Manufacturing method of OMOG photomask
In the OMOG photomask manufacturing, the patterned molybdenum silicide layer is formed using laser or electron beam direct writing scanning technology, which solves the problem of insufficient thickness and absorbance of the molybdenum silicide layer in the traditional method, and realizes the OMOG photomask efficient preparation and cost reduction.
Patent Information
- Application Number
- CN202411140685.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-01
AI Technical Summary
The traditional OMOG photomask manufacturing method cannot meet the development needs of OMOG photomasks, and the process cost is high, which affects the manufacturing cost.
By depositing the silicon layer and the molybdenum layer in sequence on the transparent substrate, forming a molybdenum-silicon stack layer and performing patterned laser or electron beam direct writing scan, the Mo atoms in the molybdenum layer are completely moved into the silicon layer to form a patterned The molybdenum silicide layer controls its thickness and content distribution, thereby increasing the absorbance and thinning the molybdenum silicide layer.
The goal of the molybdenum silicide layer has been achieved with the minimum thickness and highest absorbance, which reduces the cost of raw materials, simplifies the preparation process, and improves production efficiency and cost-effectiveness.
Smart Images

Figure CN118884776A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of integrated circuit manufacturing, and in particular to a method for manufacturing an OMOG photomask. Background Art
[0002] With the introduction of ultra-large numerical aperture 193nm lithography machines, the size of the patterns on the mask is getting smaller and smaller. Studies have found that the thicker the Cr used to block light on the mask, the stronger the interaction between the light wave and Cr, causing the optimal focus value during exposure to shift with the size of the pattern. This phenomenon is called the mask three-dimensional effect. In order to reduce the mask three-dimensional effect, molybdenum silicide (MoSi) with higher optical density (OD) is used as the material for the absorption layer. This mask using high optical density MoSi material as the absorption layer is called an opaque MoSi mask (opaque MoSi on glass, OMOG).
[0003] OMOG uses MoSi as the absorption layer. The molybdenum silicide layer provides sufficient optical density and has a high extinction coefficient (k). A very thin molybdenum silicide layer can effectively block light with a wavelength of 193nm, which can reduce the three-dimensional effect of the mask that plagues ultra-large numerical aperture immersion lithography, thereby improving pattern fidelity and resolution. In addition, the MoSi material has excellent etching performance. Ion etching can well achieve vertical side walls, which helps to provide excellent CD uniformity in the final product; in addition, the MoSi film itself has very little stress, which is of great advantage in improving the flatness of the mask and reducing the offset of the pattern. In short, the OMOG photomask has finer resolution, higher fidelity, tighter CD uniformity and better alignment.
[0004] In recent years, in order to make the molybdenum silicide layer fully absorb ultraviolet light under thinner conditions, an OMOG photomask based on multi-layer MoSi has been developed. The multi-layer MoSi has different molybdenum and silicon contents so that each layer has different optical parameters (n, k). The reflected light between the interfaces of the multi-layer molybdenum silicide layers increases, which can improve the absorption rate, so that ultraviolet light can be fully absorbed under thinner conditions. Thinner molybdenum silicide layers can reduce edge morphology effects, effectively avoid distortion, uneven peak intensity, and unequal sidelobe width caused by edge morphology effects, and can achieve better resolution and contrast.
[0005] However, the prior art uses a sputtering deposition process to form the molybdenum silicide layer of the OMOG photomask. The molybdenum and silicon contents in the MoSi film formed by sputtering deposition are fixed and the molybdenum and silicon materials are evenly distributed. The content of the single-layer molybdenum silicide layer is fixed, and the multi-layer molybdenum silicide layer can only increase the reflected light at the interface between the layers. The ability of the multi-layer molybdenum silicide layer to increase the reflected light is limited, so that although the multi-layer molybdenum silicide layer can increase the reflected light and improve the absorptivity to a certain extent, it cannot achieve the development goal of the minimum thickness and the highest absorptivity of the molybdenum silicide layer required by the OMOG photomask. In addition, the Mo and Si contents of the MoSi target material used in the sputtering deposition process are fixed, and it is difficult to adjust the Mo and Si contents in the MoSi film formed by the sputtering deposition process by adjusting the process parameters. The MoSi film with different Mo and Si contents can only be formed by replacing the MoSi target material with different Mo and Si contents. The manufacture of the OMOG photomask requires the use of multiple MoSi targets with different Mo and Si contents, and the raw material cost is high, which seriously affects the manufacturing cost of the OMOG photomask. Therefore, the traditional OMOG photomask manufacturing process cannot meet the development needs of OMOG photomasks, and the process cost is high, which affects the technical problem of OMOG photomask manufacturing cost. Summary of the invention
[0006] The purpose of the present invention is to provide a method for manufacturing an OMOG photomask to solve the technical problems that the traditional OMOG photomask manufacturing method cannot meet the development needs of the OMOG photomask and has high process cost, which affects the manufacturing cost of the OMOG photomask.
[0007] To achieve the above object, the present invention provides a method for manufacturing an OMOG photomask, comprising the following steps: providing a transparent substrate; Alternatingly depositing silicon layers and molybdenum layers on a transparent substrate to form a molybdenum-silicon stacked layer; Performing patterned laser or electron beam direct writing scanning on the molybdenum-silicon stacked layer, so that the Mo atoms in the molybdenum layer in the area scanned by the laser or electron beam are completely moved into the silicon layer to form a patterned molybdenum silicide layer, wherein the patterned molybdenum silicide layer has a preset thickness, preset Mo and Si contents, and a preset Mo atomic distribution gradient; removing the unreacted silicon layer and molybdenum layer to form an OMOG photomask; The silicon layer and the molybdenum layer are deposited by a thin film deposition process, and the thin film deposition process controls the thickness of the silicon layer and the molybdenum layer respectively according to a preset thickness, a preset Mo and Si content, and a preset Mo atomic distribution gradient.
[0008] The manufacturing method of the above-mentioned OMOG photomask first deposits a silicon layer and a molybdenum layer on a transparent substrate in sequence to form a molybdenum-silicon stacked layer. During the deposition process, the thickness of the silicon layer and the molybdenum layer are respectively controlled according to the preset thickness of the preset patterned molybdenum silicide layer, the preset Mo and Si content, and the preset Mo atomic distribution gradient. After the molybdenum-silicon stacked layer is deposited, the molybdenum-silicon stacked layer is patterned and directly scanned by laser or electron beam so that the Mo atoms in the molybdenum layer in the scanned area are completely moved to the silicon layer to form a patterned molybdenum silicide layer. This method can adjust the thickness of the finally formed patterned molybdenum silicide layer, the content of Mo and Si in the molybdenum silicide layer, and the distribution gradient of Mo atoms by controlling the thickness of the deposited silicon layer and the molybdenum layer. The patterned molybdenum silicide layer can form a change in the composition of the total continuous molybdenum-silicon layer. The distribution of Mo atoms in the patterned molybdenum silicide layer changes in a gradient, which can form a layer of internal reflection to repeatedly absorb ultraviolet light, so that the reflected light between the interfaces of the multi-layer molybdenum silicide layers can be repeatedly absorbed by each layer, and the light absorption rate can be maximized. Moreover, the manufacturing method of the above-mentioned OMOG photomask enables Mo atoms to completely move into the silicon layer and completely consume the molybdenum layer to form a patterned molybdenum silicide layer. According to calculation, the thickness of the patterned molybdenum silicide layer increased on the surface of the original silicon layer is only 1% of the thickness of the original molybdenum layer. The thickness of the final patterned molybdenum silicide layer is almost equal to the thickness of the original silicon layer. The thickness of the patterned molybdenum silicide layer can be well controlled by controlling the thickness of the original molybdenum layer and the silicon layer. Therefore, the manufacturing method of the above-mentioned OMOG photomask can improve the absorbance while reducing the thickness of the patterned molybdenum silicide layer as much as possible, and can well achieve the development goal of the OMOG photomask with the smallest thickness of the molybdenum silicide layer and the highest absorbance.
[0009] In addition, the above-mentioned method for manufacturing an OMOG photomask can form a molybdenum silicide layer with any Mo and Si content as needed, and only one elemental molybdenum target and one elemental silicon target are needed to form a plurality of molybdenum silicide layers with different Mo and Si contents, without the need to prepare a plurality of MoSi targets with different Mo and Si contents, which can effectively reduce the cost of raw materials and greatly save the manufacturing cost of the OMOG photomask. Moreover, the above-mentioned method for manufacturing an OMOG photomask performs patterned direct writing scanning on the molybdenum-silicon stacked layer by laser or electron beam, and directly forms a patterned molybdenum silicide layer after the laser or electron beam scanning, and after the patterned molybdenum silicide layer is formed, only the unreacted silicon layer and molybdenum layer need to be removed to form the OMOG photomask, and the preparation of the OMOG photomask is completed, and there is no need to perform the patterning process steps such as glue coating and exposure in the traditional OMOG photomask manufacturing process, which simplifies the OMOG photomask preparation process, can effectively improve the production efficiency of the OMOG photomask, and further save manufacturing costs.
[0010] In summary, the above-mentioned OMOG photomask manufacturing method can minimize the thickness of the molybdenum silicide layer and maximize the absorbance, and can achieve the development goal of the OMOG photomask with the smallest molybdenum silicide layer thickness and the highest absorbance, and the above-mentioned OMOG mask substrate manufacturing method can effectively reduce the process cost, which is conducive to saving the OMOG photomask manufacturing cost.
[0011] In one embodiment, the laser or electron beam is focused on the molybdenum layer.
[0012] In one embodiment, the power density of the laser or electron beam is 1 W / cm 2 ~10W / cm 2 .
[0013] In one embodiment, the surface temperature of the laser or electron beam is 400°C to 800°C.
[0014] In one embodiment, the surface temperature of the laser or electron beam is 500°C to 800°C.
[0015] In one embodiment, the scanning time of the laser or electron beam is 10 min to 30 min.
[0016] In one embodiment, the thickness of the silicon layer and the thickness of the molybdenum layer are both no greater than 30 nm.
[0017] In one embodiment, the preset Mo and Si contents are such that the content of Mo atoms is not greater than 50% of the content of Si atoms.
[0018] In one embodiment, the preset Mo and Si contents are such that the content of Mo atoms is 30% to 45% of the content of Si atoms.
[0019] In one embodiment, the thin film deposition process includes a sputtering deposition process or an atomic layer deposition process.
[0020] In one embodiment, after the step of forming a patterned molybdenum silicide layer with a preset Mo and Si content, the step of implanting at least one of nitrogen atoms, oxygen atoms or carbon atoms into the patterned molybdenum silicide layer is further included. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of a process for manufacturing an OMOG photomask according to an embodiment; Figures 2 to 5 The schematic structural diagram of an embodiment of the present invention is a schematic structural diagram of an OMOG photomask manufactured by using the method for manufacturing an OMOG photomask of the present invention.
[0022] Description of reference numerals: 10 - transparent substrate, 20 - silicon layer, 30 - molybdenum layer, 40 - molybdenum-silicon stacked layer, 50 - patterned molybdenum silicide layer, 60 - light-transmitting area, 70 - OMOG photomask. DETAILED DESCRIPTION
[0023] In the following description, a large number of specific details are given in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features known in the art are not described. It should be understood that the present invention can be implemented in different forms and should not be interpreted as being limited to the embodiments presented here. On the contrary, providing these embodiments will make the disclosure thorough and complete, and fully convey the scope of the present invention to those skilled in the art. The same reference numerals represent the same elements from beginning to end. It should be understood that when a layer is referred to as being formed on other layers, it can be directly formed on other layers, or there can be an intervening film layer. Among them, the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back" and the like is based on the orientation or positional relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, wherein "longitudinal" can be understood as a direction perpendicular to the substrate surface, and "lateral" can be understood as a direction parallel to the substrate surface. When used herein, the singular forms "a", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "include" is used to determine the presence of features, steps, operations, elements and / or parts, but does not exclude the presence or addition of one or more other features, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items. The terms "same", "equal" and "consistent" include completely equal and identical meanings, and may also include approximately the same or approximately equal meanings under allowed process errors. The terms "first" "second" and the like in the specification are used to distinguish between similar elements, and are not necessarily used to describe a specific order or time sequence. It is to be understood that, where appropriate, these terms used in this way are interchangeable, for example, so that the embodiments of the present invention described herein can be operated in other orders different from those described or shown herein. Similarly, if the method described herein includes a series of steps, the order in which the steps are presented herein is not necessarily the only order in which the steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method. If components in a certain figure are the same as components in other figures, although these components can be easily identified in all figures, in order to make the description of the figures clearer, this specification will not mark all the same component numbers in each figure.
[0024] The present invention is described more clearly and completely below by way of embodiments in conjunction with the accompanying drawings, but the present invention is not limited to the scope of the following embodiments.
[0025] Please also see Figures 1 to 5 The method for manufacturing the OMOG photomask 70 of one embodiment includes the following steps:
[0026] Step S11: providing a transparent substrate 10 .
[0027] Specifically, Figure 2 As shown, a transparent substrate 10 is first provided, and the transparent substrate 10 includes one of a quartz substrate, a soda lime substrate, a borosilicate substrate, an aluminum silicate substrate, a silicon substrate, and a silicon carbide substrate. The radial dimension of the transparent substrate 101 is between 1 inch and 100 inches, and the thickness is between 0.1 mm and 200 mm. For example, in this embodiment, the transparent substrate 10 can be a quartz substrate, and its radial dimension can be 4 inches, 6 inches, 8 inches, 12 inches, etc.
[0028] Step S12: Alternately depositing silicon layers 20 and molybdenum layers 30 on the transparent substrate 10 in sequence to form a molybdenum-silicon stacked layer 40 .
[0029] In one embodiment, the silicon layer 20 and the molybdenum layer 30 are deposited by a thin film deposition process such as a sputtering deposition process or an atomic layer deposition process. Both the sputtering deposition process and the atomic layer deposition process have a high controllability of the thickness of the deposited film, and can accurately control the thickness of the deposited silicon layer 20 and the molybdenum layer 30. In specific practical applications, a specific thin film deposition process can be selected as needed. This embodiment is not specifically limited. For the convenience of description, this embodiment is described by taking the sputtering deposition process to deposit the silicon layer 20 and the molybdenum layer 30 as an example. Specifically, the sputtering deposition process preferably adopts a low-temperature DC magnetron sputtering process. The sputtering deposition process uses an inert gas (helium and / or argon) to bombard the corresponding silicon target material or molybdenum target material so that the material is deposited on the transparent substrate 10 to form the corresponding silicon layer 20 or molybdenum layer 30. The silicon target material uses a single silicon target material including amorphous silicon and a purity of at least 99.99%, and the molybdenum target material uses a single molybdenum target material including amorphous molybdenum and a purity of at least 99.99%. Furthermore, the preset Mo and Si contents are the ratios of the Mo content and the Si content in the patterned molybdenum silicide layer 50 to be formed. Before the sputtering deposition process, the thicknesses of the silicon layer 20 and the molybdenum layer 30 are calculated according to the preset thickness of the patterned molybdenum silicide layer 50 to be formed, the preset Mo and Si contents, and the preset Mo atomic distribution gradient, and the target thicknesses of the silicon layer 20 and the molybdenum layer 30 are obtained. During the sputtering deposition process, the deposition time is controlled according to the calculated thicknesses of the silicon layer 20 and the molybdenum layer 30, and the silicon layer 20 and the molybdenum layer 30 are deposited to form the target thicknesses.
[0030] Furthermore, the sputtering deposition process first deposits the silicon layer 20 on the transparent substrate 10, and then deposits the molybdenum layer 30. When only one patterned molybdenum silicide layer 50 needs to be formed, the silicon layer 20 and the molybdenum layer 30 are sequentially deposited on the transparent substrate 10. When multiple patterned molybdenum silicide layers 50 need to be formed, the silicon layer 20 and the molybdenum layer 30 are alternately deposited on the transparent substrate 10 to form a molybdenum-silicon stacked layer 40 having at least three layers. In the molybdenum-silicon stacked layer 40 having at least three layers, the uppermost layer and the lowermost layer are both silicon layers 20, and the molybdenum layer 30 is located between two adjacent silicon layers 20. Figure 3 As shown, in this embodiment, the need to form two layers of patterned molybdenum silicide layers 50 is taken as an example. When the need to form two layers of patterned molybdenum silicide layers 50 is to form a three-layer structure of molybdenum-silicon stacked layers 40 is deposited on the transparent substrate 10. In the three-layer structure, the bottom layer and the top layer are both silicon layers 20, and the molybdenum layer 30 is located between the two silicon layers 20. Specifically, the first silicon layer 20 is first deposited on the transparent substrate 10. After the film thickness of the first silicon layer 20 reaches the target thickness, the molybdenum layer 30 is deposited on the surface of the first silicon layer 20. After the film thickness of the molybdenum layer 30 reaches the target thickness, the second silicon layer 20 is deposited on the film surface. After the film thickness of the second silicon layer 20 reaches the target thickness, the deposition operation is completed, and step S13 is executed.
[0031] Step S13: Perform patterned laser or electron beam direct writing scanning on the molybdenum silicon stacked layer 40, so that the Mo atoms in the molybdenum layer 30 in the area scanned by the laser or electron beam are completely moved to the silicon layer 20 to form a patterned molybdenum silicide layer 50, and the patterned molybdenum silicide layer 50 has a preset thickness, preset Mo and Si contents, and a preset Mo atomic distribution gradient.
[0032] Specifically, the ratio of the Mo content to the Si content in the patterned molybdenum silicide layer 50 depends on the relative amount of Mo atoms in the molybdenum layer 30 and the Si atoms in the silicon layer 20, and the thickness of the molybdenum layer 30 determines the number of Mo atoms, and the thickness of the silicon layer 20 determines the number of Si atoms. In step S12, the thickness of the silicon layer 20 and the molybdenum layer 30 is first controlled according to the preset Mo and Si contents required for the patterned molybdenum silicide layer 50 to be formed, and after the molybdenum silicon stacking layer 40 is heat-treated, the Mo atoms are completely moved to the silicon layer 20, so that the molybdenum layer 30 is completely consumed to form a patterned molybdenum silicide layer 50 with preset Mo and Si contents. Further, after the molybdenum silicon stacking layer 40 is heat-treated, the Mo atoms in the molybdenum layer 30 move from near to far into the silicon layer 20, so that the Mo atoms are distributed in a gradient in the formed patterned molybdenum silicide layer 50. More specifically, the preset Mo and Si contents in this embodiment are the average contents of Mo and Si in the patterned molybdenum silicide layer 50. The Mo atoms in the patterned molybdenum silicide layer 50 are distributed in a gradient, from the side close to the original molybdenum layer 30 to the side away from the original molybdenum layer 30, the content of Mo atoms is distributed from high to low, the Mo atom content on the side close to the original molybdenum layer 30 is slightly higher than the Mo atom content in the preset Mo and Si contents, and the Mo atom content on the side away from the original molybdenum layer 30 is slightly lower than the Mo atom content in the preset Mo and Si contents, and the average content of Mo atoms in the patterned molybdenum silicide layer 50 is equal to the Mo atom content in the preset Mo and Si contents. Furthermore, it has been calculated that after the Mo atoms are completely moved into the silicon layer 20 and completely consume the molybdenum layer 30 to form a patterned molybdenum silicide layer 50, the increased thickness of the patterned molybdenum silicide layer 50 on the surface of the original silicon layer is only 1% of the thickness of the original molybdenum layer 30. The final thickness of the patterned molybdenum silicide layer 50 is almost equal to the thickness of the original silicon layer 20. By controlling the thickness of the original molybdenum layer 30 and the silicon layer 20, the thickness of the patterned molybdenum silicide layer 50 can be well controlled.
[0033] The distribution of Mo atoms in the patterned molybdenum silicide layer 50 formed by the manufacturing method of the OMOG mask substrate of this embodiment changes in a gradient, which can form intralayer reflection and repeated absorption of ultraviolet light, and can improve the absorbance. The method is used to make a multilayer patterned molybdenum silicide layer 50 with different Mo and Si contents, which can increase the reflected light at the interface between the multilayer patterned molybdenum silicide layers 50, and the intralayer reflection and repeated absorption of ultraviolet light of each layer of the patterned molybdenum silicide layer 50 are superimposed, so that the reflected light between the interfaces of the multilayer patterned molybdenum silicide layers 50 can be repeatedly absorbed by each layer, which can maximize the absorbance. Figure 4As shown, in this embodiment, the molybdenum-silicon stacked layer 40 having a three-layer structure is subjected to heat treatment, so that the Mo atoms in the middle molybdenum layer 30 are respectively moved to the silicon layers 20 on both sides, so as to form two patterned molybdenum silicide layers 50. In this embodiment, two patterned molybdenum silicide layers 50 are formed by heat treating the molybdenum-silicon stacked layer 40 having a three-layer structure, and the thickness of the deposited molybdenum layer 30 and the two adjacent silicon layers 20 are controlled according to the preset thickness, preset Mo and Si content, and preset Mo atomic distribution gradient of the patterned molybdenum silicide layer 50 of the upper and lower layers to be formed, so as to ensure that the two patterned molybdenum silicide layers 50 of the upper and lower layers formed have the preset thickness, preset Mo and Si content, and preset Mo atomic distribution gradient. When it is necessary to form more layers of patterned molybdenum silicide layers 50, the thickness of each silicon layer 20 and molybdenum layer 30 is determined according to the preset thickness, preset Mo and Si content, and preset Mo atomic distribution gradient of the multiple patterned molybdenum silicide layers 50 to ensure that the formed multiple layers of patterned molybdenum silicide layers 50 all meet the preset thickness, preset Mo and Si content, and preset Mo atomic distribution gradient requirements.
[0034] In one embodiment, in order to achieve the overall best absorbance of the multi-layer patterned molybdenum silicide layer 50, the thickness of the silicon layer 20 on both sides of the molybdenum layer 30 is preferably opposite, that is, the thickness of the silicon layer 20 on one side of the molybdenum layer 30 is thinner, and the thickness of the silicon layer 20 on the other side of the molybdenum layer 30 is thicker. The thickness of the silicon layer 20 on both sides of the molybdenum layer 30 is different. After heat treatment, the thinner silicon layer will first reach the preset Mo and Si content level, and the entry of Mo atoms will slow down, but Mo atoms will still enter the thicker silicon layer 30 on the other side until the molybdenum layer 30 is completely exhausted. At this time, the formation of multi-layer patterned molybdenum silicide layers 50 with different Mo and Si contents increases the interlayer interface reflected light, and further superimposes the intra-layer reflection of each layer of the patterned molybdenum silicide layer 50 to repeatedly absorb ultraviolet light, which can achieve the best absorbance.
[0035] The manufacturing method of the OMOG mask substrate of the present embodiment can control the film thickness, Mo and Si content, and Mo atomic distribution gradient of the patterned molybdenum silicide layer 50 by controlling the thickness of the original silicon layer 20 and the molybdenum layer 30. The film thickness, Mo and Si content, and Mo atomic distribution gradient of the patterned molybdenum silicide layer 50 are simple and convenient to adjust.
[0036] Step S14 : removing the unreacted silicon layer 20 and molybdenum layer 30 to form an OMOG photomask 70 .
[0037] Specifically, after scanning the molybdenum-silicon stacked layer to form a patterned molybdenum silicide layer 50, an etching process is performed to remove the unreacted silicon layer 20 and the molybdenum layer 30 to form a light-transmitting region 60, thereby completing the preparation of the OMOG photomask (eg, Figure 5As shown). In this embodiment, a wet etching process is preferably used to remove the unreacted silicon layer 20 and the molybdenum layer 30. Further preferably, the etching solution is an acidic etching solution, such as SPM ((H2SO4 / H2O2)). The principle and implementation of the specific wet etching process are the same as those of the existing conventional wet etching process, and will not be described in detail in this embodiment.
[0038] The manufacturing method of the above-mentioned OMOG photomask first deposits a silicon layer 20 and a molybdenum layer 30 on a transparent substrate 10 in sequence to form a molybdenum-silicon stacked layer 40. During the deposition process, the thickness of the silicon layer 20 and the molybdenum layer 30 are respectively controlled according to a preset thickness of a preset patterned molybdenum silicide layer 50, a preset Mo and Si content, and a preset Mo atomic distribution gradient. After the deposition of the molybdenum-silicon stacked layer 40 is completed, the molybdenum-silicon stacked layer 40 is patterned by laser or electron beam direct writing scanning so that the Mo atoms in the molybdenum layer 30 in the scanned area are completely moved to the silicon layer 20 to form a patterned molybdenum silicide layer 50. The method can adjust the thickness of the finally formed patterned molybdenum silicide layer 50, the content of Mo and Si in the molybdenum silicide layer and the distribution gradient of Mo atoms by controlling the thickness of the deposited silicon layer 20 and the molybdenum layer 30. The patterned molybdenum silicide layer 50 can form a change in the overall continuous molybdenum-silicon composition. The distribution of Mo atoms in the patterned molybdenum silicide layer 50 shows a gradient change, which can form intra-layer reflection and repeated absorption of ultraviolet light, so that the reflected light between the interfaces of the multi-layer molybdenum silicide layers 50 can be repeatedly absorbed by each layer, which can maximize the absorbance. Moreover, the manufacturing method of the above-mentioned OMOG photomask enables Mo atoms to completely move into the silicon layer 20 and completely consume the molybdenum layer 30 to form a patterned molybdenum silicide layer 50. The thickness of the patterned molybdenum silicide layer 50 increased on the surface of the original silicon layer 20 is only 1% of the thickness of the original molybdenum layer 30. The thickness of the final patterned molybdenum silicide layer 50 is almost equal to the thickness of the original silicon layer 20. The thickness of the patterned molybdenum silicide layer 50 can be well controlled by controlling the thickness of the original molybdenum layer 20 and the silicon layer 30. Therefore, the manufacturing method of the above-mentioned OMOG photomask can improve the absorbance while reducing the thickness of the patterned molybdenum silicide layer 50 as much as possible, and can well achieve the development goal of the OMOG photomask required for the minimum thickness of the molybdenum silicide layer and the highest absorbance.
[0039] In addition, the above-mentioned method for manufacturing the OMOG photomask can form a molybdenum silicide layer with any Mo and Si content as needed, and only one elemental molybdenum target and one elemental silicon target are needed to form a plurality of molybdenum silicide layers with different Mo and Si contents, without the need to prepare a plurality of MoSi targets with different Mo and Si contents, which can effectively reduce the cost of raw materials and greatly save the manufacturing cost of the OMOG photomask. Moreover, the above-mentioned method for manufacturing the OMOG photomask performs patterned direct writing scanning on the molybdenum-silicon stacked layer by laser or electron beam, and directly forms a patterned molybdenum silicide layer 50 after the laser or electron beam scanning, and after the patterned molybdenum silicide layer 50 is formed, it is only necessary to remove the unreacted silicon layer 20 and the molybdenum layer 30 to form the OMOG photomask 70, and the preparation of the OMOG photomask 70 is completed, and there is no need to perform the patterning process steps such as glue coating and exposure in the traditional OMOG photomask manufacturing process, which simplifies the OMOG photomask preparation process, can effectively improve the production efficiency of the OMOG photomask, and further save the manufacturing cost.
[0040] In one embodiment, the preset Mo and Si contents are such that the content of Mo atoms is not greater than 50% of the content of Si atoms. Specifically, the preset Mo and Si contents of the patterned molybdenum silicide layer 50 are determined in advance according to the target optical parameters of the molybdenum silicide layer of the OMOG photomask. In order to avoid excessive Mo atom content and increase the thickness of the patterned molybdenum silicide layer 50, the content of Mo atoms in the patterned molybdenum silicide layer 50 is not greater than 50% of the content of Si atoms. Further, in order to effectively control the thickness of the patterned molybdenum silicide layer 50 and ensure that the content of Mo atoms in the patterned molybdenum silicide layer 50 can meet the optical parameter requirements of the molybdenum silicide layer, it is preferred that the preset Mo and Si contents are such that the content of Mo atoms is 30% to 45% of the content of Si atoms. In one embodiment, the preset Mo and Si contents are such that the content of Mo atoms is not greater than 50% of the content of Si atoms. Specifically, the preset Mo and Si contents of the patterned molybdenum silicide layer 50 are determined in advance according to the target optical parameters of the molybdenum silicide layer of the OMOG photomask. To avoid excessive Mo atomic content and increase the thickness of the patterned molybdenum silicide layer 50, the content of Mo atoms in the patterned molybdenum silicide layer 50 is not greater than 50% of the content of Si atoms. Further, to effectively control the thickness of the patterned molybdenum silicide layer 50 and ensure that the content of Mo atoms in the patterned molybdenum silicide layer 50 can meet the optical parameter requirements of the molybdenum silicide layer, it is preferred that the preset Mo and Si contents are such that the content of Mo atoms is 30% to 45% of the content of Si atoms.
[0041] In one embodiment, in order to reduce the edge morphology effect and effectively control the thickness of the finally formed patterned molybdenum silicide layer 50, the thickness of the silicon layer 20 and the thickness of the molybdenum layer 30 in the molybdenum-silicon stacked layer 40 are both no greater than 30 nm. Further, in order to ensure that each layer of the multi-layer patterned molybdenum silicide layer 50 meets the respective preset Mo and Si content requirements, the thickness of the silicon layer 20 and the thickness of the molybdenum layer 30 in the molybdenum-silicon stacked layer 40 are preferably no less than 10 nm.
[0042] In one embodiment, the focus of the laser or electron beam is focused on the molybdenum layer 30. Focusing the laser or electron beam on the molybdenum layer 30 enables the Mo atoms to move quickly and completely into the silicon layer 20, which helps to quickly form a molybdenum silicide layer with a preset Mo and Si content. Further, when the molybdenum silicon stacked layer 40 has multiple molybdenum layers 30, in order to ensure uniform energy distribution, the focus of the laser or electron beam is preferably focused on the bottommost molybdenum layer 30.
[0043] Furthermore, the manufacturing method of the OMOG photomask of the present embodiment performs patterned direct writing scanning on the molybdenum silicon stacked layer by laser or electron beam, and directly forms a patterned molybdenum silicide layer 50 after the laser or electron beam scanning. In order to achieve optimal graphic control, it is necessary to adjust the scanning area of the laser or electron beam according to the size of the graphic. In order to ensure that the scanning area of the laser or electron beam matches the image size and meets the graphic requirements, it is necessary to use a small spot laser or a small electron beam spot electron beam to scan the molybdenum silicon stacked layer 40 to form a patterned molybdenum silicide layer 50. In one embodiment, in order to ensure that the small spot laser or the electron beam of the small electron beam spot has sufficient energy to quickly form a patterned molybdenum silicide layer 50, the power density of the laser or electron beam is 1W / cm 2 ~10W / cm 2 .
[0044] In one embodiment, in order to react the molybdenum layer 30 with the silicon layer 20 and avoid evaporation of silicon and molybdenum materials, the energy and scanning speed of the laser or electron beam are controlled at a surface temperature of 400° C. to 800° C. At a temperature of 400° C. to 800° C., Mo atoms tend to move into the silicon layer 20 and form molybdenum silicide. Preferably, in order to ensure complete reaction of molybdenum and silicon, the energy and scanning speed of the laser or electron beam are controlled at a surface temperature of 500° C. to 800° C.
[0045] In one embodiment, the scanning time of the laser or electron beam is 10min~30min. Specifically, it has been verified by experiments that after the molybdenum silicon stacking layer 40 is heat-treated to consume the molybdenum layer 30, if the heating is continued for a long time, the Mo atoms in the patterned molybdenum silicide layer 50 will be evenly distributed. Although the thickness of the patterned molybdenum silicide layer 50 will not increase, the Mo atoms in the patterned molybdenum silicide layer 50 will not be distributed in a gradient, and the patterned molybdenum silicide layer 50 cannot absorb ultraviolet light by intra-layer reflection, so that the optical absorption rate of the molybdenum silicide layer 50 is poor. Therefore, after the molybdenum layer 30 is consumed, the heating is stopped after adding 5%~10% of the scanning time. In this embodiment, in order to ensure that the Mo atoms are completely moved to the silicon layer 20 to completely consume the molybdenum layer 30, and to ensure that the Mo atoms in the patterned silicide layer 50 are distributed according to the preset Mo atom distribution gradient, the time for laser or electron beam scanning of the molybdenum silicon stacking layer 40 is controlled to be 10min~30min.
[0046] In one embodiment, after step S13, the following step may be further included: injecting at least one of nitrogen atoms, oxygen atoms or carbon atoms into the patterned molybdenum silicide layer 50. In this embodiment, by injecting a small amount of at least one of nitrogen atoms, oxygen atoms or carbon atoms into the patterned molybdenum silicide layer 50, the light absorption rate of the patterned molybdenum silicide layer 50 can be further enhanced, and the adhesion of the interface between the patterned molybdenum silicide layer 50 and the transparent substrate 10 can be enhanced.
[0047] The manufacturing method of the above-mentioned OMOG photomask can minimize the thickness of the molybdenum silicide layer and maximize the absorbance, and can achieve the development goal of the minimum thickness of the molybdenum silicide layer and the highest absorbance required by the OMOG photomask. In addition, the manufacturing method of the above-mentioned OMOG mask substrate can effectively reduce the process cost, which is conducive to saving the manufacturing cost of the OMOG photomask.
[0048] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of the technical solution of the present invention.
Claims
1. A method for manufacturing an OMOG photomask, It is characterized in that The following steps are involved: providing a transparent substrate; Alternatingly depositing silicon layers and molybdenum layers on the transparent substrate in sequence to form a molybdenum-silicon stacked layer; Performing patterned laser or electron beam direct writing scanning on the molybdenum-silicon stacked layer, so that the Mo atoms in the molybdenum layer in the area scanned by the laser or the electron beam are completely moved into the silicon layer to form a patterned molybdenum silicide layer, wherein the patterned molybdenum silicide layer has a preset thickness, preset Mo and Si contents, and a preset Mo atomic distribution gradient; removing the unreacted silicon layer and molybdenum layer to form an OMOG photomask; The silicon layer and the molybdenum layer are deposited by a thin film deposition process, and the thin film deposition process controls the thickness of the silicon layer and the molybdenum layer respectively according to the preset thickness, the preset Mo and Si contents, and the preset Mo atomic distribution gradient.
2. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The laser or the electron beam is focused on the molybdenum layer.
3. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The power density of the laser or the electron beam is 1 W / cm 2 ~10W / cm 2 .
4. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The surface temperature of the laser or the electron beam is 400° C. to 800° C.
5. The method for manufacturing an OMOG photomask according to claim 4, It is characterized in that The surface temperature of the laser or the electron beam is 500° C. to 800° C.
6. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The scanning time of the laser or the electron beam is 10 min to 30 min.
7. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The thickness of the silicon layer and the thickness of the molybdenum layer are both no greater than 30 nm.
8. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The preset Mo and Si contents are such that the content of Mo atoms is not greater than 50% of the content of Si atoms.
9. The method for manufacturing an OMOG photomask according to claim 8, It is characterized in that The preset Mo and Si contents are such that the content of Mo atoms is 30% to 45% of the content of Si atoms.
10. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that The thin film deposition process includes a sputtering deposition process or an atomic layer deposition process.
11. The method for manufacturing an OMOG photomask according to claim 1, It is characterized in that After the step of forming the patterned molybdenum silicide layer with preset Mo and Si contents, the method further includes the following step: injecting at least one of nitrogen atoms, oxygen atoms or carbon atoms into the patterned molybdenum silicide layer.