Cation-mixed halogen-mixed full-inorganic perovskite single-crystal X-ray detector

By using mixed cationic halogenated all-inorganic perovskite single crystal material in X-ray detectors, the problem of insufficient response sensitivity and stability of detectors at room temperature in the prior art is solved, and high-throughput hard X-rays are achieved efficient detection and low leakage current.

CN118888618APending Publication Date: 2024-11-01SHANDONG FIRST MEDICAL UNIV & SHANDONG ACADEMY OF MEDICAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410918436.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing X-ray semiconductor detectors are difficult to achieve high response sensitivity and low detection limits at room temperature, and are costly and difficult to grow. In particular, the low carrier mobility and ion mobility of perovskite materials seriously affect performance and stability.

Method used

The Cs1-mRbmPbBr3-nIn series materials were prepared by using mixed cationic mixed halogen all-inorganic perovskite single crystal material, and the solution of Rb+ ions to replace Cs+ ions and I-ion to replace Br-ion to prepare Cs1-mRbmPbBr3-nIn series materials to improve resistivity and carrier mobility. Inhibit ion migration.

Benefits of technology

High response sensitivity, small dark current and stability to high-throughput hard X-rays are achieved, capable of operating at high electric field intensity, providing low and stable leakage currents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888618A_ABST
    Figure CN118888618A_ABST
Patent Text Reader

Abstract

The invention discloses a cation-mixed halogen-mixed full-inorganic perovskite single crystal X-ray detector, the cation-mixed halogen-mixed full-inorganic perovskite single crystal comprises two A-site cations Cs and Rb and two halogen ions Br and I. The structural formula of the cation-mixed halogen-mixed full-inorganic perovskite single crystal is Cs1-mRbmPbBr3-nIn, m is more than or equal to 0 and less than or equal to 1, and n is more than or equal to 0 and less than or equal to 3. The invention relates to the technical field of X-ray detection. According to the cation-mixed halogen-mixed full-inorganic perovskite single crystal X-ray detector, the cation-mixed halogen-mixed full-inorganic perovskite single crystal is used for preparing the X-ray detector, the cation-mixed halogen-mixed full-inorganic perovskite single crystal has large resistivity and high ion activation energy, large response sensitivity to high-flux hard X-rays (120keV) and small dark current can be achieved, and the X-ray detector can be applied to the field of X-ray detection. The lowest detection limit is low; and the stability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of X-ray detection, and in particular to a mixed-cation and mixed-halogen all-inorganic perovskite single crystal X-ray detector. Background Art

[0002] X-ray detectors are widely used in medical diagnosis, industrial production, safety detection, scientific research and other fields. Semiconductor X-ray detectors convert X-ray photons directly into electrical signals. Compared with traditional scintillator detectors, they have the advantages of high conversion efficiency, fast response speed, good response linearity, and compact and portable equipment. High-performance semiconductor materials for gamma-ray detection usually need to have a large atomic number (Z), a suitable band gap (E g ), high resistivity (ρ) and large carrier mobility lifetime product (μτ) to ensure sufficient absorption of rays, while achieving efficient photogenerated carrier collection and low noise in room temperature working environment.

[0003] Traditional X-ray semiconductor detectors face many problems: Si has a small atomic number and can only be used to detect low-energy X-rays; Ge crystals have a small band gap of 0.7 eV, so they must be operated at liquid nitrogen temperature to suppress dark current; HgI2 and PbBr2 crystals are prone to polarization effects, which seriously affect the performance and working stability of the detector; the growth of high-quality CdTe and CdZnTe crystals is difficult and the cost is high (about $2,000 / cm 3 ). Therefore, the development of semiconductor materials with high response sensitivity and low detection limit at room temperature, low cost and easy preparation of large-sized single crystals has become a research hotspot and technical challenge in the field of X-ray detection.

[0004] In recent years, halide perovskite materials (ABX3) represented by MAPbI3, CsPbBr3, etc. contain elements with high atomic numbers such as Pb, I, Br, and have band gaps usually between 1.5-2.5eV, and have high resistivity and mobility lifetime products, showing excellent and balanced semiconductor properties. In addition, compared with commercial CdTe and CdZnTe crystals, this type of crystal has a low growth temperature, short growth cycle, and lower raw material cost, and is expected to become a new generation of high-performance room temperature X-ray detection materials. Among them, all-inorganic perovskite single crystals represented by CsPbBr3 have become a research hotspot and star material in the field of perovskites due to their better stability compared to perovskite polycrystalline thin film materials and MA and FA-based organic-inorganic composite perovskite crystals. The growth of large-sized CsPbBr3 crystals mainly adopts the vertical Bridgman method, which has the advantages of raw materials not easy to volatilize, crystals not easy to be contaminated, crystal components not easy to segregate, high quality of the resulting crystals, and the ability to grow large-sized single crystals. At present, the maximum size of CsPbBr3 crystal can reach φ65×75mm, and the minimum detection limit is 0.02nGy s–1 , which is the lowest value of perovskite X-ray detectors so far, and is 5 orders of magnitude lower than the standard medical diagnosis requirement (5.5 μGy s –1 ). However, compared with commercial CdTe crystals, the carrier mobility of perovskite crystals is still low, and the ion migration is serious, which makes the device easily polarized, seriously affecting the performance and stability of the detector.

[0005] Composition regulation is an effective strategy to optimize semiconductor properties and inhibit the migration of perovskite ions. Huang Jinsong from the State University of Nebraska, Xu Yadong from Northwestern Polytechnical University, and Yang Bin from Hunan University prepared MAPbBr using the composition regulation strategy. 2.94 Cl 0.06 , CsPbBr 2.79 Cl 0.21 , Cs 1-x A series of mixed halogen or mixed cation perovskite crystals such as RbxPbBr3. By utilizing the doping compensation effect of halogen anions and utilizing lattice contraction to enhance the atomic interaction and orbital coupling between Pb and Br, the resistivity and carrier mobility of the crystal are improved. Liu Shengzhong from Shaanxi Normal University, Edward H.Sargent from the University of Toronto, Canada, Tao Xutang from Shandong University, etc. prepared FA using a component regulation strategy. 0.85 MA 0.1 Cs 0.05 PbI 2.55 Br 0.45 , Rb 0.15 Cs 0.85 PbI 1.75 Br 1.25 , CsPbBr 3-n I n By releasing lattice stress, enhancing lattice distortion and reducing the average atomic distance between the A-site cation and the halogen, the ion migration barrier of the perovskite material is increased, effectively inhibiting ion migration. Therefore, based on CsPbBr3 crystal, Rb+ ions are used to partially replace Cs + Ion, I – Ion partial replacement of Br – ions, preparing Cs with high resistivity, high carrier mobility and weak ion mobility 1-m RbB 3-n I n The solution is feasible for a series of perovskite crystals. At present, there is still a blank in the research on the growth, electrical properties and high-throughput hard X-ray detection performance of such crystals at home and abroad. Summary of the invention

[0006] 1. Technical issues to be solved

[0007] In view of the shortcomings of the prior art, the present invention provides a mixed-cation and mixed-halogen all-inorganic perovskite single crystal X-ray detector, in which the X-ray detector is prepared by using a mixed-cation and mixed-halogen all-inorganic perovskite single crystal, wherein the mixed-cation and mixed-halogen all-inorganic perovskite single crystal has a large resistivity and a high ion activation energy, and can achieve a large response sensitivity to high-flux hard X-rays (120keV), a small dark current, a low minimum detection limit and good stability.

[0008] (II) Technical solution

[0009] To achieve the above objectives, the present invention is implemented by the following technical solutions: a mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector, wherein the mixed cation mixed halogen all-inorganic perovskite single crystal includes two A-site cations, Cs and Rb, and two halogen ions, Br and I, and the structural formula is Cs 1-m R m PbB 3-n I n , where 0≤m≤1, 0≤n≤3.

[0010] Preferably, the X-ray detector of the mixed cation-mixed halogen all-inorganic perovskite single crystal comprises, from top to bottom, a cathode, a mixed cation-mixed halogen all-inorganic perovskite single crystal and an anode, and the mixed cation-mixed halogen all-inorganic perovskite single crystal is an active material for absorbing X-ray photons.

[0011] Preferably, the X-ray detector is a semiconductor mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector.

[0012] Preferably, the X-ray detector is prepared by cutting, grinding and polishing a mixed-halogen all-inorganic perovskite single crystal, and then coating electrode materials on the upper and lower surfaces of the mixed-cation mixed-halogen all-inorganic perovskite single crystal with smooth and flat surfaces.

[0013] Preferably, the cutting is performed using a STX-202A small diamond wire cutting machine, and after cutting, the crystal has a length of 2-25 mm, a width of 2-24 mm, and a thickness of 1-8 mm.

[0014] Preferably, the grinding is to place the crystal on 7000-mesh sandpaper and grind and polish it in a mixture with alcohol.

[0015] Preferably, the polishing is fine polishing using a mixture of 0.02 micron aluminum oxide polishing powder and alcohol.

[0016] Preferably, the electrode materials are Au, Ga and Al, and the formed X-ray detector structure is Au / Cs 1- m R m PbB 3-n I nSingle crystal / Au, Au / Cs 1-m R m PbB 3-n I n Single crystal / Ga, Au / Cs 1-m R m PbB 3-n I n Single crystal / Al.

[0017] Preferably, the structure of the electrode material is a single-point electrode.

[0018] The present invention is not limited to the above types.

[0019] (III) Beneficial effects

[0020] The present invention provides a mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector. Compared with the prior art, it has the following beneficial effects:

[0021] (1) The mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector is prepared by using a mixed cation mixed halogen all-inorganic perovskite single crystal, wherein the mixed cation mixed halogen all-inorganic perovskite single crystal has a large resistivity and a high ion activation energy, which can effectively improve the working stability of the detector.

[0022] (2) The mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector can effectively improve the response speed and sensitivity of the detector by using the mixed cation mixed halogen all-inorganic perovskite single crystal to prepare the X-ray detector.

[0023] (3) The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector is prepared by using a mixed cation and mixed halogen all-inorganic perovskite single crystal. The detector has a low and stable leakage current, can operate under high electric field strength, and can realize the detection of high-flux hard X-rays (>100keV). BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the structure of a dual-temperature zone Bridgman furnace for growing all-inorganic perovskite single crystals according to the present invention;

[0025] Figure 2 Cs grown in Example 1 of the present invention 0.8 R 0.2 PbBr3、Cs 0.7 R 0.3 PbB 2.7 I 0.3 , Cs 0.8 R 0.2 PbB 2.9 I 0.1 Schematic diagram of the crystal photo;

[0026] Figure 3 Cs grown in Example 2 of the present invention 0.8 R 0.2 PbBr3、Cs 0.7 R 0.3 PbB 2.7 I 0.3 , Cs 0.8 R 0.2 PbB 2.9 I 0.1 Schematic diagram of the crystal photo;

[0027] Figure 4 Cs grown in Example 3 of the present invention 0.8 R 0.2 PbBr3、Cs 0.7 R 0.3 PbB 2.7 I 0.3 , Cs 0.8 R 0.2 PbB 2.9 I 0.1 Schematic diagram of the crystal photo;

[0028] Figure 5 The present invention is based on Cs 0.8 R 0.2 Image of a single-point electrode structure detector made from PbBr3 crystal. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] See also Figure 1-5 The embodiment of the present invention provides four technical solutions: a mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector, specifically including the following embodiments:

[0031] Example 1: Cs 0.8 R 0.2 Growth method of PbBr3 crystal:

[0032] (1) Take 2.9851 g CsBr, 0.5799 g RbBr, and 6.4351 g PbBr2 and place them in a mortar, mix them evenly, grind them thoroughly, transfer them to a quartz tube, and extract them to 10 -5Pa vacuum and sealed, the sealed quartz tube is placed in a single temperature zone pit furnace for high temperature sintering, the sintering process is as follows: heating to 620°C for 6 hours, keeping the temperature for 24 hours, and cooling to room temperature for 12 hours to obtain pure phase perovskite crystal polycrystalline material;

[0033] (2) Put pure phase perovskite crystal polycrystalline material into the crystal growth quartz crucible and extract it to 10 -5 Pa vacuum and sealed, and then loaded into the growth chamber of the double temperature zone Bridgman furnace.

[0034] (3) Turn on the heating device of the dual-temperature zone Bridgman furnace growth chamber to heat the high-temperature zone and the low-temperature zone. The furnace body is heated to 650°C in the high-temperature zone and 200°C in the low-temperature zone. After the temperature of the temperature zone is stable, the crystal growth quartz crucible containing the polycrystalline material is moved up to the high-temperature zone. The quartz crucible is located in the high-temperature zone with an overheating temperature of 620°C to fully melt the polycrystalline material. The crystal growth quartz crucible containing the polycrystalline material is moved down to the low-temperature zone at a speed of 0.3 mm / h to achieve crystal growth. After the growth is completed, the furnace temperature is lowered to room temperature after 72 hours, and the crystal is taken out. The obtained Cs 0.8 R 0.2 PbBr3 crystals Figure 2 shown.

[0035] The structure of the double temperature zone Bridgman furnace is as follows Figure 1 As shown, it includes a furnace body and a rotating descending system. The furnace body includes a quartz furnace tube and a heating device. The cavity in the quartz furnace tube is a crystal growth cavity. The heating device is arranged outside the quartz furnace tube. An insulation sleeve is arranged outside the heating device of the quartz furnace tube. The insulation sleeve is a quartz tube, the inner wall of which is coated with a gold layer and is in close contact with the heating device. The wall thickness of the insulation sleeve is 3mm to 6mm. The gold layer in the insulation sleeve has a heat-insulating effect and can reflect the heat generated by the heater to the center of the furnace body.

[0036] A crystal growth quartz crucible is arranged in the crystal growth chamber; the crystal growth quartz crucible includes a funnel-shaped shoulder area and a cylindrical equal-diameter area, and the funnel-shaped shoulder area is connected to the cylindrical equal-diameter area as a whole. The cylindrical equal-diameter area can be connected to a vacuum pump and a molecular pump, and the quartz crucible can be sealed by a hydrogen-oxygen flame after being evacuated. The cone angle of the funnel-shaped shoulder area of ​​the crystal growth quartz crucible is 55-135°, and the inner diameter of the cylindrical equal-diameter area is 8-22mm. The entire crystal growth chamber is divided into a high-temperature zone, a gradient zone and a low-temperature zone from top to bottom. The heating device is a resistance wire heater, which is divided into two sections. A high-temperature resistance wire heater is arranged outside the high-temperature zone, and a low-temperature resistance wire heater is arranged outside the low-temperature zone. The distance between the high-temperature resistance wire heater and the low-temperature resistance wire heater is 3-17cm. The length of the high-temperature zone is greater than 230mm, and the length of the low-temperature zone is greater than 180mm; the diameter of the heating furnace wire is 1-4mm; the maximum heating temperature of the furnace body is 800℃, and the maximum temperature gradient is 35℃ / cm. The rotating and descending system includes a crystal growth rod and a driving device for driving the crystal growth rod to rotate and descend. The crystal growth quartz crucible is fixed on the crystal growth rod. The driving device includes a stator, a rotor arranged on the stator, and a rotating motor. The rotating motor drives the rotor to rotate. The crystal growth rod passes through the rotor and the bottom end is fixedly connected to the rotor. The rotating motor drives the rotor to rotate. One end of the crystal growth rod fixing the crystal growth crucible passes through the crystal growth cavity and is located in the crystal growth cavity.

[0037] Example 2: Cs 0.7 R 0.3 PbB 2.7 I 0.3 The crystal growth method is carried out according to the method of Example 1, except that:

[0038] In step (1), 2.5698 g CsBr, 0.8558 g RbBr, 5.3815 g PbBr2, and 1.1929 g PbI2 were used as raw materials for polycrystalline material synthesis. The polycrystalline material synthesis temperature was 610° C. The overheating temperature in step (3) was 610° C. The rest was carried out as in Example 1. 0.7 R 0.3 PbB 2.7 I 0.3 Crystal objects such as Figure 3 The structure of the dual temperature zone Bridgman furnace is the same as that of Example 1.

[0039] Example 3: Cs 0.8 R 0.2 PbB 2.9 I 0.1 The crystal growth method is carried out according to the method of Example 1, except that:

[0040] In step (1), 2.9607 g CsBr, 0.5752 g RbBr, 6.0633 g PbBr2, and 0.4008 g PbI2 were used as raw materials for polycrystalline material synthesis. The polycrystalline material synthesis temperature was 620° C. The overheating temperature in step (3) was 620° C. The rest was carried out as in Example 1. 0.8 R 0.2 PbB 2.9 I 0.1 Crystal objects such as Figure 4 The structure of the dual temperature zone Bridgman furnace is the same as that of Example 1.

[0041] Example 4: Cs 0.8 R 0.2 Preparation of PbBr3 detector:

[0042] (1) Cs of Example 1 0.8 R 0.2 PbBr3 crystals were processed by STX-202A small diamond wire cutting machine to obtain wafers with a length of 3.5 mm, a width of 3.5 mm, and a thickness of 1 mm. The wafers were roughly polished with a mixture of 7000-mesh sandpaper and alcohol, and then finely polished with a mixture of 0.02-micron aluminum oxide polishing powder and alcohol.

[0043] (2) Set the aperture to 3×3 mm 2 The mask is covered on Cs 0.8 R 0.2 The Au electrode was prepared on the upper surface of the PbBr3 crystal by sputtering, and the Ga electrode was coated on the back of the crystal to obtain Figure 5 Single point electrode detector shown.

[0044] In summary, the present invention prepares an X-ray detector by using mixed cation and mixed halogen all-inorganic perovskite single crystals, wherein the mixed cation and mixed halogen all-inorganic perovskite single crystals have large resistivity and high ion activation energy, which can effectively improve the working stability of the detector. By using mixed cation and mixed halogen all-inorganic perovskite single crystals to prepare X-ray detectors, the response speed and sensitivity of the detector can be effectively improved. By using mixed cation and mixed halogen all-inorganic perovskite single crystals to prepare X-ray detectors, the detectors have low and stable leakage current, can operate under high electric field strength, and can realize the detection of high-flux hard X-rays (>100keV).

[0045] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0046] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector, characterized in that: The mixed cation mixed halogen all-inorganic perovskite single crystal includes two A-site cations, Cs and Rb, and two halogen ions, Br and I. The structural formula is Cs 1- m R m PbB 3-n I n , where 0≤m≤1, 0≤n≤3.

2. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 1, characterized in that: The X-ray detector of the mixed cation-mixed halogen all-inorganic perovskite single crystal comprises, from top to bottom, a cathode, a mixed cation-mixed halogen all-inorganic perovskite single crystal and an anode, and the mixed cation-mixed halogen all-inorganic perovskite single crystal is an active material for absorbing X-ray photons.

3. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 1, characterized in that: The X-ray detector is a semiconductor mixed cation mixed halogen all-inorganic perovskite single crystal X-ray detector.

4. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 1, characterized in that: The X-ray detector is prepared by cutting, grinding and polishing a mixed-halogen all-inorganic perovskite single crystal, and then coating electrode materials on the upper and lower surfaces of the mixed-cation mixed-halogen all-inorganic perovskite single crystal with smooth and flat surfaces.

5. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 4, characterized in that: The cutting is performed using a STX-202A small diamond wire cutting machine. After cutting, the crystal has a length of 2-25 mm, a width of 2-24 mm, and a thickness of 1-8 mm.

6. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 4, characterized in that: The grinding is to place the crystal on 7000-mesh sandpaper and mix it with alcohol for rough grinding and polishing.

7. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 4, characterized in that: The polishing is fine polishing using a mixture of 0.02 micron aluminum oxide polishing powder and alcohol.

8. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 4, characterized in that: The electrode materials are Au, Ga and Al, and the X-ray detector structure formed is Au / Cs 1-m R m PbB 3-n I n Single crystal / Au, Au / Cs 1-m R m PbB 3-n I n Single crystal / Ga, Au / Cs 1-m R m PbB 3-n I n Single crystal / Al.

9. The mixed cation and mixed halogen all-inorganic perovskite single crystal X-ray detector according to claim 4, characterized in that: The structure of the electrode material is a single-point electrode.