Preparation method of stacked nanosheet fence field effect transistor and field effect transistor
By using the preparation method of stacked nanosheet fence field effect transistors in nanosheet fence field effect transistors, the structure is simplified and the parasitic capacitance is reduced, and the problem of limited circuit working rate in NS GAAFET devices is solved, and more efficient circuits are achieved performance.
Patent Information
- Application Number
- CN202410814338.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-01
AI Technical Summary
The device structure of nanosheet fenced field effect transistor (NS GAAFET) has a complex structure and large parasitic capacitance, which limits the improvement of its circuit operating speed.
By using the preparation method of stacked nanosheets, a plurality of silicon material nanosheets and a plurality of silicon alloy layers are deposited on the substrate, an etching is formed into a retraction cavity, and a protective layer is prepared therein to Reduce parasitic capacitance, remove high dielectric constant, and form air side walls to reduce capacitance.
The structure of NS GAAFET is simplified, the parasitic capacitance is significantly reduced, the working efficiency and speed of the circuit are improved, and the performance of the field effect tube is optimized.
Smart Images

Figure CN118888445A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a stacked nanosheet gate field effect transistor and a field effect transistor. Background Art
[0002] As the size of integrated circuits continues to shrink, traditional planar metal oxide semiconductor field effect transistors and fin field effect transistors have reached the physical limits of their structures. For technology nodes below 3nm, the gate-all-around field-effect transistor (GAAFET) has become a key structure for further miniaturization due to its excellent gate control performance and good compatibility with FinFET processes. The nanosheet structure GAAFET (NSGAAFET) in GAAFET is a more common device structure in gate-all-around devices at technology nodes below 3nm.
[0003] However, the NS GAAFET device structure in the related art is relatively complex and has a large parasitic capacitance, which is one of the main factors limiting the improvement of its circuit operating speed.
[0004] The above statements are only used to provide background information related to the present application and do not necessarily constitute prior art. Summary of the invention
[0005] In view of the technical problem that the device structure of the nanosheet gate transistor in the related art is relatively complex and has a large parasitic capacitance, which limits the operating speed of its circuit, the purpose of this application is to provide a method for preparing a stacked nanosheet gate field effect transistor and a field effect transistor, so as to simplify its structure, reduce the parasitic capacitance of the nanosheet gate transistor, and improve its circuit operating speed. In order to have a basic understanding of some aspects of the disclosed embodiments, a simple summary is given below. This summary section is not a general review, nor is it intended to identify key / important components or describe the scope of protection of these embodiments. Its only purpose is to present some concepts in a simple form as a preface to the detailed description that follows.
[0006] According to one aspect of an embodiment of the present application, a method for preparing a stacked nanosheet gate field effect transistor is provided, comprising:
[0007] Depositing on a substrate to form a stacked layer, the stacked layer comprising a plurality of silicon material nanosheet layers and a plurality of silicon alloy layers alternately stacked;
[0008] Etching the silicon alloy layer to form a first retraction cavity, wherein the first retraction cavity is located between two adjacent silicon material nanosheet layers;
[0009] A protective layer covering the inner surface of the first retraction cavity is prepared in the first retraction cavity, wherein the protective layer is recessed to form a second retraction cavity;
[0010] A gate and two source and drain electrodes are prepared on the substrate based on the second retracted cavity, and an air sidewall is formed between the gate and any of the source and drain electrodes;
[0011] The first dielectric constant medium in the first space is removed; the first space is the space in the air sidewall surrounded by the upper surface of the highest silicon material nanosheet layer, the gate, and any of the source and drain electrodes.
[0012] According to some embodiments of the present application, depositing on a substrate to form a stack includes:
[0013] Providing a silicon substrate, and sequentially performing well photolithography, ion implantation and annealing on the silicon substrate;
[0014] A stack is deposited on the surface of the annealed structure.
[0015] According to some embodiments of the present application, preparing a gate and two source and drain electrodes located on the substrate based on the second retraction cavity includes:
[0016] Prepare two solid sidewalls, a first source and drain electrode, a second source and drain electrode, and a gate electrode, wherein the plurality of silicon material nanosheet layers are located between the two solid sidewalls, and the second retracted cavities are all filled with the corresponding solid sidewalls;
[0017] The two solid side walls are removed to form two air side walls.
[0018] According to some embodiments of the present application, the step of preparing two solid side walls comprises:
[0019] depositing an amorphous silicon thin film on the substrate;
[0020] A target pattern formed by photolithography on the amorphous silicon thin film;
[0021] Depositing a hard mask layer on the amorphous silicon film having the target pattern formed thereon;
[0022] The amorphous silicon film formed with the hard mask layer is etched to form two solid sidewalls.
[0023] According to some embodiments of the present application, the step of preparing the first source and drain, the second source and drain, and the gate includes:
[0024] Removing the hard mask layer by anisotropic etching to obtain a plurality of fin structures;
[0025] Filling an insulating medium between the fin structures to form shallow trench isolation between the fin structures;
[0026] removing the depression of the shallow trench isolation;
[0027] A first source and drain, a second source and drain, and a gate are etched on the fin structure.
[0028] According to some embodiments of the present application, etching a first source and drain, a second source and drain, and a gate on the fin structure includes:
[0029] An insulating layer and a silicon layer are sequentially deposited on the surface of the uppermost silicon material nanosheet layer in the fin structure;
[0030] Etching the silicon layer to form a dummy gate structure;
[0031] Prepare sidewall structures and source and drain regions on both sides of the dummy gate structure;
[0032] forming a first source-drain electrode and a second source-drain electrode on the source-drain region;
[0033] removing the dummy gate structure to form a gate region;
[0034] removing the silicon alloy layer in the stack to release the nanosheet channel;
[0035] A gate is formed by deposition in the gate region.
[0036] According to some embodiments of the present application, a spacer structure is prepared on both sides of the dummy gate structure, including:
[0037] Depositing a sidewall isolation dielectric film;
[0038] A sidewall structure is formed by etching on the surface of the sidewall isolation dielectric film.
[0039] According to some embodiments of the present application, the method further includes: removing the protective layer.
[0040] According to some embodiments of the present application, it further includes:
[0041] Depositing to form an isolation layer, wherein the isolation layer covers the air side wall;
[0042] Etching a contact hole on the isolation layer;
[0043] A tungsten material is deposited in the contact hole to form a tungsten plug.
[0044] According to some embodiments of the present application, the protective layer is an amorphous carbon layer.
[0045] According to another aspect of an embodiment of the present application, a stacked nanosheet gate field effect transistor is provided, which is prepared by the preparation method described in any embodiment of the present application, and the stacked nanosheet gate field effect transistor includes:
[0046] substrate;
[0047] A first source and a drain and a second source and a drain located on the substrate;
[0048] A gate, located on the substrate, between the first source-drain electrode and the second source-drain electrode, and having an air sidewall formed between the first source-drain electrode and the second source-drain electrode;
[0049] A plurality of silicon material nanosheet layers are arranged in the gate at intervals, each of the silicon material nanosheet layers is respectively connected to the first source and drain and the second source and drain, and each of the silicon material nanosheet layers is parallel to the upper surface of the substrate.
[0050] The technical solution provided by one aspect of the embodiments of the present application may have the following beneficial effects:
[0051] The method for preparing a stacked nanosheet gate field effect transistor provided in an embodiment of the present application comprises depositing a stack on a substrate, wherein the stack comprises a plurality of silicon material nanosheet layers and a plurality of silicon alloy layers alternately stacked, etching the silicon alloy layer to form a first retraction cavity, wherein the first retraction cavity is located between two adjacent silicon material nanosheet layers, preparing a protective layer covering the inner surface of the first retraction cavity in the first retraction cavity, wherein the protective layer is recessed to form a second retraction cavity, and preparing a gate and two source and drain electrodes located on the substrate based on the second retraction cavity, wherein an air side wall is formed between the gate and any of the source and drain electrodes, and the first dielectric constant medium in the first space is removed; the first space is the space enclosed by the upper surface of the highest silicon material nanosheet layer, the gate, and any of the source and drain electrodes in the air side wall, and the structure of the prepared stacked nanosheet gate field effect transistor is relatively simple, the parasitic capacitance is greatly reduced, and the working efficiency of the circuit in which the stacked nanosheet gate field effect transistor is located can be improved.
[0052] The above description is only an overview of the technical solution of the embodiment of the present application. In order to more clearly understand the technical means of the embodiment of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0054] Figure 1 A schematic diagram of the three-dimensional structure of a stacked nanosheet gate field effect transistor according to an embodiment of the present application is shown.
[0055] Figure 2 A cross-sectional view of a stacked nanosheet gate field effect transistor along line XX′ according to an embodiment of the present application is shown.
[0056] Figure 3 A cross-sectional view of a stacked nanosheet gate field effect transistor along line YY' according to an embodiment of the present application is shown.
[0057] Figure 4 A flow chart of a method for preparing a stacked nanosheet gate field effect transistor according to an embodiment of the present application is shown.
[0058] Figure 5 A cross-sectional view along line XX' of a structure obtained after each step (a) to step (d) in a preparation method according to another embodiment of the present application is shown.
[0059] Figure 6 A cross-sectional view along line YY' of a structure obtained after each step (a) to step (d) in a preparation method according to another embodiment of the present application is shown.
[0060] Figure 7 A cross-sectional view along line XX' of a structure obtained after each step (e) to step (h) is performed in a preparation method according to another embodiment of the present application is shown.
[0061] Figure 8 A cross-sectional view along line YY' of a structure obtained after each step (e) to step (h) in a preparation method according to another embodiment of the present application is shown.
[0062] Fig. 9 A cross-sectional view along line XX' of a structure obtained after each step (i) to step (l) in a preparation method according to another embodiment of the present application is shown.
[0063] Fig.10 A cross-sectional view along line YY' of a structure obtained after each step (i) to (l) in a preparation method according to another embodiment of the present application is shown.
[0064] Fig.11 A cross-sectional view along line XX' of a structure obtained after each step from step (m) to step (p) in a preparation method according to another embodiment of the present application is shown.
[0065] Fig.12A cross-sectional view along line YY' of a structure obtained after each step from step (m) to step (p) in a preparation method according to another embodiment of the present application is shown.
[0066] Fig.13 A cross-sectional view along line XX' of a structure obtained after each step from step (q) to step (t) in a preparation method according to another embodiment of the present application is shown.
[0067] Fig.14 A cross-sectional view along line YY' of a structure obtained after each step from step (q) to step (t) in a preparation method according to another embodiment of the present application is shown.
[0068] Fig.15 A cross-sectional view along line XX' of a structure obtained after each step (u) to step (w) in a preparation method according to another embodiment of the present application is shown.
[0069] Fig.16 A cross-sectional view along line YY' of a structure obtained after each step (u) to step (w) in a preparation method according to another embodiment of the present application is shown. DETAILED DESCRIPTION
[0070] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0071] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as here.
[0072] GAAFET includes nanowire structure (NW GAAFET) and nanosheet structure (NS GAAFET). The nanosheet structure can obtain a larger driving current per unit projected area than the nanowire structure. Therefore, NS GAAFET has become the device structure in the gate-all-around device at technology nodes below 3nm.
[0073] The parasitic capacitance of NS GAAFET mainly includes the gate and source-drain capacitance (C gs / ), gate and substrate capacitance (Cgb ) and the parasitic capacitance of the inner and outer walls of adjacent nanosheets (C cr, ), where C gs / Since the area between the gate and the source and drain is large and the dielectric layer is thin, it becomes the main part of the parasitic capacitance.
[0074] C gs / It is not only affected by the overlapping area between the gate and the source-drain epitaxial region and the source-drain electrode, but also by the dielectric constant value of the medium between the gate and the source-drain epitaxial region and the source-drain electrode, the width of the dielectric layer, and other factors. gs / There is SiN between the gate and the source and drain epitaxial regions. x and HfO2(κ SiO2 ≈3.9), there are SiO2, SiN between the electrodes x And HfO2, among which HfO2 material has the largest κ value, which makes the parasitic capacitance at the side wall position larger, thus affecting the operating speed of the device and circuit.
[0075] A method for preparing a stacked nanosheet gate field effect transistor and a field effect transistor according to an embodiment of the present application are described below in conjunction with the accompanying drawings.
[0076] refer to Figures 1 to 3 As shown, an embodiment of the present application provides a stacked nanosheet gate field effect transistor, comprising: a substrate 8; a first source and drain electrode 1 and a second source and drain electrode 2 located on the substrate 8; a gate 3 located on the substrate 8, located between the first source and drain electrode 1 and the second source and drain electrode 2, and an air sidewall 27 is formed between the first source and drain electrode 1 and the second source and drain electrode 2; a plurality of silicon material nanosheet layers 7, arranged in the gate 3 at intervals, each silicon material nanosheet layer 7 is respectively connected to the first source and drain electrode 1 and the second source and drain electrode 2, and each silicon material nanosheet layer 7 is parallel to the upper surface of the substrate 8. The portion of the silicon material nanosheet layer 7 connected to the first source and drain electrode 1 is located outside the gate 3, and the portion of the silicon material nanosheet layer 7 connected to the second source and drain electrode 2 is located outside the gate 3. Figure 1 A straight line XX' and a straight line YY' are shown in FIG.
[0077] Each silicon material nanosheet layer 7 is connected to the first source-drain electrode 1 and the second source-drain electrode 2 through the epitaxial layer 20 .
[0078] Since air has the lowest dielectric constant, the air sidewalls 27 can greatly reduce the parasitic capacitance.
[0079] In some embodiments, the stacked nanosheet gate-all-around field effect transistor may further include:
[0080] The first insulating layer 28 covers the gate 3, the first drain-source electrode 1 and the second drain-source electrode 2; the first contact electrode 4 is arranged in the first insulating layer 28, the first end of which is in contact with the first source-drain electrode 1, and the second end of which is exposed from the top surface of the first insulating layer 28; the second contact electrode 5 is arranged in the first insulating layer 28, the first end of which is in contact with the second source-drain electrode 2, and the second end of which is exposed from the top surface of the first insulating layer 28.
[0081] Exemplarily, the stacked nanosheet gate field effect transistor further includes: an amorphous silicon layer 31 located between the gate 3 and the substrate 8 .
[0082] The stacked nanosheet gate field effect transistor of the embodiment of the present application has a simple structure, small parasitic capacitance and high operating speed.
[0083] There is a high dielectric constant material in the portion of the air side wall 27 located between two adjacent epitaxial layers 20. This portion of high dielectric constant material can increase the driving current of the field effect transistor and reduce the on-resistance of the field effect transistor, thereby optimizing the performance of the circuit formed by the field effect transistor, such as reducing the inverter delay and increasing the frequency of the ring oscillation circuit.
[0084] refer to Figure 4 As shown, another embodiment of the present application provides a method for preparing a stacked nanosheet gate field effect transistor of any of the above embodiments, which may include:
[0085] S10, depositing on a substrate to form a stacked layer, wherein the stacked layer includes a plurality of silicon material nanosheet layers and a plurality of silicon alloy layers alternately stacked.
[0086] Exemplarily, depositing a stack on a substrate may include: providing a silicon substrate, sequentially performing well lithography, ion implantation, and annealing on the silicon substrate; and depositing a stack on a surface of the annealed structure.
[0087] S20, etching the silicon alloy layer to form a first retraction cavity, wherein the first retraction cavity is located between two adjacent silicon material nanosheet layers.
[0088] Specifically, both ends of the silicon alloy layer are etched to remove a portion of the layer, thereby forming a recessed portion between two adjacent silicon material nanosheet layers, the recessed portion being the first retraction cavity.
[0089] S30, preparing a protective layer covering the inner surface of the first retraction cavity in the first retraction cavity, wherein the protective layer is recessed to form a second retraction cavity.
[0090] Specifically, the protective layer may be an amorphous carbon layer, and the thickness of the protective layer is less than 1 / 2 of the etching depth when etching the silicon alloy layer to form the first retraction cavity.
[0091] An amorphous carbon layer can be deposited in the first retraction cavity to form a protective layer, and the recessed portion on the protective layer forms a second retraction cavity. The protective layer is used to protect the high dielectric constant material from being removed. The high dielectric constant material can increase the driving current per unit projected area, thereby reducing the on-resistance of the field effect tube and optimizing the circuit performance of the field effect tube, for example, it can reduce the inverter delay and increase the frequency of the ring oscillation circuit.
[0092] S40, preparing a gate and two source and drain electrodes on the substrate based on the second retracted cavity, wherein an air sidewall is formed between the gate and any of the source and drain electrodes.
[0093] The two source and drain electrodes are respectively referred to as the first source and drain electrode and the second source and drain electrode. Exemplarily, preparing a gate electrode and two source and drain electrodes located on the substrate based on the second retraction cavity may include: preparing two solid sidewalls, a first source and drain electrode, a second source and drain electrode, and a gate electrode, wherein the plurality of silicon material nanosheet layers are located between the two solid sidewalls, and the second retraction cavity is filled with the corresponding solid sidewalls; and removing the two solid sidewalls to form two air sidewalls.
[0094] Exemplarily, preparing two solid sidewalls may include: depositing an amorphous silicon film on the substrate; photolithographically forming a target pattern on the amorphous silicon film; depositing a hard mask layer on the amorphous silicon film having the target pattern; and etching the amorphous silicon film having the hard mask layer to form two solid sidewalls.
[0095] Exemplarily, preparing a first source and drain, a second source and drain, and a gate includes: removing the hard mask layer by anisotropic etching to obtain a plurality of fin structures; filling an insulating medium between each of the fin structures to form a shallow trench isolation between each of the fin structures; removing the recess of the shallow trench isolation; and etching a first source and drain, a second source and drain, and a gate on the fin structure.
[0096] Exemplarily, a first source and drain, a second source and drain, and a gate are etched on the fin structure, including: depositing an insulating layer and a silicon layer in sequence on the surface of the uppermost silicon material nanosheet layer in the fin structure; etching the silicon layer to form a dummy gate structure; preparing a sidewall structure and a source and drain region on both sides of the dummy gate structure; forming a first source and drain and a second source and drain on the source and drain region; removing the dummy gate structure to form a gate region; removing the silicon alloy layer in the stack to release a nanosheet channel; and depositing a gate in the gate region.
[0097] Exemplarily, preparing the sidewall structures on both sides of the dummy gate structure includes: depositing a sidewall isolation dielectric film; and etching on the surface of the sidewall isolation dielectric film to form the sidewall structures.
[0098] S50, removing the first dielectric constant medium in the first space, where the first space is the space in the air sidewall surrounded by the upper surface of the highest silicon material nanosheet layer, the gate, and any of the source and drain electrodes.
[0099] The first dielectric constant medium is a medium with a dielectric constant greater than a preset value, and is a medium with a relatively high dielectric constant, that is, a high dielectric constant medium. Removing the first dielectric constant medium in the first space can reduce the parasitic capacitance of the GAAFET. In addition, the first dielectric constant medium of the part covered and protected by the protective layer in the air side wall is not removed. The first dielectric constant medium that is not removed can reduce the on-resistance of the GAAFET, reduce the delay of the circuit composed of the device, and increase the circuit frequency, such as reducing the inverter delay and increasing the ring oscillation circuit frequency.
[0100] S60: removing the protective layer.
[0101] Specifically, the protective layer can be removed by dry etching or wet etching. The protective layer can be, for example, an amorphous carbon layer. Removing the protective layer can further reduce the parasitic capacitance of the semiconductor device.
[0102] In some implementations, the preparation method may further include: depositing to form an isolation layer, the isolation layer covering the air sidewall; etching a contact hole on the isolation layer; and depositing tungsten material in the contact hole to form a tungsten plug.
[0103] refer to Figures 5 to 16 As shown, an embodiment of the present application provides a method for preparing a stacked nanosheet gate field effect transistor, which may include the following steps:
[0104] (a) Silicon substrate doping: well lithography, implantation and annealing.
[0105] A silicon substrate 8 is provided, and well lithography, ion implantation and annealing are sequentially performed on the substrate 8. In the well lithography process, a photoresist layer is covered on the surface of the substrate 8, and then a desired pattern is transferred to the photoresist layer through a mask, and the photoresist layer is exposed to light, and the part of the photoresist layer not exposed to light is removed by development to form a desired pattern.
[0106] During the ion implantation process, dopants of a preset type and concentration are implanted into the silicon substrate in the area of the pattern formed by well lithography through ion implantation technology. These dopants can change the conductive properties of the silicon substrate to form source and drain regions.
[0107] During the annealing process of the silicon substrate that has been treated with ion implantation, the silicon substrate is heated to a preset temperature to activate the dopants implanted by the ion implantation operation and repair the crystal structure of the silicon substrate implanted with the dopants, thereby reducing the crystal defects of the silicon substrate implanted with the dopants and improving the diffusion degree of the dopants.
[0108] (b) Laminated epitaxy.
[0109] The surface of the annealed structure is cleaned to remove impurities or residues on the surface of the structure, providing a substrate suitable for stacked epitaxial growth, and then multiple silicon alloy layers 30 and multiple nanosheet layers 7 are alternately deposited on the surface of the annealed structure by chemical vapor deposition (CVD) or molecular beam epitaxy (MBE) and other techniques, wherein a silicon alloy layer 30 is deposited on the substrate 8, and then a nanosheet layer 7 is deposited on the isolation layer, and then an isolation layer is deposited on the nanosheet layer, until a preset number of nanosheet layers 7 are deposited, for example, as shown in the figure, a total of three nanosheet layers 7 are formed, the silicon alloy layer 30 is SiGe material or SiGa material, and the nanosheet layer 7 is made of silicon material. The width range of the nanosheet layer 7 can be, for example, 5-50nm, and the thickness range of the nanosheet layer 7 can be, for example, 3-20nm.
[0110] During the epitaxial growth process, the thickness of the stack 7 of SiGe material or SiGa material can be adjusted by controlling the epitaxial growth conditions (such as temperature, gas pressure, and material ratio in the gas phase, etc.).
[0111] (c) Side wall transfer.
[0112] Core layer (core layer is made of amorphous silicon a-Si material) deposition and patterning (photolithography, etching) processing: using chemical vapor deposition (CVD) or physical vapor deposition (PVD) and other technologies, an amorphous silicon (a-Si) film is deposited on a silicon substrate to form a core layer 9; using photolithography technology, a photoresist is coated on the amorphous silicon film, and then a mask lithography machine is used to expose a specific pattern on the photoresist, and finally the photoresist in the unexposed area is removed using development and other processes to form the desired pattern.
[0113] Hard mask (HM) film deposition: Deposition of silicon nitride (SiN) on amorphous silicon film using chemical vapor deposition (CVD) or physical vapor deposition (PVD) techniques. x ) or silicon oxide (SiO2) or other materials to form the hard mask film 10.
[0114] Sidewall etching: The silicon nitride or silicon oxide film is patterned by placing the sample in an etching chamber and etching the film with an etching gas (such as hydrogen fluoride) to form the desired sidewall structure.
[0115] The core layer selective removal includes: using chemical solutions or plasma etching techniques to selectively remove the amorphous silicon film (core layer), leaving the required silicon nitride or silicon oxide film, thereby forming the key structure of the transistor.
[0116] (d) Fabrication of a fin structure.
[0117] The hard mask film 10 is removed by anisotropically etching SiGe / Si Fin to obtain a fin structure (the fin structure is also called a Fin structure).
[0118] Figure 5 The structure obtained after steps (a), (b), (c) and (d) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Figure 6 The structure obtained after steps (a), (b), (c) and (d) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0119] (e) Fabrication of shallow trench isolation (STI).
[0120] A low-temperature insulating dielectric layer 11 (HARP or FCVD) is deposited to fill the insulating dielectric between the fin structures to achieve isolation between the fin structures.
[0121] Specifically, a low-temperature insulating dielectric layer 11 is deposited between and around the fin structures using chemical vapor deposition (CVD) technology. HARP (High Aspect Ratio Process) or FCVD (Flowable Chemical Vapor Deposition) is usually used to achieve uniform deposition in high aspect ratio structures. This step is intended to fill the gaps between the fin structures.
[0122] The low-temperature annealing treatment makes the low-temperature insulating dielectric layer 11 more stable by heating, and enhances the adhesion between the low-temperature insulating dielectric layer 11 and the fin structure.
[0123] Specifically, the current semiconductor structure is heat treated at a controlled low temperature (usually below 500°C) to cause the molecular structure of the insulating medium to rearrange, thereby improving its density and stability.
[0124] The dielectric CMP (chemical mechanical polishing) process is to remove excess insulating dielectric from the surface of the fin structure and the chip surface to make the surface flat and ensure the accuracy of subsequent process steps.
[0125] Specifically, chemical mechanical polishing technology is used to grind the insulating dielectric layer on the surface by using mechanical abrasives in a specific chemical solution, so that the height of the fin structure and the chip surface is consistent.
[0126] The HM (hard mask) and STI recess are removed to remove residual impurities on the surface of the fin structure to ensure the purity and stability of the fin structure.
[0127] Specifically, chemical solutions or plasma treatment techniques are used to remove residues deposited between the fin structure surface and STI (shallow trench isolation), such as etching residues or oxide layers. This step may also include processing the STI area to adjust its surface morphology and properties to ensure that the next process steps proceed smoothly.
[0128] The surface morphology and depth of the STI recess can be adjusted by etching. Etching can be done by dry etching, such as plasma etching or reactive ion etching (RIE), or by wet etching, such as chemical mechanical polishing (CMP). STI (Shallow Trench Isolation) is a commonly used process technology in integrated circuit manufacturing, used to isolate different devices on an integrated circuit chip. STI recess refers to the step of retreating in the STI process. In the STI process, a layer of oxide film is first formed on the surface of the silicon wafer, and then a shallow groove is formed on the surface of the silicon wafer through photolithography and etching processes. Next, an insulating material (usually silicon dioxide SiO2) is filled in the shallow groove to achieve electrical isolation between devices. STI recess means that after filling the insulating material, it is necessary to grind it, retreat the slope, and other steps to make the insulating material and the silicon wafer surface basically flat for subsequent device manufacturing processes.
[0129] The main purpose of the STI recess step is to make the upper surface of the low-temperature insulating dielectric layer 11 obtained by filling the insulating material and the upper surface of the silicon substrate 8 be located on the same plane, thereby providing a flat surface for subsequent processes. This step is very important for ensuring that subsequent processes such as photolithography, deposition, and etching can be carried out accurately, because the flat surface can ensure the accuracy of the photolithography pattern and is also conducive to the production of metal wire connections.
[0130] (f) Fabricating a dummy gate structure.
[0131] An oxide layer 12 (the oxide layer may be a GOX material), a non-single silicon layer 13 (the non-single silicon layer 13 may be, for example, an a-Si or p-Si layer) and a hard mask layer 14 are deposited in sequence.
[0132] The step of depositing the oxide layer 12 specifically includes: using chemical vapor deposition (CVD) or physical vapor deposition (PVD) technology to deposit an insulating layer (usually silicon dioxide SiO2) on the surface of the substrate to obtain the oxide layer 12. The temperature, pressure, gas flow rate and other parameters during the deposition process are controlled to obtain the desired oxide layer thickness.
[0133] The deposition step of the non-single silicon layer 13 (amorphous silicon a-Si or polycrystalline silicon p-Si) may specifically include: using CVD or PVD technology to deposit an amorphous silicon (a-Si) or polycrystalline silicon (p-Si) layer on the oxide layer 12 to form a non-single silicon layer 13, and the non-single silicon layer 13 is used as the main part of the dummy gate structure. Parameters such as temperature, pressure and gas flow rate during the deposition process are controlled to obtain the desired silicon layer thickness.
[0134] The operation process of depositing the hard mask layer 14 may include: depositing a hard mask layer 14 on the silicon layer using CVD or PVD technology to protect the gate structure. Controlling parameters such as temperature, pressure and gas flow rate during the deposition process to obtain the desired hard mask layer thickness. The hard mask layer can be referred to as HM (i.e. hard mask).
[0135] The process of gate photolithography and etching may include: designing the gate pattern on the mask template of the photolithography layer, then exposing the pattern to the photoresist layer through a photolithography machine, developing the exposed area of the photoresist layer to dissolve or remove it, and forming a photoresist layer of the gate pattern. Using the photoresist layer pattern as a mask, the non-single silicon layer 13 and the oxide layer 12 are etched, and dry etching (such as plasma etching) or wet etching (such as chemical etching) can be used. The photoresist layer is cleaned and removed to expose the gate pattern to form a final dummy gate structure. The dummy gate structure is used to reserve space for the subsequent formation of the gate.
[0136] (g) Deposition to form a sidewall isolation dielectric film.
[0137] Deposition of isolation dielectric film: Use chemical vapor deposition (CVD) or physical vapor deposition (PVD) technology to uniformly deposit a layer of isolation dielectric film on the entire surface. Control parameters such as temperature, pressure and gas flow during the deposition process to obtain the required dielectric film thickness.
[0138] Sidewall formation: On the surface of the deposited dielectric film, a sidewall structure 15 is formed by processes such as photoresist deposition, photolithography, development and etching.
[0139] Etching of the dielectric film for sidewall isolation: Cover the dielectric film for sidewall isolation with photoresist, and expose the desired pattern on the photoresist layer through a photolithography machine. The pattern design should include the desired sidewall shape. The exposed area in the photoresist layer is developed to dissolve or remove it, forming a photoresist pattern for the dielectric film for sidewall isolation. Using the photoresist pattern as a mask, etching is performed on the dielectric film surface to form a sidewall structure 15.
[0140] The etching process can use dry etching or wet etching, depending on the material and process requirements.
[0141] The photoresist layer is removed by cleaning to expose the sidewall structure 15 formed finally.
[0142] Through the above steps, the deposition and etching operations of the sidewall isolation dielectric film are completed, forming the required sidewall structure 15. The sidewall structure 15 can be used to isolate and control the electrical properties between electronic components during the integrated circuit manufacturing process.
[0143] (h) Etching the drain and source regions 16 on the fin structure.
[0144] The fin structure is covered with photoresist, and a required pattern is exposed on the photoresist layer by a photolithography machine. The pattern includes the required source and drain region positions and shapes.
[0145] The exposed area of the photoresist layer is developed to dissolve or remove the photoresist layer, thereby forming a photoresist pattern of the source and drain regions. The photoresist pattern is used as a mask to perform etching in the fin structure region, thereby forming the source and drain regions 16 .
[0146] Through the above steps, the operation of etching the drain and source regions 16 on the fin structure is completed, forming the required source and drain regions 16. The source and drain regions 16 are used to connect the source and drain of the transistor to realize current injection and output, thereby controlling the working state of the transistor.
[0147] Figure 7 The structure obtained after steps (e), (f), (g) and (h) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Figure 8 The structure obtained after steps (e), (f), (g) and (h) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0148] (i) The silicon alloy layer 30 is etched to form the first retraction cavity 17 .
[0149] When etching the silicon alloy layer 30, the photoresist pattern is used as a mask to etch the silicon alloy layer 30 region to form a first pull-back cavity 17. The etching process can use dry etching or wet etching, depending on the material and process requirements.
[0150] The material of the silicon alloy layer 30 includes SiGe material or SiGa material, and the specific electrical characteristics of the device can be achieved through the retraction cavity 17 .
[0151] (j) depositing an amorphous carbon material (or other material) to form a protective layer 33 (the thickness of the protective layer 33 is less than 1 / 2 of the SiGe etching depth), and anisotropically etching the protective layer 33 to form a second retraction cavity 34.
[0152] Amorphous carbon layers can be prepared by techniques such as chemical vapor deposition (CVD) or physical vapor deposition (PVD). In CVD, a carbon source gas (such as methane) is decomposed and deposited on the substrate to form an amorphous carbon layer; while in PVD, carbon atoms are deposited on the substrate by evaporation or sputtering to form an amorphous carbon layer.
[0153] (k) Deposit SiNx material to form the inner sidewall isolation dielectric film 18.
[0154] Using deposition techniques such as chemical vapor deposition (CVD) or physical vapor deposition (PVD), an inner wall isolation dielectric film 18 is deposited on the inner wall surface of the SiGe pull-back cavity. Common isolation dielectric materials include silicon nitride (Si3N4) or silicon oxide (SiO2), and the material selection depends on the process and device requirements.
[0155] (l) Etching the inner sidewall isolation dielectric film 18.
[0156] After etching the inner sidewall isolation dielectric film 18, a remaining portion 19 of the film is obtained.
[0157] (m) Source and drain epitaxy to obtain the epitaxial layer 20.
[0158] Select appropriate materials for source and drain epitaxy for P / NMOS devices. For P-type MOS (PMOS), SiGe materials can be used for epitaxy; for N-type MOS (NMOS), silicon (Si) materials can be used for epitaxy. The epitaxy process uses chemical vapor deposition (CVD) or molecular beam epitaxy (MBE) and other technologies to deposit corresponding materials in the source and drain regions.
[0159] Fig. 9 The structure obtained after steps (i), (j), (k) and (l) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Fig.10 The structure obtained after steps (i), (j), (k) and (l) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0160] (n) Source and drain doping.
[0161] Inner wall etching: Etching is performed on the inner wall of the SiGe pull-back cavity using chemical etching or plasma etching techniques. The purpose of this step is to remove the SiGe material to form a smooth inner wall surface.
[0162] Source and drain doping: source and drain doping is performed on the PMOS / NMOS device respectively to obtain a doped layer 21. For PMOS, a P-type dopant (such as boron) is used to dope the source and drain regions; for NMOS, an N-type dopant (such as arsenic or phosphorus) is used to dope the source and drain regions. Doping can be performed by using ion implantation or molecular beam epitaxy to implant dopants into the source and drain regions.
[0163] (o) ILD layer deposition and planarization process.
[0164] ILD layer dielectric deposition: using chemical vapor deposition (CVD) or physical vapor deposition (PVD) and other technologies, an ILD layer dielectric layer 22 is deposited on the surface of the current semiconductor structure. The dielectric material of the ILD layer dielectric layer 22 includes silicon dioxide (SiO2), silicon nitride (Si3N4) or aluminum oxide (Al2O3). The deposited dielectric has the characteristics of being flat, uniform and dense. The deposited dielectric is planarized to ensure that the surface of the dielectric layer is flat to avoid the influence of subsequent processes.
[0165] POP CMP (Planarization Chemical Mechanical Polishing): Use the chemical mechanical polishing (CMP) process to grind the current semiconductor structure surface through a rotating polishing disk and abrasive solution. This process aims to flatten the surface of the dielectric layer and eliminate height differences. Through the above steps, the ILD layer dielectric deposition and POP CMP operations are completed, which helps to improve the flatness of the semiconductor structure surface and provide a good foundation for subsequent processes.
[0166] (p) The dummy gate structure is removed to form a gate reserved region 23 . The dummy gate structure is the aforementioned non-single silicon layer 13 .
[0167] A wet chemical etching method may be used to immerse the current semiconductor structure in a suitable etching solution, such as a hydrofluoric acid (HF) solution or a mixed acid solution, to remove the dummy gate structure.
[0168] A dry etching method may also be used, using a plasma etching process, placing the current semiconductor structure in a reaction chamber, and removing the dummy gate structure under the action of a high-energy gas.
[0169] The etching or corrosion time and conditions are controlled to ensure that only the dummy gate structure is removed without damaging other areas.
[0170] (q) Release of nanosheet channel.
[0171] A wet etching method may be used to immerse the current semiconductor structure in a suitable etching solution, such as a hydrofluoric acid (HF) solution or a mixed acid solution, to remove the dielectric material next to the nanosheet channel, that is, to remove the remaining portion of the silicon alloy layer 30 and release the nanosheet channel.
[0172] A dry etching method can also be used, using a plasma etching process, to place the current semiconductor structure in a reaction chamber, and remove the dielectric material around the nanosheet channel under the action of high-energy gas, that is, to remove the remaining portion of the silicon alloy layer 30 and release the nanosheet channel. After the remaining portion of the silicon alloy layer 30 is completely removed, a void region 24 is formed.
[0173] Fig.11 The structure obtained after steps (m), (n), (o) and (p) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Fig.12 The structure obtained after steps (m), (n), (o) and (p) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0174] (r) An amorphous silicon layer, a mixed layer 32 and a polysilicon layer 25 are formed by deposition.
[0175] An amorphous silicon layer 31 is deposited on the upper surface of the substrate 8 .
[0176] The mixed layer 32 includes, from inside to outside, an intermediate layer, a high dielectric constant layer and a first barrier layer, wherein the intermediate layer wraps the silicon material nanosheet layer 7, the high dielectric constant layer wraps the intermediate layer, and the first barrier layer includes the high dielectric constant layer.
[0177] Interlayer (IL) deposition: an insulating layer (eg SiO 2 ) is deposited on the surface of the silicon material nanosheet layer 7 . The insulating layer is called an interlayer and is used to isolate different metal layers or functional layers.
[0178] High-K (HK) material deposition: Deposition of high-K materials (such as HfO2 or ZrO2) to replace traditional SiO2 as the gate dielectric layer to reduce the leakage current and power consumption of the transistor.
[0179] Deposition of the first barrier layer (Barrier Insertion, Barrier-I for short): Deposition of a barrier layer (the material of the barrier layer may be, for example, TiN or TaN) to prevent impurity diffusion and improve the reliability of electronic devices.
[0180] Polysilicon Work Function Layer 25 (P-WFL) deposition: The polysilicon layer is deposited to adjust the work function of the transistor gate to control the performance of the electronic device.
[0181] The photoresist is applied to the surface of the current semiconductor structure. The photoresist on the chip is exposed using a photolithography machine, and an image is formed on the glue layer according to the designed photolithography pattern. The exposed photoresist is developed, and the unexposed glue layer is removed to form a structure with a photolithography pattern.
[0182] Etching operations include dry etching and wet etching, wherein dry etching uses plasma etching technology to perform precise etching on the IL / HK / Barrier-I / P-WFL layer according to the photolithography pattern to form the required structure. Wet etching uses chemical solutions to wet-etch the IL / HK / Barrier-I / P-WFL layer to achieve a specific shape and size.
[0183] (s) Preparing a metal gate MG.
[0184] N-type polysilicon work function layer (N-WFL) deposition: depositing an N-type polysilicon layer onto the surface of the current semiconductor structure to adjust the functional parameters of the transistor gate. This layer is usually used to control the conductive properties of stacked nanosheet gate field effect transistors (FETs).
[0185] Barrier-II (Barrier Insertion II) deposition: Deposition of a second barrier layer to enhance the prevention of impurity diffusion and improve the reliability of electronic devices. This barrier layer usually forms an isolation layer between the N-WFL layer.
[0186] A tungsten layer 26 is deposited on the current semiconductor structure as a metal gate. The tungsten layer 26 can fill and connect various structures in the semiconductor structure, such as interconnection lines or resistors.
[0187] (t) Metal gate polishing (CMP).
[0188] CMP refers to Chemical Mechanical Polishing. CMP is a process that flattens and smoothes the surface of semiconductor products by combining mechanical and chemical methods. It is widely used in semiconductor manufacturing, especially to form a flat connection between metal layers and insulating layers. After polishing the deposited tungsten layer 26, the upper surface of the obtained metal gate is flush with the upper surface of the ILD layer dielectric layer 22.
[0189] (u) Side wall corrosion.
[0190] After the metal gate is polished, the SiN material of the sidewall is corroded, and the SiN dielectric of the sidewall is removed to form an air sidewall 27. Air has the lowest dielectric constant, so the air sidewall 27 can significantly reduce the parasitic capacitance of the stacked nanosheet gate field effect transistor. The first space 35 is the space surrounded by the upper surface of the highest silicon material nanosheet layer, the gate 3, and any source and drain in the air sidewall 27, that is, the first space 35 is a part of the air sidewall 27. The highest silicon material nanosheet layer is the silicon material nanosheet layer farthest from the upper surface of the substrate 8 in the direction perpendicular to the upper surface of the substrate 8. In addition to the first space 35, the air sidewall 27 also includes a space located in the second retraction cavity 34.
[0191] Fig.13 The structure obtained after steps (q), (r), (s) and (t) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Fig.14 The structure obtained after steps (q), (r), (s) and (t) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0192] (v) Etching to remove the high dielectric constant layer.
[0193] After the air sidewalls 27 are formed, the High-κ layer in the first space 35 is removed by selective atomic level etching (ALE), and the high dielectric constant medium in the first space 35 is completely removed, thereby further significantly reducing the parasitic capacitance of the device.
[0194] There is still HfO2 material with a high dielectric constant between the gate and the source and drain, which causes the device parasitic capacitance to be still large. Selective atomic-level etching is performed to selectively remove the HfO2 material with a high dielectric constant on both sides of the metal gate, and the high dielectric constant medium in the first space 35 is completely removed, thereby significantly reducing the device parasitic capacitance.
[0195] Selective atomic-level etching: Using specific etching gases, such as hydrogen fluoride (HF), the etching process is precisely controlled through the alternating process of atomic layer deposition (ALD) and atomic layer etching (ALE). In each cycle, the etching gas reacts with the High-κ material and selectively removes the High-κ layer on both sides of the metal gate.
[0196] Cyclic etching process: Repeat the ALD and ALE cycles until the High-κ layer on both sides of the metal gate is completely removed and the metal material between the source, drain and gate is exposed. Etching is stopped until the required etching depth is reached or the High-κ layer is completely removed.
[0197] (w) The protective layer 33 composed of the amorphous carbon layer is removed.
[0198] Specifically, the amorphous carbon layer can be removed by dry etching or wet etching. Removing the protective layer 33 formed by the amorphous carbon layer can further reduce the parasitic capacitance of the semiconductor device.
[0199] Dry etching includes plasma etching and electron beam etching. Plasma etching includes oxygen plasma etching and reactive ion etching.
[0200] Oxygen plasma etching: Oxygen plasma reacts to generate active oxygen atoms and ions, which react with the carbon in the amorphous carbon layer to generate carbon dioxide and water, thereby removing the carbon layer.
[0201] Reactive Ion Etching (RIE): In RIE, oxygen is mixed with other gases (such as fluoride) to etch the amorphous carbon layer by combining high-energy ion bombardment and chemical reactions.
[0202] Electron beam etching involves using a high-energy electron beam to directly bombard the amorphous carbon layer, causing it to decompose and be removed. This method is usually used for finer pattern etching.
[0203] Wet etching includes chemical solution etching, specifically, etching the amorphous carbon layer using a solution of a strong oxidant (such as hydrogen peroxide, sulfuric acid, nitric acid, etc.) These chemical solutions oxidize carbon to generate soluble products (such as carbon dioxide, carbonates, etc.), thereby removing the carbon layer.
[0204] (x) An ILD layer 28 is formed by deposition.
[0205] The steps of ILD layer 28 dielectric deposition are:
[0206] Chemical vapor deposition (CVD): The substrate is placed in a reaction chamber, and the chemical gas required for the dielectric deposition of the pre-prepared ILD layer 28 is introduced to deposit the required insulating layer material on the chip surface through a thermochemical reaction.
[0207] Control deposition parameters: Control deposition parameters such as temperature, pressure, gas flow rate, etc. to ensure a uniform and dense insulating layer is deposited.
[0208] Stop deposition: After the desired deposition thickness is reached, the deposition process is stopped and the chip is removed.
[0209] The operation steps of dielectric polishing are as follows: prepare the chip that has been deposited with the dielectric of the ILD layer 28 and ensure that its surface is clean and dust-free. Place the chip in the CMP equipment and use the chemical mechanical polishing (CMP) method to gradually remove the excess dielectric material through mechanical grinding and chemical dissolution to make the surface flat.
[0210] Control grinding parameters: control the pressure, speed, abrasive particle size and chemical solution ratio during grinding to ensure precise control of the grinding process and surface quality.
[0211] After grinding, the chips are thoroughly cleaned to remove residual abrasive and chemical solutions, and the surface is inspected to ensure that the required flatness and quality are achieved.
[0212] (y) Contact and interconnection.
[0213] The steps of contact hole photolithography and etching include: preparing the chip to be photolithographically and etched, and depositing a layer of photoresist on its surface. Placing the chip in a photolithography machine, irradiating a pre-designed pattern to cause a local chemical change in the photoresist and form a photolithographic pattern. Placing the chip in an etching device, using chemical vapor etching (CPE) or physical vapor etching (PPE) technology to remove the part of the dielectric material not covered by the photoresist, thereby forming a contact hole.
[0214] The operation steps of hole silicide are as follows: prepare the chip with contact holes formed and deposit a layer of silicon material in the contact holes. Use chemical vapor etching (CPE) or physical vapor etching (PPE) technology to remove the part of the dielectric material not protected by silicide to form hole silicide. After etching, the chip is thoroughly cleaned to remove the residual etching gas and impurities, and the hole silicide is inspected to ensure that the required quality requirements are met.
[0215] Preparation steps of tungsten plug (W-Plug): prepare a chip with hole silicide formed, and deposit a layer of tungsten material in the hole silicide. Use chemical vapor etching (CPE) or physical vapor etching (PPE) technology to remove the part of the dielectric material not protected by the tungsten material to form a tungsten plug.
[0216] Fig.15 The structure obtained after steps (u), (v), (w), (x) and (y) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line X-X'. Fig.16 The structure obtained after steps (u), (v), (w), (x) and (y) is shown in FIG. Figure 1 Schematic cross-sectional view of the center line Y-Y'.
[0217] In some examples, nMOS devices are fabricated on P-type bulk silicon substrates, and pMOS devices are fabricated on N-type bulk silicon substrates; source and drain epitaxy of nMOS devices is Si-doped P, and source and drain epitaxy of pMOS devices is SiGe-doped B; STI oxide isolation is used; there is no High-κ layer on both sides of the metal gate; and the sidewall SiNx is etched with HfO2, SiO2 and Si as etching stop layers.
[0218] In some examples, a protective layer 33 composed of an amorphous carbon thin layer or other materials with the same function is used to protect the High-κ material at the inner side wall, and the High-κ layer on both sides of the metal gate is removed by selective atomic-level etching (ALE), which can further reduce the parasitic capacitance of the air side wall stacked nanosheet GAA device and improve the operating speed of the device and circuit. By first depositing a thin protective layer of amorphous carbon material or other material, and after the high dielectric constant metal gate polishing (HKMG CMP) operation, after removing the side wall material, an atomic-level etching scheme is used to realize the stripping of the High-κ material at the side wall position, and then the protective layer is removed. Among them, the part of the high dielectric constant material protected by the protective layer 33 is not removed.
[0219] The specific implementation method is as follows: after the SiGe material is etched, a sacrificial layer material is deposited. Amorphous carbon or other suitable materials can be used for deposition in this step, and the thickness is less than 1 / 2 of the GeSi etching depth; then the inner sidewall is formed until the nanosheet is released, and High-κ deposition is performed. After the air sidewall is formed, the High-κ layer on both sides of the metal gate is removed by selective atomic-level etching (ALE) corresponding to the process flow step (u), and then the protective layer is removed to form a stacked nanosheet transistor structure with the High-κ material removed at the sidewall position, thereby reducing the parasitic capacitance of the device.
[0220] Before removing the protective layer 33, in addition to the first space 35, the air side wall 27 also includes a space located in the second retraction cavity 34. The second retraction cavity 34 is formed by the depression of the protective layer 33, and the part of the high dielectric constant material protected by the protective layer 33 is not removed, so that the part of the high dielectric constant material can increase the driving current of the field effect tube and reduce the on-resistance of the field effect tube, thereby optimizing the performance of the circuit composed of the field effect tube, such as reducing the inverter delay and increasing the frequency of the ring oscillation circuit.
[0221] Another embodiment of the present application provides a stacked nanosheet gate field effect transistor, which is prepared by the preparation method of any embodiment of the present application, and the stacked nanosheet gate field effect transistor includes: a substrate; a first source and a drain and a second source and a drain located on the substrate; a gate located on the substrate, between the first source and the drain and the second source and the drain, and an air sidewall is formed between the first source and the drain and the second source and the drain; a plurality of silicon material nanosheet layers are arranged in the gate at intervals from each other, each of the silicon material nanosheet layers is respectively connected to the first source and the drain and the second source and the drain, and each of the silicon material nanosheet layers is parallel to the upper surface of the substrate.
[0222] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.
[0223] It should be understood that, although the steps in the flowchart of the accompanying drawings are displayed in sequence as indicated by the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless otherwise specified herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least a part of the steps in the flowchart of the accompanying drawings may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn or alternately with other steps or at least a part of the sub-steps or stages of other steps.
[0224] The above embodiments only express the implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a stacked nanosheet gate field effect transistor, characterized in that: include: Depositing on a substrate to form a stacked layer, the stacked layer comprising a plurality of silicon material nanosheet layers and a plurality of silicon alloy layers alternately stacked; Etching the silicon alloy layer to form a first retraction cavity, wherein the first retraction cavity is located between two adjacent silicon material nanosheet layers; A protective layer covering the inner surface of the first retraction cavity is prepared in the first retraction cavity, wherein the protective layer is recessed to form a second retraction cavity; A gate and two source and drain electrodes are prepared on the substrate based on the second retracted cavity, and an air sidewall is formed between the gate and any of the source and drain electrodes; The first dielectric constant medium in the first space is removed; the first space is the space in the air sidewall surrounded by the upper surface of the highest silicon material nanosheet layer, the gate, and any of the source and drain electrodes.
2. The method according to claim 1, characterized in that The step of depositing a stacked layer on a substrate comprises: Providing a silicon substrate, and sequentially performing well photolithography, ion implantation and annealing on the silicon substrate; A stack is deposited on the surface of the annealed structure.
3. The method according to claim 1, characterized in that The method of preparing a gate and two source and drain electrodes on the substrate based on the second retracted cavity comprises: Prepare two solid sidewalls, a first source and drain electrode, a second source and drain electrode, and a gate electrode, wherein the plurality of silicon material nanosheet layers are located between the two solid sidewalls, and the second retracted cavities are all filled with the corresponding solid sidewalls; The two solid side walls are removed to form two air side walls.
4. The method according to claim 3, characterized in that The method of preparing two solid side walls comprises: depositing an amorphous silicon thin film on the substrate; A target pattern formed by photolithography on the amorphous silicon thin film; Depositing a hard mask layer on the amorphous silicon film having the target pattern formed thereon; The amorphous silicon film formed with the hard mask layer is etched to form two solid sidewalls.
5. The method according to claim 4, characterized in that The method of preparing the first source and drain electrode, the second source and drain electrode, and the gate electrode comprises: Removing the hard mask layer by anisotropic etching to obtain a plurality of fin structures; Filling an insulating medium between the fin structures to form shallow trench isolation between the fin structures; removing the depression of the shallow trench isolation; A first source and drain, a second source and drain, and a gate are etched on the fin structure.
6. The method according to claim 5, characterized in that The etching of a first source and drain, a second source and drain, and a gate on the fin structure includes: An insulating layer and a silicon layer are sequentially deposited on the surface of the uppermost silicon material nanosheet layer in the fin structure; Etching the silicon layer to form a dummy gate structure; Prepare sidewall structures and source and drain regions on both sides of the dummy gate structure; forming a first source-drain electrode and a second source-drain electrode on the source-drain region; removing the dummy gate structure to form a gate region; removing the silicon alloy layer in the stack to release the nanosheet channel; A gate is formed by deposition in the gate region.
7. The method according to claim 6, characterized in that Producing sidewall structures on both sides of the dummy gate structure, including: Depositing a sidewall isolation dielectric film; A sidewall structure is formed by etching on the surface of the sidewall isolation dielectric film.
8. The method according to claim 1, characterized in that Also includes: The protective layer is removed.
9. The method according to claim 8, characterized in that Also includes: Depositing to form an isolation layer, wherein the isolation layer covers the air side wall; Etching a contact hole on the isolation layer; A tungsten material is deposited in the contact hole to form a tungsten plug.
10. The method according to any one of claims 1 to 9, characterized in that The protective layer is an amorphous carbon layer.
11. A stacked nanosheet gate field effect transistor, characterized in that: The stacked nanosheet gate field effect transistor is prepared by the preparation method according to any one of claims 1 to 10, and comprises: substrate; A first source and a drain and a second source and a drain located on the substrate; A gate, located on the substrate, between the first source-drain electrode and the second source-drain electrode, and having an air sidewall formed between the first source-drain electrode and the second source-drain electrode; A plurality of silicon material nanosheet layers are arranged in the gate at intervals, each of the silicon material nanosheet layers is respectively connected to the first source and drain and the second source and drain, and each of the silicon material nanosheet layers is parallel to the upper surface of the substrate.