Preparation method of laminated oxide memristor

By using a localized thermal annealing method to scan the surface of dielectric layer B with a laser, the problem of interface damage in the dielectric layer was solved, and high-performance oxide memristors were fabricated. This method is suitable for the fabrication of CMOS-compatible stacked oxide memristors, thereby improving the performance and reliability of the devices.

CN118890955APending Publication Date: 2024-11-01PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939692.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When fabricating multilayer RRAM devices, traditional thermal annealing methods can damage the dielectric layer interface, affecting device performance. Furthermore, high-temperature processing can alter the properties of the dielectric layer material, making it difficult to fabricate high-performance memristor devices in CMOS-compatible processes.

Method used

A localized thermal annealing method is adopted, which generates localized heat by scanning the surface of dielectric layer B with a laser in a pure nitrogen atmosphere to repair the interface damage between dielectric layers A and B. The material with a bandgap of dielectric layer B is selected that is smaller than that of A, and the laser wavelength is in the range of 10nm-800nm ​​to penetrate dielectric layer B to the interface for heat treatment.

Benefits of technology

It effectively mitigates dielectric layer interface damage, improves the performance and reliability of memristor devices, and is suitable for the fabrication of high-performance oxide memristors compatible with CMOS processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890955A_ABST
    Figure CN118890955A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a laminated oxide memristor, and belongs to the technical field of semiconductor (semiconductor) and CMOS (complementary metal oxide semiconductor) hybrid integrated circuits. The laminated oxide memristor comprises a bottom electrode layer, a dielectric layer A, a dielectric layer B and a top electrode layer, and after the two dielectric layers of the oxide memristor are prepared, the surfaces of the dielectric layers are annealed in a laser scanning mode in a nitrogen atmosphere. According to the invention, the interface damage of the dielectric layer can be effectively relieved, and the performance of the memristor is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor and CMOS hybrid integrated circuit, and in particular relates to an oxide memristor preparation technology compatible with existing CMOS process. Background Art

[0002] In recent years, with the gradual delay of Moore's Law and Donald's scaling law, traditional memory devices based on complementary metal oxide semiconductor (CMOS) technology have encountered bottlenecks in operating voltage, power consumption, reliability, integration process, circuit design, etc. At the same time, the shrinking ability of CMOS devices is gradually approaching the physical limit, making it difficult to meet the growing storage and computing needs. In order to cope with these problems, new semiconductor devices such as resistive random access memory (RRAM), phase change memory (PCRAM), magnetoresistive memory (MRAM) and ferroelectric memory (FeRAM) have received extensive research and attention from the industry and academia.

[0003] Among these new semiconductor devices, RRAM devices have a simple structure and a "sandwich" structure, so they have strong shrinking capability, simple manufacturing process, and are compatible with CMOS. At the same time, non-volatile RRAM has a short response time and a long retention time, and is a new type of storage device with great potential. It can be used to store relevant parameters such as weights in neural networks. In addition, according to the classic Kirchhoff's law, the cross array based on RRAM devices can realize the matrix-vector multiplication of voltage and conductivity in a highly parallel manner in an in-memory calculation manner. In particular, stacked RRAM devices have excellent continuous resistive switching characteristics due to the interface modulation effect, so they have been widely studied. However, during the preparation process, the upper and lower dielectric layers of the stacked RRAM device are grown continuously, so the surface of the lower dielectric layer will inevitably be damaged during the growth of the upper dielectric layer, causing degradation of characteristics such as consistency. Although the traditional thermal annealing method can alleviate the interface damage during the preparation process, the higher global temperature will also cause changes in the performance of the dielectric layer material itself, which is not conducive to the preparation of large-scale high-performance memristive devices. Summary of the invention

[0004] In order to optimize the interface performance without affecting the material properties of the dielectric layer, the present invention proposes a novel method for preparing a stacked oxide memristor, which can effectively alleviate the dielectric layer interface damage and improve the memristor performance.

[0005] A method for preparing a stacked oxide memristor, characterized in that the specific steps include:

[0006] 1) Preparing a bottom electrode layer on a substrate by physical vapor deposition or electroplating process;

[0007] 2) growing a dielectric layer A by physical vapor deposition, chemical vapor deposition or atomic layer deposition;

[0008] 3) growing the dielectric layer B by physical vapor deposition, chemical vapor deposition or atomic layer deposition, wherein the bandgap width of the dielectric layer B is smaller than the bandgap width of the dielectric layer A;

[0009] 4) In a pure nitrogen atmosphere, a laser with a wavelength range of 10nm-800nm ​​is used to scan the surface of the dielectric layer B. The laser passes through the dielectric layer B, generates heat at the interface between the dielectric layer A and the dielectric layer B, and alleviates the interface damage through local thermal annealing;

[0010] 5) Prepare the top electrode layer by physical vapor deposition or electroplating process.

[0011] Preferably, an adhesion layer is prepared on the bottom layer by physical vapor deposition or electroplating process, and then ground into a flat surface by chemical mechanical polishing; the adhesion layer material is selected from materials with excellent conductive properties, such as Ti, Al, TiN, Cu, W, TaN, etc., with a thickness of 5-50nm.

[0012] Preferably, the material of the bottom electrode layer and the top electrode layer is metal or a highly conductive compound, such as Al / Al, Hf / TiN, Hf / TaN, TiN / TaN, TaN / TaN, etc., with a thickness of 5-50 nm.

[0013] Preferably, the dielectric layer A and the dielectric layer B are transition metal oxides with excellent resistive switching properties, such as HfO x 、NiO x 、SrTiO x 、TaO x 、AlO x , WO x , ZnO, etc., with a thickness of 5-50nm; and the bandgap width of dielectric layer B is smaller than that of dielectric layer A, so that the laser can penetrate dielectric layer B and reach the interface between the two dielectric layers.

[0014] The beneficial effects of the present invention are as follows: In the present invention, in a pure nitrogen atmosphere, laser is used to perform local thermal annealing on the interface of the dielectric layer, and fine heat is generated at the interface, which can effectively alleviate the interface damage problem and thus improve device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1-5 It is a process flow chart proposed by the present invention.

[0016] Figure 6 yes Figure 1-Figure 5 Legend for . DETAILED DESCRIPTION

[0017] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0018] The stacked oxide memristor of the present invention comprises a bottom electrode layer, a dielectric layer A, a dielectric layer B and a top electrode layer. The materials of the bottom electrode layer and the top electrode layer are usually metal materials or highly conductive compounds. The dielectric layer A and the dielectric layer B are transition metal oxides with excellent resistive switching properties. The bandgap width of the dielectric layer B is smaller than the bandgap width of the dielectric layer A. After the two dielectric layers of the oxide memristor are prepared, the surface is annealed by laser scanning in a nitrogen atmosphere. The laser parameters need to be specifically selected according to the material parameters of the two dielectric layers (such as the bandgap width) and are based on whether the dielectric layer B can be transparent. The specific parameter range is 10nm-800nm ​​wavelength.

[0019] Below is Pt / HfO x / TiO x As an example, the stacked memristor with HfO / TiN structure x The band gap of TiO is 5.8eV. x The band gap is about 3.2 eV. The present invention is further clearly and completely explained through specific embodiments.

[0020] 1) First, a metal layer 1 is sputtered, that is, a 5 nm Ti is sputtered to form an adhesion layer; a metal layer 2 can be formed on the metal layer 1, that is, a 40 nm Pt is formed to form a bottom electrode, such as Figure 1 As shown;

[0021] 2) Growth of dielectric layer A, that is, growth of a 20nm dielectric layer HfO by physical vapor deposition or atomic layer deposition x ,like Figure 2 As shown;

[0022] 3) Growth of dielectric layer B, that is, growth of a 20nm dielectric layer TiO by physical vapor deposition or atomic layer deposition x ,like Figure 3 As shown;

[0023] 4) In pure nitrogen atmosphere, use an intensity of 0.2-0.6 J / cm 2 , a laser with a wavelength of 300nm is used to perform scanning annealing on the dielectric layer B, so that the laser penetrates the dielectric layer TiO x , for HfO x and TiO x The laser passes through the dielectric layer B and generates heat at the interface between A and B. Figure 4 As shown;

[0024] 5) Deposition of metal layer 3: Define the top electrode pattern by photolithography, sputter grow 40nm TiN as the top electrode, and then peel off to form the top electrode pattern, such as Figure 5 shown.

[0025] It should be noted that the purpose of publishing the embodiments is to help further understand the present invention, but those skilled in the art can understand that various substitutions and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the present invention should not be limited to the contents disclosed in the embodiments, and the scope of protection claimed by the present invention shall be subject to the scope defined in the claims.

Claims

1. A method for preparing a stacked oxide memristor, It is characterized in that The specific steps include: 1) Preparing a bottom electrode layer on a substrate by physical vapor deposition or electroplating process; 2) growing the dielectric layer A by physical vapor deposition, chemical vapor deposition or atomic layer deposition; 3) growing the dielectric layer B by physical vapor deposition, chemical vapor deposition or atomic layer deposition, wherein the bandgap width of the dielectric layer B is smaller than the bandgap width of the dielectric layer A; 4) In a pure nitrogen atmosphere, a laser with a wavelength range of 10nm-800nm ​​is used to scan the surface of the dielectric layer B. The laser passes through the dielectric layer B, generates heat at the interface between the dielectric layer A and the dielectric layer B, and alleviates the interface damage through local thermal annealing; 5) Prepare the top electrode layer by physical vapor deposition or electroplating process.

2. The preparation method according to claim 1, It is characterized in that In step 1), an adhesion layer is first prepared on the substrate by physical vapor deposition or electroplating process, and then a bottom electrode layer is prepared on the adhesion layer.

3. The preparation method according to claim 2, It is characterized in that The surface of the adhesion layer is made flat by chemical mechanical polishing.

4. The preparation method according to claim 2, It is characterized in that The adhesion layer material is selected from one of Ti, Al, TiN, Cu, W or TaN, and has a thickness of 5-50 nm.

5. The preparation method according to claim 1, It is characterized in that The material of the bottom electrode layer and the top electrode layer is selected from one of Al / Al, Hf / TiN, Hf / TaN, TiN / TaN or TaN / TaN, and the thickness is 5-50nm.

6. The preparation method according to claim 1, It is characterized in that The dielectric layer A and the dielectric layer B are selected from HfO x 、NiO x 、SrTiO x 、TaO x 、AlO x , WO x Or one of ZnO, with a thickness of 5-50nm.