Method for producing separator by hot pressing
By preheating outside the heating station and hot pressing in the press, using the briquette of high-thermal conductivity materials to quickly cool, the problems of difficult polymer temperature control and low production efficiency in the prior art are solved, and faster and Efficient partition production.
Patent Information
- Application Number
- CN202380026892.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-05
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-04
AI Technical Summary
The prior art is difficult to effectively control the polymer temperature when producing fuel cell separators when hot pressing, resulting in insufficient hot pressing process and low production efficiency, and high equipment complexity and cost.
The molded parts are heated and pressed outside the heating station and hot pressed in the press, and the blocks of high thermal conductivity materials are quickly cooled to form partitions, and the temperature is controlled to reduce from the first predetermined temperature to the second predetermined temperature, and optimize the thermal pressure. Process and production process.
It achieves better polymer temperature control, improves the rapidity and production efficiency of the hot pressing process, simplifies equipment design, and reduces production costs and energy consumption.
Smart Images

Figure CN118891141A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a process for producing separators by hot pressing, in particular a continuous process. Background Art
[0002] Bipolar plates (BPP), produced, for example, by combining two monopolar plates (MPP), are key components of fuel cells. They also play a role in the electrical connection to provide the required voltage of the stack.
[0003] EP3041076A1 discloses a method for producing a fuel cell separator, in which a multilayer sheet is preheated before compression molding to shorten the required molding time. The polymer component of the sheet comprises a fluorocarbon polymer, in particular FEP, PTFE, PFA or a combination thereof. The preheating temperature range is specified to be 280 to 360°C. The melting points of the three mentioned polymers are 260°C, 327°C and 315°C, so that the temperature range indicates molding when the polymer is melted, which is not optimal, however. This is discussed in WO2021 / 028000.
[0004] WO2021 / 028000 of Blue World Technologies Holding discloses a continuous production method and apparatus comprising a mixing stage for mixing a powder of a thermoplastic polymer material and an electrically conductive filler (ECF), and a subsequent kneading stage for kneading the mixture at a kneading temperature above the glass transition temperature of the thermoplastic polymer material but below the melting temperature of the thermoplastic polymer material, so as to provide a ductile but non-melting composite for inducing fibrillation in the thermoplastic polymer material. It also discloses a pre-pressing stage after the kneading stage for pre-pressing the ductile composite into a sheet, and a hot pressing stage for hot pressing the sheet into a pressed part to form a partition. The pressed part has two relatively arranged forming press plates, between which there is a sheet for being hot pressed by the two press plates. The press plates are made of a thermal conductivity greater than 100 W / (m .The sheet is made of a material of a pressure-sensitive adhesive (PSA) such as ... . On the way to the press, the temperature of the extensible quasi-endless film obtained during the kneading stage is maintained by the heated conveyor surface so that the film can be inserted into the press-form and pressed at a temperature in the range of 220°C to 274°C before the temperature decreases due to the transfer of thermal energy to the press-form.
[0005] Although the method and production equipment disclosed in WO2021 / 028000 do bring some advantages over the earlier prior art, it is desirable to further optimize the method. In particular, it is desirable to better control the temperature of the polymer during hot pressing while still achieving rapid production. Summary of the invention
[0006] It is therefore an object of the present invention to provide improvements in the art. In particular, it is an object of the present invention to provide an improved method for producing separators, in particular BPP. In particular, the object relative to WO2021 / 028000 is to better control the heating process of the polymer film during the hot pressing process. Other objects exist in high-speed production, simplicity of production equipment and methods, and reduction of size and cost of production facilities. One or more of these objects are achieved by a method for producing separators for, for example, fuel cells as explained in the claims and in the further details below.
[0007] Briefly, a method for producing a separator is provided wherein a ductile composite of a thermoplastic polymer and an electrically conductive filler is inserted into a press-formed piece which is heated to a first predetermined temperature in a heating station before being inserted into a press for hot pressing between pressing blocks which simultaneously absorb heat energy during compaction to cool the press-formed piece and the sheet forming the separator.
[0008] For the production method, an endless strip of a ductile composite is provided, the composite comprising a mixture of a thermoplastic polymer material and a conductive filler powder. Typically, the filler comprises a carbon material as a major portion of the filler. The strip is cut into sheets and cut to fit into a pressed form. For example, an endless strip is provided similar to the method disclosed and discussed in WO2021 / 028000, and the endless strip is provided with the components disclosed and discussed in WO2021 / 028000, which is incorporated by reference.
[0009] The press-formed part comprises a bottom platen and a support frame which in combination form a hollow part having lateral dimensions and a height H. In the case of a rectangular hollow part, the lateral dimensions comprise a length L and a width W. However, rectangular dimensions are not mandatory, as the partitions can in principle be circular or have other flat shapes.
[0010] The press-formed part also includes a covering press plate covering the hollow portion. When the cut and trimmed sheets are placed in the hollow portion, the covering press plate is placed on top to cover the sheets.
[0011] For example, the cover platen is tightly fitted into the hollow portion. The tight fit within the hollow portion still allows the cover platen to move smoothly into the support frame and prevents the sheet for the separator from being pressed out of the press form during the hot pressing stage where the press form is placed in the press and the platens of the form are pressed together.
[0012] The press-formed part is used to impart stiffness and flow field patterns to the separator, for example for coolant transport and / or for the flow of hydrogen or oxygen. For this reason, the press-formed part includes an embossing template in the bottom press plate and / or the cover press plate, which during compression forms one or more flow fields for the separator.
[0013] For example, when the cover platen is positioned within the hollow and rests on the sheet, a portion of the cover platen extends above the support frame a distance D. During hot pressing of the sheet into the press form, the sheet is pressed into the spacer by pressing the cover platen deeper into the hollow.
[0014] For example, the distance that the cover platen is pressed into the hollow part during hot pressing is measured and / or the pressure is measured. In such a case, the depth to which the cover platen moves into the hollow part is determined by the pressure and volume of the sheet material in the hollow part. These parameters can be adjusted to obtain the desired product.
[0015] In some embodiments, the press includes a mechanism defined to only move the cover platen a certain distance during heat pressing. An option is a toggle press mechanism, where the toggle press cannot push the cover platen further than a certain dead point in the toggle press.
[0016] In order to adjust the distance that the cover platen is pushed into the hollow portion, the distance may be determined by an adjustment mechanism, such as adjustment sheets of different thicknesses, which are selected by thickness according to the distance that the cover platen should be pressed into the hollow portion and are placed between the press and the cover platen or between the press and the bottom platen.
[0017] For example, the covering press plate is pressed into the hollow portion by a distance less than the distance D or by a distance D at most.
[0018] There is also the option that the support frame of the press-form is used as a stop for the compression in the press. For example, during pressing, the cover platen is pushed deeper into the hollow by a distance D until the cover platen is flush with the upper edge of the support frame, so that the support frame stops further compressing the sheet within the press-form. Using the upper edge of the support frame as a stop can be useful, since the size of the spacer is determined in a simple manner by the hardware, which is very precise.
[0019] In particular, when the size of the press blocks extends beyond the support frame of the press-formed part, since the support frame blocks the movement of the press blocks toward each other, it is not possible to push until the cover press plate is flush with the upper layer of the support frame. In this case, according to the preset pressure and the volume of the sheet in the hollow part, the cover press plate is pushed into the hollow part not more than the distance D. The distance D defines the maximum compression distance of the sheet during hot pressing.
[0020] The press comprises two oppositely positioned metal pressing blocks, usually made of steel, and a drive mechanism, such as an electromechanical actuator system, for pressing the two blocks towards each other. The advantage of using electromechanical actuators compared to hydraulics is much lower energy consumption and less heat generation.
[0021] The press has a pressing area between the pressing blocks, in which the press-formed parts are positioned for hot pressing. Furthermore, a conveyor is connected to the pressing area for moving the press-formed parts into and out of the pressing area. With such a conveyor, the insertion and removal of the press-formed parts into the pressing area can advantageously be automated for a smooth and fast automated production sequence.
[0022] For example, the conveyor comprises a ball conveyor table in which the balls are rotatably embedded so as to easily slide the pressed parts on the rotating balls on the table and into the press. In the pressing area, the balls are spring-loaded for being pressed into the table during pressing of the pressed parts between the pressing blocks. For reasons of stability, the platform is advantageously supported by the lower pressing blocks.
[0023] After the sheet is placed in the press-form, the press-form and the sheet inside the press-form are heated to a first predetermined temperature, which is a start temperature of hot pressing.
[0024] This temperature is above the glass transition temperature of the thermoplastic polymer material in order to make the sheet formable. If the thermoplastic material in the mixture comprises more than one polymer, a temperature above the glass transition temperature of the thermoplastic polymer material must be understood as a temperature above the glass transition temperature of all thermoplastic polymers in the mixture, which temperature is higher than the highest glass transition temperature of the thermoplastics in the mixture.
[0025] Advantageously, as discussed in WO2021 / 028000, the temperature is below the melting temperature of the thermoplastic polymer material so that the composite is compacted in a ductile but non-molten state. If the thermoplastic material in the mixture comprises more than one polymer, a temperature below the melting temperature of the thermoplastic polymer material must be understood as a temperature below the melting temperature of all thermoplastic polymers in the mixture, which temperature is below the lowest melting temperature of the thermoplastic in the mixture.
[0026] Typically, the first predetermined temperature at the start of thermal compression is in the range of 250-350°C, such as in the range of 300-350°C.
[0027] The heating of the press-formed part is carried out outside the pressing area so that it is not occupied during the heating phase. This is part of the optimization process. Only when the press-formed part and the sheet material therein have been heated to the desired temperature is the press-formed part moved by the conveyor into the pressing area between the press blocks. The main advantage of this external heating, in which both the press-formed part and the sheet material are heated while the sheet material is inside the press-formed part, is the control of the first predetermined temperature before starting the hot pressing.
[0028] In the hot pressing stage, hot pressing of the sheet is carried out in the pressed form in order to transform the sheet into a separator with a flow field. To this end, the pressing pieces are pressed towards each other for pressing on the cover press plate, for example pressing the cover press plate deeper into the hollow, in order to shape the flow pattern in the separator with the embossing template. High pressure is used, advantageously in the range of 100 to 300 MPa. Due to the high pressure, the pressing time can be advantageously short while still being effective enough for forming the flow pattern.
[0029] In this connection, it should be remembered that the temperature during pressing is rapidly transferred by heat conduction from the press plate material to the press block of the press, which is advantageously molybdenum having a high thermal conductivity, since the press block is made of metal, typically steel. By effective heat conduction from the sheet through the press plate and into the press block, the temperature of the sheet and the pressed part is reduced from a first predetermined temperature to a second predetermined temperature below the glass transition temperature of the polymer in the sheet, and rigid curing of the formed separator is induced.
[0030] For effective cooling, the compact has a thickness much greater than the platen, for example more than ten times the thickness of the platen, so that the compact has a volume sufficient to absorb the heat from the platen during the pressing action, so that the pressing also provides the necessary cooling process for the pressed part to cool the separator to the temperature at which it has solidified. The advantage of this procedure is that it speeds up the process.
[0031] For example, the time range of the cooling process is generally less than 5 seconds, optionally in the time range of 1-2 seconds.
[0032] Finally, the rigid cured separator is removed from the press-formed part.
[0033] Since the press-formed part is not heated in the pressing zone, it is convenient for a fast production line to provide one or more additional press-formed parts. During the hot pressing phase, one or more of the additional press-formed parts are filled with corresponding additional cut sheets of material, and after the press-formed part is removed from the pressing zone, another of the additional press-formed parts is inserted into the pressing zone for hot pressing the additional sheets into additional separators.
[0034] Taking the offset in WO2021 / 028000 as an example, further investigation of the various materials proposed in WO2021 / 028000 for the press plate led to the selection of molybdenum as the material for the press plate. Although molybdenum does not have the highest thermal conductivity of the four materials proposed in WO2021 / 028000, it has a very high hardness, even comparable to steel. The specific choice of molybdenum has been found to be particularly useful because the press-formed parts are subjected to very high pressures.
[0035] When comparing with WO2021 / 028000, some improvements should be particularly highlighted as follows, although aspects are at least partially described above.
[0036] The first and main improvement is that the press-formed part is heated to the desired hot pressing temperature in a specially designed heating station while the sheet is already inside the press-formed part. The heating station is outside the pressing area of the press and is inserted into the pressing area of the press for compacting the sheet only when the press-formed part has been fully heated to the first predetermined temperature. Such a procedure is not disclosed in WO2021 / 028000, where it is recorded instead that the sheet is kept at a high temperature by a roller and then inserted into the press-formed part for cooling and hot pressing, which means that the risk of hot pressing not being carried out quickly enough relative to the cooling effect of the press-formed part on the sheet. In addition, WO2021 / 028000 explains the cooling of the sheet by transferring heat energy to the press plate. However, this type of cooling is difficult to control because the temperature change of the sheet starts immediately when it contacts the press plate unless the press plate is heated to the same temperature as the sheet. In addition, the press plate must be made thick so as to have the necessary heat capacity to absorb enough heat energy from the sheet to reach a temperature below the glass transition temperature. Thus, in contrast to WO 2021 / 028000, thorough control of the first predetermined temperature at the start of the hot pressing process is ensured by heating the pressed part comprising the sheet outside the press and not only the sheet itself.
[0037] A second improvement with respect to WO2021 / 028000 has been found to be that several press-formed pieces can be in a waiting position for hot pressing with corresponding sheets inside at a predetermined first temperature, so that the hot pressing process can be carried out in a rapid sequence, with one press-formed piece inserted into the pressing area and then another press-formed piece inserted into the pressing area, thereby optimizing the production process in terms of speed. This means that the press itself does not require a heater for the press-formed pieces. This also means that the utilization of the press is optimized in terms of total production capacity.
[0038] It has been found that a third improvement over WO2021 / 028000 is to provide a press block in metal (usually steel) and of a thickness much greater than the press plate, so that heat absorbed by the press plate from the sheet is quickly transferred from the press plate by the press block pressing against it. This accelerates the cooling process.
[0039] A further improvement over WO2021 / 028000 is that the compact is maintained at a second predetermined temperature by cooling, wherein the second predetermined temperature is much lower than the first temperature of the pressed part during the start of hot pressing. The second predetermined temperature is in the range of 50-100°C, for example in the range of 60-80°C. By maintaining the compact at such a predetermined cooling temperature, the cooling process from the first predetermined temperature to the second predetermined temperature is precisely controlled at a high cooling rate. In addition, during the time when the pressed part is removed from the press, and until the next pressed part is inserted into the press, the heat energy absorbed by the compact can be effectively removed by cooling, so that the compact is quickly ready to absorb energy from the next pressed part inserted into the pressing area for the hot pressing of the next partition. This principle has also been shown to accelerate the process compared to some prior art, in which the pressed part is heated in the press. For example, the compact is effectively cooled by a coolant flowing through a cooling channel in the compact.
[0040] In a practical embodiment, the press comprises a frame having an upper frame portion and a lower frame portion. The lower portion of the frame is fastened to the lower pressing block, and the upper portion of the frame is located above the upper block, wherein during hot pressing, the actuator presses the upper block downward and away from the upper portion of the frame. The force applied to the press-form will cause the sheet material to be compacted in the press-form.
[0041] For example, the forces applied to the cover plate involve a total force of more than 1000 tons between the blocks. As an example, for a block of size 10 cm x 50 cm = 500 cm 2 The pressure of 1000 tons on the platen results in 2 tons / cm 2 =2000bar=pressure of 200MPa.
[0042] For the actuator, an electromechanical solution is preferred over a hydraulic system, since at such high pressures the energy consumption for pressing is much lower than with a hydraulic system. Optionally, the press comprises an electromechanical toggle mechanism, the spindle of which is driven by an electric actuator, the spindle moving an toggle, advantageously a double toggle, which mechanically acts between the upper part of the frame and the upper block in order to move the upper block towards the lower block relative to the upper part of the frame.
[0043] For a specific embodiment in which the thermoplastic polymer material comprises at least two thermoplastic polymers, the first predetermined temperature for starting hot pressing is adjusted to be above the highest of the glass transition temperatures of the at least two thermoplastic polymers but below the lowest melting temperature of the at least two thermoplastic polymers. Thus, all polymers are maintained at a kneading temperature above their respective glass transition temperatures so as to be ductile and below their respective melting temperatures. The temperature of the formed separator is then reduced to a second predetermined temperature below the lowest of the glass transition temperatures of the at least two thermoplastic polymers while under pressure in the press-formed piece so as to induce rigid curing of all of the at least two thermoplastic polymers before removing the rigidly cured separator from the press-formed piece.
[0044] For example, the thermoplastic polymer material comprises or consists of a first group of thermoplastic polymers and a second group of thermoplastic polymers. By selecting polymers from two different groups, physical parameters related to structural stability, toughness, and chemical inertness, etc., can be adjusted to produce an optimal thermoplastic polymer material for the separator. For example, the thermoplastic polymers of the first group are mainly used to produce structural stability, while the thermoplastic polymers of the second group are mainly used for toughness to prevent fracture. In order to produce the toughness of the composite material, the polymer selected from the second group should be fibrillable by kneading. The ratio between one or more polymers of the first group and the second group is adjusted to optimize. In some embodiments, the composite contains a larger amount of polymers of the first group than polymers of the second group.
[0045] In case the final separator should be used in HT-PEM fuel cells, both groups should have a melting point above 200° C. Furthermore, it is advantageous if the polymer of the first group has a flexural strength above 100 MPa to provide good structural stability of the separator.
[0046] A very useful candidate as a thermoplastic polymer is polyphenylene sulfide (PPS). However, polyetheretherketone (PEEK), polyetherimide (PEI), polysulfone (PSU) are useful alternatives. These polymers belong to the first group of polymers, which have high thermal stability, chemical resistance and high bending strength. As an example, PPS is a favorable binder for separators (especially MPP and BPP) because it does not dissolve in any solvent at temperatures below 200°C, and it has a high melting point in the range of 271-292°C, depending on crystallinity and molecular weight. Its melting point is significantly higher than the operating temperature of HT-PEM fuel cells, which is in the range of 120-200°C.
[0047] Candidates for the second group of polymers include tetrafluoroethylene (ETFE), fluorinated ethylene propylene (FEP), polychlorotrifluoroethylene (PCTFE), polytetrafluoroethylene (PTFE).The polymers of the second group have relatively high tensile elongation and can be fibrillated, in particular by kneading.
[0048] Advantageously, this second group is characterized by the following:
[0049] - a melting temperature above 200°C;
[0050] - continuous operating temperature of at least 120°C;
[0051] - a tensile elongation higher than 100%, for example in the range of 100% to 300% or in the range of 200% to 300%;
[0052] -Tendency to fibrillate by kneading.
[0053] Furthermore, when used in combination, the glass transition temperature of the second group should be lower than the melting temperature of the polymers of the first group.
[0054] Using two groups of polymers in a mixture creates advantages because their respective useful properties can be combined. As an example, a mixture of PPS and PTFE can be used as a combined binder for conductive fillers. In particular, when combined with PPS, PTFE is superior to other thermoplastic binders due to its high decomposition temperature (410°C), inertness, and other unique properties, including low coefficient of friction, high strength, toughness, and self-lubricity.
[0055] For reasons of low resistance, the concentration of ECF should be relatively high, for example greater than 60 wt%, such as greater than 70 wt%.
[0056] After hot pressing, further structuring by machining the separator is generally not required. For example, the method includes hot pressing the sheet into a bipolar plate with a flow channel pattern on each side of the bipolar plate. Alternatively, MPPs are produced and two of such MPPs are combined back-to-back into a single BPP, typically by gluing.
[0057] Optionally, the separators are arranged in an array with the fuel cell membrane located between the separators, the membrane separating the hydrogen fuel from the oxygen.
[0058] This production method is not only applicable to BPP, such as the BPP provided by combining two MPPs. It is also equally applicable to other separators, such as cathode plates, anode plates and cooling plates.
[0059] The invention is particularly useful for fuel cells, in particular proton exchange membrane (PEM) fuel cells, such as high temperature proton exchange membrane (HT-PEM) fuel cells. High temperature PEM fuel cells have a great advantage over low temperature PEM fuel cells in that they can be operated with impure hydrogen (e.g., reformed gas) due to their high tolerance to carbon monoxide therein. However, the relatively high operating temperatures (120-200° C.) combined with the concentrated acid medium inside the fuel cell result in the need to use an inert, thermally stable polymer to bind powdered or granular conductive fillers (ECF).
[0060] However, although the invention is particularly applicable to fuel cells, especially high temperature proton exchange membrane (HT-PEM) fuel cells, it may also be used in other electrochemical energy storage and conversion devices, such as batteries, double layer capacitors or electrolyzers.
[0061] It is to be noted that all stated concentrations and amount percentages are weight percentages (wt %). BRIEF DESCRIPTION OF THE DRAWINGS
[0062] The present invention will be explained in more detail with reference to the accompanying drawings, in which
[0063] Figure 1 An example of a fuel cell stack is shown;
[0064] Figure 2 A method for producing a separator is shown;
[0065] Figure 3A is a sketch of an exemplary pressed part in elevation view, and Figure 3B is a sketch of an exemplary press-formed part in side view;
[0066] Figure 4 An example of a conveyor is shown. DETAILED DESCRIPTION
[0067] Figure 1 An example of a fuel cell stack is shown. Figure 1The separators, illustrated as bipolar plates (BPPs), are one of the key components of fuel cells because they serve to separate the membrane electrode assemblies in the fuel cell stack while electrically connecting the fuel cells in the stack in series so that the voltage of the stack is the sum of the voltages of the cells. In a fuel cell, a fuel containing hydrogen is supplied through the anode inlet, and oxygen is supplied through the cathode inlet. Hydrogen and oxygen are combined into water, which is distributed through the cathode fuel outlet, while the remaining hydrogen is removed through the anode fuel outlet, for example, for use in a burner used in conjunction with a reformer to provide energy for the reforming process. Separators, particularly BPPs, typically have flow fields on both sides as flow guides for the gas. It is also known that separators have flow fields for coolants. For example, two monopolar plates MPPs can be combined back-to-back to form a BPP, with a coolant flow field in the volume between the two MPPs. Flow guides are typically provided in separators during production by embossing channel patterns during hot pressing.
[0068] Figure 2 A continuous process for producing a separator (eg, MPP or BPP) is illustrated.
[0069] In the mixing stage 1, the raw materials are provided from the distributor 0 and mixed in the mixer. Advantageously, a plurality of polymers are combined with the conductive filler ECF. For example, the first type of polymer is selected from a first group of polymers having high thermal stability, chemical resistance and good bending strength. Examples include polyphenylene sulfide (PPS), polyetheretherketone (PEEK), polyetherimide (PEI), polysulfone (PSU). Another polymer is selected from a second group of polymers having relatively high tensile elongation and can advantageously also be fibrillated, in particular by kneading. Examples include fluorinated ethylene propylene (FEP), polychlorotrifluoroethylene (PCTFE), polytetrafluoroethylene (PTFE). Examples of ECF are amorphous carbon, carbon black, carbon fibers, carbon nanotubes, graphene and / or graphite. For example, the ECF contains a major concentration of graphite and / or carbon black.
[0070] Optionally, a surfactant is added as a wetting agent and can help the polymer nanoparticles penetrate deeper into the pores and cracks of the ECF.To reduce the content of water and / or other liquids in the mixture, the temperature is increased to induce evaporation.
[0071] A kneading stage 2 is used after the mixing stage 1 for high-temperature kneading in a kneading container. The purpose of this kneading operation is the fibrillation of the polymer. To this end, the temperature is kept above the glass transition temperature of the fibrillated polymer to achieve fibrillation. The increase in temperature has a positive effect before the melting point of one of the polymers is reached, because the polymer in a molten condition flows too fast. It has been proven that melting one or more polymers is less useful because it leads to an increase in the area specific resistance of the produced BPP. Kneading is carried out for a sufficiently long time to cause significant fibrillation in the polymer. The time depends on the kneading process. Typical kneading times are in the range of 1-60 minutes. For the example of PTFE, the temperature must be above 130°C in order to reach the glass transition temperature of PTFE, where the PTFE is in a viscous state. In the case of a graphite / PPS / PTFE composite, the temperature should be below the melting temperature of PPS, which is 274°C.
[0072] In an extrusion stage 3 used after the kneading stage 2, the compound is extruded from the extruder as a flexible and ductile material. The compound passes through an extrusion nozzle to form an extruded composite rod, for example, having a rectangular cross section.
[0073] The extruded rods are transported on a conveyor belt to a first compression stage 4. Such a first compression stage 4 is exemplified as an inclined top pressing conveyor having a decreasing height in the direction of transport so that the height of the rods decreases as it passes through the compression stage 4. This single operation can be used to rapidly reduce the height of the rods while increasing the width to produce a quasi-endless belt of composite.
[0074] Optionally, a calendering stage 5 is added, wherein the calendering station has a reduced gap height in the subsequent calendering station to form a relatively thin sheet with a desired final thickness. Advantageously, when converted into a tape, the thickness of the rod is reduced to less than 2 mm, optionally reduced to less than 1 mm. The final thickness of the tape is optionally less than several mm, and can be made as thin as several tenths of a mm. During this calendering stage 5, nanofibril formation is further enhanced, for example in PTFE. However, the PTFE content is generally low, for example, less than 0.5 wt %. For good electrical conductivity, the carbon content is high, generally higher than 70 wt %.
[0075] During the transport phase 6, the temperature of the composite belt is maintained in order to keep it ductile, for example by adjusting the temperature of the conveyor surface and ensuring that there is heat conduction between the conveyor surface and the belt.
[0076] The sheets are cut to the required size, usually by means of knives, in the cutting and trimming stage 7. Optionally, waste material is returned to a container in stage 2 for recycling in the manufacturing process.
[0077] The cut and trimmed sheets are inserted into the pressed parts and then heated in the heating station 23 before being inserted into the press 11 of the hot pressing stage 8 providing hot pressing. For example, the start of hot pressing in the press 11 of stage 8 is carried out at a first predetermined temperature, which is generally in the range of 200°C-400°C, advantageously in the range of 300°C-350°C. However, depending on the hot pressing temperature, a useful applied pressure is between 100 and 300 MPa. The advantage of hot pressing is a short pressing-compacting time, which is optionally in the order of 1 second, optionally in the range of 0.5-2 seconds. For example, during hot pressing, the density of the pressed material increases by at least 1.5 times, for example in the range of 1.5 to 3 times, such as in the range of 2 to 2.5 times.
[0078] The press 11 used in the hot pressing stage 8 is also used to cool the sheet for the separator. In this case, the time available for shaping the separator is limited by the cooling rate of the sheet, because the shaping in the hot pressing stage should be completed before the glass transition temperature of the polymer in the sheet is reached, which is 85° C. for PPS, for example. A rapid hot pressing procedure is beneficial because the product can be pressed into its desired and final shape before one or more polymers in the composite reaches the glass transition temperature. In addition, rapid cooling of the sheet during hot pressing generally has the advantage of speeding up the production process.
[0079] For example, after hot pressing, the separator is collected in a container 9 .
[0080] exist Figure 3A An example of a press-formed part 10 for hot pressing in stage 8 is shown in the front view sketch of . A polymer sheet 14, such as MPP, is inserted into the press-formed part 10, between which press plates 13A, 13B supported by a support frame 12 are formed. At least one of the press plates 13A, 13B (but typically both) has a flow field embossed pattern for transfer to the sheet 14 during the hot pressing stage. The press-formed part 10 is positioned in a pressing area 17 between two press blocks 15A, 15B, which are pressed together by force from an actuator 16 acting on the first and upper press blocks 15A. When the first press block 15A is lowered by the force from the actuator 16, it presses on the upper press plate 13A, which is arranged to be vertically movable within the support frame 12 so as to transfer the pressure from the upper press block 15A to the sheet 14 for compressing and embossing the flow field pattern into the sheet 14.
[0081] The bottom pressing plate 13B and the support frame 12 are combined to form a hollow part with a height of H, and the polymer sheet 14 is inserted into this hollow part. Since the polymer sheet 14 has a thickness T < H, a part of the hollow part can be occupied by the covering pressing plate 13A. The latter is partially inserted into the support frame 12 and extends a distance D above the upper edge of the support frame 12, and thus can be pressed down during hot pressing.
[0082] Optionally, the upper edge of the support frame 12 serves as a movement stopper for the upper pressing block 15B. This means that the covering pressing plate 13A is pressed into the hollow part by a distance D for compressing the sheet 14 and forming the partition. Alternatively, the distance by which the covering pressing plate 13A is pressed into the hollow part is less than the distance D. For example, the pressure applied by the press in combination with the adjustment of the volume of the sheet within the hollow part determines the distance by which the covering pressing plate 13A is pressed down into the hollow part. Another option is to use a toggle press, which applies a strong force until its dead point, at which point no further reduction in the distance between the pressing blocks 15A, 15B is achieved. However, in principle, the upper pressing block 15A with its lower side assembled into the hollow part can press the covering pressing plate even deeper into the hollow part than the distance D. There are various options for such a press configuration.
[0083] The rapid hot compression process is to form the sheet 14 into a partition, MPP or BPP, with a flow field for gases and optionally for coolants. As described above, the pressing plates 13A, 13B need to be highly rigid and stable so that the partition 14 obtains the correct dimensions and shape. For this reason, the pressing plates 13A, 13B must be made of hard materials.
[0084] To prevent the material from escaping from the press-molded part 10, the pressing plates 13A, 13B need to closely abut against the inner wall of the support frame 12. In addition, the shrinkage of the pressing plates during cooling should not be different from the shrinkage of the sheet 14 during cooling.
[0085] To achieve high-speed hot pressing while cooling the formed sheet in a short time, the material for the press-molded part in the press 11 has a high thermal conductivity in order to take away the heat and thus cool the pressed MPP as quickly as possible.
[0086] Examples of such materials are molybdenum, tungsten, and some aluminum alloys, such as 2024-T351 and 7075-T651 with thermal conductivities of 143, 197, 121, and 130 W / (m . K), respectively. However, in particular, it has been found that molybdenum has advantages due to its high strength comparable to steel and its high thermal conductivity. According to the Brinell method, molybdenum has a high hardness of 225. Additionally, during cooling, molybdenum has a low degree of thermal shrinkage.
[0087] The press 11 includes a press frame 20. The press frame 20 has an upper portion 20A and side portions 20B and a lower portion 20C. The lower portion 20C is connected to the lower pressing block 15. The side portions 20B connect the lower portion 20C with the upper portion 20A of the press frame 20. When the actuator 16 acts on the upper pressing block 15B, the force applied to the upper pressing block 15B is transferred to the upper platen 13A.
[0088] Figure 3B 1 is a schematic side view of the press 11 and shows a heating station 23, which heats the press-formed part 10 to a predetermined first temperature, for example to 300° C. or higher, which is suitable for starting hot pressing before inserting the press-formed part 10 into the press 11. Once heated, the press-formed part 10 is moved into the press 11 by a conveyor 21A, as indicated by arrow 22. Once in the press 11, hot pressing is performed by pressure between two compacts 15A, 15B. The metal compacts 15A, 15B are maintained at a compact temperature that is much lower than the temperature of the press-formed part. For example, the compacts 15A, 15B are maintained at 70° C. by controlled cooling. Due to the temperature difference and the compacts 15A, 15B having a much larger volume than the press plates 13A, 13B, the press-formed part 10 is effectively cooled from both sides by the compacts 15A, 15B during hot pressing. After hot pressing, the pressed part 10A is moved out of the press 11 again on a conveyor 21A or 21B. At this stage, the sheet 14 has hardened into a rigid separator with an embossed flow field pattern. The procedure shown is fast and smooth and can be used for efficient production lines.
[0089] If the separator is produced as an MPP, the MPP can be used to assemble into a BPP in pairs if the BPP is desired as the final product. Typical assembly methods include gluing around the perimeter of two MPPs adjacent back to back. The requirements for the glue used for PEM BPPs are very similar to the polymers used in MPP composites, i.e. mechanical, thermal and chemical stability within the operating temperature range of high temperature PEM fuel cells. It should be mentioned that forming the BPP by the method described herein also allows gas flow channels and pores to be obtained during the procedure, so that no additional operations such as grinding are required.
[0090] Figure 4 An optional conveyor 21A is shown, which in this embodiment is illustrated as a ball transfer table 25. The balls 24 are supported to roll in bearings so that the press-formed parts 10 can be easily slid into and out of the press on the table 25. Figure 3A and Figure 3B Once the pressed part 10 is in the press 11 and is subjected to the pressure of the upper pressing block 15A, the pressed part 10 will be as follows Figure 4The spring loaded 26, 27 ball 24 shown is pressed into the table 25 so that the pressed part 10 rests on the upper side of the table. The lower side of the table 25 is supported by the lower pressing block 15B.
Claims
1. A method for producing a separator, the method comprising: - providing a press-formed article (10), the press-formed article comprising a bottom press plate (13B) and a support frame (12) and a hollow portion formed by the bottom press plate (13B) and the support frame (12), the hollow portion having a height H, the press-formed article (10) further comprising a cover press plate (13A) covering the hollow portion; wherein at least one of the bottom press plate (13B) and the cover press plate (13A) comprises a template for embossing a fluid flow pattern in a partition (14) formed in the press-formed article (10); - providing an endless strip of a ductile composite comprising a mixture of a thermoplastic polymer material and a conductive filler powder, - cutting and trimming a sheet (14) from the strip, the sheet (14) having a constant thickness T less than H so as to fit into the hollow, placing the cut and trimmed sheet (14) into the hollow, and placing the covering plate (13A) over the sheet (14) so as to cover the sheet (14) in the hollow, - providing a press (11) having a pressing area (17) for receiving the press-formed part (10) so as to hot-press the sheet (14) inside the press-formed part (10) in the pressing area (17), - in a hot press molding stage (8), the sheet (14) in the pressed part (10) is hot pressed into a separator by pressing the pressing plates (13A, 13B) towards each other and shaping the flow pattern in the sheet (14) with the template, - reducing the temperature of the sheet (14) to below the glass transition temperature of the thermoplastic polymer material to induce rigid curing while under pressure in the press-form (10), and then removing the sheet (14) from the press-form (10) as a rigid cured separator, It is characterized in that The press (11) is provided with two metal pressing blocks (15A, 15B) positioned opposite to each other and a drive mechanism (16) for pressing the two pressing blocks (15A, 15B) toward each other, and wherein a conveyor (21A, 21B) is connected to the pressing area (17) for moving the pressed parts (10) into and out of the pressing area (17); wherein the method comprises, - after placing the sheet (14) in the press mould (10), heating the press mould (10) and the sheet (14) while the sheet (14) is inside the press mould (10) in a heating station (23) outside the pressing area (17) to a first predetermined temperature which is above the glass transition temperature of the thermoplastic polymer material but below the melting temperature of the thermoplastic polymer material so as to press the composite into a ductile but non-molten state; - moving the press-formed part (10) into the pressing area (17) between the pressing blocks (15A, 15B) by the conveyor (21A, 21B) only after heating the press-formed part (10), then applying pressure on the press-formed part (10) by the pressing blocks (15A, 15B) and simultaneously reducing the temperature of the press-formed part (10) from the first predetermined temperature to a second predetermined temperature below the glass transition temperature by transferring thermal energy from the press-formed part (10) to both the pressing blocks (15A, 15B) during the hot pressing, - The pressed parts (10) are then removed from the pressing area (17) by means of the conveyors (21A, 21B).
2. A method according to claim 1, wherein the method includes providing an additional press-formed part in a repeated process, and filling the additional press-formed part with corresponding additional cut sheets (14) during the hot pressing of the sheet in the press-formed part (10), and after the press-formed part (10) is removed from the pressing area (17) by the conveyor (21A, 21B), the additional press-formed part is inserted into the pressing area (17) by the conveyor (21A, 21B) to hot press the additional sheet into an additional partition.
3. A method according to any preceding claim, wherein the covering plate (13A) is tightly fitted into the hollow portion, and wherein the method includes positioning the covering plate (13A) within the hollow portion and resting the covering plate (13A) on the sheet (14), a portion of the covering plate (13) extending a distance D above the support frame (12), and hot pressing the sheet (14) in the pressed part (10) into a partition by pressing the pressing blocks (15A, 15B) toward each other and pushing the covering plate (13A) deeper into the hollow portion by the pressing blocks (15A, 15B) not exceeding a distance D.
4. A method according to any preceding claim, wherein the method comprises providing the compact (15A, 15B) with a thickness not less than ten times the thickness of the press plate (13A, 13B) so that the compact (15A, 15B) has a volume sufficient to absorb heat from the press plate (13A, 13B) during simultaneous cooling and hot pressing.
5. A method according to any preceding claim, wherein the method comprises providing a cooling system for the compact (15A, 15B) and maintaining the compact (15A, 15B) at a second predetermined temperature by cooling, wherein the second temperature is below the glass transition temperature of the thermoplastic polymer.
6. A method according to any preceding claim, wherein the method comprises maintaining the compact (15A, 15B) at a second predetermined temperature in the range of 50-100°C, such as in the range of 60-80°C.
7. A method according to any preceding claim, wherein the conveyor (21A, 21B) comprises a ball transfer table (25) in which a rotating ball (24) is embedded for sliding the pressed part (10) on the rotating ball (24) on the table (25) into the press (11), wherein the ball (25) in the pressing area (17) is spring-loaded (26, 27) for being pressed into the table (25) during pressing of the pressed part (10) between the pressing blocks (15A, 15B).
8. A method according to any preceding claim, wherein the method comprises providing the base plate (13B) and the cover plate (13A) with molybdenum.
Citation Information
Patent Citations
Method and production plant for producing a separator by compacting
CN114207888A
Method of manufacturing fuel cell separator
JP2012234639A
Cited By
Plastic plate hot press molding device and using method thereof
CN119283264A