rework (PR Rework) is required due to process requirements, an ashing process is usually used to remove the photoresist. The ashing process generates oxygen plasma, and the oxygen free radicals in the plasma burn the organic components of the photoresist. Therefore, the ashing process will cause the silicon nitride layer to oxidize and thicken again. Since the thickness of the oxide layer after the photoresist layer is reworked is different from the initial oxide layer thickness, the actual photolithography conditions will also be different. If the original photolithography parameters are used for exposure, the photolithography line width will be abnormal. In addition, before phosphoric acid is used to remove the silicon nitride layer, diluted hydrofluoric acid (DHF) will be used to remove the surface oxide layer, but after the photoresist layer is reworked, the oxide layer will thicken, and the original diluted hydrofluoric acid (DHF) will not completely clean the oxide layer, resulting in the final phosphoric acid being unable to completely remove the silicon nitride layer. Therefore, the subsequent problems of abnormal photolithography line width and phosphoric acid being unable to completely remove the silicon nitride layer are caused. Summary of the invention

[0003] The object of the present invention is to provide a method for photoresist back etching to solve the problem of abnormal photolithography line width and the inability of phosphoric acid to completely remove the silicon nitride layer.

[0004] In order to solve the above technical problems, the present invention provides a method for photoresist back etching, comprising:

[0005] Providing a substrate, the substrate comprising an N-well and a PMOS device located on the N-well, and a P-well and an NMOS device located on the P-well, wherein a top surface of the PMOS device is lower than a top surface of the NMOS device;

[0006] forming a protection layer, wherein the protection layer covers the PMOS device and the NMOS device;

[0007] forming an isolation layer, wherein the isolation layer covers the protective layer;

[0008] forming a photoresist layer, wherein the photoresist layer covers the isolation layer, and the isolation layer is used to isolate the protective layer and the photoresist layer;

[0009] A photoresist etch-back process is performed to make the top surface of the PMOS device and the top surface of the NMOS device have the same height.

[0010] Optionally, after the photoresist layer is formed, when the photoresist layer needs to be remade, hydrogen is used to remove the photoresist layer.

[0011] Optionally, after removing the photoresist layer, a photoresist layer is formed again on the isolation layer.

[0012] Optionally, after the photoresist etch-back process, a first wet cleaning process is used to remove the isolation layer, and a second wet cleaning process is used to remove the protection layer.

[0013] Optionally, the solution of the first wet cleaning process includes diluted hydrofluoric acid, and the solution of the second wet cleaning process includes phosphoric acid.

[0014] Optionally, the material of the protective layer is silicon nitride.

[0015] Optionally, the material of the isolation layer is silicon oxide.

[0016] Optionally, the isolation layer is formed by a chemical vapor deposition process, a thermal oxidation process or a furnace tube diffusion process.

[0017] Optionally, the PMOS device includes a gate and a dielectric layer located on the gate and side walls on both sides of the gate, and the NMOS device includes a gate and a dielectric layer located on the gate and side walls on both sides of the gate, and the protective layer covers the side walls of the PMOS device and the side walls of the NMOS device.

[0018] Optionally, before forming the protective layer, the method further includes:

[0019] Forming a silicon germanium layer and a metal silicide layer, wherein the silicon germanium layer is located in the N well on both sides of the PMOS device, and the metal silicide layer is located on the silicon germanium layer;

[0020] A stress dielectric layer is formed, the stress dielectric layer covers the NMOS device, and a SMT process is performed to transfer the stress of the stress dielectric layer into the NMOS device.

[0021] In the photoresist back-etching method provided by the present invention, an N well and a PMOS device located on the N well and a P well and an NMOS device located on the P well are formed on the substrate, and the top surface of the PMOS device is lower than the top surface of the NMOS device, resulting in excessive loads on the NMOS device and the PMOS device. By performing the photoresist back-etching process, the top surface of the PMOS device and the top surface of the NMOS device are made to have the same height, thereby solving the problem of excessive loads on the NMOS device and the PMOS device. Before performing the photoresist back-etching process, a dense isolation layer is formed on the protective layer to isolate the protective layer and the photoresist layer, thereby avoiding the poisoning effect of silicon nitride and the photoresist, and there is no need to perform short-second oxygen treatment to improve the photoresist poisoning effect. At the same time, the isolation layer provided by the present invention has high density and stable process, and a more stable photolithography line width can be obtained in the subsequent photolithography process. Furthermore, when the photoresist layer needs to be remade, a plasma mainly composed of hydrogen is used to remove the photoresist layer to reduce the amount of surface oxidation and avoid using an ashing process to remove the photoresist, which may cause the protective layer to become oxidized and thickened again, thereby causing abnormal subsequent photolithography line width and the inability of phosphoric acid to completely remove the protective layer. That is, the isolation layer formed on the protective layer of the present invention can reduce the impact of photoresist remaking on the surface condition of the protective layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Those skilled in the art will appreciate that the accompanying drawings are provided for a better understanding of the present invention and do not constitute any limitation on the scope of the present invention.

[0023] Figure 1 It is a flow chart of a method for photoresist back etching according to an embodiment of the present invention.

[0024] Figures 2 to 7 It is a schematic diagram of the structure corresponding to the steps of the photoresist back etching method according to an embodiment of the present invention.

[0025] In the attached figure:

[0026] 10-substrate; 11-deep trench isolation structure; 12a-P well; 12b-N well; 13-NMOS device; 13a-gate oxide layer; 13b-hafnium oxide layer; 13c-barrier layer; 13d-gate; 13e-first dielectric layer; 13f-second dielectric layer; 13g-first sidewall; 13h-second sidewall; 14-PMOS device; 15-silicon germanium layer; 16-metal silicide layer; 17-protective layer; 18-isolation layer; 19-photoresist layer. DETAILED DESCRIPTION

[0027] In order to make the purpose, advantages and features of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and are not drawn to scale, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In addition, the structure shown in the drawings is often a part of the actual structure. In particular, the emphasis of each drawing is different, and sometimes different scales are used.

[0028] As used in the present invention, the singular forms "one", "an" and "the" include plural objects, the term "or" is usually used to include the meaning of "and / or", the term "several" is usually used to include the meaning of "at least one", and the term "at least two" is usually used to include the meaning of "two or more". In addition, the terms "first", "second" and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Therefore, the features defined as "first", "second" and "third" can explicitly or implicitly include one or at least two of the features. In addition, as used in the present invention, an element is arranged on another element, which usually only indicates that there is a connection, coupling, matching or transmission relationship between the two elements, and the connection, coupling, matching or transmission between the two elements can be direct or indirect through an intermediate element, and cannot be understood as indicating or implying the spatial position relationship between the two elements, that is, an element can be in any orientation such as inside, outside, above, below or on one side of another element, unless the content clearly indicates otherwise. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0029] Figure 1 FIG. 1 is a flow chart of a method for photoresist back etching according to an embodiment of the present invention. Figure 1 As shown, this embodiment provides a method for photoresist etching back, including:

[0030] Step S10, providing a substrate, the substrate comprising an N well and a PMOS device located on the N well, and a P well and an NMOS device located on the P well, wherein a top surface of the PMOS device is lower than a top surface of the NMOS device;

[0031] Step S20, forming a protection layer, wherein the protection layer covers the PMOS device and the NMOS device;

[0032] Step S30, forming an isolation layer, wherein the isolation layer covers the protection layer;

[0033] Step S40, forming a photoresist layer, wherein the photoresist layer covers the isolation layer, and the isolation layer is used to isolate the protective layer and the photoresist layer;

[0034] Step S50 , performing a photoresist etch-back process to make the top surface of the PMOS device and the top surface of the NMOS device have the same height.

[0035] Figures 2 to 7 1 is a schematic diagram of the structure corresponding to the steps of the photoresist back-etching method of the embodiment of the present invention. In order to make the above-mentioned purpose, features and beneficial effects of the present invention more obvious and easy to understand, the following is a schematic diagram of the structure corresponding to the steps of the photoresist back-etching method of the embodiment of the present invention. Figures 2 to 7 The specific embodiments of the present invention are described in detail.

[0036] like Figure 2 As shown, a substrate 10 is provided, and the substrate 10 may be single crystal silicon or polycrystalline silicon, or may be a semiconductor material such as silicon, germanium, silicon germanium, gallium arsenide, or a composite structure such as silicon on insulator. Those skilled in the art may select the type of the semiconductor substrate according to the semiconductor device formed on the semiconductor substrate, and therefore the type of the semiconductor substrate shall not limit the protection scope of the present invention.

[0037] Please continue to refer to Figure 2 , the substrate 10 includes a P well 12a and an N well 12b, and a deep trench isolation structure 11 for isolating the P well 12a and the N well 12b. An NMOS device 13 is formed on the P well 12a, and a PMOS device 14 is formed on the N well 12b. The NMOS device 13 includes a gate dielectric layer, a barrier layer 13c, a gate 13d, a first dielectric layer 13e, and a second dielectric layer 13f stacked in sequence from bottom to top. The material of the gate dielectric layer includes one or a combination of an oxide layer and a hafnium oxide layer. In this embodiment, the material of the gate dielectric layer includes a gate oxide layer 13a and a hafnium oxide layer 13b. The gate oxide layer 13a can be formed by a thermal oxidation process, and the hafnium oxide layer 13b can be formed by an atomic layer deposition process. The material of the hafnium oxide layer 13b can effectively improve the gate leakage current due to its high dielectric constant. In order to prevent the metal ions hafnium ions in the hafnium oxide layer 13b from entering the gate 13d, a barrier layer 13c is formed on the hafnium oxide layer 13b, and the material of the barrier layer 13c is, for example, titanium nitride. The material of the gate 13d is, for example, polysilicon, the material of the first dielectric layer 13e is, for example, silicon nitride, and the material of the second dielectric layer 13f is, for example, silicon oxide. The gate 13d, the first dielectric layer 13e, and the second dielectric layer 13f can all be formed by a chemical vapor deposition process.

[0038] The NMOS device 13 also includes a first sidewall 13g and a second sidewall 13h located on both sides of the gate 13d. The material of the first sidewall 13g is, for example, silicon nitride, and the material of the second sidewall 13h is, for example, silicon nitride. The materials of the first sidewall 13g and the second sidewall 13h are the same but are formed in different processes. The PMOS device 14 also includes a gate dielectric layer, a barrier layer, a gate, a first dielectric layer, a second dielectric layer, and a first sidewall and a second sidewall located on both sides of the gate, which are stacked in sequence from bottom to top. The materials and functions of each layer of the PMOS device 14 are the same as those of each layer of the NMOS device 13, and are not repeated here. It is worth emphasizing that a germanium silicon layer 15 and a metal silicide layer 16 on the germanium silicon layer 15 are also formed in the N well 12b on both sides of the PMOS device 14. The germanium silicon layer 15 is formed by an epitaxial growth process. The germanium silicon layer 15 has compressive stress, and the germanium silicon layer 15 can improve the mobility of channel holes. The formation of the metal silicide layer 16 on the silicon germanium layer 15 includes: first forming a metal silicide blocking layer (Salicide Block, SAB), the metal silicide blocking layer covers the PMOS device 14 and the NMOS device 13 and exposes the silicon germanium layer 15, and then forming the metal silicide layer 16 on the exposed silicon germanium layer 15. After the metal silicide layer 16 is formed, the remaining metal silicide blocking layer is removed. Since the silicon germanium layer 15 and the metal silicide layer 16 are formed on both sides of the PMOS device 14, the top surface of the PMOS device is lower than the top surface of the NMOS device, resulting in the problem of excessive N / P Loading (the load of the NMOS device and the PMOS device).

[0039] After forming the metal silicide layer 16, a stress memorization technique (SMT) is also performed to provide tensile stress in the gate of the NMOS device 13. Specifically, a stress dielectric layer is first formed, the stress dielectric layer covers the NMOS device 13, and then a heat treatment process is performed to transfer the stress of the stress dielectric layer to the gate of the NMOS device 13 to meet the electron mobility of the NMOS device.

[0040] like Figure 3As shown, a protective layer 17 is formed, and the protective layer 17 covers the NMOS device 13 and the PMOS device 14. Specifically, the protective layer 17 covers the second dielectric layer 13f and the second sidewall 13h of the NMOS device 13 and the second dielectric layer and the second sidewall of the PMOS device 14, as well as the surface of the substrate 10 and the deep trench isolation structure 11 located between the NMOS device 13 and the PMOS device 14. The material of the protective layer 17 is silicon nitride. It is formed by a chemical vapor deposition process. The substrate 10 includes a core area and an input-output area, and the core area and the input-output area both include the NMOS device 13 and the PMOS device 14. When the NMOS device 13 and the PMOS device 14 in the input-output area are etched, the protective layer 17 is used to protect the NMOS device 13 and the PMOS device 14 in the core area from being etched.

[0041] like Figure 4 As shown, an isolation layer 18 is formed, and the isolation layer 18 covers the protective layer 17. The material of the isolation layer 18 is silicon oxide. The isolation layer 18 is formed by a chemical vapor deposition process, a thermal oxidation process or a furnace tube diffusion process. The thickness of the isolation layer 18 is, for example, 20 angstroms to 50 angstroms. Since a photoresist is formed as a mask in the etching process, the photoresist and silicon nitride produce a poisoning effect, that is, the photoresist and the protective layer 17 produce a poisoning effect. In the prior art, an oxygen treatment process (O 2 The silicon oxide layer is formed on the surface of the silicon nitride layer by the oxygen treatment process to prevent the photoresist and silicon nitride from having a poisoning effect. However, the silicon oxide film formed by the oxygen treatment process has poor density and the process is unstable. The isolation layer 18 formed by the chemical vapor deposition process, thermal oxidation process or furnace diffusion process in this embodiment has high density and stable process, which can ensure the stability of the lithography line width in the subsequent photolithography process.

[0042] like Figure 5 As shown, a photoresist layer 19 is formed, and the photoresist layer 19 covers the isolation layer 18 . The isolation layer 18 is used to isolate the protection layer 17 from the photoresist layer 19 .

[0043] In some embodiments, the photoresist layer 19 needs to be remade. For example, when the exposure result is not good or a defect is detected, the photoresist layer 19 needs to be remade. Before the photoresist layer 19 is remade, the original photoresist layer 19 needs to be removed first. In this embodiment, a plasma mainly composed of hydrogen is used to remove the photoresist layer 19 to reduce the surface oxidation amount of the protective layer 17. In the prior art, when the photoresist layer 19 is remade, an ashing process is usually used to remove the photoresist layer 19. Oxygen plasma is generated in the ashing process, and the oxygen free radicals in the plasma burn the organic components of the photoresist. Therefore, the ashing process will cause the silicon nitride layer to oxidize and thicken again. Since the thickness of the oxide layer after the photoresist layer in the prior art is different from the initial oxide layer thickness, the actual lithography conditions will also be different. If the original lithography parameters are used for exposure, the lithography line width will be abnormal. And before phosphoric acid removes the silicon nitride layer, diluted hydrofluoric acid (DHF) will be used to remove the surface oxide layer, but the oxide layer will thicken after the photoresist layer is remade in the prior art, and the original diluted hydrofluoric acid (DHF) does not clean the oxide layer completely, resulting in the final phosphoric acid being unable to completely remove the silicon nitride layer. And the isolation layer 18 formed by chemical vapor deposition process, thermal oxidation process or furnace tube diffusion process in the present embodiment has high density and stable process, and when the photoresist is remade, a plasma mainly based on hydrogen is used to remove the photoresist layer 19 to reduce the surface oxidation amount of the protective layer 17. After the photoresist layer 19 is removed, the thickness of the isolation layer 18 will not change, and after the subsequent photoresist layer is remade, a stable lithography line width can be obtained by using the original photolithography process. The isolation layer 18 formed by chemical vapor deposition process, thermal oxidation process or furnace tube diffusion process in the present embodiment can reduce the impact of the photoresist layer remaking on the surface conditions of the protective layer 17 and the isolation layer 18.

[0044] After the photoresist layer 19 is removed, a photoresist layer 19 is formed again on the isolation layer 18 .

[0045] like Figure 6 As shown, a photoresist back-etching process is performed to back-etch the photoresist layer 19 and the portion of the PMOS device and the NMOS device below the photoresist layer 19 to an ideal thickness, so that the top surface of the PMOS device and the top surface of the NMOS device are at the same height, so as to solve the problem of excessive P / N load caused by making a germanium silicon trench in the PMOS device in the process below 40nm. The ideal thickness is lower than the initial height of the PMOS device and also lower than the initial height of the NMOS device. The portion of the PMOS device and the portion of the NMOS device that are higher than the ideal thickness are removed, so that the PMOS device and the NMOS device have the same height.

[0046] like Figure 7As shown, after the photoresist etch-back process, the remaining photoresist layer is removed. Then, the isolation layer 18 is removed by a first wet cleaning process, and the protection layer 17 is removed by a second wet cleaning process. The solution of the first wet cleaning process includes diluted hydrofluoric acid (DHF), and the solution of the second wet cleaning process includes phosphoric acid.

[0047] In other embodiments, the method of using a chemical vapor deposition process to form a highly dense and process-stable silicon oxide layer on a silicon nitride layer to avoid the poisoning effect between silicon nitride and photoresist can be applied to all processes of photoresist coating and etching on a silicon nitride layer, and this embodiment is not limited to this.

[0048] From the above, it can be seen that in the method for photoresist back-etching provided in the embodiment of the present invention, an N well and a PMOS device located on the N well and a P well and an NMOS device located on the P well are formed on the substrate, a germanium silicon layer is formed in the N well on both sides of the PMOS device, a metal silicide layer is formed on the germanium silicon layer, and the top surface of the PMOS device is lower than the top surface of the NMOS device, resulting in excessive loads on the NMOS device and the PMOS device. By performing a photoresist back-etching process so that the top surface of the PMOS device and the top surface of the NMOS device have the same height, the problem of excessive loads on the NMOS device and the PMOS device is solved. Before performing the photoresist back-etching process, a dense isolation layer is formed on the protective layer to isolate the protective layer and the photoresist layer, thereby avoiding the poisoning effect of silicon nitride and the photoresist, and there is no need to perform a short-second oxygen treatment to improve the photoresist poisoning effect. At the same time, the isolation layer provided by the present invention has high density and stable process, and a more stable photolithography line width can be obtained in the subsequent photolithography process. Furthermore, when the photoresist layer needs to be remade, a plasma mainly composed of hydrogen is used to remove the photoresist layer to reduce the amount of surface oxidation and avoid using an ashing process to remove the photoresist, which may cause the protective layer to become oxidized and thickened again, thereby causing abnormal subsequent photolithography line width and the inability of phosphoric acid to completely remove the protective layer. That is, the isolation layer formed on the protective layer of the present invention can reduce the impact of photoresist remaking on the surface condition of the protective layer.

[0049] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other. In addition, the different parts between the various embodiments can also be used in combination with each other, and the present invention is not limited to this.

[0050] In addition, it should be recognized that although the present invention has been disclosed as a preferred embodiment, the above embodiment is not intended to limit the present invention. For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still belongs to the scope of protection of the technical solution of the present invention.

Claims

1. A method for photoresist back etching, characterized in that: include: Providing a substrate, the substrate comprising an N-well and a PMOS device located on the N-well, and a P-well and an NMOS device located on the P-well, wherein a top surface of the PMOS device is lower than a top surface of the NMOS device; forming a protection layer, wherein the protection layer covers the PMOS device and the NMOS device; forming an isolation layer, wherein the isolation layer covers the protective layer; forming a photoresist layer, wherein the photoresist layer covers the isolation layer, and the isolation layer is used to isolate the protective layer and the photoresist layer; A photoresist etch-back process is performed to make the top surface of the PMOS device and the top surface of the NMOS device have the same height.

2. The method for photoresist back etching according to claim 1, characterized in that: After the photoresist layer is formed, when the photoresist layer needs to be remade, hydrogen is used to remove the photoresist layer.

3. The method for photoresist back etching according to claim 2, characterized in that: After removing the photoresist layer, a photoresist layer is formed again on the isolation layer.

4. The method for photoresist back etching according to claim 1, characterized in that: After the photoresist etch-back process, a first wet cleaning process is used to remove the isolation layer, and a second wet cleaning process is used to remove the protection layer.

5. The method for photoresist back etching according to claim 4, characterized in that: The solution of the first wet cleaning process includes diluted hydrofluoric acid, and the solution of the second wet cleaning process includes phosphoric acid.

6. The method for photoresist back etching according to claim 1, characterized in that: The material of the protection layer is silicon nitride.

7. The method for photoresist back etching according to claim 1, characterized in that: The material of the isolation layer is silicon oxide.

8. The method for photoresist back etching according to claim 1 or 7, characterized in that: The isolation layer is formed by a chemical vapor deposition process, a thermal oxidation process or a furnace diffusion process.

9. The method for photoresist back etching according to claim 1, characterized in that: The PMOS device includes a gate, a dielectric layer located on the gate, and side walls on both sides of the gate; the NMOS device includes a gate, a dielectric layer located on the gate, and side walls on both sides of the gate; the protective layer covers the side walls of the PMOS device and the side walls of the NMOS device.

10. The method for photoresist back etching according to claim 1, characterized in that: Before forming the protective layer, it also includes: Forming a silicon germanium layer and a metal silicide layer, wherein the silicon germanium layer is located in the N well on both sides of the PMOS device, and the metal silicide layer is located on the silicon germanium layer; A stress dielectric layer is formed, the stress dielectric layer covers the NMOS device, and a SMT process is performed to transfer the stress of the stress dielectric layer into the NMOS device.

Citation Information

Cited By

  • Semiconductor device and preparation method thereof

    CN119815901A

  • A semiconductor device and a method of fabricating the same

    CN119815901B