Light-emitting diode epitaxial wafer, preparation method thereof and LED
By introducing light emitting diode epitaxial sheets with specific hierarchical structures into GaN-based LEDs, the crystal quality and V-pits density are regulated, and the dislocation density control problem in GaN-based LEDs is solved, and the luminous efficiency and photoelectric performance are improved.
Patent Information
- Application Number
- CN202410964792.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
AI Technical Summary
The dislocation density of GaN-based LEDs is difficult to control, resulting in poor V-shaped pit density, affecting photoelectric performance, especially non-radiation recombination efficiency and hole transmission efficiency.
The light-emitting diode epitaxial sheet structure is adopted, including a buffer layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, a multi-quantum well layer and an electron barrier layer, and the first AlGaN layer, a Si-doped three-dimensional GaN layer, and a first AlGaN layer, The two-AlGaN layer and the three-dimensional GaN combined layer regulate crystal quality and V-pits density.
It effectively reduces the non-radiative recombination efficiency of the quantum well, improves the luminous efficiency of the light emitting diode, and simplifies the preparation process to stabilize the production of high-efficiency light emitting diode epitaxial sheets.
Smart Images

Figure CN118888656A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optoelectronic technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. Background Art
[0002] GaN-based LEDs are usually grown on heterogeneous substrates, such as sapphire, SiC and Si substrates. Because of the large lattice mismatch and thermal mismatch between GaN and the substrate, GaN-based LEDs will produce a large number of threading dislocations, so these threading dislocations lead to the generation of V-pits. Earlier, the understanding of V-pits remained at the defect level. It was believed that V-pits were a defect in the active region of the quantum well, often serving as non-radiative recombination centers and device leakage channels, which seriously affected the optoelectronic performance of GaN-based LEDs. However, with the deepening of the understanding of the V-pit problem in recent years, researchers have discovered some positive effects of V-pits in improving the optoelectronic performance of GaN-based LED devices, mainly in shielding dislocations and improving hole transport. However, the dislocation density of GaN-based LEDs cannot be well controlled at present, so the density of V-pits is also difficult to control, and V-pits cannot be used well to improve hole injection efficiency. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer, which regulates the crystal quality of the GaN epitaxial layer, regulates the V-pits density, reduces the quantum well non-radiative recombination efficiency, and improves the luminous efficiency of the light-emitting diode.
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a light emitting diode epitaxial wafer, which has a simple process and can stably prepare a light emitting diode epitaxial wafer with good luminous efficiency.
[0005] In order to solve the above technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged;
[0006] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0007] In some embodiments, the thickness of the first AlGaN layer is 5 nm to 50 nm;
[0008] The Al component of the first AlGaN layer gradually changes from high to low in a direction from the buffer layer to the undoped GaN layer.
[0009] In some embodiments, the Si-doped three-dimensional GaN layer has a thickness of 0.1 nm to 1 μm.
[0010] In some embodiments, the Si doping concentration of the Si-doped three-dimensional GaN layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0011] In some embodiments, the second AlGaN layer has a thickness of 0.5 nm to 2 μm.
[0012] In some embodiments, the growth temperature of the second AlGaN layer is gradually increased.
[0013] In some embodiments, the thickness of the three-dimensional GaN merged layer is 0.5 nm to 2 μm.
[0014] To solve the above problems, the present invention also provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0015] S1. providing a substrate;
[0016] S2, depositing a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence;
[0017] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0018] In some embodiments, the growth pressure of the first AlGaN layer is 50 torr to 300 torr, and the growth temperature is 950° C. to 1050° C.;
[0019] The growth pressure of the Si-doped three-dimensional GaN layer is 50 torr to 500 torr, and the growth temperature is 950° C. to 1080° C.;
[0020] The growth pressure of the second AlGaN layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.;
[0021] The growth pressure of the three-dimensional GaN merged layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.
[0022] Correspondingly, the present invention further provides an LED, which includes the above-mentioned light emitting diode epitaxial wafer.
[0023] The implementation of the present invention has the following beneficial effects:
[0024] The first AlGaN layer is a lattice transition layer, which reduces the lattice mismatch between the three-dimensional nucleation layer and the buffer layer and improves the crystal quality of the three-dimensional nucleation layer.
[0025] The growth temperature of Si-doped three-dimensional GaN layer is low, and the density of nucleation layer islands is low, which slows down the merging speed of islands, reduces the density of defects, and improves the crystal quality of GaN epitaxial layer. In addition, Si-doped three-dimensional GaN layer introduces low-concentration Si doping to regulate the crystal quality of three-dimensional nucleation layer, thereby regulating V-pits density. The thickness of Si-doped three-dimensional GaN layer should not be too thick, and the Si concentration should not be too high, otherwise the introduction of Si atoms will lead to a rapid decrease in the crystal quality of GaN epitaxial layer.
[0026] The growth temperature of the second AlGaN layer gradually increases, the three-dimensional structure of the nucleation layer gradually increases, and the generation of other nucleation points is reduced. The Al component promotes the three-dimensional growth of the nucleation layer and improves the crystal quality of the nucleation layer.
[0027] The growth temperature of the three-dimensional GaN merged layer is slightly higher, the lateral growth of the nucleation layer islands is accelerated, the small islands continue to grow and merge, and prepare for the subsequent deposition of the undoped GaN layer.
[0028] As described above, the present invention adjusts the crystal quality of the GaN epitaxial layer and the V-pits density by adding a three-dimensional nucleation layer, thereby reducing the quantum well non-radiative recombination efficiency and improving the luminous efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic diagram of the structure of a light emitting diode epitaxial wafer provided by the present invention;
[0030] Figure 2 A process flow chart of the method for preparing a light emitting diode epitaxial wafer provided by the present invention;
[0031] Figure 3 This is a process flow chart of step S2 of the method for preparing a light emitting diode epitaxial wafer provided by the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0033] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0034] In the present invention, “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the protection scope of the present invention.
[0035] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0036] In the present invention, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.
[0037] To solve the above problems, the present invention provides a light emitting diode epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which a buffer layer 200, a three-dimensional nucleation layer 300, a non-doped GaN layer 400, an N-type GaN layer 500, a multi-quantum well layer 600, an electron blocking layer 700, and a P-type GaN layer 800 are sequentially arranged;
[0038] The three-dimensional nucleation layer 300 includes a first AlGaN layer 310 , a Si-doped three-dimensional GaN layer 320 , a second AlGaN layer 330 , and a three-dimensional GaN merged layer 340 , which are sequentially deposited on the buffer layer 200 .
[0039] The specific structure of the three-dimensional nucleation layer 300 is as follows:
[0040] In some embodiments, the thickness of the first AlGaN layer 310 is 5nm to 50nm; exemplary thicknesses of the first AlGaN layer 310 are 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, and 45nm, but are not limited thereto. In some embodiments, the Al component of the first AlGaN layer 310 gradually changes from high to low from the buffer layer to the undoped GaN layer. The first AlGaN layer 310 is a lattice transition layer, which reduces the lattice mismatch between the three-dimensional nucleation layer and the buffer layer and improves the crystal quality of the three-dimensional nucleation layer.
[0041] In some embodiments, the thickness of the Si-doped three-dimensional GaN layer 320 is 0.1 nm to 1 μm, and exemplary thicknesses of the Si-doped three-dimensional GaN layer 320 are 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, and 0.9 μm, but are not limited thereto. In some embodiments, the Si doping concentration of the Si-doped three-dimensional GaN layer 320 is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3. In some embodiments, the growth pressure of the Si-doped three-dimensional GaN layer 320 is 50torr to 500torr, and the growth temperature is 950°C to 1080°C. The growth temperature of the Si-doped three-dimensional GaN layer is low, and the density of the nucleation layer islands is low, which slows down the merging speed of the islands, reduces the density of defects, and improves the crystal quality of the GaN epitaxial layer. In addition, the Si-doped three-dimensional GaN layer introduces a low concentration of Si doping to regulate the crystal quality of the three-dimensional nucleation layer, thereby regulating the V-pits density. The thickness of the Si-doped three-dimensional GaN layer cannot be too thick, and the Si concentration is too high, otherwise the introduction of Si atoms will cause the crystal quality of the GaN epitaxial layer to drop rapidly.
[0042] In some embodiments, the thickness of the second AlGaN layer 330 is 0.5 nm to 2 μm, and the exemplary thickness of the second AlGaN layer 330 is 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, but not limited thereto. In some embodiments, the growth temperature of the second AlGaN layer 330 is gradually increased. As the growth temperature of the second AlGaN layer gradually increases, the three-dimensional structure of the nucleation layer gradually increases, reducing the generation of other nucleation points, and the Al component promotes the three-dimensional growth of the nucleation layer, improving the crystal quality of the nucleation layer.
[0043] In some embodiments, the thickness of the three-dimensional GaN merged layer 340 is 0.5nm to 2μm, and the exemplary thickness of the three-dimensional GaN merged layer 340 is 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, but not limited thereto. In some embodiments, the growth pressure of the three-dimensional GaN merged layer 340 is 50torr to 500torr, and the growth temperature is 970℃ to 1100℃. The growth temperature of the three-dimensional GaN merged layer is slightly higher, the lateral growth of the nucleation layer island is accelerated, the small islands continue to grow and merge, and prepare for the subsequent deposition of the undoped GaN layer.
[0044] In summary, the present invention adjusts the crystal quality of the GaN epitaxial layer, adjusts the V-pits density, reduces the quantum well non-radiative recombination efficiency, and improves the luminous efficiency of the light-emitting diode by inserting a three-dimensional nucleation layer 300 with a specific structure.
[0045] Accordingly, the present invention provides a method for preparing a light emitting diode epitaxial wafer, such as Figure 2 As shown, the following steps are included:
[0046] S1, providing a substrate 100;
[0047] The substrate 100 may be selected from one of a sapphire substrate, a SiO2 sapphire composite substrate, a silicon substrate, a silicon carbide substrate, a gallium nitride substrate, and a zinc oxide substrate. Preferably, the substrate 100 is a sapphire substrate, which is a commonly used GaN-based LED substrate material. The sapphire substrate has a mature preparation process, a low price, is easy to clean and handle, and has good stability at high temperatures.
[0048] S2, sequentially depositing a buffer layer 200, a three-dimensional nucleation layer 300, a non-doped GaN layer 400, an N-type GaN layer 500, a multi-quantum well layer 600, an electron blocking layer 700, and a P-type GaN layer 800 on the substrate 100;
[0049] The three-dimensional nucleation layer 300 includes a first AlGaN layer 310 , a Si-doped three-dimensional GaN layer 320 , a second AlGaN layer 330 , and a three-dimensional GaN merged layer 340 , which are sequentially deposited on the buffer layer 200 .
[0050] like Figure 3 As shown, the above preparation method step S2 specifically includes the following steps:
[0051] S21 , depositing the buffer layer 200 on the substrate 100 .
[0052] In some embodiments, the buffer layer 200 is an AlN buffer layer.
[0053] S22 , depositing the three-dimensional nucleation layer 300 on the buffer layer 200 .
[0054] In some embodiments, the growth pressure of the first AlGaN layer is 50 torr to 300 torr, and the growth temperature is 950° C. to 1050° C.;
[0055] The growth pressure of the Si-doped three-dimensional GaN layer is 50 torr to 500 torr, and the growth temperature is 950° C. to 1080° C.;
[0056] The growth pressure of the second AlGaN layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.;
[0057] The growth pressure of the three-dimensional GaN merged layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.
[0058] Preferably, the growth temperature of the second AlGaN layer increases gradually.
[0059] S23 , depositing the undoped GaN layer 400 on the three-dimensional nucleation layer 300 .
[0060] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, N source and Ga source are introduced, and a non-doped GaN layer with a thickness of 1 μm to 5 μm is grown.
[0061] S24 , depositing the N-type GaN layer 500 on the undoped GaN layer 400 .
[0062] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.
[0063] S25 , depositing the multi-quantum well layer 600 on the N-type GaN layer 500 .
[0064] In some embodiments, the multi-quantum well layer includes a plurality of alternately stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period number of 6 to 12, wherein the growth temperature of the InGaN quantum well layer is 790°C to 810°C, the thickness is 2nm to 5nm, and the growth pressure is 50torr to 300torr, and the growth temperature of the AlGaN quantum barrier layer is 800°C to 900°C, the thickness is 5nm to 15nm, and the growth pressure is 50torr to 300torr.
[0065] S26 , depositing the electron blocking layer 700 on the multi-quantum well layer 600 .
[0066] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1000° C., the pressure is controlled at 100 torr to 300 torr, N source, Al source, Ga source, and In source are introduced to grow an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm.
[0067] S27 , depositing the P-type GaN layer 800 on the electron blocking layer 700 .
[0068] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1050° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Mg source, and a Ga source are introduced to grow the P-type GaN layer.
[0069] Accordingly, the present invention further provides an LED, which comprises the above-mentioned light-emitting diode epitaxial wafer, wherein the photoelectric efficiency of the LED is effectively improved and other electrical properties are good.
[0070] The present invention is further described below with specific embodiments:
[0071] Example 1
[0072] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0073] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0074] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0075] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0076] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0077] Example 2
[0078] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0079] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0080] Among them, the thickness of the first AlGaN layer is 15nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN merged layer is 1.3μm.
[0081] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0082] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0083] Example 3
[0084] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0085] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0086] Among them, the thickness of the first AlGaN layer is 25nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0087] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0088] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0089] Example 4
[0090] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0091] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0092] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.3μm, the thickness of the second AlGaN layer is 0.9μm, and the thickness of the three-dimensional GaN combined layer is 1.5μm.
[0093] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0094] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0095] Example 5
[0096] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0097] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0098] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.5μm, the thickness of the second AlGaN layer is 1μm, and the thickness of the three-dimensional GaN combined layer is 1.2μm.
[0099] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0100] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0101] Example 6
[0102] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0103] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0104] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0105] The Al composition of the first AlGaN layer gradually changes from 0.4 to 0.08 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.08.
[0106] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0107] Example 7
[0108] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0109] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0110] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0111] The Al composition of the first AlGaN layer gradually changes from 0.2 to 0.03 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.03.
[0112] The Si doping concentration of the Si-doped three-dimensional GaN layer is 6×10 17 atoms / cm 3 .
[0113] Example 8
[0114] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0115] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0116] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0117] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0118] The Si doping concentration of the Si-doped three-dimensional GaN layer is 7×10 17 atoms / cm 3 .
[0119] Example 9
[0120] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially formed;
[0121] The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
[0122] Among them, the thickness of the first AlGaN layer is 20nm, the thickness of the Si-doped three-dimensional GaN layer is 0.4μm, the thickness of the second AlGaN layer is 0.8μm, and the thickness of the three-dimensional GaN combined layer is 1.3μm.
[0123] The Al composition of the first AlGaN layer gradually changes from 0.3 to 0.05 from the buffer layer to the undoped GaN layer, and the Al composition of the second AlGaN layer is 0.05.
[0124] The Si doping concentration of the Si-doped three-dimensional GaN layer is 4.5×10 17 atoms / cm 3 .
[0125] Comparative Example 1
[0126] This comparative example provides a light-emitting diode epitaxial wafer, and the difference between the other embodiments and the first embodiment is that the three-dimensional nucleation layer includes a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer. The rest is the same as the first embodiment.
[0127] Comparative Example 2
[0128] This comparative example provides a light emitting diode epitaxial wafer, and the difference between the other embodiments 1 and 1 is that there is no three-dimensional nucleation layer. The rest is referred to the embodiment 1.
[0129] The light-emitting diode epitaxial wafers prepared in Examples 1 to 9 and Comparative Examples 1 to 2 were prepared into 10 mil×24 mil chips using the same chip process conditions. 300 LED chips were respectively extracted and tested at a current of 120 mA. The luminous efficiency improvement rate of each embodiment and Comparative Example 1 was calculated by comparing with Comparative Example 2 as a reference. The specific test results are shown in Table 1.
[0130] Table 1 Performance test results of LEDs obtained from Examples 1 to 9 and Comparative Examples 1 to 2
[0131]
[0132] From the above results, it can be seen that the light-emitting diode epitaxial wafer provided by the present invention is provided with a three-dimensional nucleation layer, wherein the first AlGaN layer is a lattice transition layer, which reduces the lattice mismatch between the three-dimensional nucleation layer and the buffer layer, and improves the crystal quality of the three-dimensional nucleation layer. The growth temperature of the Si-doped three-dimensional GaN layer is low, the density of the nucleation layer island is low, the merging speed of the island is slowed down, the density of defects is reduced, and the crystal quality of the GaN epitaxial layer is improved. And the Si-doped three-dimensional GaN layer introduces a low concentration of Si doping to regulate the crystal quality of the three-dimensional nucleation layer, thereby regulating the V-pits density. The thickness of the Si-doped three-dimensional GaN layer cannot be too thick, and the Si concentration is too high, otherwise the introduction of Si atoms will cause the crystal quality of the GaN epitaxial layer to drop rapidly. The growth temperature of the second AlGaN layer gradually increases, the three-dimensional structure of the nucleation layer gradually increases, and the generation of other nucleation points is reduced, while the Al component promotes the three-dimensional growth of the nucleation layer, and improves the crystal quality of the nucleation layer. The growth temperature of the three-dimensional GaN merged layer is slightly higher, the lateral growth of the nucleation layer island is accelerated, the small island continues to grow and merge, and is ready for the subsequent deposition of the undoped GaN layer. As described above, the present invention adjusts the crystal quality of the GaN epitaxial layer and the V-pits density by adding a three-dimensional nucleation layer, thereby reducing the quantum well non-radiative recombination efficiency and improving the luminous efficiency of the light-emitting diode.
[0133] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the first AlGaN layer is 5nm to 50nm; The Al component of the first AlGaN layer gradually changes from high to low in a direction from the buffer layer to the undoped GaN layer.
3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the Si-doped three-dimensional GaN layer is 0.1 nm to 1 μm.
4. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The Si doping concentration of the Si-doped three-dimensional GaN layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
5. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the second AlGaN layer is 0.5 nm to 2 μm.
6. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The growth temperature of the second AlGaN layer gradually increases.
7. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the three-dimensional GaN merged layer is 0.5 nm to 2 μm.
8. A method for preparing a light emitting diode epitaxial wafer according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. providing a substrate; S2, depositing a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence; The three-dimensional nucleation layer includes a first AlGaN layer, a Si-doped three-dimensional GaN layer, a second AlGaN layer and a three-dimensional GaN merged layer sequentially deposited on the buffer layer.
9. The method for preparing a light emitting diode epitaxial wafer according to claim 8, characterized in that: The growth pressure of the first AlGaN layer is 50 torr to 300 torr, and the growth temperature is 950° C. to 1050° C.; The growth pressure of the Si-doped three-dimensional GaN layer is 50 torr to 500 torr, and the growth temperature is 950° C. to 1080° C.; The growth pressure of the second AlGaN layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.; The growth pressure of the three-dimensional GaN merged layer is 50 torr to 500 torr, and the growth temperature is 970° C. to 1100° C.
10. An LED, characterized in that: The LED comprises the light emitting diode epitaxial wafer as claimed in any one of claims 1 to 7.
Citation Information
Cited By
Epitaxial structure, preparation method and light emitting diode
CN122318418A