High-durability membrane electrode as well as preparation method and application thereof
By adding doped perovskite radical quencher BZCY to the membrane electrode catalytic layer, the chemical degradation problem caused by free radical attack in the prior art is solved, and the preparation and performance improvement of high-durability membrane electrodes are achieved. Extends the battery life.
Patent Information
- Application Number
- CN202410922629.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
In existing proton exchange membrane fuel cells, free radicals attack the polymer chain and lead to chemical degradation. Although existing radical quenchers such as ceria can improve durability, they will hinder proton conduction and affect the performance of membrane electrodes.
The doped perovskite radical quencher BZCY is added to the membrane electrode catalytic layer slurry, and a high durable membrane electrode is prepared by hot pressing technology, and the battery performance is improved by using the high radical quenching activity of BZCY.
It significantly improves the durability of the membrane electrode, reduces the amount of free radical scavenger, improves battery performance, and extends the service life of the membrane electrode without affecting proton conduction.
Smart Images

Figure CN118888801A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a high-durability membrane electrode and a preparation method and application thereof. Background Art
[0002] During the use of proton exchange membrane fuel cells, free radicals attack the molecular chains of polymers, causing chemical degradation of the proton exchange membrane. Currently, most methods for improving the durability of proton exchange membranes are to directly add free radical quenchers to the proton exchange membrane, catalyst layer or diffusion layer. The most commonly used free radical quencher is cerium dioxide (CeO2). During the free radical scavenging process, the surface CeO2 3+ Oxidized to Ce 4+ , Ce 4+ Reduction to Ce by reaction 3+ , Ce 4+ With Ce 3+ A cycle is formed to continuously quench free radicals. However, the addition of cerium dioxide will hinder proton conduction and affect the output performance of the membrane electrode. As the amount of free radical quencher added increases, the output performance loss becomes more serious.
[0003] Prior art studies have shown that properly doping Zr in the ceria lattice 4+ 、Al 3+ or Si 4+ Cations such as cerium dioxide can improve the stability of its microstructure and its oxygen storage capacity. Doped materials have better free radical scavenging activity than undoped cerium dioxide. Perovskite material ABO3 is a new type of inorganic non-metallic material with unique physical and chemical properties. The A position is generally a rare earth or alkaline earth element ion, and the B position is a transition element ion. Both the A position and the B position can be partially replaced by other metal ions with similar radii while keeping their crystal structure basically unchanged. This type of compound has high catalytic activity and has great development potential in the fields of environmental protection and industrial catalysis. Perovskite composite oxides have a unique crystal structure, especially the crystal defect structure and performance formed after doping, which can be used in many fields such as sensors, high-temperature heating materials, solid resistors and redox catalysts that replace precious metals, and have become a research hotspot in the fields of chemistry, physics and materials. Among them, BZCY (BaZr X Ce Y Y Z O 3-δ , X+Y+Z=1) is a typical perovskite containing cerium ions. In the BZCY lattice structure, oxygen ions and cations with larger radius (Ba 2+ ) form a cubic closest packing, and the cation with a smaller radius (Ce 4+ ) is an oxygen octahedral interstitial space, each Ce 4+ and Ba 2+They have 6 and 12 oxygen ion ligands, respectively, and are prone to forming oxygen vacancies (δ).
[0004] However, to date, there has been no report on the research on adding the doped perovskite-based free radical quencher BZCY into the membrane electrode catalyst layer slurry to prepare a highly durable membrane electrode. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a highly durable membrane electrode and its preparation method and application. The present invention adds BZCY to the membrane electrode catalyst layer slurry to give full play to the advantages of BZCY's high free radical quenching activity, thereby preparing a highly durable membrane electrode and significantly improving the performance of the battery assembled with the membrane electrode.
[0006] The object of the present invention is to achieve the following:
[0007] The present invention provides a highly durable membrane electrode, which is made of a catalyst-coated membrane and a gas diffusion layer after hot pressing. The catalyst-coated membrane is made by coating a slurry containing a catalyst, a perfluorosulfonic acid resin and a doped perovskite-type free radical quencher onto the surface of a proton exchange membrane. The thickness of the membrane electrode is 300 to 500 μm, and the thickness of the catalyst-coated membrane is 10 to 40 μm.
[0008] Based on the above technical solution, further, the catalyst is Pt / C, wherein the Pt content is 30-70%, and the doped perovskite free radical quencher is BZCY, the molecular formula of BZCY is BaZr X Ce Y Y Z O 3-δ , X+Y+Z=1, Ce content 5%~50%.
[0009] Based on the above technical solution, further, the specific surface area of BZCY is 15-30m 2 / g, particle size 30~100nm.
[0010] Based on the above technical solution, further, the thickness of the gas diffusion layer is 150-250 μm.
[0011] Based on the above technical solution, further, the doped perovskite free radical quencher is calculated by the amount of cerium ions added, and the amount of cerium ions added is 0.5-5 μg / cm 2 .
[0012] The present invention also provides a method for preparing the above-mentioned high-durability membrane electrode, comprising the following steps:
[0013] (1) weighing a catalyst, a perfluorosulfonic acid resin, and a doped perovskite-based free radical quencher, adding a mixed solution of a low-boiling alcohol and water to obtain a catalyst layer slurry, and coating the catalyst layer slurry on the surface of a proton exchange membrane to prepare a catalyst coating layer;
[0014] (2) The catalyst coating layer obtained in step (1) is stacked with the gas diffusion layer, and hot pressed to obtain a membrane electrode with high durability.
[0015] Based on the above technical solution, further, the low boiling point alcohol described in step (1) includes methanol, ethanol, propanol, and the mass ratio of the low boiling point alcohol to water is 1:10 to 10:1.
[0016] Based on the above technical solution, further, the catalyst coating layer described in step (1) is prepared by spraying or direct coating.
[0017] Based on the above technical solution, further, the solid content of the slurry described in step (1) is 2 to 20%.
[0018] Based on the above technical solution, further, in step (2), the temperature of hot pressing is 100-160° C., and the pressure of hot pressing is 0.5-5 MPa.
[0019] The present invention also provides application of the above-mentioned high-durability membrane electrode in a fuel cell.
[0020] The beneficial effects of the present invention compared with the prior art are as follows:
[0021] The present invention adds a doped perovskite-type free radical quencher to the membrane electrode catalyst layer slurry, fully utilizing the advantage of its high free radical quenching activity to prepare a highly durable membrane electrode. The preparation method is simple and easy to operate, and is convenient for industrial implementation. The durability of the prepared membrane electrode is significantly improved, while the amount of free radical scavenger used is reduced, which is of great significance to the improvement of battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0023] Figure 1 This is a graph showing the change of hydrogen permeation current over time during the chemical durability test of the membrane electrodes prepared in Comparative Examples 1 to 3 and Example 1.
[0024] Figure 2 This is a graph showing the change in tail water F concentration over time during a 24-hour test of the chemical durability of the membrane electrodes prepared in Comparative Examples 1 to 3 and Example 1.
[0025] Figure 3 This is a graph showing the change in OCV over time during the chemical durability test of the membrane electrode prepared in Comparative Example 1.
[0026] Figure 4 This is a graph showing the change in OCV over time during the chemical durability test of the membrane electrode prepared in Comparative Example 2.
[0027] Figure 5 This is a graph showing the change in OCV over time during the chemical durability test of the membrane electrode prepared in Comparative Example 3.
[0028] Figure 6 This is a graph showing the change in OCV over time during the chemical durability test of the membrane electrode prepared in Example 1. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0030] Example 1
[0031] In this embodiment, a doped perovskite-based free radical quencher is added to the membrane electrode catalyst layer slurry to give full play to its advantages of high free radical quenching activity to prepare a highly durable membrane electrode. The specific steps are as follows:
[0032] (1) Prepare slurry by weighing 2 g of Pt / C (Pt content 50%) catalyst and 16 g of perfluorosulfonic acid resin, adding 0.04 g of doped perovskite free radical quencher BZCY (BaZr 0.7 Ce 0.2 Y 0.1 O 3-δ , specific surface area 15~30m 2 / g, particle size 30~100nm, Ce addition amount 1μg / cm 2 ), then low boiling point alcohol ethanol and deionized water (mass ratio is 1:1) are added and mixed in sequence to prepare a catalyst layer slurry, and the catalyst layer slurry is sprayed on the proton exchange membrane to obtain a catalyst coated membrane (CCM).
[0033] (2) Preparation of membrane electrode: CCM and 240 μm thick gas diffusion layer were hot pressed at a temperature of 140° C. and a pressure of 1.0 MPa, wherein the paper frame thickness was 100 μm and the frame thickness was 125 μm.
[0034] Comparative Example 1
[0035] The experimental process of Comparative Example 1 is the same as that of Example 1, except that no free radical quencher is added.
[0036] Comparative Example 2
[0037] The experimental process of Comparative Example 2 is the same as that of Example 1, except that the free radical quencher added in Comparative Example 2 is CeO2, and the Ce addition amount is 5 μg / cm 2 .
[0038] Comparative Example 3
[0039] The experimental process of Comparative Example 3 is the same as that of Example 1, except that the free radical quencher added in Comparative Example 3 is CeZrO4, and the Ce addition amount is 5 μg / cm 2 .
[0040] Proton exchange membrane chemical durability test: The membrane electrodes prepared in Comparative Examples 1 to 3 and Example 1 were assembled into a battery, and operated under OCV conditions at a temperature of 90° C. with the cathode and anode humidified by 30%, and the hydrogen permeation current of the membrane electrode was tested at regular intervals.
[0041] The hydrogen permeation current changes with time during the chemical durability test of the membrane electrode prepared in Comparative Examples 1 to 3 and Example 1 are shown in the figure Figure 1 shown; from Figure 1 It can be seen that the failure time of the proton exchange membrane in the membrane electrode without adding free radical scavenger is shorter (hydrogen permeation current> 10mA / cm 2 ), about 120h; the failure time of the proton exchange membrane of the sample with CeO2 added is about 209h; the failure time of the proton exchange membrane of the sample with CeZrO4 added is about 380h; the failure time of the proton exchange membrane of the sample with BZCY added is about 460h. Compared with comparative examples 1 to 3, Example 1 reduces the amount of cerium ions added, and the chemical durability of the proton exchange membrane is extended by 4 times compared with the sample without adding free radical scavengers, 2 times compared with the sample with CeO2 added, and 20% compared with the sample with CeZrO4 added. The change of tail effluent F concentration over time within 24h of the membrane electrode chemical durability test prepared by comparative examples 1 to 3 and Example 1 is shown in the figure Figure 2 As shown, from Figure 2 It can be seen that the F- concentration of the anode and cathode tail discharge of the battery assembled with the membrane electrode added with the BZCY sample within 24 hours is reduced by two orders of magnitude compared with Comparative Examples 1 to 2, and the F- concentration is not much different from that of Comparative Example 3. The OCV change over time during the chemical durability test of the membrane electrode prepared in Comparative Examples 1 to 3 and Example 1 is shown in the figure Figures 3 to 6 As shown. Figures 3 to 6 It can be seen that the open circuit voltage of the cell assembled with the membrane electrode added with the BZCY sample decreases significantly less than that of Comparative Examples 1 to 3 within the same period of time.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A highly durable membrane electrode, characterized in that: It is made of a catalyst-coated membrane and a gas diffusion layer after hot pressing. The catalyst-coated membrane is made by coating a slurry containing a catalyst, a perfluorosulfonic acid resin and a doped perovskite-type free radical quencher onto the surface of a proton exchange membrane. The thickness of the membrane electrode is 300 to 500 μm, and the thickness of the catalyst-coated membrane is 10 to 40 μm.
2. The highly durable membrane electrode according to claim 1, characterized in that: The catalyst is Pt / C, wherein the Pt content is 30-70%, and the doped perovskite free radical quencher is BZCY, the molecular formula of BZCY is BaZr X Ce Y Y Z O 3-δ , X+Y+Z=1, Ce content 5%~50%.
3. The highly durable membrane electrode according to claim 2, characterized in that: The specific surface area of BZCY is 15~30m 2 / g, particle size 30~100nm.
4. The highly durable membrane electrode according to claim 1, characterized in that: The thickness of the gas diffusion layer is 150 to 250 μm.
5. The highly durable membrane electrode according to claim 1, characterized in that: The doped perovskite free radical quencher is calculated based on the amount of cerium ions added, and the amount of cerium ions added is 0.5-5 μg / cm 2 .
6. The method for preparing a highly durable membrane electrode according to any one of claims 1 to 5, characterized in that: The steps include: (1) weighing a catalyst, a perfluorosulfonic acid resin, and a doped perovskite-based free radical quencher, adding a mixed solution of a low-boiling alcohol and water to obtain a catalyst layer slurry, and coating the catalyst layer slurry on the surface of a proton exchange membrane to prepare a catalyst coating layer; (2) The catalyst coating layer obtained in step (1) is stacked with the gas diffusion layer, and hot pressed to obtain a membrane electrode with high durability.
7. The preparation method according to claim 6, characterized in that: The low boiling point alcohol described in step (1) includes methanol, ethanol, propanol, and the volume ratio of the low boiling point alcohol to water is 1:10 to 10:1; the solid content of the slurry is 2 to 20%.
8. The preparation method according to claim 6, characterized in that: The catalyst coating layer described in step (1) is prepared by spraying or direct coating.
9. The preparation method according to claim 6, characterized in that: In step (2), the temperature of hot pressing is 100-160° C., and the pressure of hot pressing is 0.5-5 MPa.
10. Use of the highly durable membrane electrode according to any one of claims 1 to 5 in a fuel cell.