Photocurable inks for automotive interior applications and glass articles comprising same
By using high pigment content light curing ink on internal displays of automobiles and curing with narrow bandwidth UV LED light sources, the problem of insufficient adhesion in existing inks in high temperature and high humidity environments is solved, and high adhesion and high optical density are achieved Opacity layer reduces production costs.
Patent Information
- Application Number
- CN202380019129.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-29
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-01
AI Technical Summary
The light-curing ink used in displays in existing automobiles is insufficient in high temperature and high humidity environments, and it is difficult to meet the requirements of high optical density and low production costs.
Using photocuring ink containing at least 10% pigment, deposited by inkjet printheads below 65°C and cured with a narrow bandwidth UV LED light source to form an opaque layer, ensuring 500 hours of adhesion and high humidity at 85°C and 95% humidity. Optical density.
The opaque layer with high adhesion and high optical density on the internal display of the automobile is realized, reducing production costs, and suitable for high-yield inkjet printing processes.
Smart Images

Figure CN118891234A_ABST
Abstract
Description
[0001] priority
[0002] This application claims the benefit of priority under 3 5 U.S.C. §119 to U.S. Provisional Application No. 63 / 304,732 filed on January 31, 2022 and U.S. Provisional Application No. 63 / 393,532 filed on July 29, 2022, the contents of the foregoing applications being the basis of this application and being incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates to photocurable inks for automotive interior applications and glass articles containing the photocurable inks. Background Art
[0004] The interior of an automobile may include a display including a display cover glass. A display module (e.g., a liquid crystal display ("LCD") module, an organic light emitting diode ("OLED") display module, or other suitable type of display module) may be laminated to or integrated with the cover glass such that the cover glass protects the display module and / or provides one or more performance enhancing attributes (e.g., anti-glare or anti-reflective properties) to the display module. Decorative inks may be applied to areas of the cover glass to hide various components of the display (e.g., electrical and mechanical connections) and / or to provide a uniform appearance of the display when the display is powered off. Certain existing inks for decorating display cover glass may have various deficiencies that render such inks unsuitable for automotive interior applications. For example, some existing inks may be applied via a screen printing process, which may require multiple layers to provide the desired optical density and have a relatively low production volume. Other existing inks (e.g., UV curable inks) may not provide the desired optical density per unit thickness and / or may not provide adequate adhesion to the cover glass initially or after environmental testing associated with variable environmental conditions (e.g., temperature or humidity conditions) to which the automotive interior components are exposed. Therefore, there is a need for alternative inks that meet the requirements associated with automotive interior display applications. Summary of the invention
[0005] One embodiment is directed to a glass article, comprising: a glass substrate having a first major surface and a second major surface, the second major surface being opposite the first major surface; and an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink, the photocurable ink comprising at least 10 weight percent pigment, wherein: the opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than 4.0, and after being cured via exposure to curing light from an ultraviolet (“UV”) light emitting diode (“LED”), the opaque layer exhibits: a pencil hardness greater than or equal to 3H measured in accordance with ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B after being tested in accordance with ASTM 3359 at a temperature of 85° C. and a relative humidity of 95% for a period of at least 500 hours.
[0006] Another embodiment includes a display for a vehicle interior system, the display comprising: a glass substrate having a first major surface and a second major surface, the second major surface being opposite to the first major surface; an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink, the photocurable ink comprising at least 10 weight percent pigment; and a display panel disposed on the second major surface, wherein: the opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than 4.0, and after being cured via exposure to curing light from an ultraviolet (“UV”) light emitting diode (“LED”), the opaque layer exhibits: a hardness greater than 500 A as measured in accordance with ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B for a period of at least 500 hours at a temperature of 85° C. and a relative humidity of 95% when tested in accordance with ASTM 3359.
[0007] Another embodiment is directed to a method of making a glass article, the method comprising: depositing a photocurable ink onto a major surface of a glass substrate using an inkjet print head at a deposition temperature of less than or equal to 65° C., wherein during deposition, the photocurable ink has a viscosity of less than 25 cP, wherein the photocurable ink comprises at least 10 wt % of a pigment and at least 50 wt % of a reactive monomer; and curing the photocurable ink on the major surface by exposing the photocurable ink to light generated by an ultraviolet (“UV”) light emitting diode (“LED”) to form an opaque layer, wherein the curing light has a bandwidth of less than or equal to 30 nm, wherein: the opaque layer comprises a thickness of less than or equal to 25 μm and an optical density of greater than or equal to 4.0, and the opaque layer exhibits: a pencil hardness of greater than or equal to 3H measured in accordance with ASTM 3363, and an adhesion to the glass substrate of greater than or equal to 4B for a period of at least 500 hours at a temperature of 85° C. and a relative humidity of 95% when tested in accordance with ASTM 3359.
[0008] It should be understood that both the above general description and the following detailed description are exemplary only and are intended to provide an overview or framework for understanding the nature and character of the claims. The accompanying drawings are included to provide a further understanding and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate one or more embodiments and together with the description explain the principles and operation of the various embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The accompanying drawings, which are incorporated in and form a part of the specification, illustrate several aspects of the present disclosure and, together with the description, serve to explain the principles of the present disclosure. In the drawings:
[0010] Figure 1 is a perspective view of a vehicle interior having a vehicle interior system including a display according to one or more embodiments of the present disclosure;
[0011] Figure 2 Schematically depicts a method of passing through a Figure 1 A cross-sectional view of a display of a vehicle interior system along line 2-2 shown;
[0012] Figure 3 A flow chart depicting a method of forming a glass article having an opaque layer according to one or more embodiments of the present disclosure;
[0013] Figure 4 A graph depicting measured optical density as a function of opaque layer thickness for Examples 1-3 according to one or more embodiments of the present disclosure;
[0014] Figure 5 depicts a photograph of a sample formed according to Example 2 after being subjected to a cross-hatch adhesion test according to one or more embodiments of the present disclosure;
[0015] Fig. 6A depicts a photograph of a sample coated with a first commercially available UV curable ink after being subjected to high temperature and high humidity testing according to one or more embodiments of the present disclosure; and
[0016] Figure 6B depicts a photograph of a sample coated with a second commercially available UV curable ink after being subjected to high temperature and high humidity testing according to one or more embodiments of the present disclosure;
[0017] Figure 7 is a graph showing the optical density of samples as a function of the thickness of an opaque layer formed according to Example 5, according to one or more embodiments of the present disclosure; and
[0018] Figure 8 A photograph of a sample formed according to Example 5 after being subjected to a cross-hatch adhesion test according to one or more embodiments of the present disclosure is depicted. DETAILED DESCRIPTION
[0019] Referring generally to the accompanying drawings, described herein are photocurable inks that can be used to form an opaque layer on a display cover glass using a high throughput curing process. Once the photocurable ink is cured, the opaque layer can have relatively high glass adhesion and a higher optical density per unit thickness while excluding certain solvents that tend to be harmful to the environment. In embodiments, for example, the photocurable inks described herein can be cured into an opaque layer having a thickness of less than 25 μm (e.g., less than or equal to 20 μm, less than or equal to 15 μm, less than or equal to 10 μm) while providing an optical density greater than or equal to 4 (e.g., greater than or equal to 5). The photocurable ink can also be cured using a light emitting diode ("LED") light source having a relatively narrow ultraviolet ("UV") spectral output (e.g., 365±10 nm, 385±10 nm, 395±10 nm, 405±10 nm) to facilitate production efficiency. In addition, the photocurable inks described herein may also be compatible with commercially available inkjet printing processes (e.g., having an uncured viscosity of less than 25 cP at a temperature of less than or equal to 60° C.) to facilitate a relatively low-cost and high-throughput production process. The photocurable inks described herein may provide each of the above-described beneficial properties while exhibiting reliable adhesion to cover glass when subjected to environmental testing. Certain ink compositions according to the present disclosure may exhibit adhesion to cover glass of greater than or equal to 4B when subjected to a cross-hatch tape test according to ASTM 3359 (the contents of which are incorporated herein by reference).
[0020] In an embodiment, the photocurable ink of the present disclosure comprises a pigment dispersion, an optional adhesion promoter, a binder solution, a multifunctional monomer, and a photoinitiator package. The pigment dispersion comprises 20% to 50% by weight of a suitable pigment (e.g., carbon black pigment) or a suitable mixture of a pigment and 50 to 80% by weight of a first reactive monomer (e.g., a suitable acrylate monomer (e.g., neopentyl glycol diacrylate or trimethylolpropane triacrylate)). The pigment may be greater than or equal to 10% by weight (e.g., greater than or equal to 20% by weight) of the ink composition to facilitate the ink to include a relatively high optical density (e.g., greater than or equal to 4, greater than or equal to 5) at a relatively low thickness (e.g., less than or equal to 25 μm after curing). The first reactive monomer may be present in an amount greater than or equal to 40% by weight and less than or equal to 60% of the photocurable ink composition. When an adhesion promoter is included, the adhesion promoter may be 10% to 20% by weight of the ink composition and comprises a monofunctional monomer for enhancing adhesion to the cover glass. For example, the adhesion promoter may include 2-hydroxyethyl acrylate (2-HEA) monomer. The binder solution may include a suitable epoxy resin to adjust the adhesion and surface hardness of the cured opaque layer. The epoxy resin may be less than 5% by weight of the ink composition. In an embodiment, in addition to the epoxy resin, the binder solution also includes a suitable acrylate monomer as a reactive diluent. The photocurable ink may also include a multifunctional monomer to achieve a relatively high crosslinking density (e.g., to promote high surface hardness). The photoinitiator package may include one or more suitable photoinitiators to promote curing using UV LEDs. In an embodiment, the photoinitiator package includes a Norrish I-type photoinitiator and a Norrish II-type initiator to induce rapid photopolymerization of the ink composition. The combined weight % of the packaged photoinitiator may include up to 10% by weight of the ink composition. In an embodiment, the concentration of the Type I photoinitiator is greater than twice that of the Type II photoinitiator to promote photopolymerization. The photocurable ink of the present disclosure may also include less than 0.5% by weight (e.g., less than 0.1% by weight) of a suitable polymerization inhibitor to facilitate transportation and storage.
[0021] The photocurable ink of the present disclosure may also meet various environmental compliance standards. For example, in an embodiment, the photocurable ink described herein contains less than 10% by weight of volatile organic compounds, and thus meets GB 35807-2020 entitled "Limits of Volatile Organic Compounds (VOCs) in Printing Ink" (incorporated herein by reference in its entirety). In addition, the photocurable ink of the present disclosure may be free of halogenated hydrocarbons and free of solvents identified by the CAS registration number in Table 1.
[0022] Table 1
[0023]
[0024]
[0025] Such solvents are known to have potential harmful effects on the environment and / or human health. Certain existing photocurable inks include the solvents listed in Table 1 to provide UV-curable inks with relatively high optical density compatible with inkjet printing. The photocurable inks of the present disclosure provide such advantageous properties without such harmful solvents. The photocurable inks of the present disclosure provide uncured viscosities suitable for inkjet printing without adding harmful solvents, thereby facilitating relatively high throughput (e.g., greater than 20 m / s) using commercially available print heads. 2 / hour, more than 30m 2 / hour, more than 40m 2 / hour, greater than 50m 2 Unlike some other inks based on ceramic glass frits that require relatively high curing temperatures, the inkjet printing process is advantageously compatible with chemically strengthened cover glasses.
[0026] In embodiments, the composition of the photocurable inks described herein can be tailored to meet specific appearance requirements associated with design needs. For example, a cover glass containing an opaque layer composed of the photocurable inks described herein can meet any of the black shield color targets in Table 2.
[0027] Table 2
[0028]
[0029] In embodiments, an opaque layer constructed using the photocurable inks described herein may meet any combination of the values included in Table 2 within the tolerances listed in Table 3 below.
[0030] Table 3
[0031]
[0032] As shown in Tables 2 to 3, when viewed from the uncoated surface of the cover glass (e.g., from the side of the glass opposite to the side where the display is disposed), when illuminated at an angle of incidence of 10° using a CIE D65 illuminant, the cover glass containing the photocurable ink described herein can generally have a CIELAB L* value of less than or equal to 30 (less than or equal to 29, less than or equal to 28, less than or equal to 27, less than or equal to 25, less than or equal to 25), a CIELAB a* value (including specular reflection component) greater than or equal to -0.05 and less than or equal to 0.15, and a CIELAB b* value (including specular reflection component) less than or equal to -0.1 and greater than or equal to -0.3. When excluding the specular reflection component, the cover glass may exhibit a CIEL* value of less than or equal to 1, and CIELAB a* and b* values of the order of less than or equal to 0.1. Areas of the cover glass coated with the photocurable inks described herein may exhibit a dark neutral appearance to facilitate hiding various components from view.
[0033] The light-curable inks of the present disclosure can also be used to construct an opaque layer on cover glass, showing good reliability test results compared to some existing light-curable inks. Automotive interior components are subject to highly variable environmental conditions (e.g., temperature and relative humidity). In an embodiment, the opaque layer can meet one or more of the following criteria when subjected to the reliability tests listed in Table 4.
[0034] Table 4
[0035]
[0036] Investigation revealed that certain existing UV curable inkjet compatible inks crack or otherwise break down when subjected to such test conditions, rendering these inks unsuitable for use in certain automotive interior applications. For example, certain existing inks have been found to wrinkle and / or crack when subjected to Test B included in Table 4 above, whereas the light curable inks described herein meet the test criteria included in Table 4.
[0037] In addition to meeting the above reliability test requirements, the photocurable inks described herein may also meet the additional requirements provided in Table 5 to make them suitable for use in certain commercially available inkjet printers.
[0038] Table 5
[0039]
[0040] The light-curable inks described herein may also exhibit a pencil hardness of greater than or equal to 3H after being cured using a narrow-band UV LED light source emitting narrow-band (e.g., less than or equal to 20 nm bandwidth, less than or equal to 30 nm bandwidth) curing light, when measured according to ASTM 3363, entitled "Standard Test Method for Film Hardness by Pencil Test," the contents of which are incorporated herein by reference, using a 750 g weight at a 45° angle to the pencil. The use of such UV LEDs may save space and cost, and be less harmful to the environment, compared to certain existing UV curing lamps. Some existing UV curable inks may not be sufficiently cured to have such a pencil hardness while meeting the optical density requirements described herein, because the opacity of the ink inhibits curing. The photoinitiator of the ink described herein is selected to facilitate curing using a UV LED while still meeting the pencil hardness and optical density requirements described herein.
[0041] Thus, the photocurable inks described herein are able to provide a relatively high optical density per unit thickness to facilitate efficacy as a black matrix layer in a display while being compatible with high throughput inkjet printing processes and also meeting the stringent reliability testing requirements associated with automotive interior displays. The photocurable inks described herein save manufacturing costs for display cover glass while still providing a highly reliable opaque layer as shown to provide consistent color performance over the life of the component.
[0042] Figure 1A vehicle interior 1000 is shown according to an exemplary embodiment and includes three different vehicle interior systems 100, 200, 300. The vehicle interior system 100 includes a center console base 110 having a curved surface 120 including a display 230. The vehicle interior system 200 includes an instrument panel base 210 having a curved surface 220 including a display 230. The instrument panel base 210 generally includes an instrument panel 215, which may also include a curved display. The vehicle interior system 300 includes an instrument panel steering wheel base 310 having a curved surface 320 and a display 330. In one or more embodiments, the vehicle interior system may include a base that is an armrest, a pillar, a seat back, a floor, a headrest, a door panel, or any portion of the vehicle interior that includes a curved surface. In an embodiment, the display 130, 230, 330 is planar and includes a cover glass having a flat major surface. In an embodiment, one or more of the displays 130, 230, 330 is curved, and the curved display may include a curved cover glass, which may be hot-formed or cold-formed to have such a curvature. For example, such an embodiment may include an opaque layer formed by a photocurable ink described herein disposed on a cold-formed glass substrate. Such cold forming relates to any of the techniques described in U.S. Pre-Grant Publication No. 2019 / 0329531A1 entitled “Laminating thin strengthened glass to curved molded plastic surface for decorative and display cover application”, U.S. Pre-Grant Publication No. 2019 / 0315648A1 entitled “Cold-formed glass article and assembly process thereof”, U.S. Pre-Grant Publication No. 2019 / 0012033A1 entitled “Vehicle interior systems having a curved cover glass and a display or touch panel and methods for forming the same”, and U.S. Patent Application No. 17 / 214,124 entitled “Curved glass constructions and methods for forming the same” (incorporated herein by reference in their entirety).
[0043] Embodiments of the glass articles described herein may be used in any or all of the vehicle interior systems 100, 200, and 300. Figure 1 An automotive interior is shown, but various embodiments of the vehicle interior system may be incorporated into any type of vehicle, such as trains, motor vehicles (e.g., cars, trucks, buses, and the like), marine vehicles (boats, ships, submarines, and the like), and aircraft (e.g., drones, airplanes, jets, helicopters, and the like), and include manually driven vehicles, semi-autonomous vehicles, and fully autonomous vehicles. Furthermore, while the description herein is primarily directed to glass articles used in vehicle displays, it should be understood that the various embodiments described herein may be used in any type of display application.
[0044] Figure 2 Schematic diagram of a method of passing through a Figure 1 FIG. 2 is a cross-sectional view of display 230 taken along line 2-2, wherein display 230 is flat. Figure 2 An example of a display 230 is depicted, but it should be understood that the description herein with respect to Figure 1 The displays 130, 330 may have similar cross-sectional structures and include the photocurable inks described herein in a similar manner. Figure 2 The display 230 in the illustrated embodiment is flat, but embodiments are also contemplated where the display 230 is curved and the glass article 400 includes one or more curved surfaces (eg, as a result of cold or hot forming to have a suitable curved shape).
[0045] like Figure 2As shown, the glass article 400 includes at least a substrate 450 and an opaque layer 500, and optionally includes a light management layer 460. The substrate 450 has a first surface 470 facing the viewer and a second surface 480 on which the opaque layer 500 is at least partially disposed. As used herein, the term "disposed" includes coating, depositing and / or forming a material on a surface using any method known in the art. The disposed material may constitute a layer as defined herein. As used herein, the phrase "disposed on..." includes the case where the material is formed onto the surface so that the material is in direct contact with the surface, and also includes the following case: the material is formed on the surface, wherein one or more intermediate materials are located between the disposed material and the surface. One or more intermediate materials may constitute a layer as defined herein. The term "layer" may include a single layer, or may include one or more sublayers. Such sublayers may be in direct contact with each other. The sublayers may be formed of the same material or two or more different materials. In one or more alternative embodiments, such sublayers may have intermediate layers of different materials disposed therebetween. In one or more embodiments, a layer may include one or more connected and uninterrupted layers and / or one or more discontinuous and interrupted layers (i.e., layers having different materials formed adjacent to each other). A layer or sublayer may be formed by any known method in the art, including discrete deposition or continuous deposition processes. In one or more embodiments, a layer may be formed using only continuous deposition processes, or alternatively only discrete deposition processes.
[0046] In an embodiment, the substrate 450 is a glass substrate that is optionally chemically strengthened and includes a thickness of 0.05 to 2.0 mm. In one or more embodiments, the substrate 450 may be a transparent plastic (e.g., PMMA, polycarbonate, and the like), or may be a glass material (which may optionally be strengthened). As will also be discussed more fully below, in an embodiment, an opaque layer 500 is printed onto the second surface 480 of the substrate 450. In an embodiment, the opaque layer 500 is printed onto the light management layer 460 (when included). Certain existing UV curable inks have been shown to meet at least some of the requirements described herein with respect to Tables 1-4, but are shown to be incompatible with the light management layer 460 (e.g., lacking the necessary adhesion). For example, when used for an opaque layer, an existing photocurable ink may chemically react with the ink of the light management layer 460 (after deposition or after environmental testing) to change the properties of the ink layer (e.g., color, size). Existing photocurable inks may also diffuse into the light management layer 460 and reduce its performance. When used to form the opaque layer 500 and printed on the photo management layer 460, the photocurable inks described herein do not suffer from this deficiency and still provide adequate adhesion to the substrate 450 even when the photo management layer 460 is present.
[0047] In an embodiment, the glass article 400 includes a functional surface layer 490. The functional surface layer 490 can be configured to provide one or more of a variety of functions. For example, the functional surface layer 490 can be an optical coating configured to provide easy-to-clean properties, anti-glare properties, anti-reflective properties, and / or a semi-mirror coating. Such optical coatings can be produced using a single layer or multiple layers. In the case of an anti-reflective functional surface layer, multiple layers having alternating high and low refractive indices can be used to form such a layer. Non-limiting examples of low refractive index films include SiO 2 MgF 2 and Al 2 O 3 , and non-limiting examples of high refractive index films include Nb 2 O 5 、TiO 2 、ZrO 2 , HfO 2 and Y 2 O 3 . In an embodiment, the total thickness of such an optical coating (which may be disposed over an anti-glare surface or a smooth substrate surface) is 5 nm to 750 nm. In addition, in an embodiment, the functional surface layer 490 that provides easy-to-clean properties also provides an enhanced touch for touch screens and / or coatings / treatments to reduce fingerprints. In some embodiments, the functional surface layer 490 is integrated with the first surface of the substrate. For example, such a functional surface layer may include an etched surface in the first surface of the substrate 450 to provide an anti-glare surface (or a haze of, for example, 2% to 20%).
[0048] In an embodiment, the opaque layer 500 is composed of one or more photocurable inks described herein. Therefore, the opaque layer 500 can include a relatively high optical density (e.g., an optical density greater than 4) to block the transmission of light. In an embodiment, the opaque layer 500 is used to block light from passing through / through certain areas of the glass article 400. In an embodiment, the opaque layer 500 blocks functional or non-decorative elements provided for the operation of the glass article 400. In an embodiment, the opaque layer 500 is provided to outline the outline of backlit icons and / or other graphics (not depicted) to increase the contrast at the edges of such icons and / or graphics. The opaque layer 500 can be any color, but in a specific embodiment, the opaque layer 500 is black or gray. In an embodiment, the opaque layer 500 is applied above the light management layer 460 and / or above the second surface 480 of the substrate 450 via inkjet printing. Generally speaking, the thickness of the opaque layer 500 is less than or equal to 25 μm (e.g., greater than or equal to 1.0 μm and less than or equal to 25.0 μm, greater than or equal to 5.0 μm and less than or equal to 25.0 μm, greater than or equal to 5.0 μm and less than or equal to 20.0 μm, greater than or equal to 5.0 μm and less than or equal to 10.0 μm).
[0049] In an embodiment, the opaque layer 500 may be deposited directly onto the second surface 480 of the substrate 450 using a suitable inkjet process. In an embodiment, prior to the deposition of the opaque layer 500, the second surface 480 may be primed using a suitable primer (e.g., an acryloxysilane primer) to promote adhesion of the opaque layer 500 to the substrate 450. Any suitable treatment of the second surface 480 may be used to promote adhesion of the opaque layer 500 to the substrate 450.
[0050] In an embodiment, if Figure 2As shown, the glass article 400 is placed above or in front of the display 540. In one or more embodiments, the display 540 may include a touch-enabled display (including a display and a touchpad). Exemplary displays include LED displays, DLP MEMS chips, LCDs, OLEDs, transmissive displays, and the like. The glass article 400 may generally have an average transmittance of greater than or equal to 10% (e.g., greater than or equal to 20%, greater than or equal to 30%, greater than or equal to 40%, greater than or equal to 50%, greater than or equal to 60%, greater than or equal to 70%) at 380nm to 750nm. However, the high optical density of the opaque layer 500 results in a region of the glass article 400 including the opaque layer 500 having a relatively low optical transmittance (e.g., an average transmittance of less than or equal to 0.1% in the visible spectrum). Therefore, the boundary of the opaque layer 500 may define a display area 520 in which the glass article 400 exhibits a relatively high optical transmittance to facilitate visibility of an image produced by the display 540.
[0051] In the illustrated embodiment, the opaque layer 500 covers the edge 550 of the display 540 to hide the edge 550 from view through the first surface 470. The opaque layer 500 can also be used to block various other components (e.g., electrical connections, mechanical housings, and the like) from view. The opaque layer 500 generally helps the desired portion of the display 540 to be seen by a user viewing the first surface 470.
[0052] Still refer to Figure 2, when included, the light management layer 460 can be printed on the substrate 450. In an embodiment, the light management layer 460 is formed of a suitable thermal or UV curable ink. The light management layer 460 can generally reduce the optical transmittance of the glass article 400 so that the glass article 400 presents a similar appearance to the user regardless of whether the display 540 is powered on or off. For example, the light management layer 460 can block the edge of the display area 520 so that the boundary of the display area 520 is not perceived by the viewer when the display is powered off. The light management layer 460 can generally be constructed as described in international patent application WO 2019 / 055458 A1 entitled “Black Deadfront for Display Device and Methods,” WO 2020 / 205519 A1 entitled “Decorated Glass Having a Printed Ink Layer,” or WO 2021 / 118835 A1 entitled “Display Devices and Articles with Color-Matched Display and Non-Display Areas” (each of which is incorporated herein by reference in its entirety).
[0053] Figure 3 A flow chart illustrating a method 600 of forming a glass article having an opaque layer according to one or more embodiments of the present disclosure. The method 600 may be performed to manufacture the glass article described herein. Figure 2 Therefore, reference will be made to the description of Figure 2 It should be understood that other glass articles may be formed by performing the method 600 and that the method 600 is not limited to a particular number or order of process steps.
[0054] At block 602, a substrate 450 is manufactured. Any suitable glass production process may be used (e.g., a fusion down draw process, a float process, or the like). Additional details regarding glass forming methods are provided herein. At block 604, the substrate 450 is treated. For example, in an embodiment, the substrate 450 is subjected to a strengthening treatment (e.g., ion exchange strengthening, thermal strengthening). Additional details regarding the strengthening treatment that may be provided to the substrate 450 are provided herein.
[0055] In an embodiment, the treatment applied to the substrate 450 during block 602 can be used to form the functional surface layer 490. For example, in an embodiment, the substrate 450 is chemically etched so that at least the first surface 470 exhibits anti-glare properties. A suitable anti-reflective coating and / or ETC coating can also be deposited on the first surface 470 via a suitable deposition process. In an embodiment, the second surface 480 can be primed (e.g., using a suitable chemical primer or ink) to promote adhesion of the opaque layer 500. In an embodiment, the light control layer 460 can be deposited and cured onto the second surface 480 (e.g., a suitable ink can be thermally cured or cured via exposure to electromagnetic radiation).
[0056] At block 606, a photocurable ink is deposited onto the second surface 480 to begin forming the opaque layer 500. As described herein, a suitable inkjet printing device can be used to deposit droplets of suitable size onto the second surface 480 so that the photocurable ink forms a suitable pattern. Various parameters for operating the inkjet printing device (e.g., control waveform, translation rate, deposition temperature) can vary depending on the composition of the photocurable ink and the desired deposition pattern. At block 608, the photocurable ink is cured on the second surface 480 via exposure to electromagnetic radiation generated by a UV LED. In an embodiment, the UVLED emits radiation having a relatively narrow bandwidth (e.g., less than or equal to 50nm, less than or equal to 40nm, less than or equal to 30nm, less than or equal to 20nm) around a central UV wavelength (e.g., 375nm, 380nm, 385nm, 390nm, 395nm, 400nm). The operating parameters of the UVLED (e.g., output intensity, exposure period) can vary depending on various aspects of the opaque layer 500 (e.g., thickness, composition).
[0057] In an embodiment, blocks 606 and 608 may be performed when the substrate 450 comprises a planar shape. In an embodiment, blocks 606 and 608 may be performed when the substrate is in a curved shape. For example, after applying at least some of the processes described with respect to block 604, the substrate 450 may be cold formed via the methods described herein, and the opaque layer 500 may be formed on the cold formed glass substrate. In an embodiment, a suitable display panel is laminated to the glass article such that the opaque layer 500 at least partially covers the display panel.
[0058] Example
[0059] Embodiments of the present disclosure can be further understood from the following examples.
[0060] Examples 1-3
[0061] Photocurable inks with different compositions were formulated. A carbon black dispersion was added to the pigment dispersion of each of the inks. The concentration of the pigment was between 10% and 20% by weight of each of the photocurable inks. In Example 1, a pigment dispersion containing a carbon black pigment from Penn Color, Inc. was used, which included propoxylated neopentyl glycol diacrylate (PO-PPGDA) as a monomer. The carbon black pigment consisted of 10% by weight of the photocurable ink. In Example 2, a pigment dispersion containing a carbon black pigment from Penn Color, Inc. was used, which included trimethylolpropane triacrylate (TMPTA) as a monomer. The carbon black pigment consisted of 20% by weight of the photocurable ink. In Example 3, a pigment dispersion containing a carbon black pigment from Sun Color was used. The pigment dispersion of carbon black pigment of the photocurable ink comprises propoxylated neopentyl glycol diacrylate (PO-PPGDA) as a monomer. The carbon black pigment is composed of 10 wt% of the photocurable ink. The ink is jetted onto a chemically strengthened glass substrate using a research grade print head at a deposition temperature of 55°C to 65°C. The ink is deposited using a 10 pL droplet volume configured to utilize a resolution of 1270 dpi. The inkjet cartridge forms an opaque layer on the glass. Then, a UV LED centered at 395mm emits radiation to cure the ink.
[0062] The optical density of the resulting opaque layer of the samples produced according to Examples 1-3 was measured using a densitometer. Figure 4 Graph 700 depicts optical density as a function of opaque layer thickness for various samples produced. As shown by point 702, the opaque layer produced by Example 2 (having the highest weight % pigment) produced an optical density greater than 4.0 at a thickness of less than 8 μm, demonstrating the efficacy of the photocurable inks described herein. When the glass was primed with an acryloxysilane primer prior to printing, Figure 4 Each of the samples shown was also tested for adhesion and passed the adhesion test (greater than or equal to 4B adhesion when measured according to ASTM 3359).
[0063] Samples produced using the ink formulation of Example 1 were subjected to high and high humidity temperature testing by heating the samples to 85°C in an environment of 95% relative humidity for a period of 500 hours and subsequently tested for adhesion according to ASTM 3359. Figure 5 The results of the cross-hatch adhesion test are shown. As shown, the appearance of the opaque layer 802 is largely unaffected by the adhesion test, with only a small portion of the opaque layer (depicted on the bottom side of the tape 804 used for the test) being removed along the cuts. Such results indicate the reliability and durability of the light-curable inks described herein.
[0064] Example 4
[0065] Another example was formulated using the composition shown in Table 6. As shown, the ink formulated according to Example 4 contained 10 wt% carbon black pigment. The ink was jetted onto chemically strengthened glass at 60°C using a research-grade printhead, and the printed parts were then cured using UV LEDs, and the optical density and thickness were measured. The measured optical density at a thickness of 21 μm was 4.2. The ink passed the adhesion test (greater than or equal to 4B when measured according to ASTM 3359). It is believed that using a pigment dispersion with a more dilute monomer can achieve higher optical density at thinner thicknesses.
[0066] Table 6
[0067]
[0068] Example 5
[0069] Another example was formulated using the composition shown in Table 7. This example differs from the previous examples in that the photoinitiator package was modified to maintain cure while reducing the total percentage in the formulation to provide greater formulation flexibility. In an embodiment, the photoinitiator package includes an amount less than or equal to 5 wt % (e.g., greater than or equal to 2 wt % and less than or equal to 4.5 wt %, greater than or equal to 2.5 wt % and less than or equal to 4.0%) to provide formulation flexibility (e.g., to facilitate the addition of viscosity modifiers). It was observed that Sun Chemical D3310-FX-K (25% in IBOA) has a much lower viscosity than UVDJ207 (25% in PONPGDA), making it more attractive for inkjet printing. The experimental mixture design was also used to optimize the formulation for viscosity, printability, total thickness and OD. In this work, dipropylene glycol diacrylate (DPGDAM222) was found to outperform hydroxy neopentyl glycol diacrylate (HPNDA M210), especially when coupled with polydipentaerythritol hexaacrylate (DPHA M600) and vinyl methyl oxazolidinone (Vmox). DPHA M600 adds additional crosslinking to the ink and aids in curing. Vmox replaces n-vinyl caprolactam and acts as a better viscosity modifier while aiding adhesion. As shown in Table 7, the ink formulated according to Example 5 contained 11.25 wt% carbon black pigment. The ink was jetted onto chemically strengthened glass using a KM1024i SHE printhead at 50°C, the printed parts were then cured using UV LED, and the optical density and thickness were measured.
[0070] The printed parts were formed using a three-pulse waveform with a total duration of 30 μs (including a first 10 μs pulse of 1 V, a second 10 μs pulse of -1 V, and a third 10 μs pulse of 0 V). The droplet volume was from 2.9 pL to 9.0 pL. The droplet velocity was from 2.67 m / s to 2.86 m / s. The droplet angle was from 0.21° to 0.60°. Figure 7 A graph of optical density as a function of thickness for a number of samples prepared according to Example 5 is depicted. As shown, the formulation provides an optical density greater than 4.0 for thicknesses greater than 10 μm. For example, the optical density measured at a thickness of 11 μm was 4.8. Example 5 was subjected to high and high humidity temperature testing by heating the sample to 85°C in an environment of 95% relative humidity for a period of 500 hours and then tested for adhesion according to ASTM 3359. Figure 8 As shown, the ink passed the adhesion test (greater than or equal to 4B when measured according to ASTM 3359). The appearance of the opaque layer 1000 was largely unaffected by the adhesion test, with only a small portion of the opaque layer (depicted on the bottom side of the tape 1002 used for testing) being removed along the cut. Such results indicate the reliability and durability of the light-curable inks described herein.
[0071] Table 7
[0072]
[0073] Opposite Embodiment
[0074] Two commercially available UV curable inks (Inks A and B) were deposited onto pre-primed, chemically strengthened glass and tested under high temperature and high humidity testing conditions (85° C. and 95% relative humidity for 500 hours). Fig. 6A and Figure 6B The samples after testing are shown. As shown, both samples exhibit visible cracks 902, 904 due to wrinkling of the opaque layer. When exposed to high temperature conditions for a long time, the light-curable ink advantageously does not exhibit visible cracks, demonstrating the improved durability and reliability of the inks described herein.
[0075] Glass material
[0076] The various glass layers of the decorative glass discussed herein (e.g., substrate 450) can be formed from any suitable glass composition including soda-lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, alkali-containing borosilicate glass, and alkali-containing boroaluminosilicate glass.
[0077] Unless otherwise indicated, the glass compositions disclosed herein are described in terms of mole percent (mol %) analyzed on an oxide basis.
[0078] In one or more embodiments, the glass composition comprises SiO 2 The amount can range from about 66 mol % to about 80 mol %, about 67 mol % to about 80 mol %, about 68 mol % to about 80 mol %, about 69 mol % to about 80 mol %, about 70 mol % to about 80 mol %, about 72 mol % to about 80 mol %, about 65 mol % to about 78 mol %, about 65 mol % to about 76 mol %, about 65 mol % to about 75 mol %, about 65 mol % to about 74 mol %, about 65 mol % to about 72 mol %, or about 65 mol % to about 70 mol %, and all ranges and subranges therebetween.
[0079] In one or more embodiments, the glass composition includes Al 2 O 3 The amount of Al contained in the glass composition is greater than about 4 mol% or greater than about 5 mol%. 2 O 3 In one or more embodiments, Al is in the range of greater than about 7 mol% to about 15 mol%, greater than about 7 mol% to about 14 mol%, about 7 mol% to about 13 mol%, about 4 mol% to about 12 mol%, about 7 mol% to about 11 mol%, about 8 mol% to about 15 mol%, 9 mol% to about 15 mol%, about 9 mol% to about 15 mol%, about 10 mol% to about 15 mol%, about 11 mol% to about 15 mol%, or about 12 mol% to about 15 mol%, and all ranges and sub-ranges therebetween. In one or more embodiments, Al is in the range of greater than about 7 mol% to about 15 mol%, greater than about 7 mol% to about 14 mol%, about 7 mol% to about 13 mol%, about 4 mol% to about 12 mol%, about 7 mol% to about 11 mol%, about 8 mol% to about 15 mol%, about 9 mol% to about 15 mol%, about 10 mol% to about 15 mol%, about 11 mol% to about 15 mol%, or about 12 mol% to about 15 mol%, and all ranges and sub-ranges therebetween. 2 O 3 The upper limit of may be about 14 mol%, 14.2 mol%, 14.4 mol%, 14.6 mol%, or 14.8 mol%.
[0080] In one or more embodiments, the glass layer herein is described as an aluminosilicate glass article or comprises an aluminosilicate glass composition. In such embodiments, the glass composition or article formed therefrom comprises SiO 2 With Al 2 O 3 In this regard, the Al content of the glass composition or article formed therefrom is 2 O 3 The amount is about 2 mol % or greater, 2.25 mol % or greater, 2.5 mol % or greater, about 2.75 mol % or greater, about 3 mol % or greater.
[0081] In one or more embodiments, the glass composition comprises B 2 O 3(e.g., about 0.01 mol % or more). In one or more embodiments, the glass composition includes B 2 O 3 The amount of B ranges from about 0 mol% to about 5 mol%, about 0 mol% to about 4 mol%, about 0 mol% to about 3 mol%, about 0 mol% to about 2 mol%, about 0 mol% to about 1 mol%, about 0 mol% to about 0.5 mol%, about 0.1 mol% to about 5 mol%, about 0.1 mol% to about 4 mol%, about 0.1 mol% to about 3 mol%, about 0.1 mol% to about 2 mol%, about 0.1 mol% to about 1 mol%, about 0.1 mol% to about 0.5 mol%, and all ranges and sub-ranges therebetween. In one or more embodiments, the glass composition contains substantially no B. 2 O 3 .
[0082] As used herein, "substantially free" with respect to a component of a composition means that the component is not actively or intentionally added to the composition during initial formulation, but may be present as an impurity in an amount less than about 0.001 mole %.
[0083] In one or more embodiments, the glass composition optionally comprises P 2 O 5 (e.g., about 0.01 mol % or greater). In one or more embodiments, the glass composition comprises up to (and includes) 2 mol %, 1.5 mol %, 1 mol % or 0.5 mol % of P 2 O 5 In one or more embodiments, the glass composition contains substantially no P 2 O 5 .
[0084] In one or more embodiments, the glass composition comprises R 2 The total amount of O (for alkali metal oxides (such as Li 2 O、Na 2 O.K 2 O、Rb 2 O and Cs 2 The total amount of R (O) may be greater than or equal to about 8 mol%, greater than or equal to about 10 mol%, or greater than or equal to about 12 mol%. In some embodiments, the glass composition includes R 2The total amount of O is in the range of about 8 mol% to about 20 mol%, about 8 mol% to about 18 mol%, about 8 mol% to about 16 mol%, about 8 mol% to about 14 mol%, about 8 mol% to about 12 mol%, about 9 mol% to about 20 mol%, about 10 mol% to about 20 mol%, about 11 mol% to about 20 mol%, about 12 mol% to about 20 mol%, about 13 mol% to about 20 mol%, about 10 mol% to about 14 mol%, or 11 mol% to about 13 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition may be substantially free of Rb. 2 O、Cs 2 O or Rb 2 O and Cs 2 In one or more embodiments, R 2 O may contain only Li 2 O、Na 2 O and K 2 In one or more embodiments, the glass composition may include a selected from Li 2 O、Na 2 O and K 2 O, wherein the alkali metal oxide is present in an amount greater than about 8 mol % or more.
[0085] In one or more embodiments, the glass composition includes Na 2 The amount of O is greater than or equal to about 8 mol%, greater than or equal to about 10 mol%, or greater than or equal to about 12 mol%. In one or more embodiments, the composition includes Na 2 O ranges from about 8 mol % to about 20 mol %, about 8 mol % to about 18 mol %, about 8 mol % to about 16 mol %, about 8 mol % to about 14 mol %, about 8 mol % to about 12 mol %, about 9 mol % to about 20 mol %, about 10 mol % to about 20 mol %, about 11 mol % to about 20 mol %, about 12 mol % to about 20 mol %, about 13 mol % to about 20 mol %, about 10 mol % to about 14 mol %, or 11 mol % to about 16 mol %, and all ranges and subranges therebetween.
[0086] In one or more embodiments, the glass composition comprises less than about 4 mol% K 2 O, less than about 3 mol% K 2 O or less than about 1 mol% K 2 O. In some cases, the glass composition includes K 2The amount of O may range from about 0 mol% to about 4 mol%, from about 0 mol% to about 3.5 mol%, from about 0 mol% to about 3 mol%, from about 0 mol% to about 2.5 mol%, from about 0 mol% to about 2 mol%, from about 0 mol% to about 1.5 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.5 mol%, from about 0 mol% to about 0.2 mol%, from about 0 mol% to about 0.1 mol%, from about 0.5 mol% to about 4 mol%, from about 0.5 mol% to about 3.5 mol%, from about 0.5 mol% to about 3 mol%, from about 0.5 mol% to about 2.5 mol%, from about 0.5 mol% to about 2 mol%, from about 0.5 mol% to about 1.5 mol%, or from about 0.5 mol% to about 1 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition may be substantially free of K. 2 O.
[0087] In one or more embodiments, the glass composition contains substantially no Li 2 O.
[0088] In one or more embodiments, the Na in the composition 2 The amount of O can be greater than that of Li 2 O. In some cases, Na 2 The amount of O can be greater than that of Li 2 O and K 2 In one or more alternative embodiments, the Li 2 The amount of O can be greater than that of Na 2 The amount of O or Na 2 O and K 2 The combined amount of O.
[0089] In one or more embodiments, the glass composition may include a total amount of RO (being the total amount of alkaline earth metal oxides (e.g., CaO, MgO, BaO, ZnO, and SrO) in the range of about 0 mol% to about 2 mol%. In some embodiments, the glass composition includes a non-zero amount of RO up to about 2 mol%. In one or more embodiments, the glass composition includes RO in an amount of about 0 mol% to about 1.8 mol%, about 0 mol% to about 1.6 mol%, about 0 mol% to about 1.5 mol%, about 0 mol% to about 1.4 mol%, about 0 mol% to about 1.2 mol%, about 0 mol% to about 1 mol%, about 0 mol% to about 0.8 mol%, about 0 mol% to about 0.5 mol%, and all ranges and sub-ranges therebetween.
[0090] In one or more embodiments, the glass composition includes CaO in an amount of less than about 1 mol%, less than about 0.8 mol%, or less than about 0.5 mol%. In one or more embodiments, the glass composition is substantially free of CaO. In some embodiments, the glass composition includes MgO in an amount of about 0 mol% to about 7 mol%, about 0 mol% to about 6 mol%, about 0 mol% to about 5 mol%, about 0 mol% to about 4 mol%, about 0.1 mol% to about 7 mol%, about 0.1 mol% to about 6 mol%, about 0.1 mol% to about 5 mol%, about 0.1 mol% to about 4 mol%, about 1 mol% to about 7 mol%, about 2 mol% to about 6 mol%, or about 3 mol% to about 6 mol%, and all ranges and sub-ranges therebetween.
[0091] In one or more embodiments, the glass composition includes ZrO 2 The amount of ZrO is equal to or less than about 0.2 mol%, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, less than about 0.12 mol%. In one or more embodiments, the glass composition includes ZrO 2 The range is about 0.01 mol % to about 0.2 mol %, about 0.01 mol % to about 0.18 mol %, about 0.01 mol % to about 0.16 mol %, about 0.01 mol % to about 0.15 mol %, about 0.01 mol % to about 0.14 mol %, about 0.01 mol % to about 0.12 mol % or about 0.01 mol % to about 0.10 mol %, and all ranges and sub-ranges therebetween.
[0092] In one or more embodiments, the glass composition includes SnO 2 The amount of SnO is equal to or less than about 0.2 mol%, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, less than about 0.12 mol%. In one or more embodiments, the glass composition includes SnO 2 The range is about 0.01 mol % to about 0.2 mol %, about 0.01 mol % to about 0.18 mol %, about 0.01 mol % to about 0.16 mol %, about 0.01 mol % to about 0.15 mol %, about 0.01 mol % to about 0.14 mol %, about 0.01 mol % to about 0.12 mol % or about 0.01 mol % to about 0.10 mol %, and all ranges and sub-ranges therebetween.
[0093] In one or more embodiments, the glass composition may include an oxide that imparts color or hue to the glass article. In some embodiments, the glass composition includes an oxide that prevents the glass article from discoloring when exposed to ultraviolet radiation. Examples of such oxides include, but are not limited to, the following oxides: Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ce, W, and Mo.
[0094] In one or more embodiments, the glass composition comprises Fe 2 O 3 In some embodiments, the glass composition contains substantially no Fe. In one or more embodiments, the glass composition contains Fe 2 O 3 The amount of Fe is equal to or less than about 0.2 mol%, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, less than about 0.12 mol%. In one or more embodiments, the glass composition includes Fe 2 O 3 The range is about 0.01 mol % to about 0.2 mol %, about 0.01 mol % to about 0.18 mol %, about 0.01 mol % to about 0.16 mol %, about 0.01 mol % to about 0.15 mol %, about 0.01 mol % to about 0.14 mol %, about 0.01 mol % to about 0.12 mol % or about 0.01 mol % to about 0.10 mol %, and all ranges and sub-ranges therebetween.
[0095] When the glass composition contains TiO 2 When TiO 2 The amount of TiO can be about 5 mol% or less, about 2.5 mol% or less, about 2 mol% or less, or about 1 mol% or less. In one or more embodiments, the glass composition can be substantially free of TiO. 2 .
[0096] An exemplary glass composition includes SiO 2 The amount ranges from about 65 mol% to about 75 mol%, Al 2 O 3 The amount ranges from about 8 mol% to about 14 mol%, Na 2 The amount of O ranges from about 12 mol % to about 17 mol %, K 2 The amount of O ranges from about 0 mol% to about 0.2 mol%, and the amount of MgO ranges from about 1.5 mol% to about 6 mol%. Optionally, SnO disclosed elsewhere herein may be included. 2 The amount.
[0097] Strengthened glass properties
[0098] In one or more embodiments, the cold-formed glass sheet 2010 or other glass layers of any decorative glass embodiment discussed herein may be formed from a strengthened glass sheet or article. In one or more embodiments, the glass article used to form a layer of a decorative glass structure discussed herein may be strengthened to include a compressive stress extending from the surface to a depth of compression (DOC). The compressive stress region is balanced by a central portion exhibiting tensile stress. At the DOC, the stress crosses from a positive (compressive) stress to a negative (tensile) stress.
[0099] In one or more embodiments, the glass articles used to form the layers of the decorative glass structures discussed herein can be mechanically strengthened by exploiting the mismatch in thermal expansion coefficients between portions of the glass to produce regions of compressive stress and a central region exhibiting tensile stress. In some embodiments, the glass articles can be thermally strengthened by heating the glass to a temperature above the glass transition point and then rapidly quenching.
[0100] In one or more embodiments, the glass articles used to form the layers of the decorative glass structures discussed herein can be chemically strengthened by ion exchange. In the ion exchange process, ions at or near the surface of the glass article are replaced or exchanged by larger ions of the same valence or oxidation state. In those embodiments where the glass article comprises an alkali aluminosilicate glass, the ions in the surface layer of the article and the larger ions are monovalent alkali metal cations (e.g., Li+, Na+, K+, Rb+, and Cs+). Alternatively, the monovalent cations in the surface layer can be replaced by monovalent cations other than alkali metal cations (e.g., Ag+ or the like). In such embodiments, the monovalent ions (or cations) exchanged into the glass article produce stress.
[0101] The ion exchange process is typically performed by immersing the glass article in a molten salt bath (or two or more molten salt baths) containing larger ions to exchange with smaller ions in the glass article. It should be noted that aqueous salt baths may also be utilized. In addition, the composition of the bath may contain more than one type of larger ion (e.g., Na+ and K+) or a single larger ion. It will be appreciated by those skilled in the art that the parameters for the ion exchange process include, but are not limited to, the composition and temperature of the bath, the immersion time, the number of immersions of the glass article in the salt bath (or baths), the use of multiple salt baths, additional steps (such as annealing, washing, and the like), and are typically determined by the composition of the glass layer of the decorative glass structure (including the structure of the article and any crystalline phases present) and the DOC and CS of the glass layer of the desired decorative glass structure produced via strengthening.
[0102] Exemplary molten bath compositions may include nitrates, sulfates, chlorides of larger alkali metal ions. Typical nitrates include KNO 3 、NaNO 3 、LiNO 3 、NaSO 4 and combinations thereof. Depending on the glass thickness, the temperature of the bath, the glass (or monovalent ion) diffusivity, the temperature of the molten salt bath is generally in the range of about 380°C to about 450°C, and the immersion time is in the range of about 15 minutes to about 100 hours. However, temperatures and immersion times different from those described above may also be used.
[0103] In one or more embodiments, the glass article used to form a layer of decorative glass may be immersed in 100% NaNO having a temperature of about 370° C. to about 480° C. 3 , 100% KNO 3 or NaNO 3 With KNO 3 In some embodiments, the glass layer of the decorative glass may be immersed in a molten salt bath containing about 5% to about 90% KNO 3 and about 10% to about 95% NaNO 3 In one or more embodiments, after being immersed in the first bath, the glass article may be immersed in a second bath. The first and second baths may have different compositions and / or temperatures from each other. The immersion times in the first and second baths may be different. For example, the time of immersion in the first bath may be longer than the time of immersion in the second bath.
[0104] In one or more embodiments, the glass article used to form a layer of the decorative glass structure may be immersed in a NaNO containing solution having a temperature of less than about 420° C. (e.g., about 400° C. or about 380° C.). 3 With KNO 3 The molten mixed salt bath (eg, 49% / 51%, 50% / 50%, 51% / 49%) lasts less than about 5 hours, or even about 4 hours or less.
[0105] The ion exchange conditions may be tailored to provide a "spike" or increase the slope of the stress profile at or near the surface of the glass layer of the resulting decorative glass structure. The spike may result in a greater surface CS value. Due to the unique properties of the glass compositions used in the glass layers of the decorative glass structures described herein, this spike may be achieved by a single bath or multiple baths, where the baths have a single composition or a mixed composition.
[0106] In one or more embodiments, when more than one monovalent ion is exchanged into a glass article used to decorate a layer of a glass structure, different monovalent ions may be exchanged to different depths within the glass layer (and produce different amounts of stress at different depths within the glass article). The relative depths of the stress-producing ions produced may be determined and result in different characteristics of the stress profile.
[0107] CS is measured using methods known in the art, such as a surface stress meter (FSM) using a commercially available instrument such as the FSM-6000 manufactured by Orihara Industrial Co., Ltd (Japan). Surface stress measurements rely on accurate measurements of the stress optical number (SOC) associated with the birefringence of the glass. SOC is then measured by methods known in the art, such as the fiber and four point bend methods (both of which are described in ASTM standard C770-98 (2013), entitled “Standard Test Method for Measurement of Glass Stress-Optical Coefficient”, the contents of which are incorporated herein by reference), and the bulk cylinder method. As used herein, CS may be the “maximum compressive stress” of the highest compressive stress value measured within the compressive stress layer. In some embodiments, the maximum compressive stress is located at the surface of the glass article. In other embodiments, the maximum compressive stress may occur at a depth below the surface, and the compression profile given may appear as a “buried peak”.
[0108] Depending on the strengthening method and conditions, DOC can be measured by FSM or by a scattered light polarizer (SCALP) (e.g., a SCALP-04 scattered light polarizer available from Glasstress Ltd. of Tallinn, Estonia). When the glass article is chemically strengthened by an ion exchange process, either FSM or SCALP can be used, depending on which ions are exchanged into the glass article. In the case where stress in the glass article is generated by exchanging potassium ions into the glass article, FSM is used to measure DOC. In the case where stress is generated by exchanging sodium ions into the glass article, SCALP is used to measure DOC. When stress in the glass article is generated by exchanging potassium ions and sodium ions into the glass, DOC is measured by SCALP because the exchange depth of sodium is considered to indicate the DOC, while the exchange depth of potassium ions indicates the change in the magnitude of the compressive stress (but not the change in stress from compression to tension); the exchange depth of potassium ions in such glass articles is measured by FSM. Central tension or CT is the maximum tensile stress and is measured by SCALP.
[0109] In one or more embodiments, the glass article used to form the layer of the decorative glass structure can be strengthened to exhibit a DOC (as described herein) described as a portion of the thickness t of the glass article. For example, in one or more embodiments, the DOC can be equal to or greater than about 0.05t, equal to or greater than about 0.1t, equal to or greater than about 0.11t, equal to or greater than about 0.12t, equal to or greater than about 0.13t, equal to or greater than about 0.14t, equal to or greater than about 0.15t, equal to or greater than about 0.16t, equal to or greater than about 0.17t, equal to or greater than about 0.18t, equal to or greater than about 0.19t, equal to or greater than about 0.2t, equal to or greater than about 0.21t. In some embodiments, the DOC may range from about 0.08t to about 0.25t, about 0.09t to about 0.25t, about 0.18t to about 0.25t, about 0.11t to about 0.25t, about 0.12t to about 0.25t, about 0.13t to about 0.25t, about 0.14t to about 0.25t, about 0.15t to about 0.25t, about 0.08t to about 0.24t, about 0.08t to about 0.23t, about 0.08t to about 0.22t, about 0.08t to about 0.21t, about 0.08t to about 0.2t, about 0.08t to about 0.19t, about 0.08t to about 0.18t, about 0.08t to about 0.17t, about 0.08t to about 0.16t, or about 0.08t to about 0.15t. In some cases, the DOC may be about 20 μm or less. In one or more embodiments, the DOC may be about 40 μm or greater (e.g., about 40 μm to about 300 μm, about 50 μm to about 300 μm, about 60 μm to about 300 μm, about 70 μm to about 300 μm, about 80 μm to about 300 μm, about 90 μm to about 300 μm, about 100 μm to about 300 μm, about 110 μm to about 300 μm, about 120 μm to about 300 μm, about 140 μm to about 300 μm, about 150 μm to about 300 μm, about 40 μm to about 290 μm, about 50 μm to about 300 μm). um, about 40 μm to about 180 μm, about 40 μm to about 160 μm, about 40 μm to about 150 μm, about 40 μm to about 140 μm, about 40 μm to about 130 μm, about 40 μm to about 120 μm, about 40 μm to about 110 μm, or about 40 μm to about 100 μm.
[0110] In one or more embodiments, the CS of the glass article used to form a layer of the decorative glass structure (which may be found at the surface or at a depth within the glass article) may be about 200 MPa or greater, 300 MPa or greater, 400 MPa or greater, about 500 MPa or greater, about 600 MPa or greater, about 700 MPa or greater, about 800 MPa or greater, about 900 MPa or greater, about 930 MPa or greater, about 1000 MPa or greater, or about 1050 MPa or greater.
[0111] In one or more embodiments, the maximum tensile stress or central tension (CT) of the glass article used to form the layer of the decorative glass structure can be about 20 MPa or more, about 30 MPa or more, about 40 MPa or more, about 45 MPa or more, about 50 MPa or more, about 60 MPa or more, about 70 MPa or more, about 75 MPa or more, about 80 MPa or more, or about 85 MPa or more. In some embodiments, the maximum tensile stress or central tension (CT) can range from about 40 MPa to about 100 MPa.
[0112] The embodiments of the present disclosure can be further understood from the following aspects:
[0113] Aspect (1) relates to a glass article comprising: a glass substrate having a first major surface and a second major surface, the second major surface being opposite to the first major surface; and an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink, the photocurable ink comprising at least 10 weight percent of a pigment, wherein: the opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than 4.0, and after being cured by exposure to curing light from an ultraviolet (“UV”) light emitting diode (“LED”), the opaque layer exhibits: a pencil hardness greater than or equal to 3H measured in accordance with ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B after being tested in accordance with ASTM 3359 at a temperature of 85° C. and a relative humidity of 95% for a period of at least 500 hours.
[0114] Aspect (2) of the present disclosure relates to the glass article according to aspect (1), wherein the photocurable ink comprises at least 30 wt % of a pigment dispersion, the pigment dispersion comprising greater than or equal to 25 wt % of a pigment and a reactive monomer.
[0115] Aspect (3) of the present disclosure relates to the glass article according to aspect (2), wherein the pigment dispersion comprises greater than or equal to 40 wt % of the pigment.
[0116] Aspect (4) of the present disclosure relates to the glass article according to any one of aspects (1) to (3), wherein the thickness is less than or equal to 10 μm.
[0117] Aspect (5) of the present disclosure relates to a glass article according to any one of aspects (1) to (4), wherein the photocurable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
[0118] Aspect (6) of the present disclosure relates to the glass article according to any one of aspects (1)-(5), wherein the pigment comprises an average particle size of less than or equal to 200 nm.
[0119] Aspect (7) of the present disclosure relates to the glass article according to any one of aspects (1)-(6), wherein the opaque layer exhibits a cured surface tension greater than 36 dynes / cm.
[0120] Aspect (8) of the present disclosure relates to a glass article according to any one of aspects (1) to (7), wherein the opaque layer exhibits a relative humidity greater than or equal to 1×10 9 Resistivity of Ω / sq.
[0121] Aspect (9) of the present disclosure relates to the glass article according to any one of aspects (1)-(8), wherein the glass article exhibits a CIELAB SCI L* value less than or equal to 30 when illuminated by a D65 illuminant at an angle of 10°.
[0122] Aspect (10) of the present disclosure relates to a glass article according to any one of aspects (1) to (9), wherein the glass article exhibits a CIELAB SCI a* value greater than or equal to -0.05 and less than or equal to 0.15 and a CIELAB SCI b* value greater than or equal to -0.3 and less than or equal to -0.1 when illuminated by a D65 illuminant at an angle of 10°.
[0123] Aspect (11) of the present disclosure relates to a glass article according to any one of aspects (1)-(10), further comprising a light management layer disposed on the second major surface between the glass substrate and the opaque layer, wherein the light management layer is formed of ink and comprises an average optical transmittance of less than or equal to 70% at 380 nm to 750 nm.
[0124] Aspect (12) of the present disclosure relates to a glass article according to any one of aspects (1) to (11), wherein the glass substrate comprises at least one of soda-lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, or alkali-containing borosilicate glass.
[0125] Aspect (13) of the present disclosure relates to a display for a vehicle interior system, the display comprising: a glass substrate having a first major surface and a second major surface, the second major surface being opposite to the first major surface; an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink, the photocurable ink comprising at least 10 weight percent pigment; and a display panel disposed on the second major surface, wherein: the opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than 4.0, and after being cured by exposure to curing light from an ultraviolet (“UV”) light emitting diode (“LED”), the opaque layer exhibits: a pencil hardness greater than or equal to 3H measured in accordance with ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B for a period of at least 500 hours at a temperature of 85°C and a relative humidity of 95% when tested in accordance with ASTM 3359.
[0126] Aspect (14) of the present disclosure relates to a display according to aspect (14), wherein the photocurable ink comprises at least 30 wt % of a pigment dispersion, the pigment dispersion comprising greater than or equal to 25 wt % of a pigment and a reactive monomer.
[0127] Aspect (15) of the present disclosure relates to the display according to any one of aspects (13)-(14), wherein the thickness is less than or equal to 10 μm.
[0128] Aspect (16) of the present disclosure relates to a display according to any one of aspects (13) to (15), wherein the photocurable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
[0129] Aspect (17) of the present disclosure relates to a display according to any one of aspects (13)-(16), wherein the pigment comprises an average particle size less than or equal to 200 nm.
[0130] Aspect (18) of the present disclosure relates to a display according to any one of aspects (13)-(17), wherein the display exhibits a CIELAB SCI L* value less than or equal to 30 when illuminated by a D65 illuminant at an angle of 10°.
[0131] Aspect (19) of the present disclosure relates to a display according to any one of aspects (13)-(18), wherein when illuminated by a D65 illuminant at a 10° angle, the display exhibits a CIELAB SCI a* value greater than or equal to -0.05 and less than or equal to 0.15 and a CIELAB SCI b* value greater than or equal to -0.3 and less than or equal to -0.1.
[0132] Aspect (20) of the present disclosure relates to a display according to any one of aspects (13)-(19), further comprising a light management layer disposed on a second major surface between the glass substrate and the opaque layer, wherein the light management layer is formed by ink and comprises an average optical transmittance of less than or equal to 70% at 380nm to 750nm.
[0133] Aspect (21) relates to a method for manufacturing a glass article, the method comprising: depositing a photocurable ink onto a major surface of a glass substrate using an inkjet print head at a deposition temperature of less than or equal to 65° C., wherein during deposition, the photocurable ink has a viscosity of less than 25 cP, wherein the photocurable ink comprises at least 10 wt % of a pigment and at least 50 wt % of a reactive monomer; and curing the photocurable ink on the major surface by exposing the photocurable ink to curing light generated by an ultraviolet (“UV”) light emitting diode (“LED”) to form an opaque layer, wherein the curing light has a bandwidth of less than or equal to 30 nm, wherein: the opaque layer comprises a thickness of less than or equal to 25 μm and an optical density of greater than or equal to 4.0, and the opaque layer exhibits: a pencil hardness of greater than or equal to 3H measured in accordance with ASTM 3363, and an adhesion to the glass substrate of greater than or equal to 4B for a period of at least 500 hours at a temperature of 85° C. and a relative humidity of 95% when tested in accordance with ASTM 3359.
[0134] Aspect (22) relates to the method according to aspect (21), further comprising: priming the major surface of the glass substrate with an acryloxysilane primer before depositing the photocurable ink.
[0135] Aspect (23) relates to a method according to any one of aspects (21)-(22), wherein the opaque layer covers a peripheral portion of the main surface so that the glass article exhibits a higher optical transmittance of 380 nm to 750 nm in a central area excluding the opaque layer.
[0136] Aspect (24) relates to a method according to any one of aspects (21) to (23), wherein the photocurable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
[0137] Aspect (25) relates to a method according to any one of aspects (21)-(24), further comprising performing one or more additional surface treatments on additional major surfaces of the glass substrate, the one or more additional surface treatments comprising chemically etching the additional major surfaces so that the additional major surfaces exhibit anti-glare properties and depositing an anti-reflective coating onto at least one of the additional major surfaces.
[0138] Aspect (26) relates to a method according to any one of aspects (21)-(25), further comprising: before depositing the photocurable ink, depositing a photomanagement layer onto the main surface, the photomanagement layer comprising an ink that is different in composition from the photocurable ink and at least partially overlaps the opaque layer.
[0139] Unless explicitly stated otherwise, any method described herein is not intended to be construed as requiring that its steps be performed in a particular order. Thus, in the event that a method claim does not actually recite the order of its steps or the claim or description does not specifically state that the steps are limited to a particular order, no particular order is inferred. Furthermore, the articles "a / an" as used herein are intended to include one or more than one component or element and are not intended to be construed to mean only one.
[0140] Those skilled in the art will appreciate that various modifications and changes may be made without departing from the spirit or scope of the disclosed embodiments. Since those skilled in the art may devise modified combinations, sub-combinations, and variations of the disclosed embodiments that include the spirit and substance of the embodiments, the disclosed embodiments should be interpreted as including all contents within the scope of the appended claims and their equivalents.
Claims
1. A glass product comprising: A glass substrate having a first main surface and a second main surface, wherein the second main surface is opposite to the first main surface; as well as an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink, the photocurable ink comprising at least 10% by weight of a pigment, wherein: The opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than or equal to 4.0, and After curing via exposure to curing light from an ultraviolet ("UV") light emitting diode ("LED"), the opaque layer exhibits: A pencil hardness of 3H or greater as measured in accordance with ASTM 3363, and An adhesion to the glass substrate of greater than or equal to 4B after a period of at least 500 hours at a temperature of 85° C. and a relative humidity of 95% when tested according to ASTM 3359.
2. The glass article of claim 1, wherein the photocurable ink comprises at least 30 wt% of a pigment dispersion, the pigment dispersion comprising greater than or equal to 25 wt% of the pigment and a reactive monomer.
3. The glass article of claim 2, wherein the pigment dispersion comprises greater than or equal to 40 weight percent of the pigment.
4. The glass article according to any one of claims 1 to 3, wherein the thickness is less than or equal to 10 μm.
5. The glass article according to any one of claims 1 to 4, wherein the light-curable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
6. The glass article of any one of claims 1-5, wherein the pigment comprises an average particle size less than or equal to 200 nm.
7. The glass article of any one of claims 1-6, wherein the opaque layer exhibits a cured surface tension greater than 36 dynes / cm.
8. The glass article of any one of claims 1 to 7, wherein the opaque layer exhibits a relative humidity greater than or equal to 1×10 9 Resistivity of Ω / sq.
9. The glass article of any one of claims 1-8, wherein the glass article exhibits a CIELAB SCI L* value of less than or equal to 30 when illuminated by a D65 illuminant at an angle of 10°.
10. The glass article of any one of claims 1-9, wherein the glass article exhibits a CIELAB SCI a* value greater than or equal to -0.05 and less than or equal to 0.15 and a CIELAB SCI b* value greater than or equal to -0.3 and less than or equal to -0.1 when illuminated by a D65 illuminant at a 10° angle.
11. The glass article according to any one of claims 1 to 10, further comprising a light management layer disposed on the second major surface between the glass substrate and the opaque layer, wherein the light management layer is formed of ink and comprises an average optical transmittance of less than or equal to 70% at 380 nm to 750 nm.
12. The glass article of any one of claims 1-11, wherein the glass substrate comprises at least one of soda-lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, or alkali-containing borosilicate glass.
13. A display for an internal system of a vehicle, the display comprising: A glass substrate having a first main surface and a second main surface, wherein the second main surface is opposite to the first main surface; an opaque layer disposed on the second major surface, the opaque layer comprising a photocurable ink comprising at least 10% by weight of a pigment; as well as A display panel is arranged on the second main surface, wherein: The opaque layer is disposed at a peripheral region of the second major surface and extends over an edge of the display panel, The opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than or equal to 4.0, and After curing via exposure to curing light from an ultraviolet ("UV") light emitting diode ("LED"), the opaque layer exhibits: A pencil hardness of 3H or greater as measured in accordance with ASTM 3363, and Adhesion to the glass substrate of greater than or equal to 4B when tested according to ASTM 3359 at a temperature of 85°C and a relative humidity of 95% for a period of at least 500 hours.
14. The display of claim 13, wherein the photocurable ink comprises at least 30 wt% of a pigment dispersion comprising greater than or equal to 25 wt% of the pigment and a reactive monomer.
15. The display of any one of claims 13-14, wherein the thickness is less than or equal to 10 μm.
16. The display of any one of claims 13 to 15, wherein the photocurable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
17. The display of any of claims 13-16, wherein the pigment comprises an average particle size less than or equal to 200 nm.
18. The display of any one of claims 13 to 17, wherein the display exhibits a CIELAB SCIL* value less than or equal to 30 when illuminated by a D65 illuminant at an angle of 10°.
19. The display of any of claims 13-18, wherein the display exhibits a CIELAB SCIa* value greater than or equal to -0.05 and less than or equal to 0.15 and a CIELAB SCIb* value greater than or equal to -0.3 and less than or equal to -0.1 when illuminated by a D65 illuminant at a 10° angle.
20. The display of any one of claims 13-19, further comprising a light management layer disposed on the second major surface between the glass substrate and the opaque layer, wherein the light management layer is formed of ink and comprises an average optical transmittance of less than or equal to 70% at 380 nm to 750 nm.
21. A method of manufacturing a glass product, the method comprising: Depositing a photocurable ink onto a major surface of a glass substrate using an inkjet print head at a deposition temperature of less than or equal to 65° C., wherein during the deposition, the photocurable ink has a viscosity of less than 25 cP, wherein the photocurable ink comprises at least 10 wt % of a pigment and at least 50 wt % of a reactive monomer; as well as curing the light-curable ink on the major surface by exposing the light-curable ink to curing light generated by an ultraviolet ("UV") light emitting diode ("LED") to form an opaque layer, wherein the curing light has a bandwidth less than or equal to 30 nm, wherein: The opaque layer comprises a thickness less than or equal to 25 μm and an optical density greater than or equal to 4.0, and The opaque layer exhibits: A pencil hardness of 3H or greater as measured in accordance with ASTM 3363, and Adhesion to the glass substrate of greater than or equal to 4B when tested according to ASTM 3359 at a temperature of 85°C and a relative humidity of 95% for a period of at least 500 hours.
22. The method of claim 21, further comprising: Prior to depositing the photocurable ink, the major surface of the glass substrate is primed with an acryloxysilane primer.
23. The method of any one of claims 21-22, wherein the opaque layer covers a peripheral portion of the major surface such that the glass article exhibits a higher optical transmittance of 380 nm to 750 nm in a central region excluding the opaque layer.
24. The method according to any one of claims 21 to 23, wherein the light-curable ink does not contain halogenated hydrocarbons, ethylbenzene, propylene oxide, styrene, benzene, isopropyl nitrite, butyl nitrite, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol formaldehyde acetate, 2-nitropropane, 2-methyl-2-pyrrolidone, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, toluene and xylene.
25. The method of any one of claims 21-24, further comprising performing one or more additional surface treatments on additional major surfaces of the glass substrate, the one or more additional surface treatments comprising chemically etching the additional major surfaces so that the additional major surfaces exhibit anti-glare properties and depositing an anti-reflective coating onto at least one of the additional major surfaces.
26. The method of any one of claims 21-25, further comprising: Prior to depositing the photocurable ink, a photomanagement layer is deposited onto the major surface, the photomanagement layer comprising an ink that is compositionally different from the photocurable ink and at least partially overlaps the opaque layer.
Citation Information
Patent Citations
Vehicle interior systems having a curved cover glass and a display or touch panel and methods for forming the same
US20190012033A1
Cold-formed glass article and assembly process thereof
US20190315648A1
Laminating thin strengthened glass to curved molded plastic surface for decorative and display cover application
US20190329531A1
Curved glass constructions and methods for forming same
US20210308986A1
Black deadfront for displays and related display device and methods
WO2019055458A1