Zinc oxide element replacing antimony oxide

By replacing antimony oxide with tin oxide in zinc oxide components, combining zinc oxide and zinc stannate, the problem of difficult maintenance of non-linear resistance characteristics in overvoltage protection devices is solved, and the non-linear resistance characteristics of zinc oxide components are realized. The improvement of thermal stability avoids health and environmental problems of antimony oxide.

CN118891237AInactive Publication Date: 2024-11-01MEIDENSHA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380028019.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-08
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the overvoltage protection device, it is difficult to maintain non-linear resistance characteristics without using antimony oxide, and the use of antimony oxide has health and environmental problems.

Method used

By replacing antimony oxide with tin oxide, the particle size and non-linear resistance characteristics of zinc oxide particles in the sintered body are controlled, and the combination of zinc oxide, bismuth oxide and zinc stannate is used to form zinc oxide with good non-linear resistance characteristics. element.

Benefits of technology

It is achieved without using antimony oxide to obtain zinc oxide components with excellent nonlinear resistance characteristics and thermal stability, avoiding health and environmental problems, and controlling the uniform particle size of zinc oxide particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891237A_ABST
    Figure CN118891237A_ABST
Patent Text Reader

Abstract

The present invention provides a zinc oxide element having excellent nonlinear resistance characteristics (V10kA / V1mA non-linearity) by controlling the particle size of zinc oxide particles in a sintered body without containing antimony oxide. A zinc oxide element according to the present invention comprises a fired body that contains zinc oxide, bismuth oxide, and zinc stannate (Zn2SnO4). This method for producing a zinc oxide element comprises firing a raw material oxide that contains zinc oxide, bismuth oxide, and tin oxide and does not contain antimony oxide, and segregating zinc stannate (Zn2SnO4) at the grain boundary of the fired zinc oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a zinc oxide element used in an overvoltage protection device such as a lightning arrester, and in particular to a zinc oxide element using tin oxide as a raw material oxide instead of antimony oxide. Background Art

[0002] Zinc oxide type lightning arresters are widely used to suppress overvoltage caused by lightning surges on power transmission and distribution lines and substations, or as protective devices for various power equipment such as transformers. As internal components of zinc oxide type lightning arresters, sintered bodies are used, which have zinc oxide powder as the main component and several oxides such as bismuth (III) oxide, antimony (III) oxide, cobalt (III) oxide, nickel (II) oxide, manganese dioxide (MnO 2 ) etc., using an organic binder such as polyvinyl alcohol, press-forming into a cylindrical shape etc., and then firing at a high temperature of 1000°C or higher. By changing the composition and additives of the zinc oxide element and controlling the composition and particle size of the particles constituting the sintered body, the electrical properties can be improved, and therefore various developments have been made.

[0003] On the other hand, in recent years, the requirements for power transmission costs have become increasingly stringent. In order to reduce power transmission costs, there is a strong desire to miniaturize power transmission and transformation equipment. Therefore, miniaturization of overvoltage protection devices that determine the insulation level of power transformation equipment has become a top priority. The current-voltage non-linear resistor used in the overvoltage protection device generally exhibits insulation characteristics under normal voltage. On the other hand, if an abnormal voltage is applied, it has a non-linear resistance characteristic that exhibits low resistance characteristics, which is effective for suppressing overvoltage. Therefore, the protection level itself in the overvoltage protection device has become an extremely important technical factor that affects the miniaturization of the overvoltage protection device and even the miniaturization of power transmission and transformation equipment. Therefore, various improvement schemes have been proposed for the current-voltage non-linear resistor, such as various limited constituent components.

[0004] Patent document 1 shows a current-voltage nonlinear resistor, wherein miniaturization is promoted by adjusting the content of the auxiliary component, and the current-voltage nonlinear characteristics, life characteristics and surge energy tolerance are excellent, and the degree of decrease in the resistance value of the current-voltage nonlinear resistor when the temperature rises is reduced, that is, the thermal stability at high temperature is improved, which can contribute to the miniaturization of the overvoltage protection device. It is also described that by containing 0.5 to 2.5 mol% of antimony oxide (Sb 2 O 3 ), thereby forming zinc oxide and spinel particles, inhibiting the grain growth of the sintered body and utilizing the homogenization effect to improve the non-linear resistance characteristics.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5065688 Summary of the invention

[0008] Problems to be solved by the invention

[0009] As an element used in an overvoltage protection device, etc., it is necessary to provide an element that does not contain antimony oxide, which is a health and environmental concern. However, when an element is made without antimony oxide, it tends to be difficult to maintain the above-mentioned nonlinear resistance characteristics.

[0010] Based on such background, an object of the present invention is to provide a zinc oxide element which avoids the health and environmental problems caused by the use of antimony oxide and has good nonlinear resistance characteristics (V10kA / V1mA nonlinearity) by controlling the particle size of zinc oxide particles in a sintered body.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive research to solve the above-mentioned problems and have found that by replacing antimony oxide (Sb 2 O 3 ) and use tin oxide (SnO 2 ), thereby being able to control the particle size of the zinc oxide particles in the sintered body, thereby obtaining a zinc oxide element with excellent non-linear resistance characteristics, thus completing the present invention.

[0013] That is, a preferred embodiment of the present invention is a zinc oxide element having the following configuration and a method for producing the same.

[0014] [1] A zinc oxide element comprising a sintered body, wherein the sintered body comprises zinc oxide (ZnO), bismuth oxide (Bi 2 O 3 ) and zinc stannate (Zn 2 SnO 4 ).

[0015] [2] The zinc oxide element according to [1], wherein the amount of zinc stannate in the sintered body is 0.1 to 5 mol % when the total amount of metal elements in the sintered body is 100 mol %.

[0016] [3] The zinc oxide element according to [1] or [2], wherein, in any cross section of the sintered body, a value (σ / D) obtained by dividing a standard deviation (σ) of a distribution of cross-sectional areas of zinc oxide particles by an average particle size (D) of the zinc oxide particles is 0.4 or less.

[0017] [4] The zinc oxide element according to any one of [1] to [3], wherein the sintered body further contains tin oxide.

[0018] [5] The zinc oxide element according to any one of [1] to [4], wherein the sintered body does not contain antimony oxide (Sb 2 O 3 ).

[0019] [6] The zinc oxide element according to any one of [1] to [5], wherein the sintered body further contains cobalt oxide (Co 2 O 3 ), nickel oxide (NiO), manganese oxide (MnO), chromium oxide (Cr 2 O 3 ), silver oxide (Ag 2 O), silicon oxide (SiO 2 ) and boron oxide (B 2 O 3 ) is an oxidized compound of at least one of the following.

[0020] [7] The zinc oxide element according to any one of [1] to [6], wherein the sintered body further contains an oxide of at least one rare earth element selected from yttrium (Y), europium (Eu), erbium (Er), thulium (Tm), gadolinium (Gd), dysprosium (Dy), holmium (Ho) and ytterbium (Yb).

[0021] [8] A method for manufacturing a zinc oxide element, comprising: 2 O 3 ) and tin oxide (SnO 2 ), does not contain antimony oxide (Sb 2 O 3 ) is sintered to form zinc stannate (Zn 2 SnO 4 ) segregation.

[0022] [9] The production method according to [8], wherein the raw material oxide further comprises cobalt oxide (Co 2 O 3 ), nickel oxide (NiO), manganese oxide (MnO), chromium oxide (Cr 2 O 3 ), silver oxide (Ag 2 O), silicon oxide (SiO 2 ) and boron oxide (B 2 O 3 ) is an oxidized compound of at least one of the following.

[0023]

[10] The manufacturing method according to [8] or [9], wherein the raw oxide further contains an oxide of at least one rare earth element selected from yttrium (Y), europium (Eu), erbium (Er), thulium (Tm), gadolinium (Gd), dysprosium (Dy), holmium (Ho) and ytterbium (Yb).

[0024] Effects of the Invention

[0025] According to the present invention, in the absence of antimony oxide, zinc stannate (Zn 2 SnO 4 ) segregation, thereby obtaining a zinc oxide element with excellent non-linear resistance characteristics and thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a cross-sectional view showing an example of the zinc oxide element of the present invention.

[0027] Figure 2 This is a scanning electron microscope photograph showing a cross section of a sintered body of the zinc oxide element of the present invention to which tin oxide is added.

[0028] Figure 3 This is a scanning electron microscope photograph showing a cross section of a sintered body of a zinc oxide element of a comparative example to which neither tin oxide nor antimony oxide is added.

[0029] Figure 4 It is an X-ray diffraction coordinate chart showing the diffraction peak of the oxide constituting the zinc oxide element of the present invention.

[0030] Figure 5 This is a scanning electron microscope photograph showing concentric circles drawn on a cross section of the zinc oxide element of the present invention in order to measure the average particle size and standard deviation of zinc oxide particles in the zinc oxide element. The x marks on the circumferences of the concentric circles represent grain boundaries. DETAILED DESCRIPTION

[0031] In this specification, the symbol "mA" means milliampere, "kA" means kiloampere, "V" means volt, "kV" means kilovolt, and "W" means watt. In addition, "mm" means millimeter, "μm" means micrometer, and "μs" means microsecond. In this specification, "antimony oxide" is synonymous with "antimony (III) oxide", "bismuth oxide" is synonymous with "bismuth (III) oxide", "cobalt oxide" is synonymous with "cobalt (III) oxide", "nickel oxide" is synonymous with "nickel (II) oxide", and "manganese oxide" is synonymous with "manganese (II) oxide".

[0032] The zinc oxide element of the present invention comprises a sintered body, wherein the sintered body comprises zinc oxide (ZnO), bismuth oxide (Bi 2 O 3 ), and zinc stannate (Zn2 SnO 4 The present invention is characterized in that as a raw material oxide, antimony oxide (Sb 2 O 3 ) and use tin oxide (SnO 2 ). In the present invention, the fired body is obtained by firing tin oxide together with zinc oxide, bismuth oxide, etc. Zinc stannate is generated by forming spinel particles of zinc oxide and tin oxide during firing, and segregates at the grain boundaries of zinc oxide. Tin oxide is partially or completely converted into zinc stannate by firing. Therefore, the zinc oxide element of the present invention may contain tin oxide (SnO 2 The present inventors surprisingly found that zinc stannate generated by the addition of tin oxide inhibits the growth of zinc oxide particles in the sintered body, thereby obtaining zinc oxide particles with uniform and small particle sizes, thereby obtaining a zinc oxide element with good nonlinear resistance characteristics (V10kA / V1mA nonlinearity).

[0033] The contents of zinc oxide, bismuth oxide and tin oxide in the raw material oxide are preferably 90 to 99.4 mol%, 0.3 to 1 mol% and 0.1 to 5 mol%, respectively, when the total metal element is 100 mol%. In addition, the content of zinc stannate generated in the sintered body is preferably 0.1 to 5 mol%, or 0.1 to 2.5 mol%, or 0.1 to 1 mol%.

[0034] The bismuth oxide contained in the zinc oxide element segregates at the grain boundaries of the zinc oxide in the fired body, thereby forming high-resistance grain boundaries, and showing the non-linear resistance characteristics of the zinc oxide element. In addition, it is known that bismuth oxide promotes the densification of the fired body even if the firing temperature is a relatively low temperature. In the case of conventional zinc oxide elements, antimony oxide is generally added for the purpose of improving the non-linear resistance characteristics, but the zinc oxide element of the present invention preferably does not contain antimony oxide in the zinc oxide element. In the present invention, the so-called "does not contain" antimony oxide means that the content of antimony oxide in the zinc oxide element is below the detection limit or below 0.1 mol%.

[0035] The sintered body constituting the zinc oxide element of the present invention may contain cobalt oxide (Co) as a minor component in addition to the above-mentioned zinc oxide, bismuth oxide, zinc stannate and tin oxide. 2 O 3 ), nickel oxide (NiO), manganese oxide (MnO), chromium oxide (Cr 2 O 3 ), silver oxide (Ag 2 O), silicon oxide (SiO 2 ), boron oxide (B 2 O 3) and other oxidizing compounds. It is known that the oxidizing compounds are solid-dissolved in the zinc oxide crystal particles during the firing process. The metal in the oxidizing compound that is solid-dissolved in this way functions as a donor, and has a tendency to further increase the free electron density of the zinc oxide crystal particles, reduce the resistance value of the zinc oxide crystal particles themselves, and suppress the increase in voltage in the overcurrent range. Therefore, it is preferred that the above-mentioned oxidizing compounds are included in the zinc oxide element in addition to bismuth oxide. Among these, cobalt oxide, manganese oxide, nickel oxide, chromium oxide, and silicon oxide are particularly preferred from the viewpoint of easily obtaining good current nonlinear characteristics and discharge tolerance characteristics.

[0036] The content of the above-mentioned oxidized compounds in the sintered body of the zinc oxide element is preferably 0.01 to 7.0 mol%, more preferably 0.05 to 6.0 mol%, and further preferably 0.1 to 5.0 mol% in terms of metal element conversion (mol% means the mol% of the metal element of each oxidized compound when the total metal element is 100 mol%). It should be noted that the above-mentioned "when the total metal element is 100 mol%" means that the total metal elements including semimetals such as Si and B are 100 mol%.

[0037] The sintered body of the zinc oxide element may optionally contain other additives. For example, a rare earth oxide may be contained for the purpose of increasing the resistance of the zinc oxide element. As the rare earth oxide, for example, an oxide (R) of at least one rare earth element (R) such as yttrium (Y), europium (Eu), erbium (Er), thulium (Tm), gadolinium (Gd), dysprosium (Dy), holmium (Ho), ytterbium (Yb), etc. may be contained. 2 O 3 The content of the rare earth oxide in the sintered body of the zinc oxide element is preferably 0.01 to 5.0 mol %, more preferably 0.1 to 1.0 mol % (mol % means the mol % of the metal element of each rare earth oxide when the total metal element is 100 mol %) in terms of metal element conversion.

[0038] Next, the manufacturing method of the zinc oxide element of the present invention is described. Zinc oxide, bismuth oxide and tin oxide as raw material oxides, as well as the above-mentioned oxidized compounds and the above-mentioned rare earth oxides used as needed, are put into a mixing and pulverizing device together with an organic binder, and pulverized and mixed for a prescribed time to prepare a slurry. There is no particular limitation on the organic binder used in the present invention. For example, polyvinyl alcohol (PVA) and the like can be used. The prepared slurry is sprayed and granulated, for example, by a rotating disc method or a pressurized nozzle method, to prepare a granulated powder. The obtained granulated powder is filled in a mold, and is pressurized into a cylindrical shape, for example, by a hydraulic pressing machine, to prepare a molded body.

[0039] The molded body is fired at a temperature of 400 to 950° C. in the atmosphere for 1 to 3 hours to remove the binder, and fired at a temperature of 1000 to 1300° C. for 1 to 15 hours to produce a fired body. In the process after molding, an inorganic insulating material (glass frit, etc.) is applied or sprayed on the side of the fired body, and then heated at 480 to 650° C. to form an insulating layer. Furthermore, the upper and lower surfaces of the fired body are ground, and a conductive material (aluminum, silver, etc.) is sprayed on the ground surface to form an electrode.

[0040] In a preferred embodiment, the method for producing a zinc oxide element of the present invention includes the following steps.

[0041] (Matching process)

[0042] The raw material oxide includes zinc oxide as a main component, bismuth oxide (0.3 to 1 mol%), tin oxide (0.1 to 5 mol%), cobalt oxide (0.3 to 1.5 mol%), manganese oxide (0.2 to 2 mol%), and nickel oxide (0.5 to 3 mol%) as subcomponents [mol% represents the mol% of the metal element of each of the above oxide compounds when the total metal element (including semimetal) is 100 mol%)], and silver oxide (0.005 to 0.05 weight%), and boron oxide (0.005 to 0.05 weight%) [weight% represents the weight% of the metal or semimetal element of each of the above oxide compounds when the total metal element (including semimetal) is 100 weight%]. The raw material oxide is stored in a sealed manner and managed so as not to be mixed with impurities.

[0043] (Crushing process)

[0044] As raw material oxides excluding zinc oxide, bismuth oxide, tin oxide, cobalt oxide, manganese oxide, nickel oxide, silver oxide and boron oxide are taken in different orders according to the above-mentioned proportions, and put into a ball mill container together with pure water in an amount equal to the total amount of the raw material oxides by weight ratio, and pulverized by changing the pulverization time using zirconium oxide balls with a diameter of 3 mm so that the particle size D50 of the pulverized slurry becomes about 0.7 μm or less. It should be noted that the particle size of the pulverized slurry is the particle size measured using a laser diffraction particle size distribution measuring device.

[0045] (Granulation and molding process)

[0046] The pulverized slurry is mixed with 90 mol % or more of zinc oxide and water in terms of metal element, 1 wt % of an organic binder relative to the weight of zinc oxide, and aluminum nitrate (Al(NO 3 ) 3 9H 2 O) aqueous solution (with Al 3+ions, equivalent to 10 to 30 ppm by weight) are fully mixed together, and then granulated using a spray dryer or the like to obtain granulated particles with a particle size of 2.5 to 3.50 g / cm 3 The density in the range is uniaxially formed using a 51.9 mm diameter mold.

[0047] (Pre-burning process)

[0048] The obtained molded body is calcined under the condition of being kept at a maximum holding temperature of 800 to 950° C. for 3 to 20 hours. By keeping the temperature at 350 to 700° C., the added organic binder is removed.

[0049] (Firing process)

[0050] The obtained calcined body is placed in a sagger made of alumina and the like, and fired under the conditions of a maximum holding temperature of 1000-1200°C, a holding time of 1-15 hours, a heating rate of 10-70°C / hour, and a cooling rate of 10-70°C / hour. The firing process has a decreasing inflection point at 700-950°C, and the temperature is lowered at 70-100°C / hour in the subsequent interval.

[0051] (Side insulation treatment process)

[0052] 0.5 to 3.0 g of a side insulating layer slurry composed of bismuth glass, a filler for thermal expansion adjustment and an organic binder is sprayed on the side of the obtained sintered body, and a heat treatment is performed under the heat treatment conditions of a maximum holding temperature of 450 to 600° C. and a holding time of 0.5 to 3.0 hours to form an insulating layer on the side of the sintered body. At this time, the added organic binder is removed by holding at 350° C. for 1 to 3 hours.

[0053] (Grinding and electrode installation process)

[0054] After the upper and lower ends of the heat-treated body with the insulating layer are polished, aluminum electrodes are sprayed onto the polished surfaces. The structure of the completed element is shown in FIG. Figure 1 . Figure 1 1 is a cross-sectional view of a zinc oxide element 1 . An insulating layer 13 is provided on the side surface of a sintered body 11 , and electrodes 12 are provided on the upper and lower end surfaces of the sintered body 11 .

[0055] (Effect)

[0056] The zinc oxide element of the present invention does not use antimony oxide in the element raw material, but uses tin oxide as a substitute material for antimony oxide, and by appropriately selecting the pulverization conditions, sintering conditions and heat treatment conditions of the oxidized compound of the secondary component, a non-linear resistor with excellent non-linear resistance characteristics and thermal stability can be obtained. That is, by using tin oxide in the element raw material, the tin oxide forms spinel particles Zn at the zinc oxide grain boundary during sintering. 2 SnO 4 ( Figure 2 , Figure 4 ), inhibiting the grain growth of zinc oxide particles in the sintered body. As a result, the particle size of zinc oxide is uniformed, and the value (σ / D) obtained by dividing the standard deviation (σ) of the distribution based on the cross-sectional area of ​​the zinc oxide particles by the average particle size (D) of the zinc oxide particles is controlled to be below 0.4, preferably below 0.3. As the current distribution in the element is uniformed, the non-linear resistance characteristics can be improved. With regard to the non-linear resistance characteristics, the ratio (V10kA / V1mA) of the action start voltage (V1mA) to the voltage (V10kA) when a 10kA 8×20μs pulse current flows is evaluated as a non-linear coefficient. A value of 1.8 or less is obtained in the element of the present invention.

[0057] (Example)

[0058] The present invention will be described in more detail using the following examples. The examples are for illustration of the present invention, and the present invention is not limited to the invention described in these examples.

[0059] (Evaluation of the performance of zinc oxide particles)

[0060] For the manufactured zinc oxide element, the action start voltage (the voltage when an alternating current of 1mA flows, V1mA) is measured. Next, the voltage (V10kA) when an 8×20μs pulse current of 10kA flows is measured, and the ratio (V10kA / V1mA) to the action start voltage (V1mA) is evaluated as a nonlinear coefficient. The smaller the value of the nonlinear coefficient, the better the nonlinear resistance characteristics. In addition, as an evaluation of thermal stability, a constant temperature bath at 170°C is used to measure the watt loss value when an alternating voltage of 80% of the action start voltage is applied. The smaller the watt loss value at 170°C, the better the thermal stability.

[0061] (Measurement based on standard deviation (σ) of distribution of cross-sectional area of ​​zinc oxide particles / average particle size (D) of zinc oxide particles)

[0062] The average particle size (D) and standard deviation (σ) of zinc oxide particles are measured by the intercept method. First, an arbitrary cross section of the sintered body is cut out and the cut cross section is mirror-polished. Then, in order to make the particles easy to identify, heat etching is performed using an electric furnace, etc. to produce an observation surface that emphasizes the zinc oxide grain boundaries. Next, a reflected electron image is obtained using a scanning electron microscope, such as Figure 5 As shown, after drawing three concentric circles with a constant total circumference in the center of the image, the average particle size (D) of the zinc oxide particles and the standard deviation (σ) of the distribution based on the cross-sectional area are measured. The arithmetic mean of the average particle size and standard deviation of 15 points in the arbitrary observation field of view is used in each evaluation. The average particle size D of the zinc oxide particles is calculated using D=L / n (L represents the circumference of the concentric circles, and n represents the number of zinc oxide grain boundaries). The value of σ / D is obtained by dividing the standard deviation (σ) calculated by the above measurement by the average particle size (D).

[0063] Example 1

[0064] Zinc oxide as a main component, raw material oxides composed of bismuth oxide, tin oxide, cobalt oxide, manganese oxide and nickel oxide, and silver oxide and boron oxide as subcomponents are prepared, and the components are weighed so that bismuth oxide becomes 0.3-0.7 mol %, tin oxide becomes 0.60 mol %, cobalt oxide becomes 0.3-1.0 mol %, manganese oxide becomes 0.2-1.0 mol %, and nickel oxide becomes 0.5-1.5 mol % [mol % represents the mol % of the metal element of the above-mentioned each oxide compound when the whole metal element (including semimetal) is taken as 100 mol %], silver oxide becomes 0.01-0.05 weight %, and boron oxide becomes 0.005-0.03 weight % [weight % represents the weight % of the metal or semimetal element of the above-mentioned each oxide compound when the whole metal element (including semimetal) is taken as 100 weight %]. The weighed raw oxide excluding zinc oxide is placed in a ball mill container together with pure water in an amount equal to the total amount of the raw oxide in weight ratio, and crushed using zirconium oxide balls with a diameter of 3 mm. The raw oxide is crushed in such a way that the particle size D50 of the slurry after crushing becomes about 0.7 μm or less when measured using a laser diffraction particle size distribution measuring device. The crushed slurry is mixed with zinc oxide and water at a metal element conversion of 90 mol% or more, an organic binder (PVA) at a weight of 1 wt% relative to the weight of zinc oxide, aluminum nitrate (Al(NO 3 ) 3 9H 2 O) aqueous solution (with Al 3+ After being fully mixed with the above-mentioned raw materials (equivalent to 10 to 30 ppm by weight in terms of ions), granulation is performed using a spray dryer or the like, and uniaxial molding is performed using a die with a diameter of 51.9 mm.

[0065] The molded body is pre-fired at a maximum holding temperature of 800-950°C for 3-20 hours. At this time, the added organic binder is removed by holding at 350-700°C. The obtained pre-fired body is placed in a sagger and fired under the conditions of a maximum holding temperature of 1000-1100°C, a holding time of 1-10 hours, a heating rate of 20-70°C / hour, and a cooling rate of 20-70°C / hour. On the side of the obtained sintered body, 0.5-3.0g of a side insulating layer slurry composed of bismuth glass, a filler for thermal expansion adjustment and an organic binder is sprayed, and then heat-treated under the heat treatment conditions of a maximum holding temperature of 450-600°C and a holding time of 0.5-3.0 hours to provide an insulating layer on the side of the sintered body. After grinding the upper and lower end surfaces of the heat-treated body provided with the insulating layer, aluminum electrodes are sprayed and attached to the ground surface. The electrical properties of the obtained zinc oxide element are shown in Table 1, and the average particle size and σ / D of the zinc oxide particles are shown in Table 2.

[0066] Comparative Example 1

[0067] A zinc oxide element was prepared under the same conditions as in Example 1 except that tin oxide (0.60 mol %) contained in the raw material oxide was replaced with antimony oxide (0.53 mol %). The electrical properties of the obtained zinc oxide element are shown in Table 1, and the average particle size and σ / D of the zinc oxide particles are shown in Table 2.

[0068] Comparative Example 2

[0069] A zinc oxide element was produced under the same conditions as in Example 1 except that tin oxide and antimony oxide were not added to the raw material oxide. The electrical properties of the obtained zinc oxide element are shown in Table 1, and the average particle size and σ / D of the zinc oxide particles are shown in Table 2.

[0070] [Table 1]

[0071]

[0072] [Table 2]

[0073]

[0074] As shown in Table 1, the nonlinearity (V10kA / V1mA) of the element of Example 1 is 1.760, showing good nonlinear resistance characteristics. In addition, the watt loss value is 0.74, showing good thermal stability at a practical level. However, the nonlinearity (V10kA / V1mA) and watt loss value of the element of Comparative Example 2, in which neither tin oxide nor antimony oxide is added, are significantly high, indicating poor performance.

[0075] As shown in Table 2, in the element of Example 1 using tin oxide instead of antimony oxide, the σ / D of zinc oxide particles is 0.26, showing a σ / D value of the same degree as that of the element of Comparative Example 1 using antimony oxide. In the element of Comparative Example 2, however, neither tin oxide nor antimony oxide exists, and there is no particle growth inhibition effect, so σ / D becomes 0.91, and the deviation of zinc oxide particles becomes larger. It can be seen from this that in the element of Comparative Example 2, the current distribution in the element is non-uniform, and the non-linear resistance characteristics are greatly deteriorated (Table 1, Table 2).

[0076] Figure 2 The cross section of the sintered body of Example 1 in which tin oxide is added instead of antimony oxide is shown. Figure 3 The cross section of the sintered body of Comparative Example 2 in which neither tin oxide nor antimony oxide was added is shown. Figure 2 It was found that zinc stannate (Zn 2 SnO 4 ) of the particles (indicated by arrows). In addition, in the X-ray diffraction coordinate diagram ( Figure 4 ), characteristic diffraction peaks of zinc stannate were found near 29.4° and 36.0°. This confirmed that zinc stannate was generated in the sintered body.

[0077] Description of Reference Numerals

[0078] 1···Zinc oxide components

[0079] 11···Sintered body

[0080] 12···Electrode

[0081] 13···Side insulation layer

Claims

1. A zinc oxide element comprising a sintered body comprising zinc oxide, bismuth oxide and zinc stannate (Zn2SnO4).

2. The zinc oxide element according to claim 1, wherein When the entire metal element in the sintered body is taken as 100 mol %, the amount of zinc stannate in the sintered body is 0.1 to 5 mol %.

3. The zinc oxide element according to claim 1 or 2, wherein: In any cross section of the sintered body, a value (σ / D) obtained by dividing a standard deviation (σ) of a distribution of cross-sectional areas of zinc oxide particles by an average particle size (D) of the zinc oxide particles is 0.4 or less.

4. The zinc oxide element according to any one of claims 1 to 3, wherein The sintered body further contains tin oxide.

5. The zinc oxide element according to any one of claims 1 to 4, wherein The sintered body does not contain antimony oxide.

6. The zinc oxide element according to any one of claims 1 to 5, wherein The sintered body further contains at least one oxide compound selected from the group consisting of cobalt oxide, nickel oxide, manganese oxide, chromium oxide, silver oxide, silicon oxide, and boron oxide.

7. The zinc oxide element according to any one of claims 1 to 6, wherein The sintered body further contains an oxide of at least one rare earth element selected from the group consisting of yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium.

8. A method for manufacturing a zinc oxide component, comprising: A raw material oxide containing zinc oxide, bismuth oxide and tin oxide but not containing antimony oxide is sintered to segregate zinc stannate (Zn2SnO4) at the grain boundary of the sintered zinc oxide.

9. The manufacturing method according to claim 8, wherein: The raw material oxide further includes at least one oxide compound selected from the group consisting of cobalt oxide, nickel oxide, manganese oxide, chromium oxide, silver oxide, silicon oxide, and boron oxide.

10. The manufacturing method according to claim 8 or 9, wherein: The raw material oxide further includes an oxide of at least one rare earth element selected from the group consisting of yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium.

Citation Information

Patent Citations

  • Current-voltage non-linear resistor and method of manufacture thereof

    CN101752046A

  • Zinc oxide ceramics composition and its manufacture method and zinc oxide nonlinear resistance

    CN1165125A

  • Current-voltage nonlinear resistor

    CN1988064A

  • Chip type varistor and method of manufacturing the same

    US6362720B1