Branched propylene polymers
By optimizing the molecular weight and branched structure of branched propylene polymers and using copolymerization with various metallocene catalysts, the shortcomings of branched propylene polymers in terms of melt tension and ductility were solved, and branched propylene polymers with high melt tension and excellent ductility were realized.
Patent Information
- Application Number
- CN202380028332.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-01
AI Technical Summary
Existing branched propylene polymers have shortcomings in terms of melt tension and ductility, especially the low melt tension at rapid strain rates, which cannot meet the requirements of various molding properties.
By controlling the molecular weight distribution and branching distribution of branched propylene polymers, and optimizing parameters such as melt flow rate, branching index, and flow activation energy, branched polymers containing propylene and ethylene are prepared. Then, a macromonomer copolymerization method using various metallocene catalysts is employed to form polymers with appropriate branching structures.
It achieves significant improvement in polymer ductility while maintaining high melt tension, and is suitable for processes such as sheet forming, blow molding, thermoforming, and foam forming.
Smart Images

Figure BDA0005047225920000161 
Figure BDA0005047225920000331 
Figure BDA0005047225920000341
Abstract
Description
Technical Field
[0001] The present invention relates to branched propylene polymers. Background Art
[0002] In recent years, many studies have been conducted for improving the suitability of polypropylene for sheet forming, blow molding, thermoforming, foam molding, etc., each of which requires a material with relatively high melt tension, by introducing a branched structure into polypropylene.
[0003] Recently, as a method for introducing a branched structure into polypropylene, a macromonomer copolymerization method using a metallocene catalyst has been mainly proposed. The branched polypropylene obtained by the macromonomer copolymerization method is advantageous because it has fewer problems, including gel generation due to excessively crosslinked components and deterioration of ductility due to components with high molecular weight increased by crosslinking, than crosslinked polypropylene peroxidized by a crosslinking aid.
[0004] As a branched propylene-based polymer obtained by a macromonomer copolymerization method, a polyolefin composition is disclosed, which is substantially composed of isotactic polypropylene and one or more optional comonomers, wherein the total comonomer content of the polyolefin composition is from 0 mol% to 20 mol%, and the weight average branching index g' of the low molecular weight range of the polyolefin composition is less than 0.93 (see Patent Document 1). In addition, a propylene homopolymer is disclosed, characterized in that: (a) the propylene homopolymer satisfies the relationship represented by the following formula (I):
[0005] MI 5 / MI 2.16 ≥0.240×Mw / Mn+3.1(I)
[0006] (MI 5 / MI 2.16 is the melt index MI under a load of 5.0 kg 5 (g / 10 min) and melt index MI under a load of 2.16 kg 2.16 (g / 10 min), both measured at a temperature of 230° C., and Mw / Mn is the ratio between the weight average molecular weight Mw and the number average molecular weight Mn, both measured by gel permeation chromatography (GPC)), and (b) the melt tension MS (g) measured at a temperature of 230° C. and the intrinsic viscosity [η] (dl / g) measured at a temperature of 135° C. in a tetracycline solvent satisfy the relationship represented by the following formula (II):
[0007] logMS≥3.17×log[η]-0.68(II)
[0008] (wherein the intrinsic viscosity [η] is within the range of 0.1 dl / g to 15.0 dl / g). The obtained branched propylene-based polymer exhibits high melt strength and high melt tension (see Patent Document 2).
[0009] Disclosed is a branched polypropylene composition having a polydispersity of less than or equal to 4.0 and a melting point of greater than 90° C., wherein the weight average branching index g′ of the branched polypropylene composition is less than 0.95. The branched propylene-based polymer obtained thereby shows improved melt strength (see Patent Document 3).
[0010] In addition, a multi-stage polymerization process is disclosed which uses a catalyst containing two specific metallocene compounds, more specifically, by combining a metallocene compound (such as rac-SiMe 2 [2-Me-4-Ph-lnd] 2 ZrCl 2 and rac-SiMe 2 [2-Me-4-Ph-lnd] 2 HfCl 2 ) and silica on which methylaluminoxane (MAO) is supported. It is shown that the branched propylene-based polymer obtained thereby exhibits a relatively high melt tension (see Patent Document 4).
[0011] In addition, a propylene homopolymer having the following characteristics (1) to (6) is disclosed:
[0012] (1) The weight average molecular weight (Mw) obtained by GPC is 200,000 to 1,000,000;
[0013] (2) the ratio (Q value) between the weight average molecular weight (Mw) and the number average molecular weight (Mn), both obtained by GPC, is 3.5 to 10.5;
[0014] (3) α / β is 1.2 or more (where α = H 50 -Tp; β = Tp-L 50 ; Tp represents the common logarithm of the molecular weight corresponding to the peak position of the molecular weight distribution curve obtained by GPC; and L 50 and H 50 The common logarithm of the molecular weight at the 50% height position of the peak height (L 50 On the molecular weight side lower than Tp, H 50 on the higher molecular weight side than Tp);
[0015] (4) Through 13 The mm fraction of the propylene unit triad sequence obtained by C-NMR analysis was more than 90%;
[0016] (5) in temperature rising elution fractionation (TREF) measurement using o-dichlorobenzene as a solvent, a component eluting at a temperature of 90° C. or lower is 6.0% by weight or lower; and
[0017] (6) In propylene polymer 13 In C-NMR analysis, three methylene carbons (Ca, Cb and Cc) were observed at 44.0ppm to 44.1ppm, 44.7ppm to 44.8ppm and 44.8ppm to 44.9ppm; methine carbon (Cbr) was observed at 31.6ppm to 31.7ppm; and the number of methine carbons per 1000 total skeleton-forming carbon atoms was 0.1 or more (the term "total skeleton-forming carbon atoms" means all carbon atoms except methyl carbons). The propylene homopolymer showed good melt tension (see Patent Document 5).
[0018] Another method is disclosed in which a propylene-based polymer having a strain hardening index (λmax) of 2.0 or more in melt tension measurement is produced by using a catalyst containing several specific metallocene compounds, and the branched polypropylene obtained thereby shows good melt tension (see Patent Document 6).
[0019] Patent document 7 discloses a polypropylene having a multi-branching index (MBI) of at least 0.15, wherein the multi-branching index (MBI) is defined as the slope of the strain hardening index (SHI) as a function of the logarithm of the Hencky strain rate to the base 10 (Ig(dε / dt)); wherein dε / dt is the deformation rate, ε is the Hencky strain, and the strain hardening index (SHI) is measured at 180°C; wherein the strain hardening index (SHI) is defined as the logarithm of the tensile stress growth function to the base 10 (lg(ηE + ))Slope as a function of the logarithm to base 10 of the Hencky strain (lg(ε)) in the range of Hencky strain between 1 and 3.
[0020] Reference List
[0021] Patent Literature
[0022] Patent Document 1: Japanese Translation of PCT International Application No. 2001-525460
[0023] Patent Document 2: Japanese Patent Application Laid-Open (JP-A) No. H10-338717
[0024] Patent Document 3: Japanese Translation of PCT International Application No. 2002-523575
[0025] Patent Document 4: JP-A No. 2001-64314
[0026] Patent Document 5: JP-A No. 2007-154121
[0027] Patent Document 6: JP-A No. 2009-57542
[0028] Patent Document 7: Japanese Translation of PCT International Application No. 2009-533540 Summary of the invention
[0029] Problem that the invention aims to solve
[0030] However, the branched propylene-based polymers obtained by the macromonomer copolymerization method disclosed in Patent Documents 1 to 6 have the following problem: although the branched propylene-based polymers have high melt tension and improved applicability for sheet forming, blow molding, thermoforming and foaming, the ductility of the polymer melt is still insufficient.
[0031] The mechanical properties of the branched propylene-based polymer obtained by the method disclosed in Patent Document 7 are improved by increasing the content of the non-crystalline part; however, the ... -1 ) is not very high. Therefore, the branched propylene polymer cannot satisfactorily show various types of molding characteristics.
[0032] An object of the present invention is to provide a branched propylene polymer which has excellent ductility when melted and maintains the melt tension required for molding.
[0033] Solutions for solving problems
[0034] The present invention relates to the following <1> to <7> .
[0035] <1> A branched propylene polymer comprises propylene and 0 mol% to 11 mol% of ethylene and an α-olefin having 4 or more carbon atoms, and has the following characteristics (1) to (4):
[0036] Characteristics (1): A melt flow rate (MFR) of 0.1 g / 10 min to 100 g / 10 min measured at a temperature of 230° C. and a load of 2.16 kg;
[0037] Characteristic (2): The ratio (Mz / Mw) between the z-average molecular weight (Mz) and the weight-average molecular weight (Mw), both obtained by gel permeation chromatography (GPC), is 2.5 to 4.0;
[0038] Characteristic (3): In the molecular weight distribution curve obtained by 3D-GPC, the absolute molecular weight Mabs The branching index g'(1 million) at 1 million is 0.60 to 0.75; and
[0039] Property (4): The flow activation energy (Ea) kJ / mol obtained by measuring the dynamic viscoelasticity and the MFR satisfy the following formula (1):
[0040] Ea≥-12.5×log(MFR)+66 formula (1).
[0041] <2> according to <1> The branched propylene polymer further has the following characteristics (2-2):
[0042] Characteristic (2-2): In the integrated molecular weight distribution curve obtained by GPC, the ratio of the percentage of the component with a molecular weight of 2 million or more (W2 million) to the percentage of the component with a molecular weight of 1 million or more (W1 million) (W2 million / W1 million) and the MFR satisfy the following formula (2):
[0043] (W2 million / W1 million)<-0.05×log(MFR)+0.34, formula (2).
[0044] <3> according to <1> or <2> The branched propylene polymer further has the following characteristics (5) and (5-2):
[0045] Feature (5): Pass 13 The mesotriad fraction measured by C-NMR is 95.0% or more and less than 99.0%, and
[0046] Characteristic (5-2): The amount of heterologous bond (2,1 bond) is in the range of 0 mol% to 0.30 mol%, and the amount of heterologous bond (1,3 bond) is in the range of 0 mol% to 0.25 mol%.
[0047] <4> according to <1> to <3> The branched propylene polymer described in any one of the above further has the following characteristics (6):
[0048] Feature (6): Pass 13 The number of long chain branches measured by C-NMR is 0.1 to 0.5 per 1000 monomers.
[0049] <5> according to <1> to <4> The branched propylene polymer described in any one of the above further has the following characteristics (7):
[0050] Characteristic (7): In an elution curve obtained by temperature rising elution fractionation (TREF) measurement with o-dichlorobenzene (ODCB), the amount of a component eluting at a temperature of 40° C. or lower is 0.1% by mass to 2.5% by mass.
[0051] <6> according to <1> to <5> The branched propylene polymer described in any one of the above further has the following characteristics (8):
[0052] Characteristic (8): Strain hardening degree (SHI@1s -1 ) is 0.70~2.50.
[0053] <7> according to <1> to <6> The branched propylene polymer described in any one of the above further has the following characteristics (9):
[0054] Property (9): Multi-branching index (MBI) is 0.20 to 1.00.
[0055] Effects of the Invention
[0056] According to the present invention, there is provided a branched propylene-based polymer which has excellent ductility when melted and maintains the melt tension required for molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] [ Figure 1 ] Figure 1 is a diagram showing the baseline and interval of a chromatogram in GPC.
[0058] [ Figure 2 ] Figure 2 This is a graph having log(MFR) which is the logarithm of MFR as the x-axis and W2 million / W1 million as the y-axis, in which data of the branched propylene polymers obtained in Examples and Comparative Examples are plotted.
[0059] [ Figure 3 ] Figure 3 is a diagram showing an example of an integrated molecular weight distribution curve.
[0060] [ Figure 4 ] Figure 4 This is a graph with log(MFR) which is the logarithm of MFR as the x-axis and Ea as the y-axis, in which data of the branched propylene-based polymers obtained in Examples and Comparative Examples are plotted.
[0061] [ Figure 5 ] Figure 5 This is a graph having log(MFR) which is the logarithm of MFR as the x-axis and the maximum take-up rate (MaxDraw) at 230° C. as the y-axis, in which data of the branched propylene-based polymers obtained in Examples and Comparative Examples are plotted. DETAILED DESCRIPTION
[0062] The inventors have found the following design idea: in order to improve the ductility of branched propylene polymers, it is preferred to include a multi-branched molecule having a molecular structure in which multiple branches are introduced into the middle molecular weight to high molecular weight region, and reduce the ultra-high molecular weight region component with too long relaxation time. The inventors further specify the relationship between the flow activation energy (Ea) obtained by measuring the dynamic viscoelasticity and the MFR as an index of appropriate branching characteristics. As a result, they successfully obtained a branched propylene polymer with excellent ductility when melted while maintaining the fluidity and melt tension required for forming.
[0063] The branched propylene polymer of the present invention is a branched propylene polymer comprising propylene and 0 mol% to 11 mol% of ethylene and an α-olefin having 4 or more carbon atoms, and has the following characteristics (1) to (4):
[0064] Characteristics (1): A melt flow rate (MFR) of 0.1 g / 10 min to 100 g / 10 min measured at a temperature of 230° C. and a load of 2.16 kg;
[0065] Characteristic (2): The ratio (Mz / Mw) between the z-average molecular weight (Mz) and the weight-average molecular weight (Mw), both obtained by gel permeation chromatography (GPC), is 2.5 to 4.0;
[0066] Characteristic (3): In the molecular weight distribution curve obtained by 3D-GPC, the absolute molecular weight M abs The branching index g'(1 million) at 1 million is 0.60 to 0.75; and
[0067] Property (4): The flow activation energy (Ea) kJ / mol obtained by measuring the dynamic viscoelasticity and the MFR satisfy the following formula (1):
[0068] Ea≥-12.5×log(MFR)+66 formula (1).
[0069] The branched propylene polymer of the present invention has characteristics (1) to (4); the branched propylene polymer has a branched propylene structure different from that of the prior art, especially a molecular weight distribution and a branching distribution; and Ea is high relative to MFR. Therefore, the branched propylene polymer of the present invention is a branched propylene polymer that has excellent ductility when melted while maintaining fluidity and melt tension required for molding.
[0070] When there are many unrelaxed components or many components with long relaxation time in the branched propylene polymer, the melt tension increases. At the same time, it is considered that: in many parts of the polymer, local oriented crystallization proceeds from the entanglement point of the molecular chain; therefore, uneven oriented crystallization occurs and leads to poor ductility.
[0071] In the present invention, attention is paid to the relationship between Ea and MFR and it is specified as an index of branching characteristics of a branched propylene-based polymer which is excellent in ductility when melted while maintaining melt tension required for molding.
[0072] Ea is considered to be an index that the numerical value is large when the number of branches is large or when the branch length is long.
[0073] The branched propylene-based polymer of the present invention has characteristics (1) to (4); the branched propylene-based polymer has a branched propylene structure different from that of the prior art, especially the molecular weight distribution and the branching distribution; and Ea is high relative to MFR. Therefore, it is estimated that the branched propylene-based polymer contains multi-branched molecules having a molecular structure in which multiple branches are introduced into the medium molecular weight to high molecular weight region, and at the same time, the branched propylene-based polymer has a branching distribution in which the content of the unrelaxed component or the content of the component with a long relaxation time is small. The branched propylene-based polymer of the present invention as described above shows a relaxation time distribution in which the amount of the component with a somewhat short relaxation time is large and the amount of the component with an extremely long relaxation time is small. Therefore, it is estimated that the ductility is improved because local oriented crystallization starting from the molecular chain entanglement point is less likely to occur and uneven oriented crystallization can be suppressed.
[0074] Hereinafter, the present invention will be described in detail. In the present specification, "to" showing a numerical range is used to describe a range in which numerical values described before and after "to" indicate a lower limit value and an upper limit value.
[0075] In the present specification, the upper limit and lower limit indicating the numerical range may be any combination of the values. In the present specification, the preferred range of a property may be any combination of the values.
[0076] In the present invention, logarithm means common logarithm, that is, logarithm with base 10.
[0077] Furthermore, in the present invention, ductility means a property of the resin that allows the molten resin to be spread wide, thin, and uniformly or to be spread thin, long, and uniformly.
[0078] The branched propylene polymer of the present invention can be a propylene homopolymer, or it can be a copolymer of propylene and an α-olefin comonomer containing 2 to 20 carbon atoms other than propylene (such as one or more comonomers selected from ethylene, 1-butene, 1-hexene, 1-octene and 4-methyl-1-pentene).
[0079] I. Physical properties of branched propylene polymers
[0080] Features(1):
[0081] In the branched propylene-based polymer of the present invention, a melt flow rate (MFR) measured at a temperature of 230° C. and a load of 2.16 kg is 0.1 g / 10 min to 100 g / 10 min.
[0082] In the present invention, when the MFR of the branched propylene polymer is too small, the fluidity of the molten resin deteriorates and thermoforming becomes difficult. Therefore, the MFR is 0.1 g / 10 min or more, preferably 1.0 g / 10 min or more, and more preferably 3.0 g / 10 min or more.
[0083] On the other hand, when the MFR is too large, the melt tension decreases. Therefore, the MFR is 100 g / 10 minutes or less, preferably 80 g / 10 minutes or less, more preferably 60 g / 10 minutes or less, and still more preferably 40 g / 10 minutes or less. The MFR may be 32 g / 10 minutes or less, and it may be 30 g / 10 minutes or less.
[0084] In the present invention, MFR is a value obtained by pelletizing a branched propylene-based polymer and measuring the polymer according to JIS K7210-1:2014 "Plastics-Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics-Part 1: Standard method" under the following test conditions: 230°C and a load of 2.16 kg. The pelletization is performed in the same manner as in "Pelletization" described under "Examples" below.
[0085] The MFR can be adjusted by varying the polymerization temperature or pressure and / or by adding hydrogen or other chain transfer agents during the polymerization.
[0086] Features(2):
[0087] In the branched propylene-based polymer of the present invention, the ratio (Mz / Mw) between the z-average molecular weight (Mz) and the weight-average molecular weight (Mw) both obtained by gel permeation chromatography (GPC) is 2.5 to 4.0.
[0088] Mz and Mw and the number average molecular weight (Mn) used herein are indices representing the average molecular weight of a polymer. Mz is an index of the average molecular weight of the high molecular weight side increased in specific gravity; Mn is an index of the average molecular weight of the low molecular weight side increased in specific gravity; Mw is an index of the average molecular weight in between. Their ratios, i.e., Mw / Mn and Mz / Mw, are indices of the degree of molecular weight distribution of a polymer.
[0089] From the viewpoint that the component with extremely long relaxation time is present in an appropriate amount in the branched propylene polymer and the decrease in melt tension is suppressed, Mz / Mw is 2.5 to 4.0. The upper limit of Mz / Mw of the branched propylene polymer of the present invention is preferably 3.6 or less, more preferably 3.4 or less, and still more preferably 3.2 or less. The lower limit of Mz / Mw of the branched propylene polymer of the present invention is preferably 2.6 or more, more preferably 2.8 or more, and still more preferably 2.9 or more.
[0090] It is considered that when the branched propylene-based polymer of the present invention has the molecular weight distribution characteristics as described above, the component having an extremely long relaxation time can be reduced, and the ductility can be improved.
[0091] In the branched propylene polymer of the present invention, the ratio between Mw and Mn (Mw / Mn) obtained by GPC can be 3.0 to 7.0. When Mw / Mn is within this range, the excessive increase in the number of components with extremely long relaxation times is suppressed, and the melt tension is maintained. Therefore, in the branched propylene polymer of the present invention, the upper limit of Mw / Mn can be 7.0 or less, can be 6.0 or less, can be 5.0 or less, can be 4.5 or less, or can be 4.3 or less. On the other hand, from the viewpoint of suppressing the decrease in melt tension, the lower limit of Mw / Mn can be 3.0 or more, can be 3.2 or more, or can be 3.3 or more.
[0092] From the viewpoint of the fluidity of the molten resin, the Mw of the branched propylene polymer of the present invention may be 15.0×10 4 ~35.0×10 4 , which can be 18.0×10 4 ~33.0×10 4 , or it can be 20.0×10 4 ~32.0×10 4 .
[0093] The Mz, Mw, Mn, Mw / Mn, and Mz / Mw values were obtained by GPC. The method and apparatus used to measure them are as follows.
[0094] Apparatus: GPC manufactured by Waters (ALC / GPC, 150C)
[0095] Detector: IR detector MIRAN 1A manufactured by FOXBORO (measurement wavelength: 3.42 μm)
[0096] Column: AT-806MS manufactured by Showa Denko KK (3 sets)
[0097] Mobile phase solvent: o-dichlorobenzene (ODCB)
[0098] Measurement temperature: 140℃
[0099] Flow rate: 1.0mL / min
[0100] Injection volume: 0.2mL
[0101] The measurement sample preparation was performed as follows: A solution (1 mg / mL) was prepared by using a sample and ODCB (containing 0.5 mg / mL of butylated hydroxytoluene (BHT)). The sample was dissolved at 140° C. for 1 hour, thereby preparing a measurement sample.
[0102] The baseline and interval of the obtained chromatogram are as follows Figure 1 OK as shown.
[0103] The retention capacity obtained by GPC was converted to molecular weight by using a calibration curve previously generated using standard polystyrene. The standard polystyrene used was the following products manufactured by Tosoh Corporation: F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, and A1000.
[0104] A calibration curve was produced by injecting 0.2 mL of a solution in which standard polystyrene was dissolved in ODCB (containing 0.5 mg / mL of BHT) so that each of them was 0.5 mg / mL. The calibration curve used a cubic equation obtained by least squares approximation.
[0105] The viscosity equation used to convert to molecular weight is [η] = K × M α , use the following values.
[0106] PS: K = 1.38 × 10 -4 , α=0.7
[0107] PP: K = 1.03 × 10 -4 , α=0.78
[0108] The average molecular weight and molecular weight distribution (Mz, Mw, Mn, Mw / Mn and Mz / Mw) of the branched propylene polymers measured by GPC and their balance can be adjusted by polymerization conditions such as catalyst selection, polymerization temperature, monomer concentration and hydrogen amount.
[0109] Features (2-2):
[0110] In the branched propylene polymer of the present invention, in the integrated molecular weight distribution curve obtained by GPC, the ratio of the percentage of the component with a molecular weight of 2 million or more (W2 million) to the percentage of the component with a molecular weight of 1 million or more (W1 million) (W2 million / W1 million) and the MFR satisfy the following formula (2):
[0111] (W2 million / W1 million)<-0.05×log(MFR)+0.34, formula (2).
[0112] W2 million / W1 million is the ratio of the amount of the higher molecular weight component in the high molecular weight region component to the amount of the high molecular weight region component. Considering that W2 million / W1 million is a function that is negatively correlated with the increase in MFR, and based on the data of the examples and the data of the comparative examples having the same level of MFR as the examples, the relationship between W2 million / W1 million and MFR is approximately determined by formula (2), which distinguishes the examples that can solve the problem from the comparative examples of the prior art that cannot solve the problem (see Figure 2 ).
[0113] Satisfying formula (2) means that W2 million / W1 million is less than a specific value related to MFR. That is, it means that the amount of higher molecular weight components with a molecular weight of 2 million or more is relatively small relative to the amount of high molecular weight components with a molecular weight of 1 million or more.
[0114] When W200000 / W100000 related to MFR is within the above range, it is considered that excessive increase in the amount of components with long relaxation time is suppressed and ductility is maintained. Therefore, the branched propylene-based polymer of the present invention preferably satisfies formula (2).
[0115] The W100000 of the branched propylene-based polymer of the present invention may be 1.00 mass % or more and 9.50 mass % or less.
[0116] It is believed that the melt tension of the branched propylene polymer of the present invention is improved due to the presence of the high molecular weight region component. Therefore, the present invention focuses on the component with a molecular weight of 1 million or more, and in the branched propylene polymer of the present invention, W1 million may be 1.00% by mass or more, or may be 2.00% by mass or more.
[0117] At the same time, it is believed that due to the presence of an appropriate amount of high molecular weight region components, an appropriate amount of components with a long relaxation time are maintained, and ductility is also maintained. Therefore, W1000000 may be 9.50 mass % or less, 8.00 mass % or less, 6.00 mass % or less, or 5.00 mass % or less.
[0118] In addition, the W200000 of the branched propylene-based polymer of the present invention may be 2.00 mass % or less.
[0119] As above, due to the presence of an appropriate amount of very high molecular weight region components, the components with extremely long relaxation times are properly maintained, and ductility is also maintained. Therefore, the present invention focuses on components with a molecular weight of more than 2 million, and in the branched propylene polymer of the present invention, W2 million can be less than 2.00 mass %, can be less than 1.00 mass %, or can be less than 0.70 mass %. In branched propylene polymers, W2 million can be more than 0.05 mass %.
[0120] Furthermore, W200000 / W100000 of the branched propylene-based polymer of the present invention may be 0.25 or less, may be 0.20 or less, or may be 0.17 or less.
[0121] As above, when W2 million / W1 million is within the above range, it is considered that an excessive increase in the amount of a component having a long relaxation time is suppressed, and ductility is maintained.
[0122] The W200000 / W100000 of the branched propylene polymer of the present invention may be 0.02 or more, 0.03 or more, or 0.05 or more.
[0123] In the present invention, W1 million is defined as a value obtained by subtracting from 1 the integral value up to a molecular weight (M) of 1 million (Log (M) = 6.0) in an integrated molecular weight distribution curve obtained by GPC (the total amount is normalized to 1), and multiplying the value thus obtained by 100. In addition, W2 million is defined as a value obtained by subtracting from 1 the integral value up to a molecular weight (M) of 2 million (Log (M) = 6.3) in an integrated molecular weight distribution curve obtained by GPC (the total amount is normalized to 1), and multiplying the value thus obtained by 100. Figure 3 An example of an integrated molecular weight distribution curve is shown.
[0124] In the present invention, as with the above-mentioned characteristic (2), W100000 and W200000 of the branched propylene polymer can be adjusted by polymerization conditions such as catalyst selection, polymerization temperature, monomer concentration and hydrogen amount.
[0125] Features(3):
[0126] In the branched propylene polymer of the present invention, in the molecular weight distribution curve obtained by 3D-GPC, the absolute molecular weight M abs The branching index g' (1 million) at 1 million is 0.60 to 0.75.
[0127] The branching index g' is calculated from the intrinsic viscosity [η] of the polymer with long-chain branching structure. br The intrinsic viscosity [η] of a linear polymer with the same molecular weight lin The ratio ([η] br / [η] lin ) is given. When there is a long-chain branched structure in a polymer molecule, the radius of gyration decreases compared to a linear polymer molecule with the same molecular weight. As the radius of gyration decreases, the intrinsic viscosity also decreases. Therefore, g' is a value less than 1.0. Even if the amount of branched structure is the same, when the branch length is long, the radius of gyration decreases compared to a linear polymer molecule with the same molecular weight. As the radius of gyration decreases, the intrinsic viscosity also decreases. Therefore, g' is a value less than 1.0. The g' of a linear polymer is defined as 1.0.
[0128] The definition of g' is described in "Developments in Polymer Characterization-4" (edited by JV Dawkins, Applied Science Publishers, 1984), and g' is a well-known index to those skilled in the art.
[0129] By using 3D-GPC, g' can be used as M abs The function is obtained.
[0130] In the present invention, 3D-GPC is a GPC device connected to three detectors: a refractive index detector (RI), a viscosity detector (viscometer), and a multi-angle laser light scattering detector (MALLS).
[0131] In the branched propylene polymer of the present invention, the absolute molecular weight M abs The weight average molecular weight (Mw abs ) may be less than 1,000,000. In addition, from the viewpoint of obtaining high melt tension, the branched propylene polymer of the present invention preferably has a Mw abs To M abs = Branched structure of the high molecular weight region of 1 million.
[0132] Therefore, the g'(1 million) of the branched propylene polymer of the present invention is 0.75 or less, preferably 0.74 or less, and more preferably 0.72 or less. abs = 1 million, and when the branch length of the introduced branched structure is an appropriate length, it is believed that the excessive increase in the number of components with extremely long relaxation times is suppressed, and ductility can also be maintained. Therefore, g'(1 million) is 0.60 or more, preferably 0.62 or more, and more preferably 0.65 or more.
[0133] I think because in M abs Since the amount of the component having a branched structure (corresponding to the high molecular weight component) in the molecular weight region of 1000000 to 100000 is appropriately large within a specific range, the melt strength of the branched propylene-based polymer of the present invention is improved, and the strain hardening degree (SHI) and melt tension (MT) in the elongational viscosity measurement, which are nonlinear viscoelastic properties, become large. Even when the number of branches in the entire polymer is large, as long as the number of branches in the molecular weight region of 1000000 to 1000000 is appropriately large, the melt strength of the branched propylene-based polymer of the present invention is improved, and the strain hardening degree (SHI) and melt tension (MT) in the elongational viscosity measurement, which are nonlinear viscoelastic properties, become large. abs = 1,000,000, the amount of the branched component (corresponding to the high molecular weight component) in the portion with M = 1,000,000 is small, and the SHI will not increase. abs = 1,000,000, and since the branch chain length of the introduced branch structure is not too long, deterioration of the ductility of the branched propylene-based polymer can be suppressed.
[0134] Features (3-2):
[0135] In the branched propylene polymer of the present invention, as in characteristic (3), it is considered that ductility can be maintained due to the presence of an appropriate amount of a component having a long relaxation time. Therefore, in the molecular weight distribution curve obtained by 3D-GPC, Mw abs The branching index g'(Mw abs ) can be 0.70~0.90.
[0136] g'(Mw abs ) may be 0.73 or more, or it may be 0.75 or more. On the other hand, the upper limit may be 0.87 or less, or it may be 0.86 or less.
[0137] Features (3-3):
[0138] In the branched propylene polymer of the present invention, in the molecular weight distribution curve obtained by 3D-GPC, g' (Mw abs ) and g'(1 million) can satisfy the following formula (3).
[0139] 0.10 ≤g'(Mw abs )-g'(1 million) Formula (3)
[0140] It is believed that due to g'(Mw abs ) and g'(1 million) are large, the component with a long relaxation time increases, and the melt strength of the branched propylene polymer of the present invention can be increased.
[0141] In the branched propylene polymer of the present invention, in the molecular weight distribution curve obtained by 3D-GPC, g' (Mw abs) and g'(1 million) can satisfy the following formula (3-2).
[0142] g'(Mw abs )-g'(1 million)≤0.20Formula (3-2)
[0143] As described above, it is considered that in the branched propylene polymer of the present invention, g'(Mw abs ) and g'(1 million) are not too different, because the components with very long relaxation times do not increase relatively much, and the ductility improves.
[0144] Furthermore, it is considered that the branched propylene-based polymer of the present invention preferably has a branching distribution within this range because the balance between the melt strength and ductility of the entire polymer can be maintained.
[0145] By M abs The details of the method of measuring the molecular weight distribution and the branching index of each molecular weight are as follows: The following detectors are connected in the order of MALLS, RI and viscometer.
[0146] Apparatus: ALLIANCE GPCV2000 manufactured by Waters Corporation (GPC equipped with RI and viscometer), DAWN-E manufactured by Technology (MALLS)
[0147] Column: GMHHR-H(S)HT manufactured by Tosoh Corporation (2 sets)
[0148] Mobile phase solvent: 1,2,4-trichlorobenzene (to which the antioxidant IRGANOX 1076 manufactured by BASF Japan was added at a concentration of 0.5 mg / mL)
[0149] Measurement temperature: 140℃
[0150] Flow rate: 1mL / min
[0151] Sample concentration: 1 mg / mL
[0152] Injection volume: 0.2175mL
[0153] To obtain the M obtained from MALLS abs The root mean square radius of gyration (Rg) and the intrinsic viscosity ([η]) obtained from the viscometer were calculated using ASTRA version 4.73.04 (data processing software attached to MALLS) by referring to the following references.
[0154] References:
[0155] 1. Developments in Polymer Characterization, Vol. 4. Essex: Applied Science; 1984. Chapter 1.
[0156] 2. Polymer, 45, 6495-6505 (2004)
[0157] 3.Macromolecules, 33, 2424-2436 (2000)
[0158] 4.Macromolecules, 33, 6945-6952 (2000)
[0159] g' is calculated as the intrinsic viscosity ([η]) obtained by measuring the sample with a viscometer. br ) is similar to the intrinsic viscosity ([η]) obtained by measuring the linear polymer alone. lin ) of the ratio ([η] br / [η] lin ).
[0160] As the linear polymer, a commercially available homopolypropylene (NOVATEC-PP (registered trademark) manufactured by Japan Polypropylene Corporation, grade name: FY6) was used to obtain [η] lin . [η] of linear polymers lin The fact that the logarithm of has a linear relationship with the logarithm of the molecular weight is known as the Mark-Houwink-Sakurada equation. Therefore, [η] lin The value of can be obtained by appropriately extrapolating to the low molecular weight side or the high molecular weight side.
[0161] In the present invention, as in the above-mentioned characteristic (2), the g'(1 million), g'(Mw abs ) and g'(Mw abs )-g'(1 million) can be adjusted by controlling polymerization conditions such as catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount. Among them, they are preferably adjusted by catalyst species selection without particular limitation. In the macromonomer copolymerization method using a catalyst containing several metallocene compounds, it is appropriate to adjust them by catalyst species selection.
[0162] Among them, g'(Mw) that satisfies formula (3) or (3-2) abs )-g'(1 million) is preferably adjusted by catalyst selection of several catalyst species or several metallocene compounds.
[0163] For example, when a catalyst of a single catalyst species or a single metallocene compound (hereinafter, it may be referred to as a "single catalyst") is used instead of a catalyst of several catalyst species or several metallocene compounds, it is considered that formula (3) or (3-2) is not satisfied. The reason is presumed to be as follows. Because the molecular weight distribution of the macromonomer generated by a single catalyst is narrow, macromonomers with large molecular weight differences are not supplied; therefore, the value obtained by formula (3) is small, or the value obtained by formula (3-2) is large. Taking Reference Example 2 as an example (see Table 2), because g'(Mw abs ) is large, estimated to be Mw abs Components with short chain branches are not included, and the molecular weight of the macromonomer generated by this catalyst is large. On the other hand, since g'(1 million) is small, it is estimated that in the high molecular weight region (M abs = 1 million) there are branched components of macromonomers with large molecular weights. As just described, by generating a single catalyst with a narrow molecular weight distribution of macromonomers, for example, g' (Mw abs )-g'(1 million) increases and does not satisfy formula (3-2).
[0164] Features(4):
[0165] In the branched propylene polymer of the present invention, the flow activation energy (Ea) kJ / mol obtained by measuring the dynamic viscoelasticity and the MFR satisfy the following formula (1):
[0166] Ea≥-12.5×log(MFR)+66 formula (1).
[0167] It has long been known empirically that the viscosity of an object generally decreases as the temperature increases, and the logarithm of the viscosity, lnη, is proportional to the inverse of the absolute temperature 1 / T and is expressed by the following equation (Chemical Dictionary, 2nd Edition, "Andrade's Viscosity Equation").
[0168] [Mathematical formula 1]
[0169]
[0170] B: proportional constant
[0171] Ea: Flow activation energy
[0172] R: Gas constant
[0173] This energy term Ea corresponds to the activation energy in the case where the reaction rate in the Arrhenius equation of the chemical reaction is considered to flow, and is referred to as "flow activation energy".
[0174] When Ea is high, it means that the energy required for flow is large. In the case of branched propylene polymers, it is believed that when the amount of branching is large or when the branch length is long, the entanglement of the molecular chain increases, and therefore the energy for making the molecular chain flow increases. That is, Ea mainly depends on the amount and length of the long chain branches in the polymer.
[0175] In order to obtain a branched propylene polymer having excellent ductility when melted while maintaining fluidity and melt tension required for molding, the present invention focuses on Ea as an index for obtaining appropriate branching characteristics and specifies the relationship between Ea and MFR.
[0176] In the branched propylene polymer of the present invention, Ea may be 55.0 kJ / mol or more, or it may be 58.0 kJ / mol or more from the viewpoint of branching characteristics that can improve ductility when melted. On the other hand, Ea may be 70.0 kJ / mol or less.
[0177] When formula (1) is satisfied, it means the following: In the branched propylene-based polymer of the present invention, Ea obtained by measuring dynamic viscoelasticity is equal to or greater than a specific value related to MFR.
[0178] In the branched propylene-based polymer of the present invention, the value of Ea related to MFR is different from that of conventional propylene-based polymers, that is, Ea satisfies the formula (1).
[0179] When Ea, which is related to MFR, is too small, branching characteristics including branching amount, branching length, and branching distribution become inappropriate, and ductility during melting deteriorates. Therefore, the branched propylene-based polymer of the present invention satisfies the above formula (1).
[0180] More preferably, the branched propylene-based polymer of the present invention may satisfy the following formula (1-2).
[0181] Ea≥-12.5×log(MFR)+72 formula (1-2).
[0182] Generally, as the fluidity of the molten resin improves, Ea deteriorates. Therefore, a propylene-based polymer having both the desired fluidity and Ea is required, and Ea is used as an indicator of branching characteristics suitable for improving ductility when melted. A branched propylene-based polymer that satisfies formula (1) and has excellent fluidity is a polymer that cannot be achieved with conventional branched propylene-based polymers, and it can be said to be a polymer with a high balance between the fluidity and branching characteristics of the molten resin. Considering that Ea is a function that is negatively correlated with the increase in MFR, and based on the data of the embodiment and the data of Comparative Examples 1, 2 and 3 having the same level of fluidity as the embodiment, the relationship between Ea and MFR is approximately determined, distinguishing between the embodiments that can solve the problem and the comparative examples of the prior art that cannot solve the problem (see Figure 4 ).
[0183] In the branched propylene polymer of the present invention, branching characteristics including branching amount, branching length, branching distribution, etc. are suitable for improving ductility during melting. Therefore, the flow activation energy (Ea) associated with MFR is estimated to be high.
[0184] When the value of Ea related to MFR is high, it is considered that the extrusion load during molding can be reduced more than that of a branched propylene-based polymer having the same MFR.
[0185] Since the branched propylene-based polymer of the present invention satisfies the formula (1), the ductility can be improved while reducing the extrusion load during molding.
[0186] The upper limit value of Ea related to MFR is not particularly limited. It may be a value satisfying the following formula (1-3), or it may be a value satisfying the following formula (1-4).
[0187] Ea≤-12.5×log(MFR)+82 formula (1-3)
[0188] Ea≤-12.5×log(MFR)+77 formula (1-4)
[0189] Ea is a value calculated by the Arrhenius equation using the shift factor (aT) in making a master curve based on the temperature-time superposition principle in melt viscoelasticity measurement. In the present invention, the master curve is a curve showing the angular frequency (unit: rad / second) dependence of the melt complex viscosity (unit: Pa·second) at 200°C. Ea is obtained by the following method.
[0190] First, the melt complex viscosity-angular frequency curve of the branched propylene polymer is obtained at the following three temperatures (T, unit: ° C) 180 ° C, 200 ° C and 220 ° C. Based on the temperature-time superposition principle, each melt complex viscosity-angular frequency curve is superimposed on the melt complex viscosity-angular frequency curve at 200 ° C to obtain the shift factor (aT) at each temperature. According to each temperature (T) and "aT" at the temperature (T), the linear approximation of [ln(aT)] and [1 / (T+273.16)] is calculated by the least squares method (the following formula (4)). Next, Ea is obtained by the following formula (5), where "m" is the slope of the linear approximation.
[0191] ln(aT)=m(1 / (T +273.16))+n Formula (4)
[0192] Ea=|0.008314×m| Formula (5)
[0193] aT: shift factor
[0194] Ea: Flow activation energy (unit: kJ / mol)
[0195] T: Temperature (unit: °C)
[0196] In the above calculation, commercially available software can be used. As software, examples include TRIOS (manufactured by TA Instruments).
[0197] Note that "aT" is the amount of movement in the x-axis direction when the double logarithmic curve of the melt complex viscosity versus angular frequency at each temperature (T) is shifted in the x-axis (angular frequency) and y-axis (melt complex viscosity) directions and superimposed on the melt complex viscosity-angular frequency curve at 200°C.
[0198] The measurement of the melt complex viscosity-angular frequency curve is performed using a viscoelasticity measuring apparatus (such as ARES-G2 manufactured by TA Instruments) in a nitrogen atmosphere under the following conditions.
[0199] The propylene polymer was compression molded by pressing at 180° C. for 5 minutes while preventing the entry of bubbles, thereby obtaining a disc-shaped measurement sample having a thickness of 2.0 mm and a diameter of 25 mm. The measurement of the sample was performed after compressing the measurement sample having a thickness of 2.0 mm to a thickness of 1.5 mm using parallel circular plates having a diameter of 25 mm maintained at the following three temperatures: 180° C., 200° C., and 220° C.
[0200] Geometry: Parallel plates
[0201] Plate diameter: 25mm
[0202] Plate spacing: 2mm
[0203] Strain: 5%
[0204] ·Angular frequency: 0.01rad / sec~100rad / sec
[0205] In the present invention, the Ea and MFR of the branched propylene polymer can satisfy the formula (1) by controlling the polymerization conditions such as the catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount as in the above-mentioned characteristic (2). Among them, they are preferably adjusted by the catalyst species selection without particular limitation. In the macromonomer copolymerization method using a catalyst containing several metallocene compounds, it is appropriate to adjust them by the catalyst species selection.
[0206] On the contrary, when a single catalyst is used, it seems difficult to satisfy all of the following: the copolymerizability of the macromonomer is high; the molecular weight of the macromonomer is large; and the generation rate of the macromonomer is high. Therefore, when a single catalyst is used, it is believed that Ea is small because the amount of long chain branching (LCB) in the polymer is small, or because the branching length is short. For example, as shown in Reference Example 2, when the terminal vinyl rate is low, that is, when the generation rate of the macromonomer in the polymer is low and the amount of LCB is small, Ea is small.
[0207] Features(5):
[0208] In the branched propylene polymer of the present invention, 13 The meso triad fraction (mm) measured by C-NMR is preferably 95.0% or more and less than 99.0%, and
[0209] Features (5-2):
[0210] Furthermore, in the branched propylene polymer of the present invention, the amount of heterogeneous bonds ([2,1 bonds]) is preferably in the range of 0 mol% to 0.30 mol%, and the amount of heterogeneous bonds ([1,3 bonds]) is preferably in the range of 0 mol% to 0.25 mol%.
[0211] The crystallinity of branched propylene polymers is susceptible to the stereoregularity expressed as the meso triad fraction (mm) or the meso pentad fraction (mmmm) and the regioregularity expressed as [2,1 bond] and [1,3 bond]. That is, crystallization is developed by folding back lamella at regularity-deficient portions (such as stereo-irregular bonds and heterogeneous bond portions).
[0212] When the stereoregularity and regioregularity of the branched propylene-based polymer of the present invention are within the above ranges, it is considered that the crystallization process due to shear or elongation deformation improves the fluidity and melt tension during gradual cooling and solidification of the resin in the molding process.
[0213] Therefore, in order to improve the melt tension during solidification, the mm of the branched propylene-based polymer of the present invention is preferably 95.0% or more, more preferably 96.0% or more, still more preferably 97.0% or more.
[0214] On the other hand, when mm is too high, the rigidity or Young's modulus increases, and the toughness of the film may be too high. Therefore, mm of the branched propylene polymer of the present invention is preferably less than 99.0%, more preferably 98.5% or less, still more preferably 98.2% or less.
[0215] As described above, from the viewpoint of improving melt tension during solidification, the amount of [2,1 bond] of the branched propylene-based polymer of the present invention is preferably 0 mol% to 0.30 mol%, more preferably 0 mol% to 0.25 mol%, still more preferably 0 mol% to 0.20 mol%, even more preferably 0.030 mol% to 0.25 mol%, particularly preferably 0.05 mol% to 0.20 mol%. The upper limit of the amount of [2,1 bond] may be 0.15 mol% or less. In combination with the amount of [2,1 bond], the amount of [1,3 bond] of the branched propylene-based polymer of the present invention is preferably 0 mol% to 0.25 mol%, more preferably 0 mol% to 0.20 mol%, still more preferably 0 mol% to 0.15 mol%, even more preferably 0.05 mol% to 0.20 mol%, particularly preferably 0.10 mol% to 0.15 mol%.
[0216] pass 13 The measurement and calculation methods of mm, the amount of [2,1 bond], and the amount of [1,3 bond] in C-NMR measurement are as follows.
[0217] First, 200 mg of sample and 2.4 mL of solvent (o-dichlorobenzene / deuterated brominated benzene (C 6 D 5 Br)) and hexamethyldisiloxane as a chemical shift standard were put into an NMR test tube (10 mm in inner diameter) and uniformly dissolved at 150° C. by a block heater, thereby preparing a measurement sample.
[0218] ( 1 H-NMR)
[0219] Apparatus: AV400 (product name, NMR apparatus manufactured by Bruker BioSpin KK)
[0220] Probe: Cryoprobe (10mm diameter)
[0221] Sample temperature: 120°C
[0222] Pulse angle: 4.5°
[0223] Pulse interval: 2 seconds
[0224] Cumulative times: 1024 times
[0225] • Chemical shift: The chemical shift of the proton signal of hexamethyldisiloxane was set to 0.09 ppm, and this was used as a chemical shift standard for the chemical shifts of the signals of other protons.
[0226] ( 13C-NMR)
[0227] Apparatus: AV400 (product name, NMR apparatus manufactured by Bruker BioSpin KK)
[0228] Probe: Cryoprobe (10mm diameter)
[0229] Sample temperature: 120°C
[0230] Pulse angle: 45°
[0231] Pulse interval: 17.2 seconds
[0232] Cumulative times: 3072 times
[0233] Decoupling conditions: broadband decoupling method
[0234] Chemical shift: The 13 The chemical shift of the C signal was set to 1.98 ppm and this was used as the 13 The chemical shift of the signal of C is that of the chemical shift standard.
[0235] By 13 C-NMR measurements 13 The integrated intensity of the C signal is substituted into the following formula (6) to obtain the meso triad fraction (mm) of the propylene unit triad sequence.
[0236] mm(%)=I mm ×100 / (I mm +3×I mrrm ) Formula (6)
[0237] In the formula, I mm The propylene unit triad sequence belongs to the bonding type of mm 13 The integrated intensity of the C signal is calculated as the integrated intensity of the signal with a chemical shift range of 23.6 ppm to 21.1 ppm (hereinafter, it will be represented as “I 23.6-21.1 ”). mrrm The propylene unit pentad sequence belongs to the mrrm bonding type 13 The integrated intensity of the C signal is expressed as “I 19.9-19.7 ” value.
[0238] You can refer to the following literature for spectrum attribution:
[0239] "Polymer Journal", Vol. 16, p. 717 (1984), Asakura Shoten Publishing Co., Ltd.,
[0240] "Macromolecules", Vol. 8, p. 687 (1975), and
[0241] "Polymer", Vol. 30, p. 1350 (1989).
[0242] The chemical shift range may vary slightly due to the molecular weight of the polymer, etc. However, the region can be easily identified.
[0243] Use by 13 C-NMR measurements 13 The integrated intensity of the C signal is used to obtain the amount of [2,1 bond] and the amount of [1,3 bond] by the following formula.
[0244] Amount of [2,1 bond] (mol%)
[0245] =I 2,1-P ×100 / (I 1,2-P +I 2,1-P +I 1,3-P )
[0246] Amount of [1,3 bond] (mol%)
[0247] =I 1,3-P ×100 / (I 1,2-P +I 2,1-P +I 1,3-P )
[0248] In the formula, I 1,2-P ,I 2,1-P and I 1,3-P The propylene unit belongs to the bonding type of [1,2 bond] 13 The integrated intensity of the C signal and the bonding type of the propylene unit are [2,1 bond] 13 The integrated intensity of the C signal and the bonding type of the propylene unit are attributed to [1,3 bond] 13 The integrated intensity of the C signal. They are obtained as follows:
[0249] I 1,2-P =I 48.80-44.50
[0250] I 2,1-P =(I 34.68-34.63 +I 35.47-35.40 +I 35.94-35.70 ) / 2
[0251] I 1,3-P =I 37.50-37.20 / 2.
[0252] Characteristics (5) and (5-2) can be satisfied by controlling polymerization conditions such as catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount.
[0253] Features(6):
[0254] From the viewpoint of maintaining high melt tension of the branched propylene polymer of the present invention during molding, 13 The number of long chain branches (LCB number) measured by C-NMR is preferably 0.1 to 0.5 per 1000 monomers, more preferably 0.2 to 0.5 per 1000 monomers.
[0255] The LCB number is when 13 When the C-NMR normalizes the methylene carbon intensity of the propylene main chain at 49.00ppm to 44.33ppm to 1000, the number of propylene monomers per 1000 is calculated by the following formula using the signal integrated intensities of the branch point carbon (methine carbon) at 31.72ppm to 31.66ppm and the three methylene carbons bonded to the branch point carbon (methine carbon) at 44.09ppm to 44.03ppm, 44.78ppm to 44.72ppm and 44.90ppm to 44.84ppm.
[0256] Number of LCB=[(I 44.09-43.03 +I 44.78-44.72 +I 44.90-44.84 +I 31.72-31.66 ) / 4] / I 49.00-44.33
[0257] The following measurement conditions were used to obtain the LCB number except that the following measurement conditions were changed as follows 13 C-NMR measurements can be compared with the characteristic (5) 13 C-NMR measurements were performed in the same manner:
[0258] Pulse interval: 4.2 seconds
[0259] Cumulative times: 20,000 times
[0260] As with characteristic (4) above, characteristic (6) can be satisfied by controlling polymerization conditions such as catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount.
[0261] Features(7):
[0262] In the branched propylene-based polymer of the present invention, the amount of a component eluting at a temperature of 40° C. or less in an elution curve obtained by temperature-increasing elution fractionation measurement with o-dichlorobenzene is preferably 0.1% by mass to 2.5% by mass.
[0263] The component eluted at 40°C or less is a low crystalline component. When the amount of this component is large, the branched propylene-based polymer may have reduced crystallinity, resulting in a product with reduced heat resistance and rigidity. On the other hand, when the amount of this component is small, the branched propylene-based polymer formed into a film obtains excessively high rigidity and poor touch.
[0264] Therefore, in the branched propylene polymer of the present invention, the amount of the component eluting at a temperature of 40°C or lower is preferably 2.5 mass% or lower, more preferably 2.0 mass% or lower, still more preferably 1.0 mass% or lower, particularly preferably 0.7 mass% or lower.
[0265] On the other hand, when the amount of the component eluted at 40°C or less is too small, for example, the branched propylene-based polymer formed into a laminate may obtain too high rigidity, resulting in poor touch (e.g., unpleasant touch). Therefore, in the branched propylene-based polymer of the present invention, the amount of the component eluted at a temperature of 40°C or less is preferably 0.1% by mass or more, more preferably 0.2% by mass or more.
[0266] The details of the measurement method of the components eluted by TREF are as follows.
[0267] First, the sample is dissolved in ODCB at 140°C to obtain a solution. The solution is introduced into a TREF column at 140°C. The column is cooled to 100°C at a cooling rate of 8°C / min; the column is further cooled to 40°C at a cooling rate of 4°C / min; and the column is then maintained at 40°C for 10 minutes. Then, a solvent (ODCB) is flowed into the column at a flow rate of 1 mL / min for 10 minutes while the column is maintained at 40°C; further, the solvent is flowed into the column at the same flow rate for 60 minutes while the temperature of the column is linearly increased from 40°C to 140°C at a heating rate of 100°C / 60 minutes, thereby eluting the sample to obtain an elution curve. The ratio of the elution amount of the component eluted at a temperature of 40°C to the total elution amount is obtained as the amount (mass %) of the component eluted at a temperature below 40°C.
[0268] Column size: 4.3mm (diameter) × 150mm
[0269] Column packing: 100μm surface deactivated glass beads
[0270] Solvent: ODCB
[0271] Sample concentration: 5 mg / mL
[0272] Sample injection volume: 0.1mL
[0273] Solvent flow rate: 1mL / min
[0274] Detector: MIRAN-1AIR detector manufactured by FOXBORO (measurement wavelength: 3.42 μm)
[0275] In general, by using a metallocene compound as a polymerization catalyst component, the amount of components soluble below 40° C. from the branched propylene-based polymer can be kept low in TREF using ODCB. It is preferred that the amount of isomers incorporated into the catalyst complex be kept low; in catalyst preparation, the metallocene catalyst is gently contacted with the organoaluminum compound; and the temperature conditions of the polymerization reaction are not extremely high.
[0276] Features(8):
[0277] In the branched propylene polymer of the present invention, the strain hardening degree (SHI@1s -1 ) is preferably 0.70 to 2.50.
[0278] As used in this paper, SHI@1s -1 is the elongational viscosity (η) at a temperature of 180°C and a strain rate of 1.0 / s E ) is measured, in the interval between Hencky strains of 1 and 3, the logarithm of the Hencky strain (log(ε)) is plotted on the x-axis and the logarithm of the elongational viscosity (log(η)) is plotted on the y-axis E )).
[0279] From the viewpoint of improving moldability by increasing melt tension and from the viewpoint of improving ductility, the SHI@1s of the branched propylene polymer of the present invention is -1 It is preferably 0.70 to 2.50, more preferably 0.80 to 2.00, still more preferably 1.00 to 1.80.
[0280] When the SHI@1s of branched propylene polymer -1 When the SHI@1s is large enough, the elongation viscosity increases because components that do not relax at fast strain rates exist in the polymer. -1 Compared with the polymer of the branched propylene-based polymer, the elongation viscosity of the branched propylene-based polymer becomes higher, and the melt tension is increased. As a result, it is considered that the formability in sheet forming, blow molding, thermoforming and foaming is improved.
[0281] Based on this viewpoint, the SHI@1s of the branched propylene polymer of the present invention is -1 It is preferably 0.70 or more.
[0282] When the SHI@1s of branched propylene polymer -1When the SHI@1s is appropriately large, the amount of the unrelaxed component or the amount of the component with a long relaxation time is appropriately maintained; the progress of local oriented crystallization starting from the molecular chain entanglement point is suppressed; and ductility is maintained. From this point of view, the SHI@1s of the branched propylene polymer of the present invention is -1 It is preferably 2.50 or less.
[0283] The strain hardening index (SHI) can be obtained by uniaxial elongational viscosity measurement as described in Polymer, Vol. 42, p. 8663 (2001). In the present invention, SHI@1s is measured by the following method: -1 .
[0284] Device: ARES-G2 manufactured by TAInstruments
[0285] Fixture: EXTENTIONAL VISCOSITY FIXTURE manufactured by TA Instruments
[0286] Measuring temperature: 180℃
[0287] Strain rate: 1.0 / sec
[0288] Preparation of test pieces: 18 mm × 10 mm sheets (thickness 0.7 mm) were prepared by compression molding.
[0289] SHI is obtained as follows. By the above measurement method, the time-dependent variation data of the elongational viscosity are obtained at a given strain rate; the measured data are plotted on the x-axis as log(ε) and the y-axis as log(η E ) are plotted on a graph of ; the slope of the elongational viscosity in the interval between the Hencky strain of 1 and 3 is assigned from the graph; and the slope is determined as the SHI at the strain rate in the measurement conditions.
[0290] As with characteristic (4) above, characteristic (8) can be satisfied by controlling polymerization conditions such as catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount.
[0291] Features(9):
[0292] From the viewpoint of achieving excellent ductility when melted, the multi-branching index (MBI) of the branched propylene polymer is preferably more than 0.20. From the viewpoint of obtaining the stability of melt tension by suppressing the strain rate dependence of the strain hardening degree, the multi-branching index (MBI) of the branched propylene polymer of the present invention is preferably less than 1.00. The lower limit of MBI is more preferably more than 0.26. On the other hand, the upper limit is more preferably less than 0.80, still more preferably less than 0.60.
[0293] MBI is the slope when SHI of a polymer is obtained at a strain rate of 0.1 to 10 / sec and the logarithm of the strain rate (log(dε / dt)) is plotted on the x-axis and SHI at a strain rate of 0.1 to 10 / sec is plotted on the y-axis.
[0294] The SHI of a polymer varies with strain rate. MBI represents the dependence of SHI on strain rate, and it means that as the value of MBI increases, SHI greatly increases with increasing strain rate.
[0295] The MBI is obtained as follows. The SHI is measured at several strain rates in the range of 0.1 / sec to 10 / sec; the SHI measured at these strain rates is plotted on a graph with log(dε / dt) on the x-axis and SHI on the y-axis; and the slope of the approximate straight line of the graph in the strain rate range of 0.1 / sec to 10 / sec is determined as the MBI. In the present invention, the three points (SHI@0.1s -1 、SHI@1.0s -1 and SHI@10.0s -1 ) is approximated as a straight line, and the slope of the straight line is determined as MBI.
[0296] As with characteristic (4) above, characteristic (9) can be satisfied by controlling polymerization conditions such as catalyst species selection, polymerization temperature, monomer concentration and hydrogen amount.
[0297] Features (10):
[0298] From the viewpoint of obtaining a propylene polymer having excellent ductility while maintaining the melt tension required for molding, the melt tension (MT230) of the branched propylene polymer of the present invention at 230°C may be 0.3 to 15 g, or 0.5 to 15 g.
[0299] MT230 is a tension detected by a pulley using a melt tension tester (such as CAPILOGRAPH 1B manufactured by Toyo Seiki Seisaku-sho, Ltd.) when a resin is extruded into a strand and taken up on a roll under the following conditions.
[0300] Resin temperature: 230℃
[0301] Capillary: 2.0mm diameter, 40mm length
[0302] Cylinder diameter: 9.55mm
[0303] ·Drum extrusion speed: 20mm / min
[0304] ·Coiling speed: 4.0m / min
[0305] When the resin broke at a take-up speed of 4.0 m / min, the melt tension was considered "not evaluable".
[0306] Features(11):
[0307] In the branched propylene polymer of the present invention, the maximum take-up rate (MaxDraw) (m / min) at 230°C and the MFR may satisfy the relationship represented by the following formula (7).
[0308] (MaxDraw)>200×log(MFR)-38 Formula (7)
[0309] MaxDraw is when the coiling speed is 18.1 mm / s in the melt tension measurement. 2 The winding rate immediately before the linear resin breaks when the resin is extruded into a linear shape and the linear resin is wound up and wound around a roll while the acceleration is gradually increased from 4.0 m / min.
[0310] When the linear resin broke at a take-up rate of 4.0 m / min, it was considered "unevaluable".
[0311] MaxDraw can be used as an index to evaluate melt ductility. The higher the MaxDraw, the better the ductility. In the present invention, MaxDraw is measured under the following conditions.
[0312] Apparatus: Capillary Rheometer CEAST SR50 manufactured by INSTRON
[0313] Capillary: 2.0mm diameter, 40mm length
[0314] ·Diameter of cylinder: 15mm
[0315] ·Tube length: 290mm
[0316] ·Drum extrusion speed: 20mm / min
[0317] Resin temperature: 230℃
[0318] Generally, there is the following problem: as fluidity increases, ductility improves while melt tension decreases; at the same time, when fluidity increases to obtain excellent ductility, melt tension becomes insufficient. Therefore, the branched propylene polymer of the present invention is required to be a propylene polymer having both the melt tension required for molding and excellent ductility. The MaxDraw-MFR relationship defined in the above formula (7) can be used as an indicator of ductility relative to fluidity. Satisfying formula (7) indicates the following: compared with conventional propylene polymers, the ductility of the branched propylene polymer of the present invention is excellent relative to fluidity.
[0319] That is, in order to distinguish the branched propylene polymer of the present invention from the conventional propylene polymer, it is considered that the melt ductility (MaxDraw) is a function that is positively correlated with the increase of fluidity (MFR), the parameters of the function are set, and it is shown that the MaxDraw of the branched propylene polymer of the present invention is greater than the MaxDraw of the conventional propylene polymer defined by the function relative to the MFR. More specifically, based on the data of the Examples and Comparative Examples, it is assumed that the values of MaxDraw and MFR that distinguish the Examples and Comparative Examples (prior art) are then determined by the least squares method. The parameters of the relationship established between MaxDraw and MFR (see Figure 5 ).
[0320] II. Method for producing branched propylene polymer
[0321] The method for producing the branched propylene polymer of the present invention is not particularly limited as long as the branched propylene polymer having the above-mentioned properties of the present invention can be obtained by the method. A suitable method is a macromonomer copolymerization method using a catalyst containing several metallocene compounds.
[0322] In the present invention, the mechanism of the macromonomer copolymerization method using several metallocene compounds is presumed as follows.
[0323] When polymerization is initiated by using a catalyst containing a metallocene compound that forms a catalyst mainly producing a macromonomer (hereinafter, the metallocene compound is referred to as "Compound 1") and a metallocene compound that forms a catalyst mainly copolymerizing a macromonomer and a propylene monomer and producing a polymer having a branched chain (the metallocene compound is referred to as "Compound 2"), the following polymerization behavior is exhibited.
[0324] In short, by using a propylene polymerization catalyst containing compounds 1 and 2, a polymer having a range including a molecular weight region in which the molecular weight and molecular weight distribution of a polymer produced by a catalyst containing compound 1 (hereinafter, the catalyst is referred to as "catalyst 1") overlap with the molecular weight and molecular weight distribution of a polymer produced by a catalyst containing compound 2 (hereinafter, the catalyst is referred to as "catalyst 2")
[0325] In the process of forming a branched structure, when the polymer produced by catalyst 1 contains a terminal vinyl group, the polymer containing the terminal vinyl group becomes a macromonomer (hereinafter, this macromonomer is referred to as "macromonomer 1"). In addition, a copolymer of propylene and macromonomer 1 is produced by catalyst 1, and a copolymer of propylene and macromonomer 1 is produced by catalyst 2.
[0326] When the polymer produced by catalyst 2 contains a terminal vinyl group, the polymer containing the terminal vinyl group becomes a macromonomer (hereinafter, the macromonomer is referred to as "macromonomer 2"). In addition, a copolymer of propylene and macromonomer 2 is produced by catalyst 1, and a copolymer of propylene and macromonomer 2 is produced by catalyst 2.
[0327] When the polymer produced by catalyst 1 and the polymer produced by catalyst 2 become macromonomer 1 and macromonomer 2, respectively, a copolymer of propylene, macromonomer 1 and macromonomer 2 is further produced by catalyst 1, and a copolymer of propylene, macromonomer 1 and macromonomer 2 is further produced by catalyst 2.
[0328] As just described, according to the molecular weight, molecular weight distribution and terminal vinyl content of the polymer generated by catalyst 1, the copolymerizability of catalyst 1, the molecular weight, molecular weight distribution and terminal vinyl content of the polymer generated by catalyst 2, the copolymerizability of catalyst 2, the ratio between the amounts of catalysts 1 and 2, and the stereo position relationship between catalysts 1 and 2, the average molecular weight, high molecular weight and very high molecular weight of the branched propylene polymer as the final product change. In addition, the branching amount and branching distribution of the branched propylene polymer change. That is, it is considered that Mn, Mw, Mz, W1 million, W2 million, g'(1 million) and g'(Mw abs ), [g'(Mw abs )-g'(1 million)], Ea, SHI, MBI and MT changed.
[0329] The preferred method for producing the branched propylene-based polymer of the present invention is not limited by mechanism. Examples of the method include, but are not limited to, the following methods.
[0330] In the method for producing a branched propylene-based polymer of the present invention, from the viewpoint of easily satisfying the above-mentioned characteristics, it is preferred to use two catalyst components for generating a macromonomer, namely, components [A-1] and [A-2], and it is preferred to carry out polymerization by using a polymerization catalyst obtained by combining components [A-1] and [A-2] so that their types, amounts and amount ratios satisfy the following conditions.
[0331] a) The molecular weight of the polymer formed from the component [A-2] is higher than the molecular weight of the polymer formed from the component [A-1].
[0332] b) The proportion of terminal vinyl groups in the polymer produced from the component [A-1] is larger than the proportion of terminal vinyl groups in the polymer produced from the component [A-2].
[0333] c) Component [A-2] has better macromonomer copolymerizability than component [A-1].
[0334] By using a polymerization catalyst obtained by combining components [A-1] and [A-2] satisfying conditions a), b) and c), the branched propylene-based polymer of the present invention can be easily produced, which has characteristics (1) to (4), has a branched propylene structure different from that of the prior art, especially molecular weight distribution and branching distribution, and wherein Ea related to MFR is high.
[0335] By using a polymerization catalyst obtained by combining components [A-1] and [A-2] that satisfy conditions a), b) and c), it is possible to produce a branched propylene-based polymer of the present invention, which contains multi-branched molecules having a molecular structure in which many branches are introduced into the medium to high molecular weight region, and at the same time has a branching distribution in which the content of an unrelaxed component or a component with a long relaxation time is small.
[0336] In the branched propylene-based polymer of the present invention, by using a polymerization catalyst obtained by combining components [A-1] and [A-2] satisfying the conditions a), b) and c), in the step of abs Area to M abs = M of the area with an area range of 1 million abs = 1 million (high molecular weight side) (both measured by using a light scattering detector (MALLS)), the ratio of the polymer generated from component [A-2] increases. abs In the region (low molecular weight side), the ratio of the polymer generated from the component [A-1] increases.
[0337] Because conditions a) and b) are satisfied, a large amount of a macromonomer with a relatively small molecular weight (macromonomer 1) is generated from component [A-1], and a macromonomer with a relatively large molecular weight (macromonomer 2) is generated from component [A-2].
[0338] As for the branched components, in M abs = 1,000,000, the ratio of the branched component generated by copolymerizing propylene, macromonomer 1 and macromonomer 2 from component [A-2] is high. abs In the region, the ratio of the branched component generated from the component [A-1] by copolymerizing propylene, the macromonomer 1 and the macromonomer 2 is high.
[0339] In addition, since condition c) is satisfied, it is considered that in Mw abs In the region, the macromonomer of component [A-1] has poor copolymerizability, so g' (Mw abs ) is reduced. abs= 1 million, component [A-2] more effectively copolymerizes both macromonomer 1 and macromonomer 2, thereby reducing g'(1 million). As a result, it is believed that a product having g'(Mw abs A branched propylene polymer having a value of )-g'(1 million) in the range of 0.10 to 0.20.
[0340] II-1. Catalyst for polymerization
[0341] The propylene polymerization catalyst used for producing the branched propylene-based polymer of the present invention preferably comprises the following components [A-1], [A-2], [B] and [C].
[0342] Component [A-1]: a metallocene compound which, when homopolymerizing propylene at 70°C, gives a propylene homopolymer a-1 having a terminal vinyl ratio (Rv) of 0.5 or more
[0343] Component [A-2]: a metallocene compound which, when homopolymerizing propylene at 70°C, gives a propylene homopolymer a-2 having an Mn greater than that of the propylene homopolymer a-1 and an Rv of 0.1 or more and less than 0.5
[0344] Component [B]: a compound or layered silicate that can react with components [A-1] and [A-2] to form an ion pair Component [C]: an organoaluminum compound
[0345] II-1-1. Component [A-1]
[0346] Component [A-1] is a metallocene compound which, when homopolymerizing propylene at 70° C., gives a propylene homopolymer a-1 having an Rv of 0.5 or more. Component [A-1] is a metallocene compound which gives an Rv of preferably 0.65 or more, more preferably 0.75 or more, and ideally 1.0 (one of both ends of all molecular chains has a vinyl structure). By using a metallocene compound which forms a polymerization catalyst for producing a propylene homopolymer having a higher Rv, the macromonomer synthesis step can be carried out more efficiently.
[0347] The terminal vinyl ratio (Rv) and the terminal vinylidene ratio (Rvd) are determined by the following formula.
[0348] Rv=[Vi] / {(total number of terminals-number of LCBs) / 2}
[0349] Rvd = [Vd] / {(total number of terminals - number of LCBs) / 2}
[0350] (where [Vi] is obtained by 1 The number of terminal vinyl groups per 1000 monomers calculated by H-NMR; [Vd] is obtained by 1The number of terminal vinylidene groups per 1000 monomers was calculated by H-NMR; the total number of terminal groups was calculated by 1 H-NMR and 13 The total number of termini per 1000 monomers was calculated by C-NMR; and the LCB number was calculated by 13 C-NMR calculated number of LCBs per 1000 monomers).
[0351] [Relationship between reaction mechanism and terminal structure]
[0352] The relationship between the reaction mechanism of propylene homopolymerization and the terminal structure will be described below.
[0353] In propylene polymerization, generally, a chain transfer reaction called β-hydrogen elimination occurs as a termination reaction, and a polymer having a propyl-vinylidene structure (vinylidene structure) represented by the structural formula (1-b) as a termination terminal is generated. In the case of using hydrogen, chain transfer to hydrogen generally occurs preferentially, and a polymer having an isobutyl structure represented by the structural formula (1-c) as a termination terminal is generated. In the case of using a catalyst containing a metallocene compound having a specific structure, a specific chain transfer reaction called β-methyl elimination occurs, and a polymer having a 1-propenyl structure (vinyl structure) represented by the structural formula (1-a) as a termination terminal is generated (reference: Macromol. Rapid Commun. 2000, 21, 1103-1107).
[0354] As the terminal end, when chain transfer by hydrogen occurs after irregular insertion of propylene in rare cases, an n-butyl structure represented by the structural formula (1-e) is generated. In addition, as the terminal end, it is considered that when β-hydrogen elimination occurs after irregular insertion of propylene, a small amount of 1-butenyl structure represented by the structural formula (1-f) or a small amount of terminal vinylene structure (2-butenyl structure) represented by the structural formula (1-g) is generated.
[0355] When the first propylene is inserted into the central metal after chain transfer or β-hydrogen elimination by hydrogen occurs as a termination reaction, the starting terminal becomes an n-propyl structure represented by the structural formula (1-h), or when the first propylene is inserted into the central metal after β-methyl elimination occurs as a termination reaction, the starting terminal becomes an isobutyl structure represented by the structural formula (1-c).
[0356] When, in rare cases, the first propylene is irregularly inserted into the central metal after chain transfer by hydrogen occurs as a termination reaction or after β-hydrogen elimination occurs as a termination reaction, the starting terminal becomes a 2,3-dimethylbutyl structure represented by the structural formula (1-i), or when, in rare cases, the first propylene is irregularly inserted into the central metal after β-methyl elimination occurs as a termination reaction, the starting terminal becomes a 3,4-dimethylpentyl structure represented by the structural formula (1-j).
[0357] All initial termini become saturated termini. Therefore, a polymer chain cannot have two unsaturated termini at the same time.
[0358] Furthermore, a polymer having an isobutylene structure represented by the structural formula (1-d) at the terminal can be produced by isomerization.
[0359] The internal vinylidene structure represented by the structural formula (1-k) is an olefin structure generated inside the polymer chain when propylene is further inserted into an intermediate formed by hydrogen desorption after the generation of an unsaturated terminal.
[0360] Therefore, in the above structural formula, structural formula (1-c) and structural formula (1-h) each become a main saturated terminal through the main reaction, and structural formula (1-a) and structural formula (1-b) each become a main unsaturated terminal through the main reaction. Compared with the number of main terminal structures, the number of other terminal structures is very small.
[0361] In the above terminal structures, polymers having structures represented by structural formulas (1-a) and (1-f) at the terminal can be macromonomers. Structural formulas (1-a) and (1-f) also have vinyl structures at the two carbon atoms at the terminal ends; in addition, structural formulas (1-a) and (1-f) have no difference in copolymerizable functions.
[0362] However, the 1-propenyl structure is a terminal generated by the elimination of β-methyl group after the regular insertion of propylene; meanwhile, the 1-butenyl structure is a structure generated as a side reaction in which β-hydrogen elimination occurs after the irregular insertion of propylene in rare cases. Therefore, it is inferred that the amount of the 1-butenyl structure will be small relative to the amount of the 1-propenyl structure. It is believed that the generation ratio of the 1-butenyl structure to the 1-propenyl structure is similar to or less than the generation probability of the heterogeneous bond. That is, it is inferred that most of the terminal vinyl number [Vi] is the 1-propenyl structure generated by the elimination of β-methyl group after the regular insertion of propylene.
[0363] [Chemical formula 1]
[0364]
[0365] [Chemical formula 2]
[0366]
[0367] [Evaluation method of terminal vinyl ratio (Rv) and terminal vinylidene ratio (Rvd)]
[0368] The propylene polymerization conditions when the Rv and Rvd of the catalyst components are determined will be described below.
[0369] First, the inside of a 20 L autoclave tank was purged with propylene; 18.7 mL of a heptane solution of triisobutylaluminum (140 mg / mL) was fed into the tank; 0.51 NL of hydrogen was introduced into the tank; 5000 g of liquid propylene was introduced into the tank; 300 mg of a catalyst containing component [A-1] (which is the mass of a polymer excluding prepolymerization) was fed into the tank under pressure; and then polymerization was started at 70° C. for 1 hour. Finally, unreacted propylene was quickly purged to stop polymerization. Thus, a propylene polymer was obtained.
[0370] Rv is an index of the ratio of the number of terminal vinyl groups to the total number of polymer chains. Rvd is an index of the ratio of the number of terminal vinylidene groups to the total number of polymer chains. 1 H-NMR and 13 C-NMR obtains the number of unsaturated terminals and the number of saturated terminals as the number per 1000 monomers, respectively, and the total number of terminals is determined as the sum of the saturated terminals and the unsaturated terminals. 13 C-NMR obtains the LCB number as the number of every 1000 monomers. Subtract the LCB number from the total terminal number, and determine that half (1 / 2) of the number thus obtained is the total polymer number. The number [Vi] of the terminal vinyl groups as the unsaturated terminal is divided by the total polymer number, thereby calculating Rv. The number [Vd] of the terminal vinylidene groups as the unsaturated terminal is divided by the total polymer number, thereby calculating Rvd. Further details of the calculation method are as follows.
[0371] <Calculation method of saturation terminal number>
[0372] The following main saturation end numbers are obtained by the following formula. In each formula, replace 13 The integrated intensity of the C signal was used as the number of saturated termini per 1000 monomers.
[0373] Structural formula (1-c): [isobutyl] = I 异丁基 ×1000 / I 总C
[0374] Structural formula (1-e): [n-butyl] = I nbu ×1000 / I 总C
[0375] Structural formula (1-h): [n-propyl] = Inpr ×1000 / I 总C
[0376] Structural formula (1-i): [2,3-dimethylbutyl] = I 2,3-dime ×1000 / I 总C
[0377] Structural formula (1-j): [3,4-dimethylpentyl] = I 3,4-dime ×1000 / I 总C
[0378] When other types of saturated terminals other than the above-mentioned main saturated terminals are detected, the number of other types of saturated terminals is calculated as the number per 1000 monomers in the same manner as above using values described in known literature.
[0379] I 异丁基 ,I nbu ,I npr ,I 2,3-dime and I 3,4-dime The characteristic values of the signals based on the structural formulas (1-c), (1-e), (1-h), (1-i) and (1-j) are respectively represented. They are quantities represented by the following formulas.
[0380] I 异丁基 =I 23.80-23.65
[0381] I nbu =I 36.99-36.88
[0382] I npr =I 39.71-39.61
[0383] I 2,3-dime =(I 16.30-16.20 +I 43.05-43.00 ) / 2
[0384] I 3,4-dime =I 12.0-11.60
[0385] I 总C The value is a quantity expressed by the following formula.
[0386] I 总C =I 异丁基 +I nbu +I npr +I 2,3-dime +I 3,4-dime +I 1,2-P +I 2,1-P +I 1,3-P
[0387] When there are other types of saturated structures besides the above main saturated structures, all detected structure numbers are added to the above formula.
[0388] I 1,2-P is a characteristic value of a signal based on 1,2-insertion of propylene bonds; I 2,1-P is a characteristic value of a signal based on a 2,1-inserted propylene bond; and I 1,3-P It is a characteristic value of the signal based on 1,3-insertion of propylene bonds. They are quantities represented by the following formula.
[0389] I 1,2-P =I 48.80-44.50
[0390] I 2,1-P =(I 34.68-34.63 +I 35.47-35.40 +I 35.94-35.70 ) / 2
[0391] I 1,3-P =I 37.50-37.20 / 2
[0392] <Calculation method of the number of unsaturated ends>
[0393] The number of unsaturated ends is obtained by the following formula. In each formula, 1 The integrated intensity of the H signal was used as the number per 1000 monomers.
[0394] exist 1 In H-NMR, the proton signals of the unsaturated bonds of the 1-propenyl structure represented by the structural formula (1-a) and the 1-butenyl structure represented by the structural formula (1-f) are expressed by their 1 In the H-NMR spectrum, overlapping signals of 5.08 ppm to 4.85 ppm and 5.86 ppm to 5.69 ppm were detected. Therefore, the number of terminal vinyl groups, [Vi], was determined to be the total number of 1-propenyl structures and 1-butenyl structures.
[0395] Structural formula (1-a) + structural formula (1-f):
[0396] [Vi]=I vi ×1000 / I 总
[0397] In the same manner as above, the number of terminal vinylidene groups [Vd], the number of isobutylene groups [isobutylene], the number of terminal vinylene groups [terminal vinylene] and the number of internal vinylidene groups [internal vinylidene] are obtained by the following formulae.
[0398] Structural formula (1-b):
[0399] [Vd]=I vd×1000 / I 总
[0400] Structural formula (1-d):
[0401] [Isobutylene]=I ibu ×1000 / I 总
[0402] Structural formula (1-g):
[0403] [Terminal vinyl] = I vnl ×1000 / I 总
[0404] Structural formula (1-k):
[0405] [Internal vinylidene] = I ivd ×1000 / I 总
[0406] I vi ,I vd ,I ibu ,I vnl and I ivd They are characteristic values of signals based on formula (1-a) + formula (1-f), formula (1-b), formula (1-d), formula (1-g), and formula (1-k). They are quantities expressed by the following formulas.
[0407] I vi =(I 5.08-4.85 +I 5.86-5.69 ) / 3
[0408] I vd =(I 4.78-4.65 ) / 2
[0409] I ibu =I 5.26-5.08
[0410] I vnl =(I 5.58-5.26 ) / 2
[0411] I ivd =(I 4.85-4.78 ) / 2
[0412] I 总 It is a quantity represented by the following formula.
[0413] I 总 =I 主要 / 6+I vi +I vd +I ibu +I vnl +I ivd
[0414] When there are other types of unsaturated structures in addition to the above main unsaturated structures, all the detected number of ends is added to the above formula.
[0415] I 主要 is 1 the total integrated intensity of the proton signals detected at 4.00 ppm to 0.00 ppm in the 1H-NMR spectrum and bonded to the saturated carbons of the polymer chain including the ends.
[0416] <Calculation method of the number of LCBs>
[0417] The number of LCBs as the number per 1000 monomers is obtained by the method described in "Characteristic (6)".
[0418] <Calculation method of the total number of ends>
[0419] The total number of ends is 1 by 1H-NMR and 13 13C-NMR calculated total number of ends per 1000 monomers.
[0420] <Calculation methods of the terminal vinyl ratio (Rv) and the terminal vinylidene ratio (Rvd)>
[0421] Using [Vi], [Vd], the total number of ends and the number of LCBs obtained above, Rv and Rvd are calculated by the following formula.
[0422] Rv = [Vi] / { (total number of ends - number of LCBs) / 2}
[0423] Rvd = [Vd] / { (total number of ends - number of LCBs) / 2}
[0424] As component [A-1], examples include, but are not limited to, binaphthalene complexes having a bulky heterocyclic group at the 2-position of the indenyl group and an optionally substituted aryl group or a heterocyclic group containing a nitrogen atom, an oxygen atom or a sulfur atom at the 4-position. As a preferred embodiment of component [A-1], examples include, but are not limited to, the following structures.
[0425] [Chemical formula 3]
[0426]
[0427] (wherein, R 11 and R 12 each independently represent a heterocyclic group containing 4 to 16 carbon atoms and containing a nitrogen atom, an oxygen atom or a sulfur atom; R 13 and R 14Each independently represents an aryl group containing 6 to 30 carbon atoms and optionally containing one or more heteroatoms selected from halogen, silicon, oxygen, sulfur, nitrogen, boron and phosphorus, or a heterocyclic group containing 6 to 16 carbon atoms and containing a nitrogen atom, an oxygen atom or a sulfur atom; Q 11 represents a divalent hydrocarbon group containing 1 to 20 carbon atoms or a silylene group or a germylene group optionally containing a hydrocarbon group containing 1 to 20 carbon atoms; M 11 represents zirconium or hafnium; X 11 and Y 11 Each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group containing 1 to 20 carbon atoms, a silyl group containing a hydrocarbon group containing 1 to 20 carbon atoms, a halogenated hydrocarbon group containing 1 to 20 carbon atoms, an amino group, or an alkylamino group containing 1 to 20 carbon atoms.
[0428] As R 11 and R 12 The heterocyclic group having 4 to 16 carbon atoms and containing a nitrogen atom, an oxygen atom or a sulfur atom is preferably a 2-furyl group, a substituted 2-furyl group, a substituted 2-thienyl group or a substituted 2-furfuryl group, and more preferably a substituted 2-furyl group.
[0429] When R 11 and R 12 When each is a group selected from a heterocyclic group each having 4 to 16 carbon atoms and each containing a nitrogen atom, an oxygen atom or a sulfur atom, the terminal vinyl ratio (Rv) can be increased. In particular, by introducing a substituent of an appropriate size into the heterocyclic group, the relative positional relationship between the heterocyclic ring, the coordination site on the transition metal and the growing polymer chain can be made appropriate, thereby further increasing Rv.
[0430] The substituent of the substituted 2-furyl group, substituted 2-thienyl group and substituted 2-furfuryl group is preferably a hydrocarbon group having 1 to 4 carbon atoms.
[0431] R 11 and R 12 Each is particularly preferably 5-methyl-2-furyl. 11 and R 12 The same groups are preferred.
[0432] R 13 and R 14 Each independently represents an aryl group having 6 to 30 carbon atoms and optionally containing one or more heteroatoms selected from halogen, silicon, oxygen, sulfur, nitrogen, boron and phosphorus, or a heterocyclic group having 6 to 16 carbon atoms and containing a nitrogen atom, an oxygen atom or a sulfur atom.
[0433] In particular, by making R 13 and R 14 The volume is larger, and propylene polymers with higher stereoregularity, fewer heterogeneous bonds and high terminal vinyl content are obtained.
[0434] Therefore, R 13 and R 14 Each is preferably an aryl group, which optionally contains one or more of a hydrocarbon group containing 1 to 6 carbon atoms, a silyl group containing a hydrocarbon group containing 1 to 6 carbon atoms, a halogenated hydrocarbon group containing 1 to 6 carbon atoms, and a halogen atom as a substituent on the aryl ring skeleton, so that the number of carbon atoms is in the range of 6 to 16. 13 and R 14 , examples include, but are not limited to, 4-tert-butylphenyl, 2,3-dimethylphenyl, 3,5-di-tert-butylphenyl, 4-chlorophenyl, 4-trimethylsilylphenyl, 1-naphthyl, and 2-naphthyl.
[0435] R 13 and R 14 Each is more preferably a phenyl group, the phenyl group containing one or more of a hydrocarbon group containing 1 to 6 carbon atoms, a silyl group containing a hydrocarbon group containing 1 to 6 carbon atoms, a halogenated hydrocarbon group containing 1 to 6 carbon atoms, and a halogen atom as a substituent so that the number of carbon atoms is within the range of 6 to 16. The substitution site is preferably position 4 on the phenyl group. 13 and R 14 , examples include but are not limited to 4-tert-butylphenyl, 4-biphenyl, 4-chlorophenyl and 4-trimethylsilylphenyl. 13 and R 14 The same groups are preferred.
[0436] X 11 and Y 11 Each is an auxiliary ligand and reacts with component [B] to generate an active metallocene capable of olefin polymerization. 11 and Y 11 The type of ligand is not particularly limited as long as the purpose is achieved. 11 and Y 11 Each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silyl group containing a hydrocarbon group having 1 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group containing oxygen atoms having 1 to 20 carbon atoms, an amino group or an alkylamino group having 1 to 20 carbon atoms.
[0437] Q 11It represents a divalent hydrocarbon group containing 1 to 20 carbon atoms and bonded to two five-membered rings, or a silylene or germanylene group optionally containing a hydrocarbon group containing 1 to 20 carbon atoms. When two hydrocarbon groups are present on the silylene or germanylene group, they may be bonded to form a cyclic structure.
[0438] As Q 11 , examples include, but are not limited to, the following: alkylene groups such as methylene, methylmethylene, dimethylmethylene and 1,2-ethylene; arylalkylene groups such as diphenylmethylene; silylene; alkylsilylene groups such as methylsilylene, dimethylsilylene, diethylsilylene, di(n-propyl)silylene, di(isopropyl)silylene and di(cyclohexyl)silylene; (alkyl)(aryl)silylene groups such as methyl(phenyl)silylene; arylsilylene groups such as diphenylsilylene; alkyloligosilylene groups such as tetramethyldisilylene; germanylene; and alkylgermanylene, (alkyl)(aryl)germanylene and arylgermanylene groups, each of which is obtained by substituting germanium for the silicon of the above-mentioned silylene groups containing a divalent hydrocarbon group containing 1 to 20 carbon atoms. Among them, a silylene group containing a hydrocarbon group containing 1 to 20 carbon atoms or a germanium group containing a hydrocarbon group containing 1 to 20 carbon atoms is preferred, and an alkylsilylene group or an alkylgermanium group is particularly preferred.
[0439] Among the compounds represented by the general formula (a1), for example, preferred compounds are as follows.
[0440] (1) dichloro[1,1'-dimethylsilylenebis{2-(2-furyl)-4-phenylindenyl}]hafnium,
[0441] (2) dichloro[1,1'-dimethylsilylenebis{2-(2-thienyl)-4-phenylindenyl}]hafnium,
[0442] (3) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-phenylindenyl}]hafnium,
[0443] (4) dichloro[1,1'-diphenylsilylenebis{2-(5-methyl-2-furyl)-4-phenylindenyl}]hafnium,
[0444] (5) dichloro[1,1'-dimethylgermethylenebis{2-(5-methyl-2-furyl)-4-phenylindenyl}]hafnium,
[0445] (6) dichloro[1,1'-dimethylgermanylbis{2-(5-methyl-2-thienyl)-4-phenylindenyl}]hafnium,
[0446] (7) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-phenylindenyl}]hafnium,
[0447] (8) dichloro[1,1'-dimethylsilylenebis{2-(5-trimethylsilyl-2-furyl)-4-phenylindenyl}]hafnium,
[0448] (9) dichloro[1,1'-dimethylsilylenebis{2-(5-phenyl-2-furyl)-4-phenylindenyl}]hafnium,
[0449] (10) dichloro[1,1'-dimethylsilylenebis{2-(4,5-dimethyl-2-furyl)-4-phenylindenyl}]hafnium,
[0450] (11) dichloro[1,1'-dimethylsilylenebis{2-(2-benzofuranyl)-4-phenylindenyl}]hafnium,
[0451] (12) dichloro[1,1'-dimethylsilylenebis{2-(2-furfuryl)-4-phenylindenyl}]hafnium,
[0452] (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-chlorophenyl)indenyl}]hafnium,
[0453] (14) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(4-chlorophenyl)indenyl}]hafnium,
[0454] (15) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-fluorophenyl)indenyl}]hafnium,
[0455] (16) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trifluoromethylphenyl)indenyl}]hafnium,
[0456] (17) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium,
[0457] (18) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-tert-butylphenyl)indenyl}]hafnium,
[0458] (19) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium,
[0459] (20) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(4-tert-butylphenyl)indenyl}]hafnium,
[0460] (21) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)indenyl}]hafnium,
[0461] (22) dichloro[1,1'-dimethylsilylenebis{2-(2-furyl)-4-(1-naphthyl)indenyl}]hafnium,
[0462] (23) dichloro[1,1'-dimethylsilylenebis(2-(2-furyl)-4-(2-naphthyl)indenyl)]hafnium,
[0463] (24) dichloro[1,1'-dimethylsilylenebis(2-(2-furyl)-4-(2-phenanthrenyl)indenyl)]hafnium,
[0464] (25) dichloro[1,1'-dimethylsilylenebis(2-(2-furyl)-4-(9-phenanthrenyl)indenyl)]hafnium,
[0465] (26) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-biphenyl)indenyl}]hafnium,
[0466] (27) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(1-naphthyl)indenyl}]hafnium,
[0467] (28) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(2-naphthyl)indenyl}]hafnium,
[0468] (29) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(1-naphthyl)indenyl}]hafnium, and
[0469] (30) Dichloro[1,1′-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(2-naphthyl)indenyl}]hafnium.
[0470] Among them, the following compounds are more preferred:
[0471] (3) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-phenylindenyl}]hafnium,
[0472] (7) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-phenylindenyl}]hafnium,
[0473] (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-chlorophenyl)indenyl}]hafnium,
[0474] (14) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(4-chlorophenyl)indenyl}]hafnium,
[0475] furanyl)-4-(4-tert-butylphenyl)indenyl}]hafnium,
[0476] (17) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium,
[0477] (18) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-tert-butylphenyl)indenyl}]hafnium,
[0478] (19) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium,
[0479] (20) dichloro[1,1'-dimethylsilylenebis{2-(5-tert-butyl-2-
[0480] (21) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)indenyl}]hafnium,
[0481] (26) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-biphenyl)indenyl}]hafnium,
[0482] (28) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(2-naphthyl)indenyl}]hafnium, and
[0483] (30) Dichloro[1,1′-dimethylsilylenebis{2-(5-tert-butyl-2-furyl)-4-(2-naphthyl)indenyl}]hafnium.
[0484] Among them, the following compounds are still more preferred:
[0485] (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-chlorophenyl)indenyl}]hafnium,
[0486] (17) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium,
[0487] (18) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-tert-butylphenyl)indenyl}]hafnium, and
[0488] (21) Dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)indenyl}]hafnium.
[0489] II-1-2. Component [A-2]
[0490] Component [A-2] is a metallocene compound which, when propylene is homopolymerized at 70°C, gives a propylene homopolymer a-2 having an Mn greater than that of the propylene homopolymer a-1 and an Rv of 0.1 or more and less than 0.5.
[0491] Component [A-2] is a metallocene compound which forms a polymerization catalyst for copolymerizing a propylene monomer and a propylene macromonomer and for producing a propylene macromonomer.
[0492] Therefore, component [A-2] is a metallocene compound that gives an Rv of 0.1 or more, preferably 0.15 or more, more preferably 0.2 or more.
[0493] By using, as component [A-2], a metallocene compound that forms a polymerization catalyst capable of efficiently copolymerizing a macromonomer while having a high molecular weight and a low Rv, the generation of a high molecular weight branched component having a long branch is suppressed.
[0494] Therefore, component [A-2] is a metallocene compound that gives an Rv of less than 0.5, preferably 0.45 or less, and more preferably 0.3 or less.
[0495] In order to obtain an average molecular weight, molecular weight distribution and branching distribution that can make Mw, Mz and g'(1 million) which are characteristic of the branched propylene polymer of the present invention have the above-mentioned characteristics and preferably can make W2 million / W1 million satisfy the above-mentioned characteristics, component [A-2] needs to produce a polymer with a higher molecular weight than component [A-1].
[0496] Therefore, when propylene is homopolymerized at 70°C using the same amount of hydrogen, the component [A-2] is a metallocene compound that produces a polymer having a higher molecular weight than the polymer produced by the component [A-1].
[0497] In order to obtain an average molecular weight, molecular weight distribution and branching distribution that enable the branched propylene polymer of the present invention to satisfy the above-mentioned characteristics, component [A-2] preferably has better macromonomer copolymerizability than component [A-1].
[0498] Therefore, component [A-2] is preferably a metallocene compound in which, when propylene is homopolymerized at 70°C, the ratio of the number of copolymerized terminal vinyl groups forming LCB among the number of generated terminal vinyl groups {LCB number / ([Vi]+LCB number)} is greater than that of component [A-1].
[0499] By selecting the component [A-2] as described above, it is possible to preferentially cause a reaction in which a macromonomer having a relatively small molecular weight generated by the component [A-1] is copolymerized by the component [A-2].
[0500] The evaluation method of Rv and Rvd was performed in the same manner as the evaluation method of component [A-1] except that 100 mg (excluding the mass of the prepolymerized polymer) of the catalyst containing component [A-2] was polymerized by introducing 1.19 NL of hydrogen.
[0501] As with the evaluation method of Rv and Rvd, the Mw characteristics can be evaluated by generating polymers from components [A-2] and [A-1] by bulk polymerization at 70°C, measuring the polymers by GPC to obtain their Mws and comparing them.
[0502] In addition, as with the evaluation method of Rv and Rvd, by generating a polymer from components [A-2] and [A-1] by bulk polymerization at 70°C, measuring the polymer by NMR to obtain the ratio of the number of copolymerized terminal vinyl groups that form LCBs in the number of generated terminal vinyl groups {LCB number / ([Vi]+LCB number)} and comparing them, the copolymerizability characteristics of the macromonomer can be evaluated.
[0503] As described above, since the proportion of the macromonomer in the polymer produced by component [A-2] is lower than the proportion of the macromonomer in the polymer produced by component [A-1], the copolymerization amount of macromonomer 2 is suppressed. At the same time, since the copolymerizability of component [A-2] is superior to that of component [A-1], the branch length in the branched structure into which the branched propylene polymer is introduced can be adjusted by effective copolymerization of macromonomer 1. Using the branch length adjustment, a branched propylene polymer can be obtained: it has an average molecular weight, molecular weight distribution, branch distribution, branch structure and melting characteristics (Ea, SHI and MBI) that make Mw, Mz and g' (1 million) that are characteristic of the branched propylene polymer of the present invention have the above characteristics and preferably can make W2 million / W1 million satisfy the above characteristics.
[0504] As component [A-2], examples include, but are not limited to, metallocene compounds represented by the following general formula (a2):
[0505] [Chemical formula 4]
[0506]
[0507] (wherein, M is a transition metal atom selected from Groups 3, 4, 5 and 6, lanthanide and actinide of the periodic table; M is preferably titanium, zirconium or hafnium;
[0508] p is 0, 1, 2 or 3, and p is preferably 2 and equal to the formal oxidation state of the metal M minus 2;
[0509] X are the same or different, and each X is a hydrogen atom, a halogen atom or R a , OR a 、OSO 2 CF 3 ,OCOR a , SR a NR a 2 or PR a 2 Group (where R a is a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms of Groups 13 to 17 of the Periodic Table of Elements); R a Preferably, it is a linear or branched alkyl group containing 1 to 20 carbon atoms; or two Xs may form a substituted or unsubstituted butadienyl group or an OR'O group (wherein R' is a divalent group selected from an alkylene group containing 1 to 40 carbon atoms, an arylene group containing 6 to 40 carbon atoms, an alkylarylene group containing 7 to 40 carbon atoms, and an arylalkylene group containing 7 to 40 carbon atoms); X is preferably a hydrogen atom, a halogen atom or a Ra group; X is more preferably a chlorine atom or an alkyl group containing 1 to 10 carbon atoms, such as a methyl group and an ethyl group;
[0510] L is a divalent hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms from Groups 13 to 17 of the Periodic Table, or a divalent silylene group containing up to 5 silicon atoms; L is preferably selected from an alkylene group containing 1 to 40 carbon atoms, a cycloalkylene group containing 3 to 40 carbon atoms, an arylene group containing 6 to 40 carbon atoms, an alkylarylene group containing 7 to 40 carbon atoms, an arylalkylene group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms from Groups 13 to 17 of the Periodic Table, and a group such as SiMe 2 and SiPh 2 The divalent bridging group in a silylene group containing up to 5 silicon atoms; L is preferably (Z(R") 2 ) nA group (wherein Z is a carbon atom or a silicon atom; n is 1 or 2; R" is a hydrocarbon group containing 1 to 20 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table; and R" is preferably a linear or branched, cyclic or non-cyclic alkyl group containing 1 to 20 carbon atoms, an alkenyl group containing 2 to 20 carbon atoms, an alkynyl group containing 2 to 20 carbon atoms, an aryl group containing 6 to 20 carbon atoms, an alkylaryl group containing 7 to 20 carbon atoms, or an arylalkyl group containing 7 to 20 carbon atoms, all of which optionally contain heteroatoms of Groups 13 to 17 of the Periodic Table); (Z(R") 2 ) n The group is more preferably Si(CH 3 ) 2 、SiPh 2 、SiPhMe、SiMe(SiMe 3 ), CH 2 and (CH 2 ) 2 or C(CH 3 ) 2 ;
[0511] R 1 and R 2 Each is a hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table, and R 1 and R 2 are the same or different; R 1 and R 2 Each is preferably a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms of Groups 13 to 17 of the Periodic Table of Elements; R 1 and R 2 Each is more preferably a linear or branched alkyl group containing 1 to 20 carbon atoms; R 1 and R 2 Each is still more preferably methyl or ethyl;
[0512] T is the following formula (a2-T1) or (a2-T2), and T is the same or different:
[0513] [Chemical formula 5]
[0514]
[0515] (wherein an atom with the symbol "*" is combined with an atom with the same symbol in the compound of formula (a2);
[0516] R 3 is a hydrogen atom or a hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table; R 3 Preferably, it is a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms from Groups 13 to 17 of the Periodic Table of Elements; R 3 More preferably, it is a linear or branched alkyl group containing 1 to 20 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms, or an arylalkyl group containing 7 to 40 carbon atoms; R 3 Still more preferred is an aryl group containing 6 to 20 carbon atoms, which is optionally substituted with one or more alkyl groups each containing 1 to 10 carbon atoms;
[0517] R 4 and R 6 are each a hydrogen atom or a hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table, and R 4 and R 6 are the same or different; R 4 and R 6 are each a hydrogen atom, a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms, or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms of Groups 13 to 17 of the Periodic Table of Elements, and R 4 and R 6 are the same or different; R 4 and R 6 Each is preferably a hydrogen atom;
[0518] R 5 is a hydrogen atom or a hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table; R 5 Preferably, it is a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms from Groups 13 to 17 of the Periodic Table of Elements; R 5More preferably, it is a linear or branched, saturated or unsaturated alkyl group containing 1 to 20 carbon atoms; R 5 Still more preferably methyl or ethyl;
[0519] R 7 and R 8 are each a hydrogen atom or a hydrocarbon group containing 1 to 40 carbon atoms and optionally containing heteroatoms of Groups 13 to 17 of the Periodic Table, and R 7 and R 8 are the same or different; R 7 and R 8 Optionally forming a saturated or unsaturated 5-membered or 6-membered ring, and the ring optionally includes an alkyl group containing 1 to 20 carbon atoms as a substituent; R 7 and R 8 Each is preferably a hydrogen atom or a linear or branched, cyclic or acyclic alkyl group containing 1 to 40 carbon atoms, an alkenyl group containing 2 to 40 carbon atoms, an alkynyl group containing 2 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms or an arylalkyl group containing 7 to 40 carbon atoms, all of which optionally contain heteroatoms from Groups 13 to 17 of the Periodic Table of Elements;
[0520] R 8 Preferably, it is a hydrogen atom or a linear or branched, saturated or unsaturated alkyl group containing 1 to 20 carbon atoms; R 8 More preferably, it is methyl or ethyl; R 7 Preferably, it is an alkyl group containing 1 to 40 carbon atoms, an aryl group containing 6 to 40 carbon atoms, an alkylaryl group containing 7 to 40 carbon atoms, or an arylalkyl group containing 7 to 40 carbon atoms; R 7 More preferably, it is the following formula (a2-R7):
[0521] [Chemical formula 6]
[0522]
[0523] (Among them, R 7a , R 7b , R 7c , R 7d and R 7e each is a hydrogen atom or a linear or branched, cyclic or acyclic alkyl group containing 1 to 20 carbon atoms, an alkenyl group containing 2 to 20 carbon atoms, an alkynyl group containing 2 to 20 carbon atoms, an aryl group containing 6 to 20 carbon atoms, an alkylaryl group containing 7 to 20 carbon atoms or an arylalkyl group containing 7 to 20 carbon atoms, all of which optionally contain heteroatoms of Groups 13 to 17 of the Periodic Table of Elements, and R 7a , R 7b , R 7c , R7d and R 7e Can be the same or different; R 7a and R 7d Each is preferably a hydrogen atom; and R 7b , R 7c and R 7e Each is preferably a hydrogen atom or a linear or branched, cyclic or acyclic alkyl group having 1 to 10 carbon atoms. )]
[0524] In an embodiment, the compound represented by the general formula (a2) may be a compound represented by the following general formula (a3):
[0525] [Chemical formula 7]
[0526]
[0527] (Among them, M, X, p, L, R 1 , R 2 , R 7 and R 8 have the same meanings as those of formula (a2). )
[0528] In the formula (a3), M is preferably hafnium from the viewpoint that a certain proportion of vinyl groups can be formed at the terminals and that long chain branches can be generated by copolymerizing a macromonomer.
[0529] As the metallocene complex represented by the general formula [a3], examples include, but are not limited to, the following.
[0530] Dimethylsilylenebis(cyclopenta[b]thienyl)hafnium dichloride
[0531] Dimethylsilylenebis(5-methyl-cyclopenta[b]thienyl)hafnium dichloride
[0532] Dimethylsilylenebis(2,5-dimethylcyclopenta[b]thienyl)hafnium dichloride
[0533] Dimethylsilylenebis(2,3,5-trimethylcyclopenta[b]thienyl)hafnium dichloride
[0534] Dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride
[0535] Dimethylsilylenebis(2,5-dimethyl-3-(4-tert-butylphenyl)-cyclopenta[b]thienyl)hafnium dichloride
[0536] Dimethylsilylenebis(2,5-dimethyl-3-(2,5-dimethylphenyl)-cyclopenta[b]thienyl)hafnium dichloride
[0537] Dimethylsilylenebis(2,5-dimethyl-3-(3,5-dimethylphenyl)-cyclopenta[b]thienyl)hafnium dichloride
[0538] Dimethylsilylenebis(2,5-dimethyl-3-(3,5-di-tert-butylphenyl)-cyclopenta[b]thienyl)hafnium dichloride
[0539] In addition, examples include, but are not limited to, the above-mentioned exemplary compounds, wherein one or two Xs are replaced with bromine atoms, iodine atoms, methyl groups, phenyl groups, dimethylamino groups, diethylamino groups, etc. instead of chlorine atoms. When an asymmetric carbon is formed in a metallocene complex, it means one of the stereoisomers or a mixture thereof (including a racemate) unless otherwise specified.
[0540] As a method for synthesizing the metallocene complex represented by the general formula [a2], a conventionally known synthesis method can be appropriately selected and used. For example, the metallocene complex represented by the general formula [a2] can be synthesized with reference to the Japanese translation of PCT International Application Publication No. 2007-528925.
[0541] As a method for synthesizing the metallocene complex represented by the general formula [a3], a conventionally known synthesis method can be appropriately selected and used. For example, the metallocene complex represented by the general formula [a3] can be synthesized with reference to JP-A No. 2021-152155.
[0542] II-1-3. Component [B]
[0543] Component [B] is a compound or layered silicate that can react with components [A-1] and [A-2] to form an ion pair.
[0544] Component [B] may be used alone, or two or more components [B] may be used. Component [B] is preferably a layered silicate.
[0545] II-1-3-1. Compounds that can react with components [A-1] and [A-2] to form ion pairs
[0546] As the compound that can react with components [A-1] and [A-2] to form an ion pair, examples include, but are not limited to, aluminum oxide compounds and boron compounds. As the aluminum oxide compound, examples include, but are not limited to, compounds represented by the following general formulas (I) to (III).
[0547] [Chemical formula 8]
[0548]
[0549] In the general formulae (I), (II) and (III), R 91 , R101 and R 111 Each independently represents a hydrogen atom or a hydrocarbon group, preferably a hydrocarbon group containing 1 to 10 carbon atoms, and particularly preferably a hydrocarbon group containing 1 to 6 carbon atoms. 91 Can be the same or different; multiple R 101 can be the same or different; and multiple R 111 They may be the same or different. In addition, p is an integer of 0 to 40, and preferably an integer of 2 to 30.
[0550] Each compound represented by the general formula (I) and (II) is a compound called aluminoxane. Among aluminoxanes, methylaluminoxane or methylisobutylaluminoxane is preferred. Several aluminoxanes may be used in combination within each group or between groups.
[0551] In the general formula (III), R 112 It is a hydrocarbon group containing 1 to 10 (preferably 1 to 6) carbon atoms.
[0552] As the boron compound, examples include, but are not limited to, complexes of cations such as carbonium cations and ammonium cations and organic boron compounds such as triphenylboron, tri(3,5-difluorophenyl)boron, and tri(pentafluorophenyl)boron, and various organic boron compounds such as tri(pentafluorophenyl)boron.
[0553] II-1-3-2. Layered silicate
[0554] Layered silicate (hereinafter, it may be simply referred to as "silicate") is a silicate compound having a crystal structure in which plate-like crystals are stacked in parallel by ion bonding, etc. In the silicate compound, the plate-like crystals form a single layer, and interlayer ions exist between the layers.
[0555] As the layered silicate, examples include, but are not limited to, layered silicates described in "Nendo Kobutsu Gaku (Clay Mineralogy)" written by Haruo Shirozu (published by Asakura Shoten in 1988), such as layered silicates having a 1:1 layer structure composed of units consisting of one tetrahedral sheet and one octahedral sheet, and layered silicates having a 2:1 layer structure composed of units consisting of two tetrahedral sheets and one octahedral sheet sandwiched therebetween.
[0556] As the layered silicate having a 1:1 layer structure, examples include, but are not limited to, kaolin group silicates (such as dickite, nacrite, kaolinite, metahalloysite, and halloysite) and serpentine group silicates (such as chrysotile, lizardite, and antigorite).
[0557] As the layered silicate having a 2:1 layer structure, examples include, but are not limited to, montmorillonite group silicates (such as montmorillonite, beidellite, nontronite, saponite, hectorite and stevensite), vermiculite group silicates (such as vermiculite), mica group silicates (such as mica, illite, sericite and glauconite), attapulgite, sepiolite, palygorskite, bentonite, pyrophyllite, talc and chlorite group. They may form a mixed layer.
[0558] Among them, a layered silicate having a 2:1 layer structure consisting of a unit composed of two tetrahedral sheets and one octahedral sheet sandwiched therebetween as a main component is preferred, the tetrahedral sheet being mainly composed of silicon oxide, and the octahedral sheet being mainly composed of aluminum oxide. The main component is preferably a montmorillonite silicate, more preferably montmorillonite.
[0559] Layered silicates may contain exchangeable ions between the layers (interlayer ions). Such layered silicates that can exchange interlayer ions are ion-exchange layered silicates.
[0560] The interlayer ions are preferably interlayer cations such that the ions are cationic. The type of interlayer cations is not particularly limited. As main components, examples include, but are not limited to, alkali metals of Group 1 of the periodic table, such as lithium and sodium, alkaline earth metals of Group 2 of the periodic table, such as calcium and magnesium, and transition metals such as iron, cobalt, copper, nickel, zinc, ruthenium, rhodium, palladium, silver, iridium, platinum and gold.
[0561] The layered silicate may be a natural layered silicate or an artificially synthesized layered silicate.
[0562] The form of the layered silicate is not particularly limited. The layered silicate may be in a naturally occurring form, or it may be in an artificially synthesized spherical form.
[0563] The form of the naturally occurring layered silicate can be processed by operations such as comminution and granulation. It is preferred to process the form of the naturally occurring layered silicate into a spherical form by granulation. It is particularly preferred to narrow the particle size distribution of the layered silicate processed into a spherical form by operations such as classification, because good polymer particle properties are obtained.
[0564] In order to change the interlayer ions of the layered silicate into alkali metal ions, the layered silicate is preferably subjected to a chemical treatment.
[0565] The layered silicate can be chemically treated by, for example, the method described in paragraphs 0048 to 0066 of JP-A No. 2018-162391.
[0566] Component [B] preferably used in the present invention is a chemically treated layered silicate. From the viewpoint of the amount and distribution of the catalyst components [A-1] and [A-2] to be supported, the molar ratio (Al / Si) between the aluminum atoms and the silicon atoms contained in the layered silicate is preferably in the range of 0.01 to 0.25, more preferably 0.03 to 0.24, still more preferably 0.05 to 0.23.
[0567] Referring to the description of paragraph 0089 in JP-A No. 2018-162391, Al and Si in the layered silicate are measured by making a calibration curve by a chemical analysis method defined in JIS and quantifying aluminum and silicon by X-ray fluorescence.
[0568] II-1-4. Component [C]
[0569] Component [C] used in the present invention is an organoaluminum compound, and it is preferably an organoaluminum compound represented by the following general formula (IV):
[0570] (AlR b n X 3-n ) m General formula (IV)
[0571] (Among them, R b is an alkyl group containing 1 to 20 carbon atoms; X is a halogen, hydrogen, an alkoxy group or an amino group; n is an integer of 1 to 3; and m is an integer of 1 to 2.
[0572] As component [C], an organoaluminum compound may be used alone, or several organoaluminum compounds may be used in combination of two or more.
[0573] As the organoaluminum compound, examples include, but are not limited to, trimethylaluminum, triethylaluminum, tri-n-propylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, tri-n-decylaluminum, diethylaluminum chloride, diethylaluminum sesquichloride, diethylaluminum hydride, diethylaluminum ethoxide, diethylaluminum dimethylamide, diisobutylaluminum hydride, and diisobutylaluminum chloride. Among them, trialkylaluminum (represented by the general formula (IV), wherein m is 1 and n is 3) and dialkylaluminum hydride (represented by the general formula (IV), wherein m is 2; n is 1; and X is hydrogen) are preferred. More preferred is trialkylaluminum (represented by the general formula (IV), wherein R is an alkyl group containing 1 to 8 carbon atoms).
[0574] II-1-5. Preparation of catalyst
[0575] The olefin polymerization catalyst preferably used in the present invention contains the above-mentioned components [A-1], [A-2], [B] and [C]. The olefin polymerization catalyst can be obtained by contacting them inside or outside a polymerization tank. The olefin polymerization catalyst can be prepolymerized in the presence of an olefin.
[0576] The amounts of components [A-1], [A-2], [B] and [C] used may be any amounts.
[0577] For example, the total usage amount of components [A-1] and [A-2] may be in the range of 0.1 μmol to 1000 μmol, or may be in the range of 0.5 μmol to 500 μmol, relative to 1 g of component [B].
[0578] For the ratio between components [A-1] and [A-2], the ratio of the molar weight of component [A-1] to the total molar weight of components [A-1] and [A-2] is preferably more than 0.30 and less than 0.99. By changing the ratio of the molar weight, the average molecular weight, high molecular weight, very high molecular weight, branching number and branching distribution are changed. By this change, a branched propylene polymer of the present invention is obtained, wherein while maintaining the necessary branched structure, there is less component with extremely long relaxation time.
[0579] In terms of the molar ratio of aluminum in component [C] to the total transition metal in components [A-1] and [A-2], the amount of component [C] used can be 0.01 to 5×10 6 In the range of 0.1 to 1×10 4 within the range.
[0580] Components [A-1], [A-2], [B] and [C] may be contacted in any order. As the order, examples include the following.
[0581] (1) One of components [A-1] and [A-2] is brought into contact with component [B]; they are brought into contact with component [C]; and then they are brought into contact with the remaining component [A-1] or [A-2].
[0582] (2) Components [A-1] and [A-2] are contacted with component [B] separately or simultaneously, and then contacted with component [C].
[0583] (3) Components [C] and [B] are brought into contact with each other, and then components [A-1] and [A-2] are brought into contact with them sequentially or simultaneously.
[0584] (4) In the presence of component [B], components [A-1] and [A-2] are simultaneously contacted with component [C].
[0585] Among them, (4) is preferred.
[0586] In the above examples, a solvent can be used to fully contact the components. As a solvent, examples include, but are not limited to, aliphatic saturated hydrocarbons, aromatic hydrocarbons, aliphatic unsaturated hydrocarbons, halides thereof, and monomers for prepolymerization. As aliphatic saturated hydrocarbons and aromatic hydrocarbons, examples include, but are not limited to, hexane, heptane, and toluene. As a monomer for prepolymerization used as a solvent, examples include, but are not limited to, propylene.
[0587] II-1-6. Prepolymerization
[0588] The olefin polymerization catalyst may be a catalyst that has undergone prepolymerization in which a small amount of olefin is polymerized by contacting the catalyst with the olefin. The catalyst that has undergone prepolymerization has improved catalytic activity and can produce a propylene-based polymer at low cost.
[0589] The olefin used is not particularly limited. Examples of the olefin include, but are not limited to, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, 3-methyl-1-butene, vinyl cycloalkanes, and styrene. Among them, propylene is preferred.
[0590] As olefins used, it is possible to use olefins from fossil fuels, olefins from biomass, olefins from chemical recycling or mixtures thereof.
[0591] The olefin may be fed into the prepolymerization tank by any method. As the method, examples include, but are not limited to, a method of introducing the olefin at a fixed rate, a method of introducing the olefin while maintaining the olefin at a fixed pressure, a combination thereof, and a method of changing the feeding method of the olefin in a staged manner.
[0592] The prepolymerization temperature and the prepolymerization time are not particularly limited, and they are preferably in the range of -20°C to 100°C and in the range of 5 minutes to 24 hours, respectively.
[0593] As the prepolymerization ratio, the mass ratio of the prepolymerized polymer to the component [B] may be 0.01 to 100, or it may be 0.1 to 50.
[0594] During the prepolymerization, component [C] may be added.
[0595] During or after the prepolymerization, a polymer such as polyethylene and polypropylene or a solid inorganic oxide such as silica and titania may coexist.
[0596] II-2. Polymerization method of propylene-based polymer
[0597] Examples of the polymerization method for the branched propylene-based polymer of the present invention include, but are not limited to, a method of homopolymerizing propylene or copolymerizing propylene with a comonomer in the presence of a propylene polymerization catalyst comprising components [A-1], [A-2], [B], and [C].
[0598] As the polymerization mode, any method may be adopted, such as a solution polymerization method, a gas phase polymerization method, a bulk polymerization method in which propylene is used as a solvent instead of using a substantially inert solvent. Among them, the bulk polymerization method is preferred.
[0599] For example, the polymerization temperature of the bulk polymerization may be 40 to 80° C., or it may be 50 to 75° C. The polymerization pressure of the bulk polymerization may be 1.0 to 5.0 MPa, may be 1.5 to 4.0 MPa, or may be 2.0 to 3.5 MPa.
[0600] As the polymerization method, a continuous polymerization method or a batch polymerization method can be adopted. As the number of polymerization stages, a single stage polymerization or a multi-stage polymerization of two or more stages can be adopted.
[0601] The polymerization may be a homopolymerization of propylene, or it may be a copolymerization of propylene and an α-olefin comonomer containing 2 to 20 carbon atoms other than propylene. As the α-olefin comonomer, examples include, but are not limited to, one or more comonomers selected from ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene, etc. By homopolymerization of propylene, a propylene homopolymer is obtained. By copolymerization of propylene and the comonomer, a propylene copolymer is obtained.
[0602] As propylene and comonomers, propylene and comonomers respectively derived from fossil fuels, biomass or chemical recycling, or propylene and comonomers derived from a mixture thereof can be used.
[0603] [Use of hydrogen]
[0604] The branched propylene-based polymer of the present invention can be obtained by using hydrogen in the presence of a catalyst and controlling the amount of hydrogen used.
[0605] The average molecular weight and molecular weight distribution (Mz, Mw, Mn, Mw / Mn and Mz / Mw) of the branched propylene-based polymer as measured by GPC, and the balance thereof can be adjusted, for example, by controlling the amount of hydrogen used and the like.
[0606] In the method for producing a branched propylene polymer of the present invention, it is preferred that in the relationship between components [A-1] and [A-2], component [A-1] relatively acts as a catalyst component for generating a low molecular weight component, and component [A-2] relatively acts as a catalyst component for generating a high molecular weight component. As a result, the rate of change of Mz relative to the change in the amount of hydrogen becomes greater than the rate of change of Mw, and therefore, Mz / Mw can be changed without a large change in Mw / Mn.
[0607] For example, when the amount of hydrogen increases, the rate of change in molecular weight reduction of the polymer produced by component [A-2], which produces a high molecular weight, is large relative to the polymer produced by component [A-1], which produces a low molecular weight. When component [A-1] is relatively more activated than component [A-2], the molecular weight distribution changes so that the percentage of polymer produced by component [A-1] is greater than the percentage of polymer produced by component [A-2]. Due to this change in molecular weight distribution, Mz and Mz / Mw can be made smaller without a large change in Mw and Mw / Mn.
[0608] On the other hand, when the amount of hydrogen is reduced, the rate of change in molecular weight increase of the polymer produced by the component [A-2] that produces a high molecular weight is large relative to the polymer produced by the component [A-1] that produces a low molecular weight. Due to this change in molecular weight distribution, Mz and Mz / Mw can be made larger without a large change in Mw and Mw / Mn.
[0609] [How to use the catalyst]
[0610] In the case of continuously polymerizing the branched propylene-based polymer of the present invention, when at least hydrogen and propylene are continuously introduced into the polymerization reactor, it is preferred that the catalyst is continuously introduced.
[0611] [Polymer slurry concentration]
[0612] For example, when the branched propylene polymer of the present invention is produced by bulk continuous polymerization, the amount of polymer contained in the polymerization reactor can be kept constant (steady state) by controlling the amount of propylene introduced into the polymerization reactor and the amount of recovered polymer and unreacted propylene.
[0613] At this time, the ratio of the amount of polymer to the mass of propylene in the polymerization reactor (ie, polymer slurry concentration) is constant.
[0614] However, even when the polymer slurry concentration is constant, the polymer concentration varies depending on the height of the position in the propylene solution when the polymer settles slightly. In this case, the hydrogen consumption rate varies depending on the position, resulting in a broadening of the molecular weight and branching distribution.
[0615] Therefore, in the method for producing a branched propylene-based polymer of the present invention, the polymer slurry concentration is preferably 55% by mass or less, more preferably 50% by mass or less, still more preferably 45% by mass or less.
[0616] In the method for producing a branched propylene polymer of the present invention, the polymer slurry concentration is preferably 30% by mass or more, more preferably 35% by mass or more, and still more preferably 40% by mass or more.
[0617] III. Uses of branched propylene polymers
[0618] The branched propylene-based polymer of the present invention can be used as a molding material after it is made into a powder form, a pellet form cut into particles after heating and melt kneading, or the like.
[0619] Branched propylene polymers of the present invention can be mixed with additives and resins. As additives, examples include, but are not limited to, antioxidants, UV absorbers, antistatic agents, nucleating agents, lubricants, flame retardants, anti-caking agents, colorants, inorganic fillers and organic fillers. As resins, examples include, but are not limited to, various synthetic and natural resins.
[0620] Branched propylene polymer of the present invention can be shaped by any type of polypropylene forming method. As forming method, example includes but is not limited to injection molding, extrusion molding, foaming and blow molding. As the molded product that can be made by the above method, example includes but is not limited to various molded products, such as industrial parts, containers, unstretched films, uniaxially stretched films, biaxially stretched films, sheets, tubing and fibers of injection molding.
[0621] In the branched propylene-based polymer of the present invention, there are fewer components with extremely long relaxation time while maintaining necessary melt tension. Therefore, a branched propylene-based polymer having excellent ductility when melted is provided, and it can be applied to applications requiring ductility.
[0622] Furthermore, the branched propylene-based polymer of the present invention may be blended with other resins when used.
[0623] Example
[0624] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. The present invention is not limited to these Examples unless it exceeds the gist thereof.
[0625] In the following examples, before using the autoclave, the autoclave was fully dried by introducing nitrogen while heating the autoclave. In addition, the catalyst preparation and polymerization were all carried out in an inert gas.
[0626] (1) Synthesis of catalyst component (A)
[0627] (1-1) Synthesis Example 1: Synthesis of Catalyst Component [A-1]
[0628] (Complex 1)
[0629] Synthesis of racemic dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium:
[0630] According to the method of Synthesis Example 1 in JP-A No. 2012-149160, racemic dichloro[1,1′-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium was synthesized.
[0631] (1-2) Synthesis Example 2: Synthesis of Catalyst Component [A-2]
[0632] (Complex 2)
[0633] 1) Synthesis of racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (complex 2):
[0634] (1-a) Synthesis of 2,5-dimethyl-3-phenyl-hydrogenated cyclopenta[b]thiophene:
[0635] The synthesis was carried out with reference to the method described in Example 1 of the Japanese translation of PCT International Application No. 2003-517010.
[0636] (1-b) Synthesis of dimethylbis(2,5-dimethyl-3-phenyl-hydrocyclopenta[b]thiophene)silane:
[0637] First, 2,5-dimethyl-3-phenyl-hydrocyclopentadien[b]thiophene (8.8 g, 39 mmol) and THF (200 ml) were placed in a 500 ml glass reaction vessel, and the mixture was cooled to -70 ° C. Next, n-butyl lithium-n-hexane solution (1.55 mol / L, 25 ml, 39 mmol) was added thereto in a dropwise manner. After the dropwise addition, the mixture was stirred for 2 hours while the mixture temperature was gradually restored to room temperature. The mixture was cooled to -70 ° C again; 1-methylimidazole (0.15 ml, 1.9 mmol) was added thereto; and a THF solution containing dimethyldichlorosilane (2.5 g, 19 mmol) was added thereto in a dropwise manner. After the dropwise addition, the mixture was stirred overnight while the mixture temperature was gradually restored to room temperature.
[0638] Distilled water was added to the reaction solution thus obtained. The mixture thus obtained was transferred to a separatory funnel and washed with brine until neutral. Sodium sulfate was added thereto, and the reaction solution was left overnight to dry. The sodium sulfate was filtered; the solvent was distilled under reduced pressure; the solid thus obtained was purified by a silica gel column to obtain a white powder of dimethylbis(2,5-dimethyl-3-phenyl-hydrocyclopenta[b]thiophene)silane (9.8 g, yield 99%).
[0639] (1-c) Synthesis of racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (complex A):
[0640] First, dimethylbis(2,5-dimethyl-3-phenyl-hydrocyclopentadienyl[b]thiophene)silane (6.1 g, 12 mmol) and ether (200 ml) were placed in a 500 ml glass reaction vessel. In a dry ice-methanol bath, the mixture was cooled to -70°C. n-Butyl lithium-n-hexane solution (1.55 mol / L, 16 ml, 24 mmol) was added thereto in a dropwise manner. After the dropwise addition, the mixture was returned to room temperature and then stirred for 2 hours. The solvent of the resulting reaction solution was concentrated to about 20 ml under reduced pressure; toluene (250 ml) and THF (10 ml) were added thereto; the mixture was cooled to -70°C in a dry ice-methanol bath; and hafnium tetrachloride (3.8 g, 12 mmol) was then added thereto. Next, the mixture was stirred overnight while the mixture temperature was gradually returned to room temperature.
[0641] The solvent was distilled from the mixture under reduced pressure, and the solid thus obtained was recrystallized with toluene / hexane to obtain racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (purity 97%) in the form of yellow crystals (0.87 g, yield 10%).
[0642] By proton nuclear magnetic resonance ( 1 The identification values of the obtained racemate obtained by H-NMR are shown below.
[0643] 1 H-NMR (CDCl 3 )Recognition results
[0644] Racemate: δ1.06 (s, 6H), δ2.42 (s, 6H), δ2.59 (s, 6H), δ8.51 (s, 2H), δ7.28-δ7.33 (m, 2H), δ7.39-δ7.43 (m, 4H), δ7.46-δ7.50 (m, 4H)
[0645] (1-3) Synthesis Example 3: Synthesis of Comparative Catalyst Component [CA-2]
[0646] (Complex 3)
[0647] Synthesis of racemic dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium:
[0648] According to the method of Example 7 in JP-A No. H11-240909, racemic dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium was synthesized.
[0649] (2) Synthesis Example of Component (B): Chemical Treatment of Ion-Exchange Layered Silicate
[0650] First, 645.1 g of distilled water and 82.6 g of 98% sulfuric acid were fed into a 1 L three-necked flask equipped with a stirring blade and a reflux device, and the temperature of the mixture was increased to 95°C.
[0651] Next, 100 g of commercially available montmorillonite (BENCLAY KK manufactured by Mizusawa Industrial Chemicals, Ltd., Al: 9.78 mass%, Si: 31.79 mass%, Mg: 3.18 mass%, Al / Si (molar ratio): 0.320, average particle size: 14 μm) was added thereto, and the mixture was reacted at 95° C. for 320 minutes. After 320 minutes, 0.5 L of distilled water was added to stop the reaction. Then, the mixture was filtered to obtain 255 g of a solid in the form of a cake.
[0652] 1 g of the cake contained 0.31 g of chemically treated montmorillonite (intermediate). The chemical composition of the chemically treated montmorillonite (intermediate) is as follows.
[0653] Al: 7.68 mass%, Si: 36.05 mass%, Mg: 2.13 mass%, Al / Si (molar ratio): 0.222
[0654] The cake was mixed with 1545 g of distilled water and slurried. The temperature of the obtained slurry was raised to 40° C. 5.734 g of lithium hydroxide hydrate in solid form was added to the slurry. Then, the slurry was reacted at 40° C. for 1 hour. After 1 hour, the reacted slurry was filtered and then washed 3 times with 1 L of distilled water to obtain a solid in the form of a cake again.
[0655] The obtained cake-like solid was pre-dried at 90°C overnight under normal pressure, and then dried at 200°C using an oil bath under reduced pressure for more than 2 hours after the bumping subsided, thereby obtaining 80 g of chemically treated montmorillonite. The chemical composition of the chemically treated montmorillonite is as follows.
[0656] Al: 7.68 mass%, Si: 36.05 mass%, Mg: 2.13 mass%, Al / Si (molar ratio): 0.222, Li: 0.53 mass%
[0657] (3) Preparation of Catalyst
[0658] (3-1) Synthesis Example of Catalyst 1
[0659] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (66 mL) and slurried. Next, triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0660] In another flask (volume 200 mL), racemic dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (105 μmol) produced in the synthesis example of catalyst component [A-1] was dissolved in toluene (21 mL) to prepare a solution (solution 1). In addition, in another flask (volume 200 mL), racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (complex 2) (45 μmol) produced in the synthesis example of catalyst component [A-2] was dissolved in toluene (9 mL) to prepare a solution (solution 2).
[0661] Triisobutylaluminum (0.42 mmol: 0.6 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, Solution 1 (21 mL) was added thereto, and they were stirred at room temperature for 20 minutes.
[0662] Next, triisobutylaluminum (0.18 mmol: 0.25 mL of a heptane solution having a concentration of 143 mg / mL) was further added thereto. Then, Solution 2 was added thereto, and they were stirred at room temperature for 1 hour.
[0663] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0664] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0665] The catalyst slurry was dried under reduced pressure for 1 hour to obtain 28.2 g of a prepolymerized catalyst (catalyst 1). The prepolymerization ratio of the catalyst (a value obtained by dividing the amount of prepolymerized polymer by the amount of solid catalyst) was 1.82.
[0666] (3-2) Synthesis Example of Catalyst 2
[0667] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (66 mL) and slurried. Next, triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0668] In another flask (volume 200 mL), racemic dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (105 μmol) produced in the synthesis example of catalyst component [A-1] was dissolved in toluene (21 mL) to prepare a solution (solution 1). In addition, in another flask (volume 200 mL), racemic dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium (complex 3) (45 μmol) produced in the synthesis example of comparative catalyst component [CA-2] was dissolved in toluene (9 mL) to prepare a solution (solution 2).
[0669] Triisobutylaluminum (0.42 mmol: 0.6 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, Solution 1 (21 mL) was added thereto, and they were stirred at room temperature for 20 minutes.
[0670] Next, triisobutylaluminum (0.18 mmol: 0.25 mL of a heptane solution having a concentration of 143 mg / mL) was further added thereto. Then, Solution 2 was added thereto, and they were stirred at room temperature for 1 hour.
[0671] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0672] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0673] The catalyst slurry was dried under reduced pressure for 1 hour to obtain 30.9 g of a prepolymerized catalyst (catalyst 2). The prepolymerization ratio of the catalyst was 2.09.
[0674] (3-3) Synthesis Example of Catalyst 3
[0675] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (66 mL) and slurried. Next, triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0676] In another flask (volume 200 mL), racemic dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (75 μmol) produced in the synthesis example of catalyst component [A-1] was dissolved in toluene (15 mL) to prepare a solution (solution 1). In addition, in another flask (volume 200 mL), racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (complex 2) (75 μmol) produced in the synthesis example of catalyst component [A-2] was dissolved in toluene (15 mL) to prepare a solution (solution 2).
[0677] Triisobutylaluminum (0.42 mmol: 0.6 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, Solution 1 (21 mL) was added thereto, and they were stirred at room temperature for 20 minutes.
[0678] Next, triisobutylaluminum (0.18 mmol: 0.25 mL of a heptane solution having a concentration of 143 mg / mL) was further added thereto. Then, Solution 2 was added thereto, and they were stirred at room temperature for 1 hour.
[0679] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0680] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0681] The catalyst slurry was dried under reduced pressure for 1 hour to obtain 28.5 g of a prepolymerized catalyst (catalyst 3). The prepolymerization ratio of the catalyst was 1.85.
[0682] (4) Embodiment
[0683] [Example 1]
[0684] (polymerization)
[0685] The 20L autoclave was used after being purged with propylene inside the tank and cooled to room temperature. Next, 18.7mL of a heptane solution of triisobutylaluminum (140mg / mL) and 5000g of liquid propylene were introduced into the polymerization tank. Next, the temperature inside the tank was raised to 63°C. Then, 700mg of catalyst 1 (which is the mass of the polymer not including the prepolymerization) was fed into the polymerization tank under pressure by high-pressure argon to initiate polymerization, and the temperature inside the tank was quickly raised to 70°C. The temperature was maintained at 70°C, and after 1 hour from the start of polymerization, unreacted propylene was quickly purged to stop polymerization. Thus, about 1687g of propylene homopolymer was obtained. The results of GPC, 3D-GPC and 13 The obtained polymer was measured by C-NMR.
[0686] (Granulation)
[0687] Relative to 100 parts by mass of the branched propylene-based polymer thus obtained, 0.125 parts by mass of a phenol-based antioxidant IRGANOX 1010 (tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane manufactured by BASF Japan Ltd.) and 0.125 parts by mass of a phosphite-based antioxidant IRGAFOS168 (tris(2,4-di-tert-butylphenyl)phosphite manufactured by BASF Japan Ltd.) were used. They were mixed at room temperature for 3 minutes by using a high-speed stirring mixer HENSCHEL MIXER (manufactured by Nippon Coke & Engineering Co., Ltd.). Then, the mixture was melt-kneaded by using a twin-screw extruder KZW-25 (product name, manufactured by Technovel Corporation) under the following conditions: the screw rotation frequency of the extruder was set to 400 rpm, and the kneading temperature under the hopper was set in stages as follows: 80° C., 120° C., and 230° C. (maintaining the temperature to the outlet of the die). The molten resin extruded from the strand die of the extruder was pulled while cooling and solidifying the resin in a cooling water bath. The strands were cut and pelletized by using a strand cutter.
[0688] The MFR of the obtained pellets was 4.5 g / 10 minutes. The obtained pellets were used to measure Ea, MT, elongational viscosity, TREF and MaxDraw. The evaluation results of each property are shown in Table 1.
[0689] [Example 2]
[0690] Polymerization was performed in the same manner as in Example 1, except that 500 mg (excluding the mass of the prepolymerized polymer) of the catalyst 1 and 0.09 NL of hydrogen were introduced. As a result, 1750 g of a polymer was obtained.
[0691] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 9.0 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0692] [Example 3]
[0693] Except that 400 mg (excluding the mass of the prepolymerized polymer) of the catalyst 1 and 0.43 NL of hydrogen were introduced, polymerization was performed in the same manner as in Example 1. As a result, 2109 g of a polymer was obtained.
[0694] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 21 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0695] [Example 4]
[0696] Polymerization was performed in the same manner as in Example 1, except that 100 mg (excluding the mass of the prepolymerized polymer) of Catalyst 1 and 1.87 NL of hydrogen were introduced, and the polymerization time was changed to 3 hours. As a result, 1960 g of a polymer was obtained.
[0697] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 32 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0698] [Example 5]
[0699] Polymerization was performed in the same manner as in Example 4, except that 160 mg (excluding the mass of the prepolymerized polymer) of Catalyst 3 was introduced instead of Catalyst 1 and 0.51 NL of hydrogen was introduced. As a result, 2026 g of a polymer was obtained.
[0700] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 1.2 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0701] [Example 6]
[0702] Polymerization was performed in the same manner as in Example 4, except that 90 mg (excluding the mass of the prepolymerized polymer) of Catalyst 3 was introduced instead of Catalyst 1 and 1.36 NL of hydrogen was introduced. As a result, 1852 g of a polymer was obtained.
[0703] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 2.7 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0704] [Comparative Example 1]
[0705] 20L autoclave is used after purging with propylene inside the tank and cooling to room temperature. Next, 18.7mL of triisobutylaluminum heptane solution (140mg / mL) and 0.68NL of hydrogen are introduced into the polymerization tank, followed by 5000g of liquid propylene. Next, the temperature inside the tank is raised to 63°C. Then, 310mg of catalyst 2 (which is the mass of the polymer not including prepolymerization) is fed into the polymerization tank under pressure by high-pressure argon to initiate polymerization, and the temperature inside the tank is quickly raised to 70°C. The temperature is maintained at 70°C, and after 1 hour from the start of polymerization, unreacted propylene is quickly purged to stop polymerization. Therefore, 2288g of propylene homopolymer is obtained.
[0706] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 3.3 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0707] [Comparative Example 2]
[0708] Except that 230 mg (excluding the mass of the prepolymerized polymer) of Catalyst 2 and 1.02 NL of hydrogen were introduced, polymerization was performed in the same manner as in Comparative Example 1. As a result, 1978 g of a polymer was obtained.
[0709] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 9.9 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0710] [Comparative Example 3]
[0711] Except that 220 mg (excluding the mass of the prepolymerized polymer) of Catalyst 2 and 1.11 NL of hydrogen were introduced, polymerization was performed in the same manner as in Comparative Example 1. As a result, 1936 g of a polymer was obtained.
[0712] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 15.0 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0713] [Comparative Example 4]
[0714] Except that 360 mg (excluding the mass of the prepolymerized polymer) of Catalyst 2 and 0.51 NL of hydrogen were introduced, polymerization was performed in the same manner as in Comparative Example 1. As a result, 1872 g of a polymer was obtained.
[0715] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 0.8 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0716] [Comparative Example 5]
[0717] Except that 200 mg (excluding the mass of the prepolymerized polymer) of the catalyst 2 and 0.94 NL of hydrogen were introduced, polymerization was performed in the same manner as in Comparative Example 1. As a result, 2000 g of a polymer was obtained.
[0718] The obtained polymer was pelletized in the same manner as in Example 1. As a result, the MFR of the obtained pellets was 40 g / 10 minutes. The results of evaluating various properties in the same manner as in Example 1 are shown in Table 1.
[0719] [Reference Example 1]: Performance evaluation of complex 1 as catalyst component (A)
[0720] (Preparation of Catalyst R1)
[0721] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (65 mL) and slurried. Next, triisobutylaluminum (25 mmol: 35 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0722] In another flask (volume 200 mL), racemic dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (0.15 mmol) synthesized in Synthesis Example 1 was dissolved in toluene (30 mL) to prepare a solution.
[0723] Triisobutylaluminum (0.60 mmol: 0.85 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, the solution was added thereto, and they were stirred at room temperature for 60 minutes.
[0724] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0725] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0726] The catalyst slurry was dried under reduced pressure for 40 minutes to obtain 29.5 g of a prepolymerized catalyst (catalyst R1). The prepolymerization ratio of the catalyst was 1.95.
[0727] (polymerization)
[0728] 20L autoclave is used after purging with propylene inside the tank and cooling to room temperature. Next, 18.7mL of triisobutylaluminum heptane solution (140mg / mL) and 0.51NL of hydrogen are introduced into the polymerization tank, followed by 5000g of liquid propylene. Next, the temperature inside the tank is raised to 63°C. Then, 300mg of catalyst R1 (which is the mass of the polymer not including prepolymerization) is fed into the polymerization tank under pressure by high-pressure argon to initiate polymerization, and the temperature inside the tank is quickly raised to 70°C. The temperature is maintained at 70°C, and after 1 hour from the start of polymerization, unreacted propylene is quickly purged to stop polymerization. Therefore, 1740g of propylene homopolymer is obtained. The resulting polymer is measured by MFR, GPC and NMR. The results are shown in Table 2.
[0729] [Reference Example 2]: Performance evaluation of complex 2 as catalyst component (A)
[0730] (Preparation of Catalyst R2)
[0731] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (66 mL) and slurried. Next, triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0732] In another flask (volume 200 mL), racemic dimethylsilylenebis(2,5-dimethyl-3-phenyl-cyclopenta[b]thienyl)hafnium dichloride (complex 2) (0.15 mmol) synthesized in Synthesis Example 2 was dissolved in toluene (30 mL) to prepare a solution.
[0733] Triisobutylaluminum (0.60 mmol: 0.85 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, the solution was added thereto, and they were stirred at room temperature for 60 minutes.
[0734] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0735] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0736] The catalyst slurry was dried under reduced pressure for 1 hour to obtain 32.0 g of a prepolymerized catalyst (catalyst R2). The prepolymerization ratio of the catalyst was 2.20.
[0737] (polymerization)
[0738] Except that 100 mg (excluding the mass of the prepolymerized polymer) of catalyst R2 was introduced instead of catalyst R1 and 1.19 NL of hydrogen was introduced, polymerization was carried out in the same manner as in Reference Example 1. As a result, 1153 g of polymer was obtained. The obtained polymer was measured by MFR, GPC and NMR. The results are shown in Table 2.
[0739] [Reference Example 3]: Performance evaluation of complex 3 as catalyst component (A)
[0740] (Preparation of Catalyst R3)
[0741] First, 10 g of the chemically treated montmorillonite obtained above was fed into a three-necked flask (volume 1 L). The chemically treated montmorillonite was mixed with heptane (66 mL) and slurried. Next, triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution of 143 mg / mL) was added to the slurry, and they were stirred for 1 hour. Then, the slurry was washed with heptane to reach a residual liquid rate of 1 / 100, thereby adjusting the total volume of the slurry to 50 mL.
[0742] In another flask (volume 200 mL), racemic dichloro[1,1′-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium (complex 3) (0.15 mmol) synthesized in Synthesis Example 3 was dissolved in toluene (30 mL) to prepare a solution.
[0743] Triisobutylaluminum (0.60 mmol: 0.85 mL of a heptane solution having a concentration of 143 mg / mL) was added to the 1 L flask containing the chemically treated montmorillonite. Then, the solution was added thereto, and they were stirred at room temperature for 60 minutes.
[0744] Then, 170 mL of heptane was added to the mixture. The slurry thus obtained was introduced into a 1 L autoclave.
[0745] After the internal temperature of the autoclave was controlled at 40° C., prepolymerization was performed while feeding propylene at a rate of 5 g / hour and maintaining the internal temperature at 40° C. for 4 hours. Then, the propylene feeding was stopped, and the remaining polymerization reaction was performed for 1 hour. After the supernatant of the catalyst slurry thus obtained was removed therefrom by decantation, triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution having a concentration of 143 mg / mL) was added to the residue thus left, and they were stirred for 5 minutes.
[0746] The catalyst slurry was dried under reduced pressure for 1 hour to obtain 31.0 g of a prepolymerized catalyst (catalyst R3). The prepolymerization ratio of the catalyst was 2.10.
[0747] (polymerization)
[0748] Except that 300 mg (excluding the mass of the prepolymerized polymer) of catalyst R3 was introduced instead of catalyst R1 and 0.51 NL of hydrogen was introduced, polymerization was carried out in the same manner as in Reference Example 1. As a result, 1570 g of polymer was obtained. The obtained polymer was measured by MFR, GPC and NMR. The results are shown in Table 2.
[0749] From the results of Reference Examples 1 to 3 shown in Table 2, the following is revealed. Complex 1 of Synthesis Example 1 can be used as a metallocene compound for obtaining the following propylene homopolymer a-1 when propylene homopolymerization of component [A-1] is carried out at 70°C: the terminal vinyl ratio (Rv) is 0.5 or more. Complex 2 of Synthesis Example 2 can be used as a metallocene compound for obtaining the following propylene homopolymer a-2 when propylene homopolymerization of component [A-2] is carried out at 70°C: the number average molecular weight (Mn) is greater than that of propylene homopolymer a-1; Rv is greater than 0.1 and less than 0.5; and the ratio of the number of copolymerized terminal vinyls forming LCB in the number of generated terminal vinyls of propylene homopolymer a-2 {LCB number / ([Vi]+LCB number)} is greater than that of propylene homopolymer a-1.
[0750] Complex 3 of Synthesis Example 3 is a metallocene compound that gives the following propylene homopolymer when propylene homopolymerization is carried out at 70°C: Although Mn is larger than that of propylene homopolymer a-1, Rv is 0.
[0751] (5) Measurement and evaluation methods
[0752] For the branched propylene polymers obtained in Examples 1 to 6 and Comparative Examples 1 to 5 and the propylene polymers obtained in Reference Examples 1 to 3, the following parameters (5-1) to (5-12) were measured and calculated by the methods described in the present specification.
[0753] (5-1) MFR was measured; further, using the measured MFR value, each value was obtained by calculating the right side of equations (1), (2) and (7).
[0754] (5-2) Mn, Mw, Mz, Mw / Mn and Mz / Mw obtained by GPC
[0755] (5-3) W1 million, W2 million, and W2 million / W1 million in the integrated molecular weight distribution curve obtained by GPC
[0756] (5-4) Mw obtained by 3D-GPC abs , g'(1 million), g'(Mw abs ) and [g'(Mw abs )-g'(1 million)]
[0757] (5-5) Ea in dynamic viscoelasticity measurement
[0758] (5-6) Pass 13 mm, amount of [2,1 bond] and amount of [1,3 bond] measured by C-NMR
[0759] (5-7) Pass 13 LCB number measured by C-NMR
[0760] (5-8) Amount of components eluted at a temperature below 40°C in the elution curve obtained by TREF (40°C soluble content in TREF)
[0761] (5-9) SHI@1.0s obtained by elongational viscosity measurement -1 and MBI
[0762] (5-10) Melt tension (MT230)
[0763] (5-11)MaxDraw
[0764] (5-12) [Vi], terminal vinyl ratio, LCB number / ([Vi] + LCB number)
[0765] (6) Evaluation results
[0766] The results of the examples, comparative examples and reference examples are shown in Table 1, Table 2, Figure 2 , Figure 4 and Figure 5 middle.
[0767] [Table 1]
[0768]
[0769] [Table 2]
[0770]
[0771] As shown in Table 1, the branched propylene polymers of Comparative Examples 1 to 5 do not have the molecular weight distribution and branching distribution specified in the present invention, and they have high melt tension. abs = 1 million, the amount of components with branches is small. Therefore, it is estimated that there are many components with extremely long relaxation times, and Ea, which is correlated with MFR, is low. As a result, it is considered that the ductility during melting is poor.
[0772] At the same time, as shown in Table 1, all the branched propylene polymers of Examples 1 to 6 satisfy characteristics (1) to (4), and they have a branched propylene structure different from the conventional structure, especially in terms of molecular weight distribution and branching distribution. In addition, for the branched propylene polymers of Examples 1 to 6, MFR is 1.2 g / 10 minutes to 32 g / 10 minutes; MT is 0.4 g to 5.3 g; and when they maintain the melt tension required for molding, MaxDraw is 112 m / minute or more and greater than 600 m / minute. As just described, the branched propylene polymers of Examples 1 to 6 are excellent in ductility when melted while maintaining the fluidity and melt tension required for molding. It is shown that the MaxDraw and MFR of the branched propylene polymers of Examples 1 to 6 satisfy the relationship represented by formula (7) and the ductility is excellent relative to the MFR.
Claims
1. A branched propylene polymer comprising propylene and 0 mol% to 11 mol% of ethylene and an α-olefin having 4 or more carbon atoms, and having the following characteristics (1) to (4): Characteristics (1): A melt flow rate (MFR) of 0.1 g / 10 min to 100 g / 10 min measured at a temperature of 230° C. and a load of 2.16 kg; Characteristic (2): the ratio Mz / Mw between the z-average molecular weight Mz and the weight-average molecular weight Mw, both obtained by gel permeation chromatography GPC, is 2.5 to 4.0; Characteristic (3): In the molecular weight distribution curve obtained by 3D-GPC, the absolute molecular weight M abs The branching index g'(1 million) at 1 million is 0.60 to 0.75; and Property (4): The flow activation energy Ea kJ / mol obtained by measuring the dynamic viscoelasticity and the MFR satisfy the following formula (1): Ea≥-12.5×log(MFR)+66 formula (1).
2. The branched propylene polymer according to claim 1, further having the following characteristics (2-2): Characteristic (2-2): In the integrated molecular weight distribution curve obtained by GPC, the ratio of the percentage of components with a molecular weight of 2 million or more, W2 million, to the percentage of components with a molecular weight of 1 million or more, W1 million, W2 million / W1 million, and MFR satisfy the following formula (2): (W2 million / W1 million)<-0.05×log(MFR)+0.34, formula (2).
3. The branched propylene polymer according to claim 1 or 2, further having the following characteristics (5) and (5-2): Feature (5): Pass 13 The meso triad fraction measured by C-NMR is 95.0% or more and less than 99.0%, and Characteristic (5-2): The amount of heterogeneous 2,1 bonds is in the range of 0 mol% to 0.30 mol%, and the amount of heterogeneous 1,3 bonds is in the range of 0 mol% to 0.25 mol%.
4. The branched propylene polymer according to claim 1 or 2, further having the following characteristics (6): Feature (6): Pass 13 The number of long chain branches measured by C-NMR is 0.1 to 0.5 per 1000 monomers.
5. The branched propylene polymer according to claim 1 or 2, further having the following characteristics (7): Characteristic (7): In the elution curve obtained by temperature-increasing elution fractionation measurement with o-dichlorobenzene, the amount of a component eluting at a temperature of 40° C. or lower is 0.1% by mass to 2.5% by mass.
6. The branched propylene polymer according to claim 1 or 2, further having the following characteristics (8): Characteristic (8): The degree of strain hardening at a strain rate dε / dt of 1.0 / sec is 0.70 to 2.
50.
7. The branched propylene polymer according to claim 1 or 2, further having the following characteristics (9): Characteristic (9): The multi-branching index is 0.20 to 1.00.