Thermosetting prepreg and manufacturing method thereof

By using different compositions of thermosetting resin compositions in the thermosetting prepreg and adjusting the curing agent distribution, the problem of taking into account the mechanical properties and operability of the thermosetting prepreg is solved, and a high-performance composite material is achieved.

CN118891314APending Publication Date: 2024-11-01TEIJIN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028615.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing thermosetting prepregs have challenges in achieving excellent mechanical properties and operability, and are difficult to take into account at the same time.

Method used

The first and second thermosetting resin compositions with different compositions are used, the first composition is impregnated in the central region of the fiber sheet, the second composition is impregnated in the outer region, and by adjusting the equivalent ratio and viscosity of the curing agent, Ensure excellent mechanical properties and operability after thermal curing.

Benefits of technology

Excellent mechanical properties and good operability of the thermosetting prepreg are achieved, and the performance of the composite material is improved, especially in terms of conductivity and viscosity of the thickness direction of the laminated body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891314A_ABST
    Figure CN118891314A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a thermosetting prepreg having good mechanical properties, in particular, good handling properties. The present invention relates to a thermosetting prepreg having: a fibrous sheet; a first thermosetting resin composition that is impregnated into a central region in the thickness direction of the fiber sheet in a cross section perpendicular to the plane direction of the fiber sheet; and a second thermosetting resin composition impregnated into an outer region in the thickness direction of the fiber sheet in a cross section perpendicular to the plane direction of the fiber sheet, and the first and second thermosetting resin compositions each contain a thermosetting resin and a curing agent, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to thermosetting prepregs and methods for manufacturing them. In particular, this disclosure relates to thermosetting prepregs that can be used to manufacture carbon fiber reinforced plastics (CFRPs) for applications such as aircraft, and methods for manufacturing them. Background Technology

[0002] Carbon fiber reinforced composites (also known as composites or CFRPs) are composed of carbon fibers as reinforcing fibers and matrix resins. They are characterized by being lightweight, high-strength, and having a high elastic modulus, and are widely used in aircraft, sports and leisure, and general industries.

[0003] In most cases, this composite material is manufactured using a prepreg that integrates carbon fibers and a matrix resin. For example, composite materials can be manufactured by laminating multiple prepregs.

[0004] Development efforts are underway to improve the properties of composite materials made from prepregs. For example, composite materials typically manufactured by laminating prepregs often include resin layers composed of a matrix resin between the layers of stacked carbon fiber layers. However, the matrix resins commonly used in composite materials often have low electrical conductivity, resulting in sometimes low conductivity in the thickness direction of the composite material.

[0005] Patent documents 1 and 2 describe the mixing of metal particles or carbon particles into the matrix resin of a composite material.

[0006] As a prepreg, there is thermosetting prepreg. Thermosetting prepreg, for example, has a composition in which a thermosetting resin such as epoxy resin is impregnated into a reinforcing fiber sheet such as carbon fiber sheet. For example, composite materials can be manufactured by laminating multiple (e.g., 24 layers) thermosetting prepregs and then performing a thermosetting treatment.

[0007] Patent Document 3 discloses a prepreg comprising: a primary prepreg consisting of reinforcing fibers and a resin composition (I) impregnated within a layer of reinforcing fibers; and a surface layer consisting of a resin composition (II) formed on one or both sides of the primary prepreg. According to Patent Document 3, the resin composition (I) comprises an epoxy resin and a thermoplastic resin, and the resin composition (II) comprises an epoxy resin and conductive particles.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent Application Publication No. 6-344519;

[0011] Patent Document 2: Japanese Patent Application Publication No. 8-34864;

[0012] Patent document 3: International Publication No. 2014 / 050896. Summary of the Invention

[0013] The problem that the invention aims to solve

[0014] Achieving excellent mechanical properties has been difficult in conventional thermosetting prepregs. Furthermore, achieving good workability in addition to excellent mechanical properties has also been challenging in conventional thermosetting prepregs.

[0015] The purpose of this disclosure is to provide thermosetting prepregs with excellent mechanical properties, and in particular, good workability, and a method for manufacturing the same.

[0016] Methods for solving problems

[0017] The above-mentioned problems can be solved by the following solutions involved in this invention:

[0018] <Option 1>

[0019] Thermosetting prepregs have the following characteristics:

[0020] Fiber sheets;

[0021] A first thermosetting resin composition, which impregnates into the central region of the fiber sheet in the thickness direction of the fiber sheet in a cross-section perpendicular to the surface direction of the fiber sheet; and

[0022] The second thermosetting resin composition is impregnated into the outer region of the fiber sheet in the thickness direction of the fiber sheet in a cross-section perpendicular to the surface direction of the fiber sheet, and

[0023] The first and second thermosetting resin compositions described above each comprise a thermosetting resin and a curing agent.

[0024] The equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0025] <Option 2>

[0026] In the thermosetting prepreg described in Scheme 1, the ratio of the thickness of the central region to the total thickness of the central region and the outer region in a cross section perpendicular to the plane of the fiber sheet is 10 to 90%.

[0027] <Option 3>

[0028] The thermosetting prepreg of Scheme 1 or 2, wherein the first and second thermosetting resin compositions further comprise a thermoplastic resin and a conductive material, respectively.

[0029] <Option 4>

[0030] The thermosetting prepreg of any one of Schemes 1 to 3, wherein the second thermosetting resin composition is impregnated into the outer region of the fiber sheet and disposed on the surface of the fiber sheet.

[0031] <Option 5>

[0032] The thermosetting prepreg of Scheme 4, wherein the second thermosetting resin composition disposed on the surface of the fiber sheet has resin particles.

[0033] <Option 6>

[0034] The thermosetting prepreg of Scheme 4 or 5, wherein the second thermosetting resin composition disposed on the surface of the fiber sheet comprises an additional conductive material.

[0035] <Option 7>

[0036] The thermosetting prepreg of any one of Schemes 1 to 6, wherein the viscosity of the first thermosetting resin composition at 50°C is higher than the viscosity of the second thermosetting resin composition at 50°C.

[0037] <Option 8>

[0038] The thermosetting prepreg of any one of Schemes 1 to 7, wherein the viscosity of the first thermosetting resin composition is 500 to 10000 Pa·s at 50°C.

[0039] The viscosity of the second thermosetting resin composition described above is 100 to 1000 Pa·s at 50°C.

[0040] <Option 9>

[0041] The thermosetting prepreg according to any one of Schemes 1 to 8, wherein the thermosetting prepreg is heat-cured at 180°C for 120 minutes,

[0042] In a cross-section perpendicular to the plane of the aforementioned fiber sheet, there exists a region where the crosslinking density of the aforementioned thermosetting resin decreases from the center of the fiber sheet in the thickness direction toward the surface.

[0043] <Option 10>

[0044] The thermosetting prepreg of any one of Schemes 1 to 9, wherein the thermosetting resin is an epoxy resin.

[0045] <Option 11>

[0046] A thermosetting prepreg laminate having a structure formed by laminating two or more thermosetting prepregs as described in any one of Schemes 1 to 10.

[0047] <Option 12>

[0048] A method for manufacturing thermosetting prepregs, comprising the following:

[0049] (a) Providing a thermosetting prepreg precursor sheet, wherein the precursor sheet has a fiber sheet and first and second thermosetting resin compositions impregnated in the fiber sheet and respectively comprising a thermosetting resin and a curing agent, wherein in a cross-section perpendicular to the surface direction of the fiber sheet, the first thermosetting resin composition impregnates a first outer region in the thickness direction of the fiber sheet, and the second thermosetting resin composition impregnates a second outer region in the thickness direction of the fiber sheet, opposite to the first outer region; and

[0050] (b) Overlap two of the above-mentioned thermosetting prepreg precursor sheets, thereby making the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet opposite to the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet.

[0051] Here, in the above-mentioned thermosetting prepreg precursor sheet, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0052] <Option 13>

[0053] A method for manufacturing thermosetting prepreg precursor sheets, comprising:

[0054] Provide fiber sheets;

[0055] A first thermosetting resin composition comprising a thermosetting resin and a curing agent is provided;

[0056] A second thermosetting resin composition comprising a thermosetting resin and a curing agent is provided;

[0057] The first thermosetting resin composition is disposed on one main surface of the aforementioned fiber sheet;

[0058] The second thermosetting resin composition is disposed on another main surface of the aforementioned fiber sheet; and

[0059] The first thermosetting resin composition and the second thermosetting resin composition are at least partially impregnated into the fiber sheet.

[0060] The equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0061] <Option 14>

[0062] The method of Scheme 13, wherein the sheet-like first thermosetting resin composition has a unit area weight (g / m²) 2 The unit area weight (g / m²) of M1 and the sheet-like second thermosetting resin composition described above 2 The ratio of M1 to M2 (M1 / M2) is 0.25 to 4.0.

[0063] <Option 15>

[0064] The method of embodiment 13 or 14, wherein the second thermosetting resin composition further comprises resin particles.

[0065] Invention Effects

[0066] According to the invention disclosed herein, thermosetting prepregs with excellent mechanical properties and methods for manufacturing the same can be provided. In particular, according to the invention disclosed herein, thermosetting prepregs with excellent mechanical properties and good workability and methods for manufacturing the same can be provided. Attached Figure Description

[0067] [ Figure 1 ] Figure 1 This shows a schematic cross-sectional view of a thermosetting prepreg according to one embodiment of the present disclosure.

[0068] [ Figure 2 ] Figure 2 This diagram shows a conceptual illustration of one embodiment of a method for manufacturing the thermosetting prepregs disclosed herein.

[0069] [ Figure 3 ] Figure 3 A conceptual diagram showing one embodiment of a method for manufacturing a thermosetting prepreg precursor sheet as disclosed herein. Detailed Implementation

[0070] The thermosetting prepregs disclosed herein have the following characteristics:

[0071] Fiber sheets;

[0072] A first thermosetting resin composition, which impregnates into the central region of the fiber sheet in the thickness direction of a cross section perpendicular to the surface direction of the fiber sheet; and

[0073] The second thermosetting resin composition is impregnated in a cross-section perpendicular to the surface direction of the fiber sheet into the outer region of the fiber sheet in the thickness direction.

[0074] Furthermore, the first and second thermosetting resin compositions each comprise a thermosetting resin and a curing agent.

[0075] The equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0076] The thermosetting prepregs involved in this invention will be specifically described below with reference to the accompanying drawings. The drawings are schematic diagrams used to help understand the invention, are not to scale, and do not limit the invention.

[0077] Figure 1 This is a schematic cross-sectional schematic diagram of one embodiment of the thermosetting prepreg involved in this disclosure, showing the cross-section of the thermosetting prepreg when cut with a cross section perpendicular to the surface direction of the fiber sheet. Figure 1 The T indicates the thickness direction of the thermosetting prepreg.

[0078] Figure 1 The thermosetting prepreg 100 described herein includes a fiber sheet 110. The fiber sheet 110 is, in particular, a carbon fiber sheet. A first thermosetting resin composition 112 is impregnated into the central region (B) of the fiber sheet 110 in the thickness direction. The first thermosetting resin composition 112 includes a thermosetting resin and a curing agent, and optionally contains a thermoplastic resin and a conductive material.

[0079] Additionally, the thermosetting prepreg 100 has a second thermosetting resin composition 122 impregnated into the outer region (A) in the thickness direction of the fiber sheet 110. The second thermosetting resin composition 122 contains a thermosetting resin and a curing agent, and optionally also contains a thermoplastic resin and a conductive material.

[0080] exist Figure 1 In the thermosetting prepreg 100 involved, the second thermosetting resin composition 122 is disposed on the surface of the fiber sheet 110. Figure 1 In this process, a second thermosetting resin composition 122 disposed on the surface forms a resin layer 120. Figure 1 The resin layer 120 has resin particles 150.

[0081] exist Figure 1 In the thermosetting prepreg 100, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition. Therefore, in the thermosetting prepreg 100, the equivalent ratio of the curing agent in the central region (B) of the thermosetting prepreg is greater than the equivalent ratio of the curing agent in the outer region (A).

[0082] It should be noted that the "equivalent ratio" of the curing agent in the thermosetting resin composition can be calculated using the following formula 1:

[0083] Equivalent ratio of curing agent = (total moles of active hydrogen in curing agent) / (total moles of polymerizable groups in thermosetting resin) ... (Equation 1)

[0084] Especially when the thermosetting resin is epoxy resin, the equivalent ratio of the curing agent can be calculated using the following formula 1':

[0085] Equivalent ratio of curing agent = (total moles of active hydrogen in curing agent) / (total moles of epoxy groups in epoxy resin) ... (Equation 1')

[0086] Although not intended to be theoretically limited, it is believed that when the thermosetting prepregs involved in this disclosure are subjected to thermosetting treatment as described above, a higher crosslinking density of the thermosetting resin can be obtained inside the fiber sheet, thereby improving the elasticity of the matrix resin and resulting in improved mechanical properties.

[0087] In particular, in the thermosetting prepreg 100, in a cross section perpendicular to the plane of the fiber sheet, the ratio of the thickness of the central region to the total thickness of the central and outer regions is 10 to 90%.

[0088] In one embodiment of this disclosure, at least one of the first thermosetting resin composition 112 and the second thermosetting resin composition 122 further comprises a thermoplastic resin and / or a conductive material (particularly conductive particles). The inclusion of a conductive material further improves the conductivity of the thermosetting prepreg. Additionally, the inclusion of a thermoplastic resin further improves the workability of the thermosetting prepreg. It should be noted that the workability of the thermosetting prepreg specifically refers to its workability when automatically stacking multiple thermosetting prepregs (automatic stacking capability).

[0089] In another embodiment of this disclosure, the viscosity of the first thermosetting resin composition at 50°C may be higher than that of the second thermosetting resin composition at 50°C. In this case, particularly good tack is considered to be obtained, and particularly good operability (especially automatic lamination) of the thermosetting prepreg can be achieved.

[0090] In particular, the viscosity of the first thermosetting resin composition at 50°C is 500–10000 Pa·s, and the viscosity of the second thermosetting resin composition at 50°C is 100–1000 Pa·s.

[0091] There are no particular limitations on the manufacturing method of the thermosetting prepregs involved in this disclosure, and in particular, they can be manufactured by the manufacturing method of the thermosetting prepregs involved in this disclosure described below.

[0092] The method for manufacturing the thermosetting prepreg disclosed herein includes the following steps (a) and (b):

[0093] (a) Providing a thermosetting prepreg precursor sheet, wherein the precursor sheet has a fiber sheet and first and second thermosetting resin compositions impregnated in the fiber sheet and respectively comprising a thermosetting resin and a curing agent, wherein in a cross-section perpendicular to the surface direction of the fiber sheet, the first thermosetting resin composition impregnates a first outer region in the thickness direction of the fiber sheet, and the second thermosetting resin composition impregnates a second outer region in the thickness direction of the fiber sheet opposite to the first outer region; and

[0094] (b) Overlap two thermosetting prepreg precursor sheets such that the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet is opposite to the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet.

[0095] Here, in the thermosetting prepreg precursor sheet, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0096] Typically, in prepregs, the required functions of the fiber sheet portion and the resin layer portion differ, and therefore their required physical properties also differ. In previous methods, achieving such site-specific optimized physical properties was not easy.

[0097] In contrast, the method for manufacturing thermosetting prepregs disclosed herein uses a precursor sheet comprising multiple resin compositions with different compositions. That is, according to the manufacturing method disclosed herein, thermosetting prepregs are manufactured using precursor sheets impregnated with multiple resin compositions with different compositions, thereby enabling the production of thermosetting prepregs with site-specific optimized physical properties.

[0098] Furthermore, in conventional methods for manufacturing thermosetting prepregs, when the resin composition is impregnated into the fiber sheet, the degree of impregnation of the resin composition into the central portion of the fiber sheet is reduced due to the impregnation properties of the resin composition. In particular, when the degree of curing agent impregnation in the central region of the fiber sheet is low, the mechanical properties of the fiber sheet are reduced.

[0099] In contrast, in the method described above in this disclosure, a thermosetting prepreg is manufactured by overlapping two thermosetting prepreg precursor sheets, and at this time, the outer regions of the resin composition having a larger equivalent amount of curing agent in the two outer regions in the thickness direction of the precursor sheets overlap each other. According to this method, the amount of curing agent distributed in the center of the resulting thermosetting prepreg can be increased.

[0100] Figure 2 This invention conceptually illustrates a manufacturing method involved in one embodiment of the present disclosure. Figure 2The thermosetting prepreg precursor sheet 200 has a fiber sheet 210. A first outer region (B') in the thickness direction of the fiber sheet 210 is impregnated with a first thermosetting resin composition 212. Additionally, a second outer region (A') in the thickness direction of the fiber sheet 210 is impregnated with a second thermosetting resin composition 222. It should be noted that in... Figure 2 In this embodiment, a second thermosetting resin composition 222 is disposed on the main surface of the fiber sheet 210 to form a resin layer 220. The resin layer 220 has resin particles 250. Figure 2 In the thermosetting prepreg precursor sheet 200, the equivalent ratio of the curing agent in the first thermosetting resin composition 212 is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition 222.

[0101] exist Figure 2 In the described method, two thermosetting prepreg precursor sheets 200a and 200b are further overlapped, thereby positioning the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet 200a opposite to the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet 200b. Particularly preferably, the surfaces adjacent to the first outer regions are brought into direct contact with each other or via a resin composition. Preferably, the two thermosetting prepreg precursor sheets 200a and 200b may be overlapped, followed by a process for integrating them, such as heating and pressurizing.

[0102] According to the manufacturing method disclosed herein, a thermosetting prepreg 100 can be obtained in which the amount of curing agent in the central region of the thickness direction in a cross section perpendicular to the surface direction of the sheet is greater than the amount of curing agent in the outer region of the thickness direction.

[0103] There are no particular limitations on the method for manufacturing thermosetting prepreg precursor sheets, and in particular, they can be manufactured by the method for manufacturing thermosetting prepreg precursor sheets according to this disclosure, which includes the following steps:

[0104] Provide fiber sheets;

[0105] A first thermosetting resin composition comprising a thermosetting resin and a curing agent is provided;

[0106] A second thermosetting resin composition comprising a thermosetting resin and a curing agent is provided;

[0107] A first thermosetting resin composition is disposed on one main surface of the fiber sheet;

[0108] A second thermosetting resin composition is disposed on another main surface of the fiber sheet; and

[0109] The first thermosetting resin composition and the second thermosetting resin composition are at least partially impregnated into the fiber sheet.

[0110] Here, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0111] Figure 3 This is a conceptual diagram illustrating one embodiment of a method for manufacturing a thermosetting prepreg precursor sheet as disclosed herein.

[0112] exist Figure 3 In the method involved, a fiber sheet 310 having a first main surface 314 and a second main surface 316 is provided. A sheet 320 formed of a first thermosetting resin composition 322 is disposed on the first main surface 314, and a sheet 330 formed of a second thermosetting resin composition 332 is disposed on the second main surface 316. Here, the equivalent ratio of curing agent contained in the first thermosetting resin composition 322 is greater than the equivalent ratio of curing agent contained in the second thermosetting resin composition 332. It should be noted that... Figure 3 The sheet 330 contains resin particles 350.

[0113] Moreover, for the intermediate laminate 340 formed by such operation, heat and / or pressure can be applied, for example, using hot rollers, so that the resin compositions 322 and 332 can each be at least partially impregnated into the fiber sheet 310 to obtain a thermosetting prepreg precursor sheet 200.

[0114] According to this method, the first thermosetting resin composition and the second thermosetting resin composition can be simultaneously impregnated into the fiber sheet. Therefore, compared with the case where the first thermosetting resin composition is impregnated into the fiber sheet first and then the second thermosetting resin composition is impregnated, the impregnation of the second thermosetting resin composition into the fiber sheet can be further improved.

[0115] The following provides a detailed description of the embodiments and constituent elements of the present invention.

[0116] Thermosetting Prepregs

[0117] The thermosetting prepreg disclosed herein comprises fiber sheets, a first thermosetting resin composition, and a second thermosetting resin composition.

[0118] Regarding this disclosure, the fiber area weight of the thermosetting prepreg can be, for example, 50 to 1000 g / m². 2 100~800g / m 2 Especially 200-600g / m 2 The thickness of thermosetting prepregs can be, for example, 0.02 mm to 3.6 mm, 0.04 mm to 2.9 mm, or 0.08 mm to 2.2 mm.

[0119] <Fiber Sheets>

[0120] The fiber sheets contained in the thermosetting prepregs disclosed herein are particularly reinforced fiber sheets composed of reinforcing fibers. The reinforced fiber sheets are preferably carbon fiber sheets.

[0121] Examples of reinforcing fibers include: carbon fiber, glass fiber, aramid fiber, silicon carbide fiber, polyester fiber, ceramic fiber, alumina fiber, boron fiber, metal fiber, mineral fiber, rock fiber, and slag fiber. Among these reinforcing fibers, carbon fiber, glass fiber, and aramid fiber are preferred, and carbon fiber that provides a composite material with good relative strength, relative elastic modulus, lightweight, and high strength is even more preferred. Among carbon fibers, polyacrylonitrile (PAN) based carbon fibers with excellent tensile strength are particularly preferred.

[0122] When using carbon fiber as the reinforcing fiber, its tensile modulus is preferably 170 GPa to 600 GPa, particularly preferably 220 GPa to 450 GPa. Furthermore, the tensile strength is preferably 3920 MPa or higher. There is no particular limitation on the upper limit of the tensile strength; for example, it can be below 10000 MPa. By using such carbon fiber, the mechanical properties of the composite material can be improved. It should be noted that the tensile strength and tensile modulus of the carbon fiber can be measured according to standard JIS R 7608.

[0123] Examples of fiber sheets include: sheets formed by pulling multiple fibers (especially reinforcing fibers) in one direction, two-way fabrics such as plain or twill fabrics, multi-axial fabrics, non-woven fabrics, pads, braided tapes, knitted fabrics, and paper made by papermaking fibers (especially reinforcing fibers).

[0124] The thickness of the fiber sheet can be 0.02–3.6 mm, 0.04–2.9 mm, or 0.08–2.2 mm. The weight per unit area of ​​the fiber sheet can be 50–1000 g / m². 2 Preferred concentration: 100–800 g / m 2 More preferably 200-600g / m 2 The distance between fibers in the fiber sheet is preferably less than 10 μm.

[0125] The content of fiber sheet in the thermosetting prepreg is preferably 40-80% by mass, particularly 45-75% by mass, and even more particularly 50-70% by mass, relative to the thermosetting prepreg as a whole.

[0126] <Resin Composition>

[0127] The fiber sheet is impregnated with a first thermosetting resin composition in its central region in the thickness direction, and with a second thermosetting resin composition in its outer region in the thickness direction.

[0128] (Central area and outer area)

[0129] In one embodiment of this disclosure, in a cross-section perpendicular to the plane of the fiber sheet, the thickness of the central region is 10% to 90% of the total thickness of the central and outer regions. Typically, the fiber sheet has two main surfaces, and the outer regions of the fiber sheet are particularly those extending along the two main surfaces of the fiber sheet respectively.

[0130] (Viscosity)

[0131] Preferably, the viscosity (V1 (Pa·s) of the first thermosetting resin composition at 50°C is higher than the viscosity (V2 (Pa·s) of the second thermosetting resin composition at 50°C), and in particular, the difference in their viscosities (V1-V2) is 10 or more, 25 or more, 50 or more, 75 or more, 100 or more, 150 or more, 200 or more, 250 or more, 300 or more, 400 or more, or 500 or more. The upper limit of the viscosity difference (V1-V2) can be, for example, 3000 or less, 2600 or less, 2000 or less, 1500 or less, 1000 or less, or 750 or less.

[0132] The viscosity of the first thermosetting resin composition at 50°C is preferably 500–10000 Pa·s or 550–5000 Pa·s, more preferably 600–3000 Pa·s or 600–2000 Pa·s, further preferably 650–1500 Pa·s or 650–1000 Pa·s, and most preferably 700–900 Pa·s. When the viscosity of the first thermosetting resin composition at 50°C is within this range, particularly good impregnation of the resin composition in fiber sheets can be obtained.

[0133] The viscosity of the second thermosetting resin composition at 50°C is preferably 100–1250 Pa·s, 100–1000 Pa·s, or 200–1000 Pa·s, more preferably 400–800 Pa·s, and even more preferably 500–750 Pa·s. When the viscosity of the second thermosetting resin composition at 50°C is within this range, particularly good impregnation of the resin composition in fiber sheets can be obtained, and in addition, particularly good workability of the thermosetting prepreg can be obtained.

[0134] Viscosity can be obtained from the temperature-viscosity profile measured using a rheometer.

[0135] The viscosity of the thermosetting resin composition can be adjusted by selecting the amount and / or type of thermosetting resin and / or curing agent contained in the thermosetting resin composition, and can also be adjusted by selecting the amount and / or type of thermoplastic resin, resin particles and / or conductive material contained herein at will.

[0136] The first thermosetting resin composition and the second thermosetting resin composition each comprise at least a thermosetting resin and a curing agent. These resin compositions may further comprise a thermoplastic resin and / or a conductive material.

[0137] (Thermosetting resin)

[0138] Thermosetting resins can be cross-linked by heating in the presence of a curing agent to form a three-dimensional molecular structure (e.g., a mesh structure). Thermosetting resins may contain heat-curable monomers and / or oligomers, and / or prepolymers. Examples of thermosetting resins include epoxy resins and polyurethane resins, especially epoxy resins. A single thermosetting resin may be used alone, or two or more may be used in combination.

[0139] Epoxy resins crosslink through a curing reaction with a curing agent, forming a network structure. Examples of epoxy resins include: conventionally known epoxy resins, particularly epoxy resins with aromatic groups within the molecule, and especially difunctional or trifunctional epoxy resins having either a glycidylamine structure or a glycidyl ether structure. Alicyclic epoxy resins can also be listed.

[0140] Examples of epoxy resins with a glycidylamine structure include: various isomers of N,N,N',N'-tetraglycidyldiaminodiphenylmethane, N,N,O-triglycidyl-p-aminophenol, N,N,O-triglycidyl-m-aminophenol, N,N,O-triglycidyl-3-methyl-4-aminophenol, and triglycidylaminocresol.

[0141] Examples of epoxy resins with a glycidyl ether structure include: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenolic varnish type epoxy resin, and cresol varnish type epoxy resin.

[0142] These epoxy resins may have non-reactive substituents for aromatic ring structures, etc., as needed. Examples of such non-reactive substituents include: alkyl groups such as methyl, ethyl, and isopropyl; aromatic groups such as phenyl; alkoxy groups; aralkyl groups; and halogen groups (chlorine, bromine, etc.).

[0143] Examples of trifunctional epoxy resins include: N,N,O-triglycidyl-p-aminophenol and N,N,O-triglycidyl-m-aminophenol.

[0144] These epoxy resins can be used alone or in combination of two or more. It should be noted that, for example, a so-called B-stage epoxy resin that has been pre-reacted with a curing agent or the like can also be used. When either the first thermosetting resin composition or the second thermosetting resin composition contains an epoxy resin as a thermosetting resin, they can be the same or different from each other.

[0145] Thermosetting resins can impart good mechanical properties and viscosity to thermosetting prepregs.

[0146] (Curing agent)

[0147] Curing agents, particularly those for thermosetting resins, such as epoxy resins or polyurethane resins, are used. Examples of curing agents for epoxy resins include dicyandiamide, various isomers of aromatic amine curing agents, and aminobenzoic acid esters. A single curing agent may be used, or two or more may be used in combination. Furthermore, the first thermosetting resin composition and the second thermosetting resin composition may have the same curing agent, or they may have different curing agents.

[0148] Dicyandiamide is preferred due to its excellent storage stability in prepregs. Furthermore, from the viewpoint of providing cured products with high heat resistance, aromatic diamine compounds such as 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, and 4,4'-diaminodiphenylmethane, and their derivatives with non-reactive substituents, are particularly preferred. Examples of non-reactive substituents include: alkyl groups such as methyl, ethyl, and isopropyl; aromatic groups such as phenyl; alkoxy groups; aralkyl groups; and halogen groups (chlorine, bromine, etc.).

[0149] Examples of aminobenzoic esters include: trimethylene glycol di-p-aminobenzoate and neopentyl glycol di-p-aminobenzoate. When using them as curing agents, the heat resistance of the composite material is sometimes poor; on the other hand, composite materials with particularly excellent tensile elongation can sometimes be obtained.

[0150] Thermosetting resins and curing agents can improve the mechanical properties (especially elastic modulus and strength) and / or heat resistance of the matrix resin of thermosetting prepregs.

[0151] (Equivalent ratio)

[0152] The equivalent ratio of the curing agent in the first thermosetting resin composition is preferably 0.70 to 1.00, more preferably 0.75 to 0.90. When the equivalent ratio of the curing agent is within this range, particularly good workability of the thermosetting prepreg and physical properties (especially mechanical properties) of the composite material formed from the thermosetting prepreg can be obtained.

[0153] The equivalent ratio of the curing agent in the second thermosetting resin composition is preferably 0.50 to 0.90, more preferably 0.60 to 0.80. When the equivalent ratio of the curing agent is within this range, particularly good workability of the thermosetting prepreg and physical properties (especially mechanical properties) of the composite material formed from the thermosetting prepreg can be obtained.

[0154] The difference (E1-E2) between the equivalent ratio (E1) of the curing agent in the first thermosetting resin composition and the equivalent ratio (E2) of the curing agent in the second thermosetting resin composition may be 0.01 or more, 0.05 or more, or 0.10 or more, and / or may be 1.0 or less, 0.50 or less, 0.40 or less, 0.30 or less, 0.20 or less, 0.18 or less, or 0.16 or less.

[0155] The content of curing agent in the thermosetting resin composition may be 5-70 parts by weight, 10-60 parts by weight, 20-50 parts by weight, or 30-45 parts by weight relative to 100 parts by weight of thermosetting resin.

[0156] (Crosslink density)

[0157] In particular, when the thermosetting prepreg disclosed herein is heat-cured at 180°C for 120 minutes, in a cross section perpendicular to the surface direction of the fiber sheet, there exists a region where the crosslinking density of the aforementioned thermosetting resin decreases from the center of the fiber sheet in the thickness direction toward the surface.

[0158] Crosslinking density (ρ) of thermosetting resin in a cross section perpendicular to the surface direction of the fiber sheet crosslink (Unit: mol / m) 3 The glass transition temperature (Tg) of the cured resin composition can be determined by the rubber state formula shown in equation (2) after measuring the glass transition temperature (Tg) based on DMA (Dynamic Viscoelasticity Measurement).

[0159] Ρ crosslink =E' / 3φRT Equation (2)

[0160] In equation (2), E' represents the energy storage elastic modulus at Tg+50℃ (unit: Pa), φ represents the pre-coefficient (here, φ=1 (unit: dimensionless)), R represents the body constant (8.31J / K·mol), and T represents the temperature at Tg+50℃ (unit: K).

[0161] DMA was measured using a dynamic viscoelasticity measuring device, such as the Rheogel-4000 (manufactured by UBM Corporation), under the conditions of double-support bending mode, strain amplitude of 5 μm, heating rate of 5 °C / min, air, and frequency of 1 Hz. The ONSET of the obtained energy storage modulus was taken as Tg.

[0162] (Thermoplastic resin)

[0163] Thermoplastic resin is preferably a thermoplastic resin that is soluble relative to thermosetting resin. Thermoplastic resin is particularly epoxy-soluble thermoplastic resin. It should be noted that, in addition to containing soluble thermoplastic resin (particularly epoxy-soluble thermoplastic resin), the resin composition may also contain a composition of insoluble thermoplastic resin (particularly epoxy-insoluble thermoplastic resin) that is insoluble relative to thermosetting resin. One type of thermoplastic resin may be used alone, or two or more types may be used in combination.

[0164] Thermoplastic resins can improve the impregnation of thermosetting resin compositions in fiber sheets. Additionally, thermoplastic resins can increase the tackiness of thermosetting prepregs. Furthermore, thermoplastic resins can improve the mechanical properties (especially toughness) of the matrix resin in thermosetting prepregs.

[0165] There is no particular limitation on the amount of thermoplastic resin in the resin composition, and it can be set according to the desired viscosity of the thermosetting resin composition, etc. For example, the amount of thermoplastic resin in the first and second thermosetting resin compositions can be 1 to 60 parts by weight relative to 100 parts by weight of thermosetting resin (especially epoxy resin), and more particularly 2 to 50 parts by weight, 5 to 40 parts by weight, 10 to 30 parts by weight, or 15 to 25 parts by weight, respectively.

[0166] In one embodiment covered in this disclosure,

[0167] The first thermosetting resin composition may contain 1 to 50 parts by weight, 2 to 40 parts by weight, 5 to 30 parts by weight, or 10 to 25 parts by weight of a soluble thermoplastic resin (especially an epoxy resin-soluble thermoplastic resin) relative to 100 parts by weight of a thermosetting resin (especially an epoxy resin), and / or

[0168] The second thermosetting resin composition may contain, relative to 100 parts by weight, 1 to 50 parts by weight, 2 to 40 parts by weight, 5 to 30 parts by weight, or 10 to 25 parts by weight of a soluble thermoplastic resin (especially epoxy resin soluble thermoplastic resin) and 1 to 50 parts by weight, 2 to 40 parts by weight, 5 to 30 parts by weight, 8 to 25 parts by weight, or 10 to 20 parts by weight of an insoluble thermoplastic resin composition (especially epoxy resin insoluble thermoplastic resin composition).

[0169] (Epoxy resin soluble thermoplastic resin)

[0170] Epoxy-soluble thermoplastic resins are thermoplastic resins that can be partially or wholly dissolved in epoxy resins by heating or the like. Preferably, the epoxy-soluble thermoplastic resin is a resin that dissolves in epoxy resins in 80% or more by mass at 190°C. Examples of epoxy-soluble thermoplastic resins include: polyethersulfone, polysulfone, polyetherimide, and polycarbonate. These can be used alone or in combination of two or more. Insoluble thermoplastic resin compositions (epoxy-insoluble thermoplastic resin compositions) are described later.

[0171] There are no particular limitations on the form of the epoxy resin-soluble thermoplastic resin. It should be noted that, especially in resin compositions used in the manufacture of thermosetting prepregs, the epoxy resin-soluble thermoplastic resin is preferably in particulate form, preferably with an average particle size of 1–50 μm, particularly 3–30 μm. It should be noted that the average particle size of the particulate thermoplastic resin can be measured using a laser diffraction / scattering particle size distribution measuring device.

[0172] When both the first thermosetting resin composition and the second thermosetting resin composition contain thermoplastic resin, they may be the same as each other or they may be different from each other.

[0173] (Conductive materials)

[0174] Conductive materials can improve the conductivity of thermosetting prepregs by being present in fiber sheets, especially in resin layers.

[0175] The conductive material is any particle that functions as a conductor with good conductivity, and there are no particular limitations. Preferably, it is a material that can be dispersed in the resin composition and can improve the conductivity of the thermosetting prepreg.

[0176] Conductive materials, especially conductive particles. The conductive particles preferably have a volume resistivity of 10⁻¹⁰ to 10⁻¹⁰. -9 Ωcm, more preferably 1 to 10 -9 Ωcm, preferably 10 -1 ~10 -9 Ωcm particles.

[0177] Examples of conductive particles include: conductive polymer particles, carbon particles, metal particles, coated conductive particles, and carbon fiber particles. These can be used individually or in combination.

[0178] Examples of conductive polymer particles include: polyacetylene particles, polyaniline particles, polypyrrole particles, polythiophene particles, polyisothioindene particles, and polyethylene dioxythiophene particles.

[0179] Examples of carbon particles include: carbon black, carbon nanotubes (CNTs), carbon nanostructures (CNS), carbon nanofibers, expanded graphite, flake graphite, graphite powder, graphite particles, graphene sheets, and ground carbon fibers. Examples of ground carbon fibers include: ground fibers of PAN-based carbon fibers, pitch-based carbon fibers, and phenol-based carbon fibers. Among these, ground fibers of pitch-based carbon fibers are preferred. The carbon fiber content of the ground carbon fibers is preferably 94% by mass or more.

[0180] There are no particular limitations on the metal particles. When carbon fiber is used as the reinforcing fiber, from the viewpoint of preventing corrosion caused by the potential difference with the carbon fiber, particles of platinum, gold, silver, copper, tin, nickel, titanium, cobalt, zinc, iron, chromium, and aluminum, particles of alloys with these metals as the main components, tin oxide, indium oxide, and indium tin oxide (ITO) are preferred. Among these, from the viewpoint of exhibiting high conductivity and stability, particles of platinum, gold, silver, copper, tin, nickel, and titanium, and particles of alloys with these metals as the main components are more preferred, and particles of silver, copper, and nickel are particularly preferred.

[0181] Examples of preferred conductive particles include carbon nanotubes, carbon nanostructures, carbon black, ground carbon fibers, and silver nanoparticles.

[0182] The conductive material preferably has a size that allows it to diffuse into the fiber sheet as the resin composition is impregnated. The conductive material is preferably granular (i.e., conductive particles), for example having an average particle size of 1–1000 nm or 1–500 nm, preferably 2–200 nm, 3–100 nm, 4–50 nm or 5–25 nm.

[0183] Regarding conductive particles with smaller particle sizes (e.g., less than 1 μm), it is believed that the conductive particles are dispersed in both the fiber sheet and the resin layer, which can further improve the conductivity of the composite material formed from the prepreg.

[0184] The average particle size of conductive materials refers to the 50% particle size of the particle size distribution measured using a laser diffraction / scattering particle size distribution measuring device (D). 50 The value of ).

[0185] The content of conductive material (especially conductive particles) can be 0.01 to 10 parts by weight, preferably 0.05 to 5 parts by weight, and more preferably 0.10 to 1 part by weight, relative to 100 parts by weight of thermosetting resin (especially epoxy resin) contained in the resin composition. When it is 0.01 parts by weight or more, the effect of improving the conductivity of the prepreg and composite material becomes particularly good. When it is 10 parts by weight or less, a significant increase in the viscosity of the resin composition can be prevented, ensuring good workability of the prepreg.

[0186] When both the first thermosetting resin composition and the second thermosetting resin composition contain conductive materials, they may be the same as each other or they may be different from each other.

[0187] (Additional conductive material)

[0188] In addition to the conductive material described above, the thermosetting prepreg may also have an additional conductive material. This additional conductive material is particularly intended to be present in a second thermosetting resin composition (particularly the resin layer described below) present on the surface of the fiber sheet. In other words, in one embodiment of this disclosure, the second thermosetting resin composition disposed on the surface of the fiber sheet comprises an additional conductive material.

[0189] Examples of additional conductive materials include: carbon fiber, pitch-carbon fiber, ground fiber (especially carbon ground fiber), and silver aggregates. These can be used alone or in combination.

[0190] The added conductive material preferably has an average length of 1 μm or more, more preferably 1.5 μm or more, more preferably 2 μm or more, and particularly preferably 4 μm or more. There is no particular upper limit to the average length of the added conductive material; for example, it can be less than 10 mm, less than 1 mm, less than 300 μm, less than 200 μm, or less than 100 μm. When the added conductive material has such a length, it is difficult for it to penetrate into the fiber sheet, and as a result, it tends to remain on the surface of the fiber sheet (especially in the resin layer). The added conductive material present on the surface of the fiber sheet (especially in the resin layer) can further improve the overall conductivity of the thermosetting prepreg.

[0191] The average length of the added conductive material can be calculated by measuring the lengths of more than 30 pieces of the added conductive material in images obtained using an electron microscope or optical microscope, and averaging the measurements. It should be noted that if the added conductive material is granular, its average diameter or average particle size can be used as the average length.

[0192] When both the first thermosetting resin composition and the second thermosetting resin composition contain additional conductive material, they may be the same as each other or different from each other.

[0193] (Resin layer)

[0194] In one embodiment of the thermosetting prepreg disclosed herein, a second thermosetting resin composition is impregnated into an outer region of the fiber sheet and disposed on the surface of the fiber sheet. In particular, the second thermosetting resin composition forms a resin layer (surface resin layer) on the surface of the fiber sheet.

[0195] The resin layer is preferably laminated on the main surface of the fiber sheet, and more preferably directly laminated on the main surface of the fiber sheet.

[0196] The thickness of the resin layer is preferably 5–50 μm, particularly 10–40 μm. With a thickness of 5 μm or more, thermosetting prepregs with particularly good adhesion are sometimes obtained. With a thickness of 50 μm or less, thermosetting prepregs with particularly good workability are sometimes obtained, and in addition, particularly good moldability can be ensured when manufacturing composite materials.

[0197] (Resin particles)

[0198] The second thermoplastic resin composition (particularly the resin layer) disposed on the surface of the fiber sheet may contain resin particles. The resin particles are preferably dispersed within the resin layer. These resin particles, present in the resin layer between the fiber sheets in a laminate made by laminating thermosetting prepregs, are also specifically referred to as "interlaminar particles."

[0199] The resin particles contained in the resin layer have the effect of improving the interlaminar toughness of composite materials formed from thermosetting prepregs (especially carbon fiber reinforced composites).

[0200] The resin particles contained in the resin layer may be composed of thermoplastic resin. Preferably, the resin particles are insoluble relative to thermosetting resin, and in particular, are composed of epoxy-insoluble thermoplastic resin.

[0201] (Epoxy resin insoluble thermoplastic resin)

[0202] Insoluble epoxy resins are thermoplastic resins that are substantially insoluble in epoxy resins at or below the temperature at which the composite material is molded. Specifically, they refer to thermoplastic resins whose particle size does not change when resin particles are added to epoxy resin and stirred at the temperature at which the composite material is formed. It should be noted that the typical molding temperature for composite materials is 100–190°C.

[0203] Examples of epoxy-insoluble thermoplastic resins include: polyamides, polyacetals, polyphenylene ethers, polyphenylene sulfides, polyesters, polyamide-imides, polyimides, polyetherketones, polyetheretherketones, polyethylene naphthalate, polyether nitrile, and polybenzimidazole. Among these, polyamides, polyamide-imides, and polyimides are preferred due to their high toughness and heat resistance. These can be used alone or in combination of two or more. Furthermore, copolymers of these resins can also be used.

[0204] In particular, amorphous polyimides or polyamides such as Nylon 6 (registered trademark) (a polyamide obtained through the ring-opening polycondensation of caprolactam), Nylon 12 (registered trademark) (a polyamide obtained through the ring-opening polycondensation of laurolactam), and amorphous Nylon (registered trademark) can be used. By using these polyamides, it is possible to obtain composite materials with particularly good heat resistance.

[0205] The average particle size of the resin particles contained in the resin layer is preferably 5 to 50 μm, particularly 10 to 40 μm.

[0206] The average particle size of resin particles can be measured using a laser diffraction / scattering particle size distribution measuring device.

[0207] (Other ingredients)

[0208] The thermosetting resin composition may contain other components as long as it does not impair the purpose and effect of the present invention. Examples of such other components include: amine compounds such as tertiary amines and imidazoles, phosphorus compounds such as phosphine and phosphonium, curing accelerators such as N,N-dimethylurea derivatives, reactive diluents, fillers, antioxidants, flame retardants, pigments, and various other additives. These other components are preferably 5% by mass or less or 1% by mass or less relative to the thermosetting resin composition.

[0209] <Polymer Membrane>

[0210] The thermosetting prepregs disclosed herein may have release paper or polymer film, such as polyethylene film, on one or both sides. The release paper or polymer film may serve to protect the thermosetting prepreg. The release paper or polymer film may be removed when manufacturing laminates (especially fiber-reinforced composites) from the thermosetting prepreg.

[0211] <Layered Body>

[0212] The thermosetting prepregs disclosed herein can be laminated by performing arbitrary thermosetting treatment to form a laminate. This laminate is particularly a fiber-reinforced composite material, and more particularly a carbon fiber-reinforced composite material. The laminate (thermosetting prepreg laminate) has a structure formed by laminating two or more thermosetting prepregs according to the present invention. The number of layers of the thermosetting prepreg forming this laminate can be, for example, 2 to 200, 5 to 100, or 10 to 50.

[0213] The laminate can be sheet-like, for example, it can have a thickness of 1mm to 100mm, 2mm to 50mm, 3mm to 25mm or 4mm to 10mm.

[0214] Such laminates can be manufactured by methods known in the past, such as manual lamination, automated tape lamination (ATL), automated fiber preparation, vacuum bagging, autoclave curing, curing other than autoclave curing, fluid-assisted processing, pressure-supported processes, matching mold processes, simple pressure curing, pressure cooker curing, and continuous manual pressurization.

[0215] Specifically, for example, the laminate (especially fiber-reinforced composite material) can be formed by laminating multiple thermosetting prepregs involved in the present invention, pressurizing them to 0.2 to 1.0 MPa in an autoclave, and heating them at 150 to 204°C for 1 to 8 hours.

[0216] The laminates (especially fiber-reinforced composites) involved in this invention preferably have a thickness-direction conductivity of 3.5 kΩ·cm or less, more preferably 0.3 kΩ·cm or less, and particularly preferably 0.2 kΩ·cm or less, based on the measurement method described in the examples. There is no particular limitation on the lower limit of the thickness-direction conductivity; for example, it can be 0.1 Ω·cm or more, or 1.0 Ω·cm or more.

[0217] Manufacturing Method of Thermosetting Prepregs

[0218] There are no particular limitations on the method for manufacturing the thermosetting prepregs involved in this disclosure. The thermosetting prepregs involved in this disclosure can be manufactured, for example, by manufacturing thermosetting prepreg precursor sheets according to the manufacturing method described below, and by overlapping the thermosetting prepreg precursor sheets.

[0219] <Method for manufacturing thermosetting prepregs by overlapping precursor sheets>

[0220] One embodiment of the method for manufacturing the thermosetting prepreg disclosed herein includes the following steps (a) and (b):

[0221] (a) Providing a thermosetting prepreg precursor sheet (precursor providing process), wherein the precursor sheet comprises: a fiber sheet, and first and second thermosetting resin compositions impregnated into the fiber sheet and respectively comprising a thermosetting resin and a curing agent, wherein in a cross-section perpendicular to the surface direction of the fiber sheet, the first thermosetting resin composition impregnates a first outer region in the thickness direction of the fiber sheet, and the second thermosetting resin composition impregnates a second outer region in the thickness direction of the fiber sheet, opposite to the first outer region; and

[0222] (b) Two thermosetting prepreg precursor sheets are overlapped, such that the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet faces the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet, forming a thermosetting prepreg (overlapping process).

[0223] Here, in the thermosetting prepreg precursor sheet, the equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0224] (Precursor provision process)

[0225] In the precursor supply process, one or more (particularly two) thermosetting prepreg precursor sheets are provided. Regarding the fiber sheet, the first thermosetting resin composition, and the second thermosetting resin composition contained in the thermosetting prepreg precursor sheet, refer to the above description concerning thermosetting prepregs.

[0226] (Overlapping processes)

[0227] In the overlapping process, two thermosetting prepreg precursor sheets are overlapped such that the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet is opposite to the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet.

[0228] That is, in the laminate obtained by overlapping two thermosetting prepreg precursor sheets, the first outer regions of the two thermosetting prepreg precursor sheets face each other, while the second outer regions of the two thermosetting prepregs face away from each other.

[0229] At this point, the two thermosetting prepreg precursor sheets can be two separate thermosetting prepreg precursor sheets, or they can be two parts of one thermosetting prepreg precursor sheet. That is, for example, the above-mentioned overlap can be achieved by bending one precursor sheet.

[0230] Preferably, when overlapping two precursor sheets in the overlapping process, the fiber orientation of the fiber sheets is preferably aligned. In particular, when the fiber sheets are composed of fibers drawn in one direction, the fiber orientation of the fiber sheets in the two precursor sheets is preferably substantially along the same direction. By doing so, the resin composition remaining between the two overlapping precursor sheets can be reduced or substantially eliminated.

[0231] Preferably, during the aforementioned overlap, the amount of resin composition between the two first outer regions of the two thermosetting prepreg precursor sheets is reduced. More preferably, there is substantially no resin composition between the surface of one thermosetting prepreg precursor sheet adjacent to the first outer region and the surface of the other thermosetting prepreg precursor sheet adjacent to the first outer region, thereby allowing the fiber sheets of the two thermosetting prepreg precursor sheets to come into contact with each other.

[0232] (Heating and pressurizing treatment)

[0233] In the preferred embodiment disclosed herein, after two thermosetting prepreg precursor sheets are overlapped, a process for integrating them (e.g., heating and pressurizing) is performed to obtain a thermosetting prepreg. For this heating and pressurizing process, for example, a hot roller can be used. Regarding the heating and pressurizing conditions, the heating temperature is preferably 40–140°C, and the pressurizing conditions are preferably 0.1–200 N / cm, particularly 5–100 N / cm.

[0234] According to the method of this disclosure described above, in which two thermosetting prepreg precursor sheets are overlapped to manufacture a thermosetting prepreg, the side with a larger equivalent amount of curing agent in the outer regions of the two thermosetting prepreg precursor sheets exists in the central region of the thermosetting prepreg obtained as a result of the overlap. Therefore, according to the method of this disclosure, the thermosetting prepreg of this disclosure can be obtained relatively easily and efficiently.

[0235] The method for manufacturing the thermosetting prepreg disclosed herein may include a step of applying release paper or a polymer film to both or one (one or two main surfaces) of the thermosetting prepreg. Specifically, in one embodiment of this disclosure, the thermosetting prepreg obtained by overlapping two thermosetting prepreg precursor sheets may be provided in a state where both or one side is covered with release paper or a polymer film. The release paper or polymer film may in particular be configured to cover the entirety of both or one (one or two main surfaces) of the thermosetting prepreg. Examples of polymer films include, for instance, polyethylene film.

[0236] <Method for manufacturing thermosetting prepreg precursor sheets>

[0237] The thermosetting prepreg precursor sheet that can be used in the above method can be manufactured by the following method, which includes:

[0238] Provide fiber sheets (sheet supply process);

[0239] A first thermosetting resin composition comprising a thermosetting resin and a curing agent is provided (the first resin composition providing process);

[0240] Provide a second thermosetting resin composition comprising a thermosetting resin and a curing agent (the process of providing the second resin composition);

[0241] A first thermosetting resin composition is prepared on one main surface of the fiber sheet (first resin composition preparation step);

[0242] A second thermosetting resin composition is prepared on another main surface of the fiber sheet (second resin composition preparation step); and

[0243] The first thermosetting resin composition and the second thermosetting resin composition are at least partially impregnated into the fiber sheet to form a thermosetting prepreg precursor sheet (impregnation process).

[0244] The equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0245] (Sheet supply process)

[0246] In the sheet supply process, fiber sheets are provided. Regarding the fiber sheets, please refer to the above description of thermosetting prepregs. It should be noted that the thickness of this fiber sheet can be 0.01–1.8 mm, 0.02–1.5 mm, or 0.04–1.1 mm. Furthermore, the area weight of this fiber sheet can be 25–500 g / m². 2 Preferred concentration: 50–400 g / m 2 More preferably 100-300g / m 2 .

[0247] (First resin composition supply process, second resin composition supply process)

[0248] In the first resin composition providing step and the second resin composition providing step, a first thermosetting resin composition and a second thermosetting resin composition are provided, respectively. These resin compositions comprise a thermosetting resin and a curing agent, and may optionally further comprise a thermoplastic resin and a conductive material. For information regarding the resin compositions and their constituent elements, please refer to the above description concerning thermosetting prepregs.

[0249] Thermosetting resin compositions can be manufactured by mixing the constituent components. The mixing temperature should be appropriately adjusted considering the viscosity, thermal properties, and curing temperature of the resins being mixed, and is preferably below the curing initiation temperature, between 50 and 120°C. Mixing can be carried out in one stage or in multiple stages. There is no particular limitation on the mixing order of the constituent components of the resin composition.

[0250] As a mixing machinery device for mixing, known devices can be used, such as roller mills, planetary mixers, kneaders, extruders, Banbury mixers, etc.

[0251] The thermosetting resin composition provided in the process may be, for example, in sheet form.

[0252] There are no particular limitations on the method for producing thermosetting resin compositions in sheet form (hereinafter also referred to as "resin composition sheets" or "resin sheets"), and they can be produced by known methods. For example, they can be produced by applying (casting, casting, etc.) to a support such as release paper or release sheet using a die coater, applicator, reverse roller coater, comma coater, doctor blade coater, etc.

[0253] Specifically, for example, a sheet of thermosetting resin composition can be made by coating the prepared thermosetting resin composition onto release paper using a thin film coating machine, drying it to form a sheet, and then peeling it off from the release paper.

[0254] When the thermosetting resin composition contains epoxy resin, the processing temperature for making the sheet is generally preferably 70 to 160°C, more preferably 75 to 140°C.

[0255] The thickness of the resin sheet is preferably 2–500 μm, more preferably 5–100 μm. The weight per unit area of ​​the resin sheet can be 10–200 g / m². 2 The preferred value is 20–100 g / m³. 2 More preferably, 30–75 g / m 2 .

[0256] Preferably, the viscosity (V1 (Pa·s) of the first thermosetting resin composition at 50°C is higher than the viscosity (V2 (Pa·s) of the second thermosetting resin composition at 50°C), and particularly the difference in their viscosities (V1-V2) is 10 or more, 25 or more, 50 or more, 75 or more, 100 or more, 150 or more, 200 or more, 250 or more, 300 or more, 400 or more, or 500 or more. The upper limit of the viscosity difference (V1-V2) can be, for example, 3000 or less, 2600 or less, 2000 or less, 1500 or less, 1000 or less, or 750 or less.

[0257] The viscosity of the first thermosetting resin composition at 50°C is preferably 500–10000 Pa·s or 550–5000 Pa·s, more preferably 600–3000 Pa·s or 600–2000 Pa·s, further preferably 650–1500 Pa·s or 650–1000 Pa·s, and most preferably 700–900 Pa·s.

[0258] The viscosity of the second thermosetting resin composition at 50°C is preferably 100–1250 Pa·s, 100–1000 Pa·s, or 200–1000 Pa·s, more preferably 400–800 Pa·s, and even more preferably 500–750 Pa·s.

[0259] (First resin composition preparation step, second resin composition preparation step)

[0260] In the first resin composition preparation step and the second resin composition preparation step, a first thermosetting resin composition and a second thermosetting resin composition are respectively prepared on the first main surface and the second main surface of the fiber sheet. In this step, for example, sheet-like (e.g., in the form of a resin film) first and second thermosetting resin compositions can be laminated on the main surface of the fiber sheet, particularly directly.

[0261] When the first thermosetting resin composition and the second thermosetting resin composition are in sheet form, the unit area weight M1 (g / m²) of the sheet-form first thermosetting resin composition is... 2 The unit area weight M2 (g / m²) of the second thermosetting resin composition in sheet form with the first thermosetting resin composition 2 The ratio (M1 / M2) can be 0.25 to 4.0, preferably 0.3 to 3.0 or further 0.5 to 2.0.

[0262] In one embodiment of the invention, the sheet-like first thermosetting resin composition has a unit area weight (g / m²) 2 M1 is greater than the unit area weight (g / m²) of the sheet-like second thermosetting resin composition. 2 M2. In this case, prepregs exhibiting particularly good viscosity and composite compressive properties are sometimes obtained. In this scheme, the ratio (M1 / M2) can be, for example, 1.2 to 3.0, 1.4 to 2.8, or 1.6 to 2.6.

[0263] In another embodiment of the invention, the unit area weight (g / m²) of the sheet-like first thermosetting resin composition is... 2 M1 is less than the unit area weight (g / m²) of the sheet-like second thermosetting resin composition. 2 M2. In this case, prepregs exhibiting particularly good composite compressive strength after impact are sometimes obtained. Additionally, cases where exceptionally excellent electrical conductivity (especially in the thickness direction) can be achieved are also possible. In this embodiment, the ratio (M1 / M2) can be, for example, 0.2–0.9, 0.3–0.8, or 0.4–0.7.

[0264] (Immersion process)

[0265] In the impregnation process, the first thermosetting resin composition and the second thermosetting resin composition are at least partially impregnated into the fiber sheet.

[0266] There are no particular limitations on the method of impregnating the thermosetting resin composition into the fiber sheet, but the following method is preferred: impregnating the fiber sheet with a resin composition whose viscosity is reduced by heating (dry method).

[0267] In this impregnation process, for example, heat and pressure are arbitrarily applied to the intermediate laminate obtained after the first resin composition preparation process and the second resin composition preparation process described above, namely, the intermediate laminate composed of the sheet of the first thermosetting resin composition, the fiber sheet, and the sheet of the second thermosetting resin composition, to impregnate it with the resin composition. To impart heat and pressure, hot pressing can be performed, for example, using a hot roller, or impregnation can be performed by passing the intermediate laminate between two rollers while it is being heated.

[0268] The heating temperature for the impregnation treatment can be appropriately determined by taking into account the viscosity of the thermosetting resin composition, curing temperature, etc. When the thermosetting resin composition contains epoxy resin, the heating temperature is preferably 70 to 160°C, more preferably 90 to 140°C.

[0269] The preferred impregnation time is 10 to 300 seconds.

[0270] The pressure conditions for the impregnation treatment can be appropriately determined by taking into account the viscosity of the thermosetting resin composition, curing temperature, etc. Preferably, the pressure conditions for the impregnation treatment are linear pressures of 1 to 245 N / cm (0.1 to 25 kg / cm), more preferably 9.8 to 147 N / cm (1 to 15 kg / cm) or 9.8 to 50 N / cm (1 to 5 kg / cm).

[0271] The impregnation treatment can be performed once or multiple times.

[0272] In the impregnation process, the first thermosetting resin composition and the second thermosetting resin composition may be completely impregnated into the fiber sheet, or a portion of the first thermosetting resin composition and / or the second thermosetting resin composition may remain on the surface of the fiber sheet. The resin composition remaining on the surface of the fiber sheet may form a resin layer.

[0273] In one embodiment of this disclosure, the first thermosetting resin composition is substantially completely impregnated into the fiber sheet, while a portion of the second thermosetting resin composition remains on the surface without impregnating the fiber sheet, thus forming a resin layer. Therefore, the area weight of the fiber sheet, the heating / pressurization conditions, and / or the viscosity of the resin composition can be appropriately adjusted. Furthermore, the formation of the resin layer can be promoted by adding interlayer particles to the thermosetting resin composition.

[0274] <Method for manufacturing thermosetting prepregs by progressive impregnation of the first and second resin compositions>

[0275] The thermosetting prepreg disclosed herein can also be manufactured by sequentially impregnating the first and second thermosetting resins into the fiber sheet (hereinafter, this method is referred to as the "stepwise impregnation method").

[0276] Specifically, the method includes:

[0277] Provide fiber sheets (sheet supply process);

[0278] A first thermosetting resin composition comprising a thermosetting resin and a curing agent is provided (the first resin composition providing process);

[0279] Provide a second thermosetting resin composition comprising a thermosetting resin and a curing agent (the process of providing the second resin composition);

[0280] A first thermosetting resin composition is applied to the main surface of the fiber sheet (first resin composition application step);

[0281] The first thermosetting resin composition is at least partially impregnated into the fiber sheet (first resin composition impregnation step);

[0282] A second thermosetting resin composition is disposed on the main surface of the fiber sheet impregnated with the first thermosetting resin composition (second resin composition disposal step); and

[0283] The second thermosetting resin composition is at least partially impregnated into the fiber sheet to form a thermosetting prepreg (second resin composition impregnation step).

[0284] The equivalent ratio of the curing agent in the first thermosetting resin composition is greater than the equivalent ratio of the curing agent in the second thermosetting resin composition.

[0285] (Step-by-step impregnation method: sheet feeding process)

[0286] In the sheet supply process, fiber sheets are provided. Regarding the fiber sheets, please refer to the above description of thermosetting prepregs. It should be noted that the thickness of this fiber sheet can be 0.01–4.0 mm, 0.05–2.0 mm, or 0.1–1.0 mm. Furthermore, the area weight of this fiber sheet can be 70–600 g / m². 2 Preferred concentration: 100–500 g / m 2 More preferably 200-450 g / m 2 .

[0287] (Stepwise impregnation method: First resin composition supply step, second resin composition supply step)

[0288] In the first resin composition providing step and the second resin composition providing step, a first thermosetting resin composition and a second thermosetting resin composition are provided, respectively. These resin compositions comprise a thermosetting resin and a curing agent, and may optionally further contain a thermoplastic resin and a conductive material. These thermosetting resin compositions may, for example, be in sheet form. For information regarding the resin compositions and their constituent elements, refer to the above description concerning thermosetting prepregs.

[0289] Sheet-shaped thermosetting resin compositions (resin composition sheets or resin sheets) can be produced in the same manner as described above. For example, a sheet of thermosetting resin composition can be produced by coating the prepared curable resin composition onto release paper using a film coating machine, drying it to form a sheet, and then peeling it off from the release paper.

[0290] (Stepwise impregnation method: First resin composition preparation step)

[0291] In the first resin composition preparation step, a first thermosetting resin composition is prepared on the first main surface and / or the second main surface (preferably the first and second main surfaces) of the fiber sheet. In this step, for example, two sheet-like (e.g., in the form of a resin film) first thermosetting resin compositions may be prepared on the two main surfaces of the fiber sheet respectively.

[0292] (Step-by-step impregnation method: the first resin composition impregnation process)

[0293] In the first resin composition impregnation step, the first thermosetting resin composition is at least partially impregnated into the fiber sheet. In this step, for example, heat and pressure are applied to a fiber sheet (first intermediate laminate) on which the first thermosetting resin composition is disposed on both main surfaces, to impregnate it with the resin composition. To impart heat and pressure, hot pressing can be performed, for example, using hot rollers, or impregnation can be achieved by passing the first intermediate laminate between two rollers while it is being heated.

[0294] (Stepwise impregnation method: Second resin composition preparation step)

[0295] In the second resin composition preparation step, the second thermosetting resin composition is prepared on the first main surface and / or the second main surface (preferably the first and second main surfaces) of the fiber sheet impregnated with the first thermosetting resin composition. In this step, for example, two sheet-like (e.g., in the form of a resin film) second thermosetting resin compositions may be laminated on the two main surfaces of the fiber sheet respectively.

[0296] (Step-by-step impregnation method: the second resin composition impregnation process)

[0297] In the second resin composition impregnation step, the second thermosetting resin composition is at least partially impregnated into the fiber sheet. In this step, heat and pressure are applied, for example, to a fiber sheet (second intermediate laminate) impregnated with the first thermosetting resin composition and having the second thermosetting resin composition on both sides thereon, to impregnate it with the resin composition. To impart heat and pressure, hot pressing can be used, for example, with hot rollers, or impregnation can be performed by passing the material between two rollers while it is being heated.

[0298] According to the above method, the thermosetting prepreg disclosed herein can be manufactured, wherein a resin composition having a lower curing agent equivalent ratio is impregnated into the outer region of a fiber sheet impregnated with a resin composition having a higher curing agent equivalent ratio, and thus the curing agent equivalent ratio in the central region is larger.

[0299] Typically, when a resin composition sheet is added to a fiber sheet that has already been impregnated with a resin composition, and then heated and pressurized, it is believed that the resin composition that has been pre-impregnated into the fiber sheet hinders the impregnation of the additional resin composition into the fiber sheet.

[0300] In contrast, in a fiber sheet impregnated with a first thermosetting resin composition, to ensure sufficient impregnation of the second thermosetting resin composition, the amount of the first thermosetting resin composition impregnated into the fiber sheet can be reduced, for example. In this case, since gaps may exist in the fiber sheet through which the second thermosetting resin composition can be impregnated, the second thermosetting resin composition can be impregnated more easily.

[0301] Therefore, relative to the fiber sheet, for example, the first thermosetting resin composition impregnated into the fiber sheet may be more than 10% by mass, more than 12% by mass, or more than 14% by mass, and / or may be less than 30% by mass, less than 30% by mass, less than 28% by mass, less than 26% by mass, less than 24% by mass, or less than 22% by mass.

[0302] Additionally, for example, the total area weight (g / cm²) of the sheet of the first thermosetting resin composition disposed on the fiber sheet in the first resin composition preparation step. 2 Weight per unit area of ​​fiber sheet (g / cm²) 2 It can be 10% or more, 12% or more, 14% or more, or 16% or more, and / or it can be less than 30%, less than 30%, less than 28%, less than 26%, or less than 24%.

[0303] Furthermore, to impregnate the second thermosetting resin composition into the fiber sheet already impregnated with the first thermosetting resin composition, the heating temperature in the impregnation process of the second resin composition can be set to 70–140°C, and the pressure conditions can be set to 9.8–245 N / cm. It is believed that by performing the impregnation treatment under these conditions, the viscosity of the thermosetting resin composition decreases, and the impregnation of the second thermosetting resin composition is promoted.

[0304] Example

[0305] The present invention will be described in more detail below through examples, but the present invention is not limited to the examples. The components and test methods used in the examples and comparative examples are described below.

[0306] Viscosity

[0307] Regarding viscosity, a rheometer (product name: ARES-G2) manufactured by TA Instruments was used. The thickness of the resin composition between the parallel plates was set to 0.5 mm with a diameter of 25 mm. The viscosity was measured up to 180 °C at an angular velocity of 10 radians / second and a heating rate of 2 °C / min. The resin viscosity was determined by the temperature-viscosity curve.

[0308] <Infiltration Level>

[0309] The impregnation level of the prepreg, i.e., the degree to which the resin composition is impregnated in the fiber sheet, can be studied by determining the water absorption rate (WPU) according to the water absorption rate test. Specifically, it follows these steps:

[0310] One layer of prepreg was cut into 100mm × 100mm pieces. After removing the inner paper, the mass (W1) of one layer of prepreg was measured for each sample. Next, the prepreg was firmly fixed in the WPU device with the fiber direction at 0° perpendicular to the water surface. With the fixed prepreg vertically positioned in the device, 5mm of the prepreg was immersed in room temperature water in a laboratory environment of 23°C and 50% relative humidity. After immersion for 5 minutes, the sample was removed from the water, excess water on the outside was removed, and the mass (W2) of the sample was measured again. The percentage of water absorption from the initial state (WPU) was obtained using the following formula (3).

[0311] WPU=(W1-W2) / W1 Equation (3)

[0312] The percentage of water absorption (WPU%) was calculated from the average weight of three samples. The samples were then evaluated according to the following criteria.

[0313] ◎: WPU is less than 3%;

[0314] 〇: WPU is 3% or more but less than 5%;

[0315] △: WPU is 5% or more but less than 10%;

[0316] ×: WPU is above 10%.

[0317] <Viscosity>

[0318] The tackiness of the prepreg was evaluated using a tackiness testing apparatus (manufactured by Resuka Co., Ltd., product name: TAC-II). Specifically, the prepreg was placed on a test platform maintained at 27°C, and an initial load of 100 gf was applied using a φ5 stainless steel cylindrical tack probe maintained at 27°C. The maximum load (F0 and F1) at a test speed of 10 mm / s was determined. 14 ).

[0319] For freshly manufactured prepreg (F0) and prepreg stored at 26.7°C and 65% humidity for 14 days (F... 14 ), respectively, a viscosity probe test was performed. The viscosity retention rate was calculated using the following formula (4), and the calculation result was expressed according to the following standard:

[0320] Viscosity retention rate = 100·(F0-F 14 Formula (4) / F0

[0321] ◎: The load after manufacturing is above 500gf, and the viscosity retention rate after 14 days of storage is above 80%.

[0322] 〇: The load after manufacturing is above 500gf, and the viscosity retention rate after 14 days of storage is above 50% and less than 80%.

[0323] △: The load after manufacturing is above 500gf, and the viscosity retention rate after 14 days of storage is above 25% and less than 50%.

[0324] ×: The load after manufacturing is above 500gf, and the viscosity retention rate after storage for 14 days is less than 25%.

[0325] <Compression Characteristics>

[0326] The compression characteristics are as follows:

[0327] The prepreg was cut into 360mm squares and stacked to obtain a stacked structure [+45 / 0 / -45 / 90]. nS The laminated body was formed using a conventional vacuum autoclave molding method, under pressure of 0.59 MPa and temperature of 180°C for 2 hours. The resulting molded body was cut into pieces with a width of 38.10 mm and a length of 304.8 mm to prepare test pieces. A 6.35 mm diameter hole was then drilled in the center of each test piece to obtain a test piece for open-hole compressive strength (OHC) testing. Using this test piece, the compressive strength (OHC) was determined according to SACMA SRM 3R-94. The crosshead speed of the test piece compression testing machine was set to 1 mm / min, and five test pieces were tested.

[0328] <Post-impact compressive strength>

[0329] The post-impact compressive strength is determined as follows:

[0330] The prepreg was cut into 360mm squares and stacked to obtain a stacked structure [+45 / 0 / -45 / 90]. nSThe laminated body was formed using a conventional vacuum autoclave molding method, under a pressure of 0.59 MPa and a temperature of 180°C for 2 hours. The resulting molded body was cut into pieces with a width of 100 mm and a length of 150 mm to obtain test pieces for the compressive strength after impact (CAI) test. Using these test pieces, an impact of 30 J was applied according to SACMA SRM 2R-94 to cause damage, and the compressive strength after impact (CAI) was then measured. The crosshead speed of the test piece compression tester was set to 1 mm / min, and five test pieces were tested.

[0331] <Conductivity in the thickness direction>

[0332] The thickness-direction electrical conductivity (volume resistivity) was measured using a digital ohmmeter (Adexaile Corporation, AX-111A) on a composite material manufactured according to the following operations, measuring the volume resistivity in the Z-direction (thickness direction). Volume resistivity is the inherent resistance of a given material. The Z-direction volume resistivity ρ of the material is calculated using the following formula.

[0333] ρ=RA / L

[0334] R: Resistance (Ω) of a uniform test piece of the material;

[0335] L: Thickness of the test piece (m);

[0336] A: Cross-sectional area of ​​the test piece (m²) 2 ).

[0337] The fabrication of the composite material and the measurement of its conductivity in the thickness direction were carried out as follows:

[0338] The prepreg was cut and stacked to obtain a laminated structure [+45 / 0 / -45 / 90]. 2S The laminated body was formed using a vacuum autoclave molding method, under a pressure of 0.59 MPa and a temperature of 180°C for 2 hours. The resulting molded body was cut into dimensions of 40 mm wide × 40 mm long. The upper and lower surfaces of the molded body were ground with sandpaper until the carbon fibers were exposed, and finally, the surface was finished with 2000 grit sandpaper. Afterward, the unground sides were covered with fluorine tape, and the ground upper and lower surfaces were copper-plated using an electrolytic electroplating method with copper sulfate as the electrolyte and copper as the electrode plate. The resulting test piece was sandwiched between gold-plated electrodes with a width of 50 mm and a length of 50 mm, and a load of 0.06 MPa was applied to the test piece. The resistance value in the Z direction was measured using a digital ohmmeter, and the conductivity in the thickness direction was calculated using the above formula.

[0339] [Element]

[0340] The components involved in the examples and comparative examples are as follows.

[0341] (Epoxy resin)

[0342] Epoxy resin [A]

[0343] A-1: Tetraglycidyl-4,4'-diaminodiphenylmethane (hereinafter referred to as "TGDDM") (manufactured by Nippon Steel Chemical & Material Co., Ltd., product name: YH-404);

[0344] A-2: Bisphenol A-diglycidyl ether (hereinafter referred to as "DGBPA") (manufactured by Nippon Steel Chemical & Material Co., Ltd., product name: YD-8125);

[0345] A-3: GAN (manufactured by Nippon Kayaku Co., Ltd.);

[0346] A-4: GOT (manufactured by Nippon Kayaku Co., Ltd.);

[0347] A-5: Triglycidyl-m-aminophenol (hereinafter referred to as "m-TGAP") (Araldite manufactured by Huntsman, product name: MY0600);

[0348] (Curing agent (amine-based curing agent))

[0349] B-1: 4,4-Diaminodiphenyl sulfone (hereinafter referred to as "44DDS") (manufactured by Wakayama Seika Kogyo Co., Ltd., product name: Seikacure-S);

[0350] B-2: 3,3'-Diaminodiphenyl sulfone (hereinafter referred to as "33DDS") (manufactured by Konishi Chemical Industry Co., Ltd., product name: 33DAS);

[0351] B-3: 3,3'-Diaminodiphenylsulfone pulverized material (pulverized material obtained by adjusting 33DDS to an average particle size of 5μm using a pulverizer, hereinafter referred to as "33DDS pulverized material");

[0352] (Epoxy resin soluble thermoplastic resin)

[0353] C-1: Polyethersulfone (hereinafter referred to as "PES") (manufactured by Sumitomo Chemical Industry Co., Ltd., product name: SumikaExcel PES-5003MP, average particle size 50μm);

[0354] (Epoxy resin insoluble thermoplastic resin (interlaminar particles))

[0355] D-1: Polyamide resin (hereinafter referred to as "PA1010") (manufactured by Daicel-Evonik, product name: MSP-A7723, average particle size 18μm);

[0356] D-2: Polyamide 12 (hereinafter referred to as "PA12") (manufactured by Daicel-Evonik, product name: MSP-A7673, average particle size 20μm);

[0357] (Conductive materials)

[0358] E-1: Carbon nanotubes (hereinafter referred to as "CNT") (manufactured by Nanocyl, product name: NC7000, average particle size 9.5nm);

[0359] E-2: Carbon nanostructures (hereinafter referred to as "CNS") (manufactured by Cabot Corporation, product name: AthlosSR1200 CNS, average particle size 10-20nm);

[0360] E-3: Ground fiber (manufactured by Mitsubishi Resin Corporation, product name: DIALEAD K223HM, pitch-based carbon fiber ground fiber with an aspect ratio of 18 and an average fiber length of 200μm (catalog value));

[0361] (Carbon fiber)

[0362] • "Tenax (registered trademark)" IMS65 E23 830tex: (carbon fiber strand, tensile strength of 5800MPa, tensile modulus of elasticity of 290GPa, manufactured by Teijin Co., Ltd.);

[0363] • "Tenax (registered trademark)" ITS55 E23 1600tex: (carbon fiber bundle, tensile strength of 5200MPa, tensile modulus of elasticity of 280GPa, manufactured by Teijin Co., Ltd.)

[0364] Examples 1-4 and Comparative Examples 1-3

[0365] The thermosetting prepregs involved in Examples 1-4 and Comparative Examples 1-3 were manufactured, and their physical properties were evaluated.

[0366] <Example 1>

[0367] (Preparation of resin composition 1)

[0368] Using a mixing apparatus, 18 parts by weight of PES, a soluble thermoplastic resin for epoxy resin, were added to 70 parts by weight of TGDDM, 25 parts by weight of DGBPA, and 5 parts by weight of GAN as epoxy resin. The mixture was stirred at 120°C for 60 minutes using a planetary mixer to completely dissolve the PES in the epoxy resin. The resin temperature was then cooled to below 80°C to prepare an epoxy resin composition. Subsequently, 40 parts by weight of curing agent as shown in Table 1 below were added to the above resin using a roller mill and the mixture was mixed to prepare resin composition 1.

[0369] (Preparation of sheets of resin composition 1)

[0370] The prepared resin composition 1 was coated onto release paper using a thin film coating machine to produce 48 g / m² resin. 2 A sheet (resin film) of resin composition 1.

[0371] (Preparation of resin composition 2)

[0372] Using a mixing apparatus, 15 parts by mass of PES (a soluble thermoplastic resin for epoxy resin) and 13 parts by mass of heat-treated PA1010 granules were added to 70 parts by mass of TGDDM, 25 parts by mass of DGBPA, and 5 parts by mass of GAN (as epoxy resin). The mixture was stirred at 120°C for 60 minutes using a planetary mixer to completely dissolve the PES in the epoxy resin. The resin temperature was then cooled to below 80°C to prepare an epoxy resin composition. Subsequently, 34 parts by mass of curing agent as shown in Table 1 below were added to the above resin using a roller mill and the mixture was kneaded to prepare resin composition 2.

[0373] (Preparation of sheets of resin composition 2)

[0374] The prepared resin composition 2 was coated onto release paper using a thin film coating machine to produce 48 g / m² resin. 2 The sheet (resin film) of resin composition 2.

[0375] (Preparation of thermosetting prepreg precursor sheets)

[0376] Next, carbon fiber sheets were prepared by arranging carbon fiber bundles (manufactured by Teijin Corporation, product name: IMS65) as reinforcing fibers in one direction. A sheet of resin composition 1 and a sheet of resin composition 2 prepared above were overlapped on each side of the carbon fiber sheet. Then, the sheets were heated and pressurized using hot rollers at 110°C and 15 N / cm to impregnate resin composition 1 and resin composition 2 into the carbon fiber sheets, resulting in a carbon fiber with an area weight of 190 g / m². 2A unidirectional prepreg precursor sheet with a matrix resin mass fraction of 35.0% (the thermosetting prepreg precursor sheet involved in Example 1).

[0377] Two thermosetting prepreg precursor sheets prepared above were prepared and overlapped with the sides of their main surfaces impregnated with resin composition 1 facing each other. They were then heated and pressurized using hot rollers at 50°C and 15 N / cm to integrate the two precursor sheets, resulting in carbon fiber with a unit area weight of 380 g / m². 2 A unidirectional prepreg sheet with a matrix resin mass fraction of 35.0% (the thermosetting prepreg involved in Example 1). The evaluation results of the properties of the prepreg involved in Example 1 are shown in Table 1 below.

[0378] A composite material was manufactured using the thermosetting prepreg described in Example 1. Specifically, 24 sheets of the thermosetting prepreg described in Example 1 were laminated in a [45° / 0° / -45° / 90°] 3s configuration and then thermosetting was performed to manufacture the composite material. The evaluation results of the properties of the resulting composite material are described in Table 1 below.

[0379] <Example 2A>

[0380] Except for changing the unit area weight of the resin film as described in Table 1 below, the thermosetting prepreg of Example 2A was manufactured in the same manner as in Example 1 above. Using the obtained thermosetting prepreg of Example 2A, a composite material was manufactured in the same manner as in Example 1 above. The evaluation results of the properties of the obtained prepreg and composite material are described in Table 1 below.

[0381] <Example 2B>

[0382] Except for variations in the amount of interlayer particles and the unit area weight of resin compositions 1 and 2 as described in Table 1 below, the thermosetting prepreg of Example 2B was manufactured in the same manner as in Example 2A described above. Using the obtained thermosetting prepreg of Example 2B, a composite material was manufactured in the same manner as in Example 1 described above. The evaluation results of the properties of the obtained prepreg and composite material are recorded in Table 1 below.

[0383] <Example 3>

[0384] Except for changing the composition of the resin composition to the types and amounts listed in Table 1 below, the thermosetting prepreg of Example 3 was manufactured in the same manner as in Example 1. Using the obtained thermosetting prepreg, a composite material was manufactured in the same manner as in Example 1 above. The evaluation results of the properties of the obtained prepreg and composite material are described in Table 1 below.

[0385] <Example 4>

[0386] (Preparation of resin composition 1')

[0387] Using a mixing apparatus, 20 parts by weight of PES, a soluble thermoplastic resin for epoxy resin, were added to 45 parts by weight of TGDDM, 50 parts by weight of DGBPA, and 5 parts by weight of GAN as epoxy resin. The mixture was stirred at 120°C for 60 minutes using a planetary mixer to completely dissolve the PES in the epoxy resin. The resin temperature was then cooled to below 80°C to prepare an epoxy resin composition. Subsequently, 36 parts by weight of curing agent as shown in Table 1 below were added to the above resin using a roller mill and the mixture was mixed to prepare resin composition 1'.

[0388] (Preparation of sheets of resin composition 1')

[0389] The prepared resin composition 1' was coated onto release paper using a thin film coating machine to produce 68 g / m 2 A sheet of resin composition 1'.

[0390] (Preparation of resin composition 2')

[0391] Using a mixing apparatus, 20 parts by weight of PES (a soluble thermoplastic resin for epoxy resin) and 35 parts by weight of heat-treated PA1010 granules were added to 45 parts by weight of GDDM (as epoxy resin), 50 parts by weight of DGBPA, and 5 parts by weight of GOT (as epoxy resin). The mixture was stirred at 120°C for 60 minutes using a planetary mixer to completely dissolve the PES in the epoxy resin. The resin temperature was then cooled to below 80°C to prepare an epoxy resin composition. Subsequently, 32 parts by weight of curing agent (as shown in Table 1 below) were added to the above resin using a roller mill and the mixture was kneaded to prepare resin composition 2'.

[0392] (Preparation of the sheet of resin composition 2')

[0393] The prepared resin composition 2' was coated onto release paper using a thin film coating machine to produce 68 g / m 2 The sheet of resin composition 2'.

[0394] (Preparation of thermosetting prepreg precursor sheets)

[0395] Next, carbon fiber sheets were prepared by arranging carbon fiber bundles (manufactured by Teijin Corporation, product name: IMS65) as reinforcing fibers in one direction. A sheet of resin composition 1' and a sheet of resin composition 2' prepared above were overlapped on each side of the carbon fiber sheet. Then, the sheets were heated and pressurized using hot rollers at 110°C and 15 N / cm to impregnate the carbon fiber sheets with resin composition 1' and resin composition 2', resulting in carbon fibers with a basis weight of 260 g / m². 2 A unidirectional prepreg precursor sheet with a matrix resin mass fraction of 35.0% (the thermosetting prepreg precursor sheet involved in Example 4).

[0396] Two thermosetting prepreg precursor sheets prepared above were prepared and overlapped with the sides of their main surfaces impregnated with resin composition 1' facing each other. The sheets were then heated and pressurized using hot rollers at 80°C and 50 N / cm to integrate the two precursor sheets, resulting in carbon fiber with a unit area weight of 520 g / m². 2 A unidirectional prepreg sheet with a matrix resin mass fraction of 35.0% (the thermosetting prepreg involved in Example 4).

[0397] A composite material was manufactured using the thermosetting prepreg described in Example 4. Specifically, 16 sheets of the thermosetting prepreg described in Example 4 were laminated in a [45° / 0° / -45° / 90°] 2s configuration and then thermosetting was performed to manufacture the composite material. The evaluation results of the properties of the resulting composite material are described in Table 1 below.

[0398] <Comparative Example 1>

[0399] Except for changing the content of the curing agent as described in Table 1 below, the thermosetting prepreg of Comparative Example 1 was manufactured in the same manner as in Example 1 above. Using the manufactured thermosetting prepreg, a composite material was manufactured in the same manner as in Example 1 above. The properties of the obtained prepreg and composite material are described in Table 1 below.

[0400] <Comparative Example 2>

[0401] Resin composition 1 was prepared using the same method as in Example 1.

[0402] The prepared resin composition 1 was coated onto the release paper using a thin film coating machine and dried to form a sheet. Two sheets were then peeled off from the release paper, producing two sheets with a unit area weight of 96 g / m². 2 A sheet of resin composition 1.

[0403] Next, two sheets of the resin composition 1 prepared above were placed on each side of a carbon fiber sheet in which carbon fiber bundles (manufactured by Teijin Corporation, product name: IMS65) used as reinforcing fibers were arranged in one direction. Then, by heating and pressurizing with hot rollers at 110°C and 15 N / cm, the resin composition 1 was impregnated into the carbon fiber sheets, producing carbon fibers with a basis weight of 380 g / m². 2 The unidirectional prepreg sheet involved in Comparative Example 2, with a matrix resin mass fraction of 35.0% (the thermosetting prepreg involved in Comparative Example 2), is shown in Table 1 below. The performance evaluation results of the prepreg involved in Comparative Example 2 are shown in Table 1 below.

[0404] Using the thermosetting prepreg described in Comparative Example 2, a composite material was manufactured in the same manner as in Example 1 described above, and its properties were evaluated. The properties of the resulting composite material are described in Table 1 below.

[0405] <Comparative Example 3>

[0406] Except that a sheet of resin composition 2 was used instead of a sheet of resin composition 1, the thermosetting prepreg of Comparative Example 3 was prepared in the same manner as in Comparative Example 2 described above. Using the prepared thermosetting prepreg, a composite material was manufactured in the same manner as in Example 1 described above. The properties of the obtained prepreg and composite material are described in Table 1 below.

[0407] [Table 1]

[0408] Table 1

[0409]

[0410] As shown in Table 1, compared with the thermosetting prepregs of Comparative Examples 2 and 3, which were made using only one type of resin composition, the thermosetting prepregs of Examples 1-4 exhibited preferred workability (penetration level and tackiness) resulting from the resin with a smaller equivalent ratio of curing agent, and preferred mechanical properties (compression properties and post-impact compression properties) resulting from the resin with a larger equivalent ratio of curing agent.

[0411] Furthermore, the thermosetting prepreg of Comparative Example 1 exhibited inferior mechanical properties compared to Examples 1-4. In the prepreg of Comparative Example 1, the equivalent ratio of the curing agent in the first resin composition impregnated into the central region was less than the equivalent ratio of the curing agent in the second resin composition impregnated into the outer region. While not intended to be theoretically limiting, it is believed that in Comparative Example 1, the mechanical properties were insufficient because a sufficient crosslinking density of the thermosetting resin in the central region could not be ensured.

[0412] <<Example 5>>

[0413] The thermosetting prepreg involved in Example 5 was manufactured, and its physical properties were evaluated. In Example 5, the prepreg was manufactured using only one fiber sheet, as follows.

[0414] Resin composition 1 was prepared using the same method as in Example 1.

[0415] The prepared resin composition 1 was coated onto the release paper using a thin film coating machine and dried to form a sheet. Two sheets were then peeled off from the release paper, producing two sheets with a unit area weight of 48 g / m². 2 A sheet of resin composition 1.

[0416] Resin composition 2 was prepared using the same method as in Example 1.

[0417] The prepared resin composition 2 was coated onto the release paper using a thin film coating machine and dried to form a sheet. The sheet was then peeled off from the release paper, producing two sheets with a unit area weight of 48 g / m². 2 The sheet of resin composition 2.

[0418] Next, two sheets of the resin composition 1 prepared above were placed on each side of a carbon fiber sheet in which carbon fiber bundles (manufactured by Teijin Corporation, product name: IMS65) used as reinforcing fibers were arranged in one direction. Then, by heating and pressurizing with hot rollers at 110°C and 15 N / cm, the resin composition 1 was impregnated into the carbon fiber sheets, producing carbon fibers with a basis weight of 380 g / m². 2 Unidirectional prepreg sheets with a matrix resin mass fraction of 20.5%.

[0419] Next, two sheets of the prepared resin composition 2 were respectively placed on both sides of the carbon fiber sheet impregnated with resin composition 1. Then, by heating and pressurizing with hot rollers at 80°C and 15 N / cm, the resin composition 2 was impregnated into the carbon fiber sheet, producing a carbon fiber with a unit area weight of 380 g / m². 2 The unidirectional prepreg sheet (the thermosetting prepreg involved in Example 5) with a matrix resin mass fraction of 35.0% is shown in Table 2 below. The performance evaluation results of the prepreg involved in Example 5 are shown in Table 2 below.

[0420] Using the thermosetting prepreg described in Example 5, a composite material was manufactured in the same manner as in Example 1 described above, and its properties were evaluated. The properties of the resulting composite material are described in Table 2 below.

[0421] [Table 2]

[0422] Table 2

[0423]

[0424] As shown in Table 2, compared to Comparative Examples 2 and 3, which used only a single resin composition, the prepreg of Example 5, obtained by impregnating resin composition 1 with a larger curing agent equivalent ratio followed by impregnation of resin composition 2 with a smaller curing agent equivalent ratio, exhibits excellent prepreg and composite material properties. While not intended to be theoretically limiting, it is believed that these effects of Example 5 are due to the use of two resin compositions with different curing agent contents. In particular, it is believed that the crosslinking density of the thermosetting resin in the central region is higher in the prepreg of Example 5, resulting in good mechanical properties. It should be noted that in manufacturing Example 5, because the amount of resin composition 1 impregnated into the fiber sheet was relatively reduced, resin composition 2 was better impregnated into the fiber sheet impregnated with resin composition 1.

[0425] Examples 6A and 6B, and Examples 7-11

[0426] In Examples 6A and 6B, and Examples 7 to 11, the effects of adding conductive materials were evaluated.

[0427] <Example 6A>

[0428] Except for adjusting the resin composition according to the components and amounts described in Table 3 below, and changing the type of carbon fiber used as the reinforcing fiber (manufactured by Teijin Corporation, product name: ITS55 E2324K), the thermosetting prepreg of Example 6A was manufactured in the same manner as in Example 1 above. Using the obtained thermosetting prepreg of Example 6A, a composite material was manufactured in the same manner as in Example 1 above. The evaluation results of the properties of the obtained prepreg and composite material are described in Table 3 below.

[0429] <Example 6B>

[0430] In addition to the unit area weight M1 (g / m²) of the sheet-like resin composition 1 2 The unit area weight M2 (g / m²) of the thermosetting resin composition 2 with sheet form 2 Except for changing the ratio (M1 / M2) to 0.57, the thermosetting prepreg involved in Example 6B was manufactured in the same manner as in Example 6A, and evaluated in the same manner as in Example 6A. The results are recorded in Table 3 below.

[0431] <Examples 7-11>

[0432] Except for preparing the resin composition according to the components and amounts described in Table 3 below and adding the conductive material described in Table 3 below (the conductive material further added in Example 8), the thermosetting prepregs involved in Examples 7 to 11 were manufactured in the same manner as in Example 6A. It should be noted that the conductive material was added to the resin after being loaded with the curing dosage shown in Table 3 below using a roller mill. The evaluation results of the properties of the thermosetting prepregs involved in Examples 7 to 11 and the composites manufactured from these prepregs in the same manner as in Example 1 are recorded in Table 3 below.

[0433] <Comparative Examples 4-5>

[0434] Except for preparing the resin composition according to the components and amounts described in Table 3 below, the thermosetting prepregs of Comparative Examples 4 and 5 were manufactured in the same manner as in Example 7 above. The evaluation results of the properties of the thermosetting prepregs of Comparative Examples 4 and 5 and the composites manufactured from these prepregs in the same manner as in Example 1 above are recorded in Table 3 below.

[0435] [Table 3]

[0436] Table 3

[0437]

[0438] As shown in Table 3, the thermosetting prepregs of Examples 6A and 6B, as well as Examples 7-11, exhibit sufficient thickness-direction conductivity. In particular, Examples 7-11, which contain conductive material, show exceptionally good thickness-direction conductivity compared to Example 6A, which does not contain conductive material. Furthermore, the thermosetting prepreg of Example 8, which includes additional conductive material with larger dimensions in addition to the conductive material, further exhibits good thickness-direction conductivity compared to the case without the additional conductive material.

[0439] Furthermore, Examples 7-11 exhibit conductivity equal to or better than Comparative Examples 4 and 5, and also show composite material properties superior to those of Comparative Examples 4 and 5. In Comparative Example 4, the curing agent equivalent ratios of the first resin composition and the second resin composition were the same, and there was no difference between the curing agent equivalent ratio in the outer region and the central region of the prepreg. In Comparative Example 5, since the curing agent equivalent ratio of the first resin composition was smaller than that of the second resin composition, a resin composition with a larger curing agent equivalent ratio was present in the outer region of the prepreg. In contrast, in Examples 7-11, a resin composition (the first resin composition) with a higher curing agent equivalent ratio was present in the central region of the prepreg. Although not intended to be theoretically limited, it is believed that in the composite materials involved in Examples 7-11, the crosslinking density is higher in the central region of the prepreg constituting the composite material, resulting in composite material properties superior to those of Comparative Examples 4 and 5.

[0440] Furthermore, as shown in Table 3, in Example 6B where the ratio of the resin film to its unit area weight (M1 / M2) during the manufacture of the prepreg was 0.57, superior thickness-direction conductivity was confirmed compared to that in Example 6A where the ratio was 1.00.

[0441] Symbol Explanation

[0442] 100: Thermosetting prepreg;

[0443] 110, 210, 310: Fiber sheets;

[0444] 120, 220: Resin layer;

[0445] 112, 212, 322: First thermosetting resin composition;

[0446] 122, 222, 332: Second thermosetting resin composition;

[0447] 150, 250, 350: Resin granules;

[0448] 200, 200a, 200b: Thermosetting prepreg precursor sheets;

[0449] 314: First primary surface;

[0450] 316: Second primary surface;

[0451] 320: Sheet of the first thermosetting resin composition; 330: Sheet of the second thermosetting resin composition; 340: Intermediate laminate;

[0452] A: Outer region:

[0453] B: Central Area:

[0454] A': The second outermost region of the fiber sheet;

[0455] B': The first outermost region of the fiber sheet;

[0456] T: Thickness direction.

Claims

1. A thermosetting prepreg having: Fiber sheets; a first thermosetting resin composition which is impregnated into a central region in a thickness direction of the fiber sheet in a cross section perpendicular to a surface direction of the fiber sheet; and a second thermosetting resin composition which is impregnated into an outer region in a thickness direction of the fiber sheet in a cross section perpendicular to the surface direction of the fiber sheet, and The first and second thermosetting resin compositions respectively contain a thermosetting resin and a curing agent. The equivalent ratio of the curing agent in the first thermosetting resin composition is larger than the equivalent ratio of the curing agent in the second thermosetting resin composition.

2. The thermosetting prepreg according to claim 1, in, In a cross section perpendicular to a surface direction of the fiber sheet, a ratio of a thickness of the central region to a total thickness of the central region and the outer regions is 10 to 90%.

3. The thermosetting prepreg according to claim 1 or 2, in, The first and second thermosetting resin compositions further contain a thermoplastic resin and a conductive material, respectively.

4. The thermosetting prepreg according to any one of claims 1 to 3, in, The second thermosetting resin composition is impregnated into the outer region of the fiber sheet and is disposed on the surface of the fiber sheet.

5. The thermosetting prepreg according to claim 4, in, The second thermosetting resin composition disposed on the surface of the fiber sheet has resin particles.

6. The thermosetting prepreg according to claim 4 or 5, in, The second thermosetting resin composition disposed on the surface of the fiber sheet contains an additional conductive material.

7. The thermosetting prepreg according to any one of claims 1 to 6, in, The viscosity of the first thermosetting resin composition at 50°C is higher than the viscosity of the second thermosetting resin composition at 50°C.

8. The thermosetting prepreg according to any one of claims 1 to 7, in, The viscosity of the first thermosetting resin composition at 50° C. is 500 to 10,000 Pa·s. The viscosity of the second thermosetting resin composition at 50° C. is 100 to 1000 Pa·s.

9. The thermosetting prepreg according to any one of claims 1 to 8, in, When the thermosetting prepreg is heat-cured at 180°C for 120 minutes, In a cross section perpendicular to the surface direction of the fiber sheet, there is a region where the crosslinking density of the thermosetting resin decreases from the center toward the surface in the thickness direction of the fiber sheet.

10. The thermosetting prepreg according to any one of claims 1 to 9, in, The above-mentioned thermosetting resin is epoxy resin. 11 . A thermosetting prepreg laminate having a structure in which two or more thermosetting prepregs according to claim 1 are laminated.

12. A method for producing a thermosetting prepreg, comprising: (a) providing a thermosetting prepreg precursor sheet, wherein the precursor sheet comprises a fiber sheet, and first and second thermosetting resin compositions impregnated into the fiber sheet and containing a thermosetting resin and a curing agent, respectively, wherein in a cross section perpendicular to a surface direction of the fiber sheet, the first thermosetting resin composition is impregnated into a first outer region in a thickness direction of the fiber sheet, and the second thermosetting resin composition is impregnated into a second outer region in a thickness direction of the fiber sheet on the opposite side to the first outer region. ; as well as (b) overlapping two of the thermosetting prepreg precursor sheets so that the first outer region of the fiber sheet of one thermosetting prepreg precursor sheet faces the first outer region of the fiber sheet of the other thermosetting prepreg precursor sheet; Here, in the thermosetting prepreg precursor sheet, the equivalent ratio of the curing agent in the first thermosetting resin composition is larger than the equivalent ratio of the curing agent in the second thermosetting resin composition.

13. A method for producing a thermosetting prepreg precursor sheet, wherein include: providing a fiber sheet; Providing a first thermosetting resin composition comprising a thermosetting resin and a curing agent; providing a second thermosetting resin composition comprising a thermosetting resin and a curing agent; Disposing the first thermosetting resin composition on one main surface of the fiber sheet; Disposing the second thermosetting resin composition on the other main surface of the fiber sheet; as well as impregnating the fiber sheet with the first thermosetting resin composition and the second thermosetting resin composition at least partially, The equivalent ratio of the curing agent in the first thermosetting resin composition is larger than the equivalent ratio of the curing agent in the second thermosetting resin composition.

14. The method of claim 13, in, The weight per unit area (g / m2) of the first thermosetting resin composition in sheet form 2 ) M1 and the weight per unit area of ​​the second thermosetting resin composition in sheet form (g / m 2 )M2 ratio (M1 / M2) is 0.25~4.

0.

15. The method according to claim 13 or 14, in, The second thermosetting resin composition further includes resin particles.