Trans-type electric control dimming film and preparation method and application thereof

Through the mixing system of double epoxy liquid crystal monomer and single epoxy liquid crystal monomer and special photoinitiator, the problems of long curing time and low mechanical strength of the trans electronically controlled dimming film are solved, and high mechanical performance is achieved And the rapidly prepared trans electronically controlled dimming film, suitable for automotive glass and lenses and other scenarios.

CN118884745APending Publication Date: 2024-11-01UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105847.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing trans electronically controlled dimming film has a long curing time and low mechanical strength, making it difficult to meet the needs of large-scale production and use.

Method used

Using a hybrid system of double epoxy liquid crystal monomer and single epoxy liquid crystal monomer, combined with a special cationic photoinitiator, the polymerization time is shortened and the polymer content is increased through ultraviolet curing technology to form a trans form with high mechanical properties. Electrically controlled dimming film.

Benefits of technology

It significantly shortens the preparation time of the trans electronically controlled dimming film, improves its mechanical strength and mechanical properties, and is suitable for application scenarios such as automotive glass and lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118884745A_ABST
    Figure CN118884745A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of liquid crystal materials, and discloses a trans-type electric control dimming film and a preparation method and application thereof. The trans-type electric control dimming film comprises a first transparent conductive film, a polymer liquid crystal composite material layer and a second transparent conductive film which are sequentially stacked in the thickness direction. The polymer liquid crystal composite material comprises the following raw materials: a double-epoxy liquid crystal monomer and / or a single-epoxy liquid crystal monomer, negative liquid crystal and a cationic photoinitiator, the polymer liquid crystal composite material comprises the following components in parts by weight: 2-40 parts of a double-epoxy liquid crystal monomer, 0-24 parts of a single-epoxy liquid crystal monomer, 56-94 parts of negative liquid crystal and 3-5 parts of a cationic photoinitiator. Through the combination of a mixed system of the double epoxy liquid crystal monomer and the single epoxy liquid crystal monomer and the special photoinitiator, the mechanical property of the polymer liquid crystal composite material is improved, and meanwhile, the content and the polymerization speed of the polymer in the trans-electronic control dimming film are improved; the obtained trans-type electric control dimming film has good electro-optical performance and mechanical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of liquid crystal materials, and in particular to a reverse electrically controlled dimming film and a preparation method and application thereof. Background Art

[0002] The electrically controlled dimming film can be switched between a transparent state and a light scattering state by adjusting the voltage. It has been widely used in the fields of building exterior walls, automobile glass, etc. There are two types of electrically controlled dimming films: formal electrically controlled dimming film and reverse electrically controlled dimming film. The formal electrically controlled dimming film currently used in large-scale production is a non-transparent state with a light scattering state under normal conditions, and a transparent state with a light transmitting state when powered on. However, in most usage scenarios, such as automobile glass and goggles, the use time of the transparent state is much longer than that of the non-transparent state. In these application scenarios, the reverse electrically controlled dimming film, which is transparent under normal conditions and a non-transparent state with a light scattering state when powered on, is more suitable than the formal electrically controlled dimming film.

[0003] At present, the reverse electric dimming film is mainly based on the polymerization of negative liquid crystal and acrylate-based polymer system. It induces free radical polymerization through ultraviolet light irradiation, and a relatively fine polymer network structure is formed inside. However, when the polymer content is low, the reverse electric dimming film obtained by polymerization of negative liquid crystal and acrylate-based polymer system has a small number of vertical fibers, a large domain density, and thin fibers in the network structure of the negative liquid crystal and acrylate-based polymer system, and its mechanical properties such as tensile strength and bending resistance are poor; as the polymer content increases, the mechanical properties also improve, but when the mechanical properties are improved to a certain extent or reach the standard for large-scale preparation and use, due to the excessive polymer content in the system, the vertical fiber domain density in the polymer network is small, and the polymer network has a strong anchoring effect on the liquid crystal small molecules. When power is applied, the liquid crystal small molecules cannot be driven by the electric field, and the sample cannot switch between the light transmission state and the light scattering state, resulting in the reverse electric dimming film cannot be used normally.

[0004] Epoxy resin has high corrosion resistance, good adhesion and excellent mechanical properties, and has been widely used in semiconductor materials, protective coatings and other places. The polymer network used as the electrically controlled dimming film after polymerization is expected to improve the mechanical properties of the reverse electrically controlled dimming film. At present, the methods for preparing polymers by negative liquid crystal and epoxy resin mainly include thermal curing and photocuring. However, both curing methods have the problem of long polymerization time. For example, photoinitiator 6976 is added to the mixture of negative liquid crystal and epoxy monomer E6M, and a liquid crystal / epoxy monomer mixture material with excellent mechanical properties is prepared by ultraviolet light curing. The polymerization time reaches 2 hours, and the content of E6M in the polymer is only up to 10wt%. On the one hand, the long curing time leads to low production efficiency; on the other hand, due to the low content of epoxy monomer, the mechanical strength of the reverse electrically controlled dimming film is still low. Summary of the invention

[0005] The present application provides a reverse electric-controlled dimming film and a preparation method and application thereof, aiming to solve the problems of long curing time and low mechanical strength of the existing epoxy resin-based reverse electric-controlled dimming film.

[0006] In order to achieve the above objectives, the present application adopts the following technical solutions.

[0007] In a first aspect of the present application, a reverse electrically controlled dimming film is provided, comprising a first transparent conductive film, a polymer liquid crystal composite material layer, and a second transparent conductive film which are sequentially stacked in a thickness direction;

[0008] The raw materials of the polymer liquid crystal composite material include diepoxy liquid crystal monomers and / or monoepoxy liquid crystal monomers, negative liquid crystals and cationic photoinitiators;

[0009] The polymer liquid crystal composite material comprises, by weight, 2 to 40 parts of diepoxy liquid crystal monomers, 0 to 24 parts of monoepoxy liquid crystal monomers, 56 to 94 parts of negative liquid crystals, and 3 to 5 parts of cationic photoinitiators.

[0010] In some embodiments, the mass ratio of the diepoxy liquid crystalline monomer to the monoepoxy liquid crystalline monomer is (5:0) to (1:4).

[0011] In some embodiments, the cationic photoinitiator includes photoinitiator 1173, and photoinitiator 1176 or photoinitiator 6976.

[0012] In some embodiments, the cationic photoinitiator includes photoinitiator 1173 and photoinitiator 1176, and the mass ratio of the two is 1:1.

[0013] In some embodiments, the negative liquid crystal is a negative nematic liquid crystal, which has a crystallization point of less than -40°C, a clearing point of more than 100°C, a birefringence of more than 0.1, a dielectric anisotropy of less than -0.5, and a viscosity of less than 200 mPa.s.

[0014] In some embodiments, the chemical structure of the diepoxy liquid crystal monomer is:

[0015]

[0016] Wherein m = 1 to 9; n = 1 to 9;

[0017] The chemical structure of the monoepoxy liquid crystal monomer is:

[0018]

[0019] Wherein m=1~9.

[0020] The second aspect of the present application provides a method for preparing the above-mentioned reverse electrically controlled dimming film, comprising:

[0021] The raw materials of the polymer liquid crystal composite material are mixed evenly according to a proportion, added between the first transparent conductive film and the second transparent conductive film, and cured by ultraviolet radiation to obtain a reverse electric control dimming film.

[0022] In some embodiments, the distance between the first transparent conductive film and the second transparent conductive film is 8-40 μm.

[0023] In some embodiments, the UV curing temperature is -20°C to 100°C, the time is 1 to 20 minutes, and the light intensity is 10 to 300 mW / cm 2 .

[0024] The third aspect of the present application provides the use of the above-mentioned reverse electrically controlled dimming film in automobile glass or lenses.

[0025] Compared with the prior art, the beneficial effects of this application are:

[0026] The present application increases the mechanical properties of the polymer liquid crystal composite material by using a mixed system of diepoxy liquid crystal monomers and monoepoxy liquid crystal monomers and a special photoinitiator combination, while also increasing the polymer content in the trans-electrically controlled dimming film. The resulting trans-electrically controlled dimming film has good electro-optical and mechanical properties, high mechanical strength, and good bending and stretching resistance.

[0027] The present application greatly improves the polymerization speed of the diepoxy liquid crystal monomer and the monoepoxy liquid crystal monomer through a special photoinitiator combination, shortens the preparation time of the reverse electrically controlled dimming film, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 1;

[0030] Figure 2 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 1;

[0031] Figure 3 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 2;

[0032] Figure 4 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 2;

[0033] Figure 5 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 3;

[0034] Figure 6 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 3;

[0035] Figure 7 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 4;

[0036] Figure 8 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 4;

[0037] Fig. 9 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 5;

[0038] Fig.10 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 5;

[0039] Fig.11 is a voltage-transmittance curve of the reverse electric-controlled dimming film of Example 6;

[0040] Fig.12 Graph showing the threshold voltage and saturation voltage of the reverse electrically controlled dimming film of Example 6;

[0041] Fig.13 The voltage-transmittance curve of the reverse electric-controlled dimming film of comparative example 1;

[0042] Fig.14 The voltage-transmittance curve of the reverse electric-controlled dimming film of comparative example 2;

[0043] Fig.15 This is a diagram showing the mechanical tensile test results of the reverse electrically controlled dimming film of the present application;

[0044] Fig.16 is a scanning electron microscope image of the reverse electrically controlled dimming film of Example 1;

[0045] Fig.17 This is a scanning electron microscope image of the reverse electrically controlled dimming film of Example 2;

[0046] Fig.18 This is a scanning electron microscope image of the reverse electrically controlled dimming film of Example 5. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0048] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0049] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0050] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0051] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0052] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0053] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0054] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0055] In a first aspect, the present application provides a reverse electrically controlled dimming film, comprising a first transparent conductive film, a polymer liquid crystal composite material layer and a second transparent conductive film stacked in sequence along the thickness direction; wherein the first transparent conductive layer and the second transparent conductive layer are preferably ITO.

[0056] The raw materials of the polymer liquid crystal composite material include diepoxy liquid crystal monomers and / or monoepoxy liquid crystal monomers, negative liquid crystals and cationic photoinitiators;

[0057] The polymer liquid crystal composite material comprises, by weight, 2 to 40 parts of diepoxy liquid crystal monomers, 0 to 24 parts of monoepoxy liquid crystal monomers, 56 to 94 parts of negative liquid crystals, and 3 to 5 parts of cationic photoinitiators.

[0058] The present application increases the mechanical properties of the polymer liquid crystal composite material by using a mixed system of a diepoxy liquid crystal monomer and a monoepoxy liquid crystal monomer. Unlike the prior art which uses acrylate monomers to induce polymerization via a free radical photoinitiator, the free energy required for the polymerization of epoxy resin in the present application is relatively high, and it is difficult for a free radical photoinitiator to promote the polymerization reaction, so the present application uses a cationic initiator to initiate the polymerization reaction.

[0059] In the present application, the ends of the diepoxy liquid crystalline monomer and the monoepoxy liquid crystalline monomer have epoxy groups, wherein the chemical structure of the diepoxy liquid crystalline monomer is:

[0060]

[0061] Wherein m = 1 to 9; n = 1 to 9;

[0062] The chemical structure of the monoepoxy liquid crystal monomer is:

[0063]

[0064] Wherein m=1~9.

[0065] In the present application, the polymer monomer adopts a mixture of a diepoxy liquid crystal monomer and a monoepoxy liquid crystal monomer. In the embodiment of the present application, the diepoxy liquid crystal monomer is preferably bis[4-(5,6-epoxyhexyloxy)]benzoic acid 1,4-phenylene ester; the monoepoxy liquid crystal monomer is 4-(5,6-epoxyhexyloxy)benzoic acid 4-methoxyphenyl ester. In the embodiment of the present application, the mass ratio of the diepoxy liquid crystal monomer to the monoepoxy liquid crystal monomer is preferably (5:0) to (1:4).

[0066] In the present application, the cationic photoinitiator includes photoinitiator 1173, and photoinitiator 1176 or photoinitiator 6976, preferably a mixture of photoinitiator 1173 and photoinitiator 1176 in a mass ratio of 1:1. In the ultraviolet light curing reaction, photoinitiator 1173 decomposes under ultraviolet light to generate phenylcarbonyl and 2-hydroxypropane-2-yl radicals, which are then oxidized by photoinitiator 1176 to form phenylcarbonyl carbon cations, and finally initiate the polymerization reaction of epoxy groups under the action of carbon cations, prompting the curing polymerization reaction to proceed rapidly. Based on the mixed initiator used in this application, that is, a mixture of photoinitiator 1173 and photoinitiator 1176 in a mass ratio of 1:1, the rapid polymerization of the mixed system of diepoxy liquid crystal monomers and monoepoxy liquid crystal monomers can be achieved, not only shortening the polymerization time from 2h to less than 20min, but also the fastest is only 1min; and the content of epoxy liquid crystal monomers in the polymer is increased from 10wt% to 30%, which greatly improves the mechanical properties of the trans-electrically controlled dimming film.

[0067] In the present application, the cationic photoinitiator may also include at least one of 4-(phenylthio)phenyldiphenylsulfonium hexafluorophosphate, 4-(phenylthio)phenyldiphenylsulfonium hexafluoroantimonate, 4-isobutylphenyl-4'-methylphenyliodonium hexafluorophosphate, 4-isobutylphenyl-4'-methylphenyliodonium hexafluoroantimonate, a mixture of triarylsulfonium hexafluorophosphates, a mixed solution of 4-isobutylphenyl-4'-methylphenyliodonium hexafluorophosphate, 4-isobutylphenyl-4'-methylphenyliodonium hexafluorophosphate or a mixed solution of η6-isopropylphenylferrocene (II) hexafluorophosphate.

[0068] In the present application, the chemical structures of the photoinitiator 1173, the photoinitiator 1176 and the photoinitiator 6976 are shown below:

[0069]

[0070] In the present application, the negative liquid crystal is a negative nematic phase liquid crystal, with a crystallization point of less than -40°C, a clearing point of more than 100°C, a birefringence of more than 0.1, a dielectric anisotropy of less than -0.5, and a viscosity of less than 200 mPa.s. In the embodiment of the present application, the negative liquid crystal is selected from liquid crystal GXV-7822-180.

[0071] In a second aspect, the present application provides a method for preparing the above-mentioned reverse electrically controlled dimming film, comprising:

[0072] The raw materials of the polymer liquid crystal composite material are mixed evenly according to a proportion, added between the first transparent conductive film and the second transparent conductive film, and cured by ultraviolet radiation to obtain a reverse electric control dimming film.

[0073] Specifically, the raw materials of the polymer liquid crystal composite material are mixed uniformly according to a ratio and added to a liquid crystal box, the surface of which is deposited with a conductive glass film, and the surface of the conductive glass film is coated with a vertical alignment layer prepared by DMOAP or PI. In the present application, the conductive glass layer of the liquid crystal box is preferably ITO, and the thickness between the two conductive glass films is 8 to 40 μm.

[0074] In this application, the liquid crystal cell is placed in a light intensity range of 10 to 300 mW / cm 2 The mixed photoinitiator of the present invention is used to irradiate the di-epoxy liquid crystal monomer and the mono-epoxy liquid crystal monomer under ultraviolet light, and the monomer undergoes polymerization reaction and solidifies. The temperature of the ultraviolet light irradiation curing is -20°C to 100°C, and the irradiation curing time is 1 to 20 minutes, so that the reverse electric control dimming film can be obtained, which greatly shortens the irradiation curing time.

[0075] The present application is further described below by way of examples.

[0076] In the examples of the present application, all raw materials can be purchased on the market or prepared according to conventional methods well known to those skilled in the art.

[0077] In the embodiment of the present application, the diepoxy liquid crystal monomer is E6M, the monoepoxy liquid crystal monomer is E6PM, the negative liquid crystal is GXV-7822-180, and the cationic photoinitiator is a mixed initiator of photoinitiator 1173 and photoinitiator 1176 in a mass ratio of 1:1.

[0078] Among them, the crystallization point of liquid crystal GXV-7822-180 is less than -40°C, the clearing point is greater than 100°C, the birefringence is greater than 0.1, the dielectric anisotropy is less than -0.5, and the viscosity is less than 200mPa.s.

[0079] Example 1

[0080] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0081] S1. E6M, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 are mixed according to the amounts in Table 1. After being fully stirred, they are poured into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0082] Table 1 Raw material components and dosage of Example 1

[0083]

[0084] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0085] Example 2

[0086] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0087] S1. E6M, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 are mixed according to the amounts in Table 2. After being fully stirred, they are poured into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0088] Table 2 Raw material components and dosage of Example 2

[0089]

[0090]

[0091] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0092] Example 3

[0093] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0094] S1. E6M, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 are mixed according to the amounts in Table 3. After being fully stirred, they are poured into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0095] Table 3 Raw material components and dosage of Example 3

[0096]

[0097] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0098] Example 4

[0099] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0100] S1. Mix E6M, E6PM, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 according to the amounts in Table 4. After being fully stirred, pour them into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0101] Table 4 Raw material components and dosage of Example 4

[0102]

[0103]

[0104] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0105] Example 5

[0106] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0107] S1. Mix E6M, E6PM, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 according to the amounts in Table 5. After being fully stirred, pour them into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0108] Table 5 Raw material components and dosage of Example 5

[0109]

[0110] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0111] Example 6

[0112] This embodiment provides a method for preparing a reverse electric-controlled dimming film, comprising:

[0113] S1. Mix E6M, E6PM, negative liquid crystal GXV-7822-180, photoinitiator 1173 and photoinitiator 1176 according to the amounts in Table 6. After being fully stirred, pour them into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0114] Table 6 Raw material components and dosage of Example 6

[0115]

[0116] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 The film was cured by ultraviolet radiation for 600 seconds under an ultraviolet light intensity of , to obtain a reverse electrically controlled dimming film.

[0117] In order to verify the effect of the mixed initiator in the embodiment of the present application, two groups of comparative examples were conducted, in which the mixed initiator in the embodiment was replaced with a single initiator containing only the photoinitiator 1176, and the reverse electrically controlled dimming film was prepared by UV radiation curing. Since the E6M monomer content in the slow reaction initiated by the photoinitiator 1176 is at most 15wt%, and the liquid crystal has no electro-optical performance when it exceeds 15wt%, the content of the E6M monomer in the comparative example does not exceed 15wt%.

[0118] Comparative Example 1

[0119] Table 7 Raw material components and dosage of comparative example 1

[0120] Monomer (wt.%) Liquid crystal (wt.%) UV photoinitiator (wt.%) E6M GXV-7822-180 Photoinitiator 1176 10 86 4

[0121] S1. E6M, negative liquid crystal GXV-7822-180 and photoinitiator 1176 are mixed according to the amounts in Table 7. After being fully stirred, they are poured into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0122] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 Under ultraviolet light intensity of , ultraviolet radiation curing is carried out for 2 hours to obtain a reverse electrically controlled dimming film.

[0123] Comparative Example 2

[0124] Table 8 Raw material components and dosage of comparative example 2

[0125] Monomer (wt.%) Liquid crystal (wt.%) UV photoinitiator (wt.%) E6M GXV-7822-180 Photoinitiator 1176 15 81 4

[0126] S1. E6M, negative liquid crystal GXV-7822-180 and photoinitiator 1176 are mixed according to the amounts in Table 8. After being fully stirred, they are poured into a liquid crystal box made of two pieces of conductive glass with indium tin oxide plated on the inner side. The liquid crystal box is oriented to orient the liquid crystal molecules vertically. The thickness of the liquid crystal box is 20.0 μm.

[0127] S2, the liquid crystal box in step S1 is heated at 25°C and 140 mW / cm 2 Under ultraviolet light intensity of , ultraviolet radiation curing is carried out for 2 hours to obtain a reverse electrically controlled dimming film.

[0128] Compared with Examples 1-6, the single photoinitiator of Comparative Example 1-2 requires 2 hours to complete UV radiation curing, which is much higher than the 600 seconds of Examples 1-6. The present application uses a mixed initiator, which greatly accelerates the UV radiation curing speed and shortens the UV radiation curing time.

[0129] The performance of the reverse electrically controlled dimming films prepared in Examples 1 to 6 was characterized, including:

[0130] (1) Liquid crystal comprehensive parameter test: The reverse electric control dimming films prepared in Examples 1 to 6 were tested using a liquid crystal comprehensive parameter tester LCT-P1000 to test their voltage-transmittance curves, threshold voltage and saturation voltage diagrams.

[0131] In this application, T off It indicates the light transmittance of the reverse electric control dimming film when no electric field is applied (off-state transmittance); T on It indicates the light transmittance (on-state transmittance) of the reverse electric control dimming film when an electric field of 100V is applied; V th Indicates the threshold voltage, which refers to when the light transmittance of the electrically controlled dimming film reaches T off The voltage required for 90% of sat Indicates the saturation voltage, which means when the light transmittance of the electronically controlled dimming film reaches T off The voltage required to achieve 10% of the required value; CR represents the contrast ratio, which is calculated as follows: CR = T off / T on .

[0132] Figure 1 is a voltage-transmittance curve of the reverse electric control dimming film of Example 1, Figure 2 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 1. Figure 1 and Figure 2It can be seen that the initial transmittance of the reverse electrically controlled dimming film of Example 1 is 72.3932% when not powered, the transmittance is 0.6277% when powered at 100V, and the contrast is 115.36; its threshold voltage is 30.134V, and the saturation voltage is 44.66V.

[0133] Figure 3 is a voltage-transmittance curve of the reverse electric control dimming film of Example 2, Figure 4 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 2. Figure 3 and Figure 4 It can be seen that the initial transmittance of the reverse electrically controlled dimming film of Example 2 is 73.4778% when not powered, the transmittance is 0.6957% when powered at 100V, and the contrast is 105.56; its threshold voltage is 35.875V, and the saturation voltage is 58.662V.

[0134] Figure 5 is a voltage-transmittance curve of the reverse electric control dimming film of Example 3, Figure 6 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 3. Figure 5 and Figure 6 It can be seen that the initial transmittance of the reverse electric control dimming film of Example 3 is 71.3962% when not powered, the transmittance is 15.978% when powered at 100V, and the contrast is 4.46; its threshold voltage is 54.838V, and the saturation voltage is 92.311V.

[0135] Figure 7 is a voltage-transmittance curve of the reverse electric control dimming film of Example 4, Figure 8 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 4. Figure 7 and Figure 8 It can be seen that the initial transmittance of the reverse electrically controlled dimming film of Example 4 is 69.7956% when not powered, the transmittance is 1.2004% when powered at 100V, the contrast is 58.03, the threshold voltage is 25.066V, and the saturation voltage is 38.507V.

[0136] Fig. 9 is a voltage-transmittance curve of the reverse electric control dimming film of Example 5, Fig.10 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 5. Fig. 9 and Fig.10 It can be seen that the initial transmittance of the reverse electric control dimming film of Example 5 is 72.8028% when not powered, the transmittance is 0.5864% when powered at 100V, the contrast is 123.99, the threshold voltage of Example 5 is 33.909V, and the saturation voltage is 50.656V.

[0137] Fig.11 is a voltage-transmittance curve of the reverse electric control dimming film of Example 6, Fig.12 The threshold voltage and saturation voltage diagram of the reverse electric control dimming film of Example 6. Fig.11 and Fig.12 It can be seen that the initial transmittance of the reverse electrically controlled dimming film of Example 6 is 65.5612% when not powered, the transmittance is 3.0218% when powered at 100V, and the contrast is 21.7; its threshold voltage is 33.628V, and the saturation voltage is 74.437V.

[0138] Fig.13 The voltage-transmittance curve of the reverse electric control dimming film of comparative example 1 shows that the initial transmittance is 73.1367% when no power is applied, but when the voltage is 12V, the transmittance drops sharply; Fig.14 1 is a voltage-transmittance curve of the reverse electrically controlled dimming film of comparative example 2, and its initial transmittance when no power is applied is 63.7245%.

[0139] From the above data, it can be seen that the transverse electrically controlled dimming films prepared in Examples 1-6 all have a good threshold voltage and saturation voltage, as well as good transmittance. However, the transverse electrically controlled dimming films prepared in Comparative Examples 1-2 have a lower transmittance performance than the transverse electrically controlled dimming films in the examples.

[0140] In the trans-electrically controlled dimming film prepared in Example 1-6, when the epoxy resin is the double epoxy resin monomer E6M, as the epoxy resin content increases, the contrast of the trans-electrically controlled dimming film decreases, the transmittance increases, and the threshold voltage and saturation voltage increase. When the total amount of epoxy resin remains unchanged, the trans-electrically controlled dimming film whose epoxy resin is a mixture of E6M and E6PM has a lower threshold voltage and saturation voltage than the trans-electrically controlled dimming film whose epoxy resin uses E6M. That is, adding E6PM to E6M can effectively reduce the threshold voltage and saturation voltage of the trans-electrically controlled dimming film.

[0141] When the mass ratio of E6M and E6PM is 3:2 and the total proportion is 25%, for example, the reverse electrically controlled dimming film prepared in Example 5 has an initial transmittance of 72.8028% when not powered, a transmittance of 0.5864% when powered at 100V, a contrast ratio of 123.99, a threshold voltage of 33.909V, and a saturation voltage of 50.656V in Example 5, which has the best photoelectric performance.

[0142] (2) Mechanical properties test

[0143] The reverse electrically controlled dimming films prepared in Examples 1-6 and Comparative Examples 1-2 were stretched by a mechanical stretching machine, and the yield stress limit was tested. Fig.15 shown.

[0144] according to Fig.15 It can be seen that the stress limits of the reverse dimming film samples of Examples 1-6 are 464.17 KPa, 848.73 KPa, 2562.46 KPa, 128.17 KPa, 337.52 KPa and 284.2 KPa respectively.

[0145] All have high tensile properties; the stress limits of comparative examples 1 and 2 are 20.34 KPa and 36.51 KPa, which are much lower than the reverse dimming film of the embodiment of the present application.

[0146] When the polymer monomer of the reverse dimming film of Examples 1-6 is pure E6M, the stress limit increases with the increase of the E6M content; when the polymer monomer is a mixture of E6M and E6PM and the ratio remains unchanged, the stress limit increases with the increase of the total content of E6M and E6PM; when the total content of the polymer monomer is constant, the stress limit of the film with the addition of E6PM is lower than the stress limit of pure E6M.

[0147] (3) Scanning electron microscope test

[0148] The reverse electrically controlled dimming film samples prepared in Examples 1, 2 and 5 were cut into small pieces respectively. To facilitate observation of the polymer network, the sample pieces were immersed in cyclohexane to remove the liquid crystal. The samples were then subjected to gold spraying and observed under a scanning electron microscope.

[0149] The scanning electron microscope images of the samples of Examples 1, 2, and 5 are as follows: Fig.16 , 17 , 18. From Fig.16 and Fig.17 It can be seen that when the polymer monomer is pure E6M, as the E6M content increases, the polymer fiber network between the two conductive substrates becomes denser and the domain density increases. Fig.18 It can be seen that when E6PM is added, the polymer fiber network becomes sparse and the domain density decreases, which verifies that the stress limit of the sample with added E6PM is lower than that of pure E6M.

[0150] In the present application, when the polymer monomer is pure E6M, as the E6M content increases, the density of the polymer fiber network between the two conductive substrates increases, the stress limit of the trans-electrically controlled dimming film is enhanced, and the mechanical properties are enhanced. With the addition of E6PM, the driving voltage of the trans-electrically controlled dimming film is reduced, but the polymer fiber network between the two conductive substrates also becomes sparse, resulting in reduced tensile properties. In actual use, the raw materials of the trans-electrically controlled dimming film can be adjusted according to the requirements for driving voltage or tensile properties to meet the needs. For example, when a lower driving voltage is required, E6M and E6PM can be used; when higher tensile properties are required, single E6M can be used.

[0151] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.

Claims

1. A reverse electric control dimming film, It is characterized in that It comprises a first transparent conductive film, a polymer liquid crystal composite material layer and a second transparent conductive film which are sequentially stacked in the thickness direction; The raw materials of the polymer liquid crystal composite material include diepoxy liquid crystal monomers and / or monoepoxy liquid crystal monomers, negative liquid crystals and cationic photoinitiators; The polymer liquid crystal composite material comprises, by weight, 2 to 40 parts of diepoxy liquid crystal monomers, 0 to 24 parts of monoepoxy liquid crystal monomers, 56 to 94 parts of negative liquid crystals, and 3 to 5 parts of cationic photoinitiators.

2. The reverse electrically controlled dimming film according to claim 1, It is characterized in that The mass ratio of the diepoxy liquid crystalline monomer to the monoepoxy liquid crystalline monomer is (5:0) to (1:4).

3. The reverse electrically controlled dimming film according to claim 1, It is characterized in that The cationic photoinitiator includes photoinitiator 1173, and photoinitiator 1176 or photoinitiator 6976.

4. The reverse electrically controlled dimming film according to claim 3, It is characterized in that The cationic photoinitiator includes photoinitiator 1173 and photoinitiator 1176, and the mass ratio of the two is 1:

1.

5. The reverse electrically controlled dimming film according to claim 1, It is characterized in that The negative liquid crystal is a negative nematic phase liquid crystal, with a crystallization point of less than -40°C, a clearing point of more than 100°C, a birefringence of more than 0.1, a dielectric anisotropy of less than -0.5, and a viscosity of less than 200 mPa.s.

6. The reverse electrically controlled dimming film according to claim 1, It is characterized in that The chemical structure of the diepoxy liquid crystal monomer is: Wherein, m=1 to 9; n=1 to 9; The chemical structure of the monoepoxy liquid crystal monomer is: Among them, m=1~9.

7. The method for preparing the reverse electrically controlled dimming film according to any one of claims 1 to 6, It is characterized in that include: The raw materials of the polymer liquid crystal composite material are mixed evenly according to a proportion, added between the first transparent conductive film and the second transparent conductive film, and cured by ultraviolet radiation to obtain a reverse electric control dimming film.

8. The preparation method according to claim 7, It is characterized in that The distance between the first transparent conductive film and the second transparent conductive film is 8-40 μm.

9. The preparation method according to claim 7, It is characterized in that The temperature of the ultraviolet light curing is -20°C to 100°C, the time is 1 to 20 minutes, and the light intensity is 10 to 300 mW / cm 2 .