Resin composition, molding material, and molded article
By adding aluminum hydroxide, expanded graphite, and a specific ratio of phosphorus- and nitrogen-containing flame retardants to the resin composition, the problems of insufficient heat insulation and moldability of resin molding materials in battery containers are solved, and molded products with high strength and resistance to discoloration at high temperatures are achieved.
Patent Information
- Application Number
- CN202380026400.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-01
AI Technical Summary
Existing resin molding materials struggle to simultaneously meet the requirements of thermal insulation and moldability when making lightweight battery containers, especially in situations where it is necessary to prevent the spread of vehicle fires.
A resin composition containing resin components, aluminum hydroxide, expanded graphite, and flame retardants is used. The flame retardants consist of phosphorus-containing and nitrogen-containing flame retardants, and the proportions of each component are controlled to optimize thermal insulation and formability.
It produces molded products with excellent heat insulation and formability, which can maintain strength at high temperatures and reduce discoloration after combustion, and are suitable for applications such as battery boxes for electric vehicles.
Smart Images

Figure BDA0005033963320000261 
Figure BDA0005033963320000271 
Figure BDA0005033963320000281
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a molding material, and a molded body. Background Art
[0002] Conventionally, molded articles formed from molding materials (particularly sheet molding compounds (SMC)) containing resin components (eg, unsaturated polyester resins) have been particularly excellent in appearance, mechanical properties, water resistance, and corrosion resistance and are used in a wide range of fields.
[0003] Furthermore, as such a molding material, for example, a thermoplastic polyester resin composition containing a thermoplastic polyester resin, a phosphorus-based flame retardant, and a nitrogen-based flame retardant has been proposed (for example, see Patent Document 1 below).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2021-14478 Summary of the Invention
[0007] Problems to be solved by the invention
[0008] In recent years, with the increasing use of electric vehicles, large-capacity batteries have been installed in vehicles. To reduce weight, the battery containers (battery cases) are being made of resin. These resins are required to have superior thermal insulation properties to prevent the spread of vehicle fires.
[0009] Furthermore, when a molded article is produced using a resin composition, moldability is required.
[0010] The present invention provides a resin composition for producing a molded article having excellent thermal insulation and moldability, a molding material for producing a molded article having excellent thermal insulation and moldability, and a molded article having excellent thermal insulation and moldability.
[0011] Means for solving problems
[0012] The present invention [1] is a resin composition comprising a resin component, aluminum hydroxide, expanded graphite and a flame retardant, wherein the flame retardant comprises a phosphorus-containing flame retardant and a nitrogen-containing flame retardant.
[0013] The content of the expanded graphite is 1.0 part by mass or more and less than 5.0 parts by mass relative to 100 parts by mass of the resin component.
[0014] The phosphorus content of the phosphorus-containing flame retardant is 1.5 parts by mass or more and 4.5 parts by mass or less relative to 100 parts by mass of the resin component.
[0015] The mass ratio of the nitrogen content of the nitrogen-containing flame retardant relative to 100 parts by mass of the resin component to the phosphorus content of the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component is 0.5 or more and 3.0 or less.
[0016] A mass ratio of the content of the expanded graphite relative to 100 parts by mass of the resin component to the content of phosphorus in the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component is 0.5 to 2.0.
[0017] The present invention [2] comprises the resin composition described in [1] above, wherein the nitrogen content of the nitrogen-containing flame retardant is 2.0 parts by mass or more and 3.0 parts by mass or less relative to 100 parts by mass of the resin component.
[0018] The present invention [3] includes a molding material comprising the resin composition described in [1] or [2] above and reinforcing fibers.
[0019] The present invention [4] includes a molded article comprising a cured product of the molding material described in the above [3].
[0020] Effects of the Invention
[0021] The resin composition of the present invention comprises expanded graphite and a flame retardant, wherein the flame retardant comprises a phosphorus-containing flame retardant and a nitrogen-containing flame retardant. Furthermore, in the resin composition, the mass ratio of the content of the expanded graphite, the phosphorus content of the phosphorus-containing flame retardant, the nitrogen content of the nitrogen-containing flame retardant relative to the phosphorus content of the phosphorus-containing flame retardant, and the mass ratio of the content of the expanded graphite relative to the phosphorus content of the phosphorus-containing flame retardant are within a predetermined range. Therefore, a molded product having excellent thermal insulation and formability can be manufactured.
[0022] The molding material of the present invention comprises the resin composition of the present invention, and therefore, can produce a molded article having excellent heat insulation and moldability.
[0023] The molded article of the present invention comprises a cured product of the molding material of the present invention and therefore has excellent thermal insulation and moldability. DETAILED DESCRIPTION
[0024] The resin composition of the present invention comprises a resin component, aluminum hydroxide, expanded graphite and a flame retardant.
[0025] <Resin Components>
[0026] The resin component contains a radical polymerizable resin.
[0027] [Free radical polymerizable resin]
[0028] Examples of the radical polymerizable resin include unsaturated polyester resins, vinyl ester resins, and urethane (meth)acrylates. From the perspective of excellent physical properties (toughness, strength, durability, weather resistance, hot water resistance, and transparency), preferred free radical polymerizable resins include unsaturated polyester resins and vinyl ester resins.
[0029] The unsaturated polyester resin comprises an unsaturated polyester and a polymerizable monomer. That is, the unsaturated polyester resin is an unsaturated polyester resin composition comprising an unsaturated polyester and a polymerizable monomer.
[0030] Unsaturated polyesters are condensation products of polybasic acids and polyols.
[0031] The polybasic acid includes a polybasic acid having ethylenically unsaturated double bonds (hereinafter referred to as a polybasic acid containing ethylenically unsaturated bonds) as an essential component and a polybasic acid not having ethylenically unsaturated double bonds (hereinafter referred to as a polybasic acid not containing ethylenically unsaturated bonds) as an optional component.
[0032] Examples of the polybasic acid containing an ethylenically unsaturated bond include ethylenically unsaturated aliphatic dibasic acids and anhydrides thereof, halides of ethylenically unsaturated aliphatic dibasic acids, and alkyl esters of ethylenically unsaturated aliphatic dibasic acids.
[0033] Examples of ethylenically unsaturated aliphatic dibasic acids include maleic acid, fumaric acid, itaconic acid, and dihydromuconic acid. Examples of polybasic acids containing ethylenically unsaturated bonds include acid anhydrides derived from the above-mentioned ethylenically unsaturated aliphatic dibasic acids. Examples of acid anhydrides derived from ethylenically unsaturated aliphatic dibasic acids include maleic anhydride. Preferred polybasic acids containing ethylenically unsaturated bonds include maleic anhydride.
[0034] Examples of the polybasic acid containing no ethylenically unsaturated bond include saturated aliphatic polybasic acids, saturated alicyclic polybasic acids, aromatic polybasic acids, anhydrides of these acids, halides of these acids, and alkyl esters of these acids.
[0035] Examples of the saturated aliphatic polybasic acid include saturated aliphatic dibasic acids.
[0036] Examples of saturated aliphatic dibasic acids include oxalic acid, malonic acid, succinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, hexylsuccinic acid, glutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylsuccinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. Saturated aliphatic polybasic acids include acid anhydrides derived from the above-mentioned saturated aliphatic dibasic acids. Examples of acid anhydrides derived from saturated aliphatic dibasic acids include oxalic anhydride and succinic anhydride.
[0037] Examples of the saturated alicyclic polybasic acid include saturated alicyclic dibasic acids.
[0038] Examples of saturated alicyclic dibasic acids include chlorotriazine (HET) acid, 1,2-hexahydrophthalic acid, 1,1-cyclobutanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid (cis- or trans-1,4-cyclohexanedicarboxylic acid, or mixtures thereof). Examples of saturated alicyclic polybasic acids include acid anhydrides derived from the above-mentioned saturated alicyclic dibasic acids. Examples of acid anhydrides derived from saturated alicyclic dibasic acids include chlorotriazine anhydride.
[0039] Examples of the aromatic polybasic acid include aromatic dibasic acids.
[0040] Examples of aromatic dibasic acids include phthalic acid (o-phthalic acid, isophthalic acid, terephthalic acid), trimellitic acid, and pyromellitic acid. Examples of aromatic polybasic acids include acid anhydrides derived from the above aromatic dibasic acids. Examples of acid anhydrides derived from aromatic dibasic acids include phthalic anhydride. Preferred aromatic dibasic acids include isophthalic acid.
[0041] Examples of the polybasic acid containing no ethylenically unsaturated bond include aromatic polybasic acids.
[0042] The polybasic acid can be used alone or in combination of two or more.
[0043] When the polybasic acid includes a polybasic acid containing an ethylenically unsaturated bond and a polybasic acid not containing an ethylenically unsaturated bond, the mixing ratio of the polybasic acid containing an ethylenically unsaturated bond is, for example, 20 mol% or more, preferably 50 mol% or more, based on 100 mol of all polybasic acids.
[0044] Examples of the polyol include diol and triol.
[0045] Examples of diols include aliphatic diols, alicyclic diols, and aromatic diols. Examples of aliphatic diols include alkanediols and ether diols. Examples of alkanediols include ethylene glycol, propylene glycol (1,2-propylene glycol or 1,3-propylene glycol, or a mixture thereof), butanediol (1,2-butylene glycol or 1,3-butylene glycol or 1,4-butylene glycol, or a mixture thereof), 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2,2-trimethylpentanediol, and 3,3-dihydroxymethylheptane. Examples of ether diols include diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of the alicyclic diol include cyclohexanediol (1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, or a mixture thereof), cyclohexanedimethanol (1,2-cyclohexanediethanol, 1,3-cyclohexanediethanol, 1,4-cyclohexanediethanol, or a mixture thereof), cyclohexanediethanol (1,2-cyclohexanediethanol, 1,3-cyclohexanediethanol, 1,4-cyclohexanediethanol, or a mixture thereof), and hydrogenated bisphenol A. Examples of the aromatic diol include ethylene oxide adducts of bisphenol A and propylene oxide adducts of bisphenol A.
[0046] Examples of the triol include glycerin, trimethylolpropane, and triisopropanolamine.
[0047] As the polyol, preferably, a diol can be used. As the polyol, more preferably, an aliphatic diol can be used. As the polyol, even more preferably, an alkanediol can be used. As the polyol, particularly preferably, propylene glycol and neopentyl glycol can be used.
[0048] The polyols can be used alone or in combination of two or more.
[0049] Unsaturated polyesters are obtained by polycondensation of polybasic acids and polyols.
[0050] In order to polycondense the polybasic acid and the polyol, the polybasic acid and the polyol are first mixed in the following equivalent ratio.
[0051] The equivalent ratio of the polyol to the polybasic acid (hydroxyl group of the polyol / carboxyl group of the polybasic acid) is, for example, 0.9 or more, preferably 0.95 or more, and for example, 1.2 or less, preferably 1.1 or less.
[0052] After the polybasic acid and the polyol are mixed, they are reacted with stirring under normal pressure in a nitrogen atmosphere at a reaction temperature of, for example, 150°C or higher, preferably 190°C or higher, and, for example, 250°C or lower, preferably 230°C or lower.
[0053] In the above reaction, a known solvent and a known reaction catalyst may be added as needed.
[0054] Thus, an unsaturated polyester is obtained.
[0055] The acid value of the unsaturated polyester (measurement method: in accordance with JIS K6901 (2008)) is, for example, 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and, for example, less than 40 mgKOH / g, preferably 30 mgKOH / g or less.
[0056] The weight average molecular weight of the unsaturated polyester is, for example, 2000 or more, preferably 4000 or more, and for example, 25000 or less, preferably 20000 or less.
[0057] The weight average molecular weight is a polystyrene-equivalent weight average molecular weight based on GPC (gel permeation chromatography). The weight average molecular weight can be determined by GPC measurement of the unsaturated polyester.
[0058] Examples of the polymerizable monomer include styrene-based monomers and (meth)acrylate-based monomers.
[0059] Examples of the styrene-based monomers include styrene, vinyltoluene, tert-butylstyrene, and chlorostyrene.
[0060] Examples of (meth)acrylate monomers include alkyl (meth)acrylates, allyl (meth)acrylates, ring-containing (meth)acrylates, hydroxyalkyl (meth)acrylates, alkoxyalkyl (meth)acrylates, aminoalkyl (meth)acrylates, fluoroalkyl (meth)acrylates, and multifunctional (meth)acrylates. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and octadecyl (meth)acrylate. Examples of allyl (meth)acrylates include allyl (meth)acrylate. Examples of (meth)acrylates containing a ring structure include cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate. Examples of hydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Examples of alkoxyalkyl (meth)acrylates include 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate. Examples of aminoalkyl (meth)acrylates include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and acid chlorides thereof. Examples of fluoroalkyl (meth)acrylates include trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate. Examples of the polyfunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0061] As the polymerizable monomer, preferably, a styrene-based monomer is used, and more preferably, styrene is used.
[0062] The polymerizable monomers can be used alone or in combination of two or more.
[0063] The unsaturated polyester resin is prepared by dissolving the unsaturated polyester in a polymerizable monomer (preferably styrene) and, if necessary, adding an additive (polymerization inhibitor (described later) (preferably hydroquinone).
[0064] In the preparation of the unsaturated polyester resin, the mixing ratio of the polymerizable monomer relative to 100 parts by mass of the unsaturated polyester is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and, for example, 100 parts by mass or less. Furthermore, the mixing ratio of the polymerization inhibitor relative to 100 parts by mass of the unsaturated polyester is, for example, 0.001 parts by mass or more, preferably 0.005 parts by mass or more, and, for example, 0.1 parts by mass or less, preferably 0.05 parts by mass or less.
[0065] Furthermore, after preparing the unsaturated polyester resin, when mixing the unsaturated polyester resin with other components (vinyl ester resin, low shrinkage agent (described later), aluminum hydroxide, expanded graphite, flame retardant and additives (described later)), a polymerizable monomer may be further added.
[0066] The vinyl ester resin contains vinyl ester and a polymerizable monomer. That is, the vinyl ester resin is a vinyl ester resin composition containing vinyl ester and a polymerizable monomer.
[0067] Vinyl esters are the reaction products of epoxy resins and unsaturated monobasic acids.
[0068] Examples of the epoxy resin include bisphenol epoxy resins and novolac epoxy resins. Preferred examples of the epoxy resin include bisphenol epoxy resins.
[0069] Bisphenol-type epoxy resins are, for example, reaction products of a phenol component and an epoxy component. Examples of the phenol component include bisphenol compounds (e.g., bisphenol A). Examples of the epoxy component include bisphenol A-type epoxy compounds.
[0070] In order to obtain a bisphenol-type epoxy resin, a phenol component and an epoxy component are reacted. Specifically, a phenol component and an epoxy component are mixed and reacted.
[0071] In the above reaction, the mixing ratio of the epoxy component per 1 equivalent of the phenol component is, for example, 1.5 equivalents or more, preferably 2.0 equivalents or more, more preferably 3.0 equivalents or more, and for example, 5.0 equivalents or less, preferably 4.0 equivalents or less.
[0072] In the above reaction, a catalyst may be added as needed.
[0073] Examples of the catalyst include amines, quaternary ammonium salts, imidazoles, and phosphines. Examples of amines include triethylamine and benzyldimethylamine. Examples of quaternary ammonium salts include tetramethylammonium chloride and triethylbenzylammonium chloride. Examples of imidazoles include 2-ethyl-4-imidazole. Examples of phosphines include triphenylphosphine.
[0074] As the catalyst, preferably, a quaternary ammonium salt is used, and more preferably, triethylbenzylammonium chloride is used.
[0075] These catalysts can be used alone or in combination of two or more.
[0076] The mixing ratio of the catalyst relative to 100 parts by mass of the total amount of the phenol component and the epoxy component is, for example, 0.01 parts by mass or more, and for example, 1.0 parts by mass or less, and preferably 0.1 parts by mass or less.
[0077] The above reaction is carried out in the presence of an inert gas, and the reaction temperature is, for example, 100° C. or higher, preferably 130° C. or higher, and for example, 180° C. or lower.
[0078] In this way, a bisphenol-type epoxy resin can be obtained.
[0079] The epoxy equivalent of the bisphenol epoxy resin is, for example, 150 g / eq or more, preferably 250 g / eq or more, and, for example, 800 g / eq or less, preferably 400 g / eq or less, more preferably 350 g / eq or less.
[0080] The epoxy equivalent when two bisphenol epoxy resins are used in combination is the epoxy equivalent of all bisphenol epoxy resins obtained by multiplying the epoxy equivalent of each bisphenol epoxy resin by the mass ratio of each bisphenol epoxy resin to the total amount of bisphenol epoxy resins.
[0081] Moreover, as the epoxy resin, a commercially available product can also be used.
[0082] Examples of the unsaturated monobasic acid include monocarboxylic acid and reaction products of an alcohol having at least one unsaturated group in its molecule and a dibasic acid anhydride.
[0083] Examples of the monocarboxylic acid include (meth)acrylic acid, crotonic acid, cinnamic acid, and sorbic acid. (Meth)acrylic acid is synonymous with methacrylic acid and / or acrylic acid.
[0084] Examples of the dibasic acid anhydride include maleic anhydride, succinic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, and hexahydrophthalic anhydride. Examples of the alcohol having an unsaturated group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, pentaerythritol tri(meth)acrylate, and glycerol di(meth)acrylate.
[0085] The unsaturated monobasic acid is preferably a monocarboxylic acid, more preferably (meth)acrylic acid, and still more preferably methacrylic acid.
[0086] The unsaturated monobasic acid can be used alone or in combination of two or more.
[0087] In the reaction of the epoxy resin and the unsaturated monobasic acid, the epoxy group of the epoxy resin undergoes an addition reaction with the unsaturated monobasic acid.
[0088] In the above reaction, the equivalent of the carboxyl group of the unsaturated monobasic acid to the epoxy group of the epoxy resin is, for example, 0.8 or more, preferably 1.0 or more, and for example, 1.5 or less, preferably 1.2 or less.
[0089] In the above reaction, a catalyst may be added as needed.
[0090] The catalyst may be the same catalyst as that used in the reaction between the phenol component and the epoxy component. Preferably, the catalyst is a quaternary ammonium salt, and more preferably, triethylbenzylammonium chloride.
[0091] The mixing ratio of the catalyst relative to 100 parts by mass of the epoxy resin is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and, for example, 1.0 parts by mass or less, preferably 0.6 parts by mass or less.
[0092] In the above reaction, a polymerization inhibitor (described later) (preferably hydroquinone) may be added as needed.
[0093] The mixing ratio of the polymerization inhibitor relative to 100 parts by mass of the epoxy resin is, for example, 0.001 parts by mass or more, preferably 0.05 parts by mass or more, and for example, 0.5 parts by mass or less, preferably 0.1 parts by mass or less.
[0094] The above reaction is carried out in the presence of oxygen, and the reaction temperature is, for example, 80°C or higher, preferably 100°C or higher, and for example, 150°C or lower, preferably 130°C or lower.
[0095] Alternatively, the above reaction may be carried out after the reaction between the phenol component and the epoxy component.
[0096] Thus, vinyl ester can be obtained.
[0097] The acid value of the vinyl ester (measurement method: in accordance with JIS K6901 (2008)) can be determined by the charge ratio of the epoxy resin and the unsaturated monobasic acid, and is, for example, 1 mgKOH / g or more, and 20 mgKOH / g or less, preferably 10 mgKOH / g or less.
[0098] Examples of the polymerizable monomer include the polymerizable monomers exemplified for the unsaturated polyester resin, preferably a styrene-based monomer, and more preferably styrene.
[0099] The vinyl ester resin can be prepared by dissolving a vinyl ester in a polymerizable monomer. In the preparation of the vinyl ester resin, the proportion of the polymerizable monomer is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and for example, 80 parts by mass or less, per 100 parts by mass of the vinyl ester.
[0100] After preparing the vinyl ester resin, when mixing the vinyl ester resin with other components (unsaturated polyester resin, low shrinkage agent (described later), aluminum hydroxide, expanded graphite, flame retardant and additives (described later)), a polymerizable monomer may be further added.
[0101] The radical polymerizable resin may be used alone or in combination of two or more. Preferably, an unsaturated polyester resin and a vinyl ester resin are used in combination. When an unsaturated polyester resin and a vinyl ester resin are used in combination, the proportion of the unsaturated polyester resin relative to 100 parts by mass of the total amount of the unsaturated polyester and the vinyl ester is, for example, 70 parts by mass or more, preferably 80 parts by mass or more, and for example, 90 parts by mass or less. Furthermore, the proportion of the vinyl ester resin is, for example, 10 parts by mass or more, and for example, 30 parts by mass or less, and preferably 20 parts by mass or less.
[0102] The mixing ratio of the radical polymerizable resin relative to 100 parts by mass of the resin component is, for example, 40 parts by mass or more, preferably 55 parts by mass or more, and, for example, 80 parts by mass or less, preferably 70 parts by mass or less.
[0103] [Low shrinkage agent]
[0104] The resin component preferably contains a low shrinkage agent.
[0105] Examples of the low-shrinkage agent include polyethylene, polystyrene, styrene-based thermoplastic elastomers, cross-linked polystyrene, polyvinyl acetate-polystyrene block copolymers, polyvinyl acetate, polymethyl methacrylate, and saturated polyester resins. Preferred examples of the low-shrinkage agent include polyethylene, polystyrene, styrene-based thermoplastic elastomers, polyvinyl acetate, and saturated polyester resins.
[0106] Examples of the styrene-based thermoplastic elastomer include styrene-butadiene block copolymer elastomers, styrene-isoprene block copolymer elastomers, styrene-ethylene / butylene block copolymer elastomers, and styrene-ethylene / propylene block copolymer elastomers. Preferred styrene-butadiene block copolymer elastomers include styrene-butadiene block copolymer elastomers.
[0107] Furthermore, as the styrene-based thermoplastic elastomer, a commercially available product may also be used. Examples of such commercially available products include D1101, D1102, D1155, DKX405, DKX410, DKX415, D1192, D1161, D1171, G1651, G1652, G1654, G1701, and G1730 (all manufactured by Kraton Polymers Inc.), Asaprene T411, Asaprene T432, Tufprene A, Tufprene 125, Tufprene 126S, Tufprene 315, Tufprene 912, Tuftec H1141, Tuftec H1041, Tuftec H1043, and Tuftec H1052 (all manufactured by Asahi Kasei Corporation), and SEPTON 1001 and 1201 (all manufactured by Kuraray Co., Ltd.).
[0108] The styrene content in the styrene-based thermoplastic elastomer is, for example, 5 mass % or more, and for example, 80 mass % or less.
[0109] The saturated polyester resin can be obtained by dissolving a saturated polyester in a polymerizable monomer.
[0110] The saturated polyester is a polymerization product of the above-mentioned polyacid not containing an ethylenically unsaturated bond and the above-mentioned polyol.
[0111] Preferred examples of the polybasic acid containing no ethylenically unsaturated bond include adipic acid and isophthalic acid.
[0112] As the polyol, preferably, diol is used, and more preferably, neopentyl glycol is used.
[0113] Saturated polyester can be obtained by polycondensing (condensation polymerization) a polybasic acid not containing an ethylenically unsaturated bond with a polyol.
[0114] When a polyacid containing no ethylenically unsaturated bonds is polycondensed with a polyol (condensation polymerization), the equivalent ratio of the polyol to the polyacid (hydroxyl group of the polyol / carboxyl group of the polyacid) is, for example, 0.9 or more, preferably 0.95 or more, and for example, 1.2 or less, preferably 1.1 or less, and the mixture is stirred under normal pressure and a nitrogen atmosphere.
[0115] The reaction temperature is, for example, 150° C. or higher, preferably 190° C. or higher, and, for example, 250° C. or lower, preferably 230° C. or lower.
[0116] The reaction time is, for example, 8 hours or longer, and, for example, 30 hours or shorter.
[0117] In the above reaction, a known solvent and a known catalyst may be added as needed.
[0118] In this way, a saturated polyester can be obtained.
[0119] The acid value of the saturated polyester (measurement method: in accordance with JIS K6901 (2008)) is, for example, 5 mgKOH / g or more and, for example, less than 40 mgKOH / g.
[0120] Then, the saturated polyester is dissolved in a polymerizable monomer (preferably styrene), and an additive (polymerization inhibitor (described later) (preferably hydroquinone)) is added as needed to prepare a saturated polyester resin.
[0121] In the preparation of the saturated polyester resin, the mixing ratio of the polymerizable monomer is, for example, 35 parts by mass or more, and for example, 150 parts by mass or less, relative to 100 parts by mass of the saturated polyester. Furthermore, the mixing ratio of the polymerization inhibitor is, for example, 0.001 parts by mass or more, and preferably 0.005 parts by mass or more, and for example, 0.1 parts by mass or less, and preferably 0.05 parts by mass or less, relative to 100 parts by mass of the saturated polyester.
[0122] The number average molecular weight of the low shrinkage agent is, for example, 5,000 or more, preferably 10,000 or more, and, for example, 200,000 or less, preferably 100,000 or less.
[0123] The low shrinkage agent may be used alone or in combination of two or more.
[0124] Alternatively, the low shrinkage agent can be dissolved in a polymerizable monomer to prepare a polymerizable monomer solution of the low shrinkage agent.
[0125] In the polymerizable monomer solution of the low-shrinkage agent, the solid content concentration of the low-shrinkage agent is, for example, 20 mass % or more, and for example, 70 mass % or less.
[0126] The mixing ratio of the low shrinkage agent relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 20 parts by mass or less.
[0127] The resin component preferably contains a radical polymerizable resin and a low shrinkage agent. More preferably, the resin component consists of a radical polymerizable resin and a low shrinkage agent.
[0128] <Aluminum hydroxide>
[0129] Aluminum hydroxide is added to impart flame retardancy and to provide transparency and depth.
[0130] The mixing ratio of aluminum hydroxide is 30 parts by mass or more, preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and 300 parts by mass or less, preferably 200 parts by mass or less, per 100 parts by mass of the resin component.
[0131] The average particle size of aluminum hydroxide is, for example, 1 μm or more, and for example, 50 μm or less, and preferably 25 μm or less.
[0132] The average particle size of aluminum hydroxide can be determined by preparing a particle size distribution curve using a laser diffraction-scattering particle size distribution analyzer and calculating the particle size corresponding to 50% by mass.
[0133] Expanded Graphite
[0134] Expanded graphite is a graphite intercalation compound formed by intercalating sulfuric acid or other substances between the layers of flaky natural graphite. Expanded graphite expands at temperatures of approximately 150-300°C, causing the interlayers to expand.
[0135] The average particle size of the expanded graphite is 150 μm or less, preferably 100 μm or less, and for example, 10 μm or more, preferably 50 μm or more.
[0136] The average particle size of expanded graphite can be determined by observing 50 arbitrary expanded graphites with an optical microscope, measuring the maximum diameter (long diameter) and the particle diameter in a direction perpendicular to the maximum diameter (short diameter), and calculating the average of the long diameter and the short diameter.
[0137] As the expanded graphite, a commercially available product may be used, and a specific example thereof is 9510045 produced by Ito Graphite Industries, Ltd.
[0138] The mixing ratio of expanded graphite will be described later.
[0139] Flame retardants
[0140] Flame retardants include phosphorus-containing flame retardants and nitrogen-containing flame retardants.
[0141] Examples of the phosphorus-containing flame retardant include red phosphorus, phosphoric acid esters, polyphosphates, and metal phosphonates.
[0142] Examples of the phosphoric acid ester include trimethyl phosphate, triethyl phosphate, tributyl phosphate, and tricresyl phosphate.
[0143] Examples of the polyphosphate include ammonium polyphosphate and aluminum polyphosphate.
[0144] Examples of the metal phosphonate salt include tris(diethylphosphonate)aluminum and tris(methylethylphosphonate)aluminum.
[0145] Furthermore, commercially available phosphorus-containing flame retardants can be used, and specific examples thereof include the OP series (specifically, Exolit OP1230 (aluminum tris(diethylphosphonate)), manufactured by Clariant Chemicals).
[0146] As the phosphorus-containing flame retardant, preferably, a phosphonic acid metal salt is used, and more preferably, tris(diethylphosphonate)aluminum is used.
[0147] The phosphorus-containing flame retardants can be used alone or in combination of two or more.
[0148] The phosphorus-containing flame retardant is incorporated in an amount of, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and for example, 25 parts by mass or less, preferably 20 parts by mass or less, and more preferably 18 parts by mass or less per 100 parts by mass of the resin component.
[0149] The phosphorus content of the phosphorus-containing flame retardant will be described later.
[0150] Nitrogen-containing flame retardants are additives used to inhibit the thermal decomposition of phosphorus-containing flame retardants. Specifically, nitrogen-containing flame retardants generate gas during thermal decomposition. This gas inhibits the thermal decomposition of the phosphorus-containing flame retardant. As a result, thermal insulation properties (post-combustion discoloration properties (described later)) can be improved.
[0151] Examples of nitrogen-containing flame retardants include triazine compounds.
[0152] The triazine compound is a compound having a triazine skeleton. Examples of the triazine compound include melamine, methylguanamine, benzoguanamine, melam, melem, succinoguanamine, ethylenebis(melamine), melamine polyphosphate, guanamine, and melamine cyanurate.
[0153] Furthermore, a commercially available nitrogen-containing flame retardant may be used, and a specific example thereof is MC-4000 (melamine cyanurate, manufactured by Nissan Chemical Industries, Ltd.).
[0154] As the nitrogen-containing flame retardant, preferably, a triazine compound is used, and as the nitrogen-containing flame retardant, more preferably, melamine cyanurate is used.
[0155] The nitrogen-containing flame retardants can be used alone or in combination of two or more.
[0156] The mixing ratio of the nitrogen-containing flame retardant relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 4 parts by mass or more, and, for example, 25 parts by mass or less, preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and further preferably 12 parts by mass or less.
[0157] The nitrogen content of the nitrogen-containing flame retardant will be described later.
[0158] In addition, the flame retardant may contain other flame retardants in addition to the phosphorus-containing flame retardant and the nitrogen-containing flame retardant.
[0159] Examples of other flame retardants include halogen flame retardants, antimony trioxide, zinc stannate, and zinc borate.
[0160] Other flame retardants may be used alone or in combination of two or more.
[0161] The flame retardant preferably does not contain other flame retardants and is composed of a phosphorus-containing flame retardant and a nitrogen-containing flame retardant.
[0162] Furthermore, the resin composition can be obtained by mixing a resin component, aluminum hydroxide, expanded graphite, and a flame retardant.
[0163] Furthermore, additives may be blended into the resin composition as needed within a range that does not impair the effects of the present invention.
[0164] Examples of additives include polymerization inhibitors, curing agents, wetting and dispersing agents, colorants, mold release agents, thickeners, pattern materials, antimicrobial agents, hydrophilic agents, photocatalysts, ultraviolet absorbers, ultraviolet stabilizers, separation inhibitors, silane coupling agents, antistatic agents, thixotropic agents, thixotropic stabilizers, fillers (excluding aluminum hydroxide), and polymerization accelerators. These additives may be used alone or in combination of two or more.
[0165] The polymerization inhibitor is added to adjust the pot life and curing reaction.
[0166] Examples of polymerization inhibitors include hydroquinone compounds, benzoquinone compounds, catechol compounds, phenolic compounds, and N-oxyl compounds. Preferred polymerization inhibitors include benzoquinone compounds. Examples of benzoquinone compounds include p-benzoquinone and methyl-p-benzoquinone. Preferred benzoquinone compounds include p-benzoquinone.
[0167] The mixing ratio of the polymerization inhibitor relative to 100 parts by mass of the resin component is, for example, 0.001 parts by mass or more, preferably 0.1 parts by mass or more, and for example, 0.5 parts by mass or less.
[0168] As a curing agent, for example, peroxides can be mentioned. As peroxides, for example, benzoyl peroxide, tert-butyl peroxyisopropyl carbonate, tert-amyl peroxyisopropyl monocarbonate, tert-hexyl peroxyisopropyl monocarbonate, 1,1-bis(tert-butylperoxy)cyclohexane, tert-butyl peroxy-2-ethylhexanoate, amyl peroxy-2-ethylhexanoate, 2-ethylhexyl peroxy-2-ethylhexanoate, tert-butyl peroxybenzoate, tert-hexyl peroxybenzoate and tert-hexyl peroxyacetate can be mentioned. As a curing agent, tert-butyl peroxyisopropyl carbonate can be preferably mentioned.
[0169] The curing agent can be used alone or in combination of two or more.
[0170] The mixing ratio of the curing agent relative to 100 parts by mass of the resin component is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and, for example, 5 parts by mass or less, preferably 2 parts by mass or less.
[0171] The wetting and dispersing agent is formulated to optimize the viscosity of the resin composition.
[0172] Examples of the wetting and dispersing agent include copolymers having an acid group, phosphoric acid polyesters, and alkylammonium salts.
[0173] As the copolymer having an acid group, specifically, BYK-W995, BYK-W996, BYK-W9010 (all manufactured by BYK-CHEMIE) and the like can be used.
[0174] Examples of the alkylammonium salt include alkylammonium salts of high molecular weight copolymers, and specifically BYK-9076 manufactured by BYK-CHEMIE, which has an amine value of 44 mg / KOH / g and an acid value of 38 mg / KOH / g, can be used.
[0175] The wetting and dispersing agents may be used alone or in combination of two or more. Preferred examples of the wetting and dispersing agents include combinations of copolymers having an acid group and alkylammonium salts.
[0176] The mixing ratio of the wetting and dispersing agent per 100 parts by mass of the resin component is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more, more preferably 1 part by mass or more, and for example, 5 parts by mass or less, preferably 2 parts by mass or less.
[0177] The colorant is not particularly limited, and examples of the colorant include polyester toners mixed with known pigments such as titanium oxide, carbon black, red iron oxide, and phthalocyanine blue.
[0178] As the colorant, preferably, polyester toner is used.
[0179] The coloring agents can be used alone or in combination of two or more.
[0180] The mixing ratio of the colorant relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 20 parts by mass or less.
[0181] Examples of release agents include fatty acids, fatty acid metal salts, liquid waxes, fluoropolymers, and silicon-based polymers. Examples of fatty acids include stearic acid and lauric acid. Examples of fatty acid metal salts include zinc stearate and calcium stearate.
[0182] As the release agent, preferably, a fatty acid metal salt is used, and more preferably, zinc stearate is used.
[0183] The release agents can be used alone or in combination of two or more.
[0184] The mixing ratio of the release agent relative to 100 parts by mass of the resin component is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less.
[0185] The thickener is added to thicken the resin composition to a viscosity suitable for heat compression molding. The thickener is preferably added before (preferably immediately before) impregnation of reinforcing fibers (described later) with the resin composition.
[0186] Examples of thickeners include alkaline earth metal oxides and alkaline earth metal hydroxides. Examples of alkaline earth metal oxides include magnesium oxide. Examples of alkaline earth metal hydroxides include magnesium hydroxide and calcium hydroxide.
[0187] Preferred examples of thickeners include alkaline earth metal oxides, and more preferred examples of thickeners include magnesium oxide.
[0188] The thickeners can be used alone or in combination of two or more.
[0189] The mixing ratio of the thickener relative to 100 parts by mass of the resin component is, for example, 0.5 parts by mass or more, and for example, 10 parts by mass or less, or preferably 3 parts by mass or less.
[0190] Through the above, a resin composition can be obtained.
[0191] Furthermore, in this resin composition, the content of expanded graphite, the phosphorus content of the phosphorus-containing flame retardant, the mass ratio of the nitrogen content of the nitrogen-containing flame retardant to the phosphorus content of the phosphorus-containing flame retardant (nitrogen content / phosphorus content), and the mass ratio of the expanded graphite content to the phosphorus content of the phosphorus-containing flame retardant (expanded graphite content / phosphorus content) are adjusted to within predetermined ranges.
[0192] The heat insulation and moldability can be improved. The heat insulation can be estimated based on the post-combustion strength measured by the combustion test described below and the post-combustion discoloration measured by the flame resistance test described below.
[0193] Post-combustion strength refers to the strength of a molded article obtained using the resin composition after heating under predetermined conditions. If the thermal insulation is excellent, the strength is maintained even after heating. On the other hand, if the thermal insulation is poor, the strength may decrease after heating, causing the molded article to deform.
[0194] In addition, the post-combustion discoloration property indicates whether a molded article obtained using the resin composition changes color when exposed to a flame under predetermined conditions. If the heat insulation property is excellent, no color change occurs, while if the heat insulation property is low, color change occurs.
[0195] Specifically, the blending ratio of the expanded graphite per 100 parts by mass of the resin component is 1.0 parts by mass or more, preferably 1.5 parts by mass or more, more preferably 2.0 parts by mass or more, even more preferably 2.5 parts by mass or more, and particularly preferably 2.7 parts by mass or more, and is less than 5.0 parts by mass, preferably 4.8 parts by mass or less, more preferably 4.5 parts by mass or less, and even more preferably 4.3 parts by mass or less.
[0196] When the blending ratio of the expanded graphite is not less than the above lower limit, excellent heat insulating properties (discoloration after combustion) are achieved.
[0197] On the other hand, if the blending ratio of the expanded graphite is less than the above lower limit, the heat insulating properties (discoloration after combustion) will be reduced.
[0198] If the expanded graphite content is less than the upper limit, the thermal insulation (post-combustion strength) is excellent. On the other hand, if the expanded graphite content is greater than the upper limit, the thermal insulation (post-combustion strength) is reduced.
[0199] If the expanded graphite content is below the upper limit, the thermal insulation (post-combustion strength) is excellent. On the other hand, if the expanded graphite content exceeds the upper limit, the thermal insulation (post-combustion strength) is reduced.
[0200] In addition, the phosphorus content of the phosphorus-containing flame retardant is 1.5 parts by mass or more, preferably 2.0 parts by mass or more, more preferably 2.5 parts by mass or more, further preferably 3.0 parts by mass or more, particularly preferably 3.5 parts by mass or more, and is 4.5 parts by mass or less, preferably 4.0 parts by mass or less, relative to 100 parts by mass of the resin component.
[0201] When the phosphorus content is at least the above lower limit, excellent heat insulating properties (discoloration after burning and strength after burning) will be achieved.
[0202] On the other hand, if the phosphorus content is less than the lower limit, heat insulation properties (discoloration after burning and strength after burning) are reduced.
[0203] Moreover, when the phosphorus content is at most the upper limit, excellent moldability is achieved.
[0204] On the other hand, when the phosphorus content exceeds the upper limit, moldability decreases.
[0205] The phosphorus content of the phosphorus-containing flame retardant can be calculated by multiplying the phosphorus content of the phosphorus-containing flame retardant by the phosphorus content. The phosphorus content can be calculated by multiplying the phosphorus content in the molecular formula of the phosphorus-containing flame retardant by the atomic weight of phosphorus and dividing the result by the molecular weight of the phosphorus-containing flame retardant.
[0206] In addition, the mass ratio of the nitrogen content of the nitrogen-containing flame retardant relative to 100 parts by mass of the resin component to the phosphorus content of the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component (nitrogen content / phosphorus content) is 0.5 or more, preferably 0.6 or more, and is 3.0 or less, preferably 2.5 or less, more preferably 2.0 or less, further preferably 1.5 or less, and particularly preferably 1.0 or less.
[0207] When the mass ratio (nitrogen content / phosphorus content) is at least the above lower limit, the heat insulating properties (discoloration after burning) will be excellent.
[0208] On the other hand, if the mass ratio (nitrogen content / phosphorus content) is less than the lower limit, the heat insulating properties (discoloration after combustion) decrease.
[0209] Moreover, when the said mass ratio (nitrogen content / phosphorus content) is below the said upper limit, the heat insulation property (discoloration property after burning) becomes excellent.
[0210] On the other hand, when the mass ratio (nitrogen content / phosphorus content) exceeds the upper limit, the heat insulating properties (discoloration after combustion) decrease.
[0211] The nitrogen content of the nitrogen-containing flame retardant can be calculated by multiplying the nitrogen content by the nitrogen content. The nitrogen content can be calculated by multiplying the number of nitrogen atoms in the molecular formula of the nitrogen-containing flame retardant by the atomic weight of nitrogen and dividing the obtained amount by the molecular weight of the nitrogen-containing flame retardant.
[0212] The mass ratio of the content of the expanded graphite relative to 100 parts by mass of the resin component to the content of phosphorus in the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component (expanded graphite content / phosphorus content) is 0.5 or more, preferably 0.7 or more, and is 2.0 or less, preferably 1.5 or less, and more preferably 1.0 or less.
[0213] When the mass ratio (expanded graphite content / phosphorus content) is not less than the above lower limit, excellent heat insulating properties (post-combustion discoloration properties) will be achieved.
[0214] On the other hand, if the mass ratio (expanded graphite content / phosphorus content) is less than the lower limit, the heat insulating properties (post-combustion discoloration properties) are reduced.
[0215] Moreover, when the mass ratio (content of expanded graphite / content of phosphorus) is equal to or less than the upper limit, the thermal insulation properties (post-combustion strength) are excellent.
[0216] On the other hand, when the mass ratio (expanded graphite content / phosphorus content) exceeds the upper limit, the thermal insulation properties (post-combustion strength) decrease.
[0217] In addition, the above-mentioned mass ratio can be calculated by dividing the content (added amount) of expanded graphite by the above-mentioned content of phosphorus.
[0218] In addition, as a ratio other than the above ratio, the nitrogen content of the nitrogen-containing flame retardant is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, more preferably 2.3 parts by mass or more, and, for example, 5.0 parts by mass or less, preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less, and further preferably 2.8 parts by mass or less, relative to 100 parts by mass of the resin component.
[0219] When the nitrogen content is at least the above lower limit, excellent heat insulating properties (discoloration after burning) will be achieved.
[0220] Moreover, when the nitrogen content is not more than the above upper limit, the heat insulating properties (discoloration after combustion) are excellent.
[0221] Furthermore, the resin composition can produce a molded article having excellent heat insulation and moldability.
[0222] In order to produce a molded article using such a resin composition, a molding material is first prepared.
[0223] In order to prepare a molding material, reinforcing fibers are blended into a resin composition.
[0224] Examples of reinforcing fibers include inorganic fibers, organic fibers, and natural fibers. Examples of inorganic fibers include glass fibers, carbon fibers, metal fibers, and ceramic fibers. Examples of organic fibers include polyvinyl alcohol fibers, polyester fibers, polyamide fibers, fluororesin fibers, and phenol fibers. Examples of natural fibers include hemp and kenaf.
[0225] Preferred examples of reinforcing fibers include inorganic fibers, and more preferred examples of reinforcing fibers include glass fibers.
[0226] Examples of the shape of the reinforcing fibers include cloth (e.g., roving cloth), mat (e.g., chopped strand mat, preformable mat, continuous strand mat, and surfacing mat), tow yarn, roving, nonwoven fabric, and paper.
[0227] The length of the reinforcing fibers is not particularly limited, and is, for example, 1.5 mm or more, preferably 5 mm or more, more preferably 15 mm or more from the viewpoint of improving strength, and is, for example, 80 mm or less, preferably 40 mm or less.
[0228] The molding material is obtained as, for example, a sheet-shaped molding material by impregnating reinforcing fibers with the resin composition.
[0229] As a method for preparing the molding material, known methods can be used. Specifically, SMC (sheet molding compound), TMC (thick molding compound), and BMC (bulk molding compound) can be used. SMC is preferred.
[0230] The content ratio of the reinforcing fibers relative to the molding material is, for example, 15 mass % or more, and for example, 60 mass % or less.
[0231] In this manner, a molding material containing the resin composition and the reinforcing fibers can be obtained.
[0232] Next, the molding material is aged in order to increase its viscosity so as to enable heat compression molding (described later).
[0233] During the aging, the aging temperature is, for example, 20° C. or higher and 50° C. or lower.
[0234] The aging time is, for example, 8 hours or longer, and for example, 120 hours or shorter.
[0235] Thus, the molding material is maintained in, for example, a sheet-like shape. In other words, the molding material has a sheet shape.
[0236] Furthermore, the molded article can be obtained by heating and compression molding a molding material using a known method.
[0237] The conditions for heat compression molding can be appropriately set depending on the purpose and application. In heat compression molding, the molding temperature is, for example, 100°C or higher, and for example, 200°C or lower. The molding pressure is, for example, 0.1 MPa or higher, preferably 1 MPa or higher, more preferably 5 MPa or higher, and for example, 20 MPa or lower, and preferably 15 MPa or lower.
[0238] Thus, the molding material is shaped and solidified to obtain a molded product.
[0239] This molded article contains a cured product of the molding material and therefore has excellent thermal insulation properties.
[0240] The thickness of the molded article is, for example, 0.1 mm or more, preferably 1.0 mm or more, and, for example, 10 mm or less, preferably 5 mm or less.
[0241] Such molded products can be widely used in, for example, building materials, housings, casting materials, mechanical parts (such as battery boxes for electric vehicles), electronic and electrical parts, and various components of vehicles, ships, and aircraft.
[0242] In particular, battery packs for electric vehicles may require excellent heat insulation to slow down the spread of fire in the event of a vehicle fire.
[0243] On the other hand, the molded article has excellent heat insulation properties and can therefore be suitably used in battery cases for electric vehicles.
[0244] Effects
[0245] Resin combination includes expanded graphite and flame retardant, as flame retardant, including phosphorus-containing flame retardant and nitrogen-containing flame retardant. Moreover, in this resin combination, the mass ratio (nitrogen content / phosphorus content) of the content of expanded graphite, the content of phosphorus of phosphorus-containing flame retardant, the content of nitrogen of nitrogen-containing flame retardant relative to the content of phosphorus of phosphorus-containing flame retardant and the mass ratio (content of expanded graphite / phosphorus content) of the content of expanded graphite relative to the content of phosphorus of phosphorus-containing flame retardant are predetermined ranges. Therefore, it is possible to produce a molded product with excellent heat insulation and formability.
[0246] Specifically, as described above, the heat insulating property can be estimated from the post-combustion strength and the post-combustion discoloration.
[0247] As mentioned above, expanded graphite expands at temperatures of approximately 150-300°C, causing the interlayers to expand. The expanded graphite forms a heat-insulating layer, improving thermal insulation properties. Therefore, if the proportion of expanded graphite is low, discoloration after combustion tends to decrease.
[0248] On the other hand, the mechanical strength of expanded graphite decreases after expansion. Therefore, if the blending ratio of expanded graphite is high, the strength after combustion tends to decrease.
[0249] Therefore, in this resin composition, by adjusting the blending ratio of expanded graphite within a predetermined range, both post-combustion discoloration resistance and post-combustion strength can be achieved, and as a result, the heat insulating properties can be improved.
[0250] Furthermore, phosphorus-containing flame retardants impart flame retardancy, and therefore, if the phosphorus content of the phosphorus-containing flame retardant is low, the heat insulating properties (discoloration after combustion and strength after combustion) tend to decrease.
[0251] On the other hand, when the phosphorus content of the phosphorus-containing flame retardant increases, moldability tends to decrease.
[0252] Therefore, in this resin composition, by setting the phosphorus content of the phosphorus-containing flame retardant within a predetermined range, it is possible to achieve both thermal insulation and moldability.
[0253] Furthermore, as described above, the gas generated by the thermal decomposition of the nitrogen-containing flame retardant inhibits the thermal decomposition of the phosphorus-containing flame retardant.
[0254] Therefore, if the nitrogen-containing flame retardant is present in a sufficient amount relative to the phosphorus-containing flame retardant, thermal decomposition of the phosphorus-containing flame retardant can be suppressed, and as a result, the post-combustion discoloration property can be improved.
[0255] In other words, if the mass ratio of the nitrogen content of the nitrogen-containing flame retardant to the phosphorus content of the phosphorus-containing flame retardant (nitrogen content / phosphorus content) becomes smaller (the nitrogen-containing flame retardant is less than the phosphorus-containing flame retardant), the discoloration after combustion decreases.
[0256] On the other hand, if the mass ratio of the nitrogen content of the nitrogen-containing flame retardant to the phosphorus content of the phosphorus-containing flame retardant (nitrogen content / phosphorus content) increases (more nitrogen-containing flame retardant than phosphorus-containing flame retardant), the post-combustion discoloration property decreases.
[0257] In this resin composition, since the mass ratio of the nitrogen content of the nitrogen-containing flame retardant to the phosphorus content of the phosphorus-containing flame retardant (nitrogen content / phosphorus content) is within a predetermined range, the post-combustion discoloration property can be improved.
[0258] Furthermore, if the mass ratio of the expanded graphite content to the phosphorus content of the phosphorus-containing flame retardant (expanded graphite content / phosphorus content) is low (the phosphorus content of the phosphorus-containing flame retardant is higher than that of the expanded graphite), phosphorus inhibits the expansion of the expanded graphite, thereby reducing thermal insulation properties and post-combustion discoloration properties.
[0259] On the other hand, if the mass ratio of the expanded graphite content to the phosphorus content of the phosphorus-containing flame retardant (expanded graphite content / phosphorus content) is large (the phosphorus content of the phosphorus-containing flame retardant is low relative to the expanded graphite), the layer formed by the expansion of the expanded graphite is likely to collapse during combustion, thereby reducing thermal insulation properties and post-combustion strength.
[0260] In this resin composition, since the mass ratio of the expanded graphite content to the phosphorus content of the phosphorus-containing flame retardant (expanded graphite content / phosphorus content) is within a predetermined range, the heat insulation properties (post-combustion discoloration and post-combustion strength) can be improved.
[0261] In summary, in this resin composition, by setting the content of expanded graphite, the phosphorus content of the phosphorus-containing flame retardant, the mass ratio of the nitrogen content of the nitrogen-containing flame retardant to the phosphorus content of the phosphorus-containing flame retardant (nitrogen content / phosphorus content), and the mass ratio of the content of expanded graphite to the phosphorus content of the phosphorus-containing flame retardant (expanded graphite content / phosphorus content) to within predetermined ranges, it is possible to achieve a balance between thermal insulation and moldability.
[0262] The molding material contains the above-mentioned resin composition, and thus, a molded product having excellent heat insulation and moldability can be produced.
[0263] The molded product comprises a cured product of the above-mentioned molding material, and therefore has excellent thermal insulation and moldability.
[0264] Example
[0265] The specific numerical values of the mixing ratio (content ratio), physical property values, parameters, etc. used in the following descriptions may replace the upper limit values (defined as "less than" or "less than") or lower limit values (defined as "more than" or "more than") of the corresponding mixing ratio (content ratio), physical property values, parameters, etc. described in the above "Specific Embodiments". In addition, unless otherwise specified in the following descriptions, "parts" and "%" are based on mass.
[0266] <Details of ingredients>
[0267] The details of the active ingredients used in the following Examples and Comparative Examples are shown below.
[0268] Unsaturated polyester resin 1: unsaturated polyester resin of Synthesis Example 1, styrene content 40% by mass
[0269] Unsaturated polyester resin 2: unsaturated polyester resin of Synthesis Example 2, styrene content 40% by mass
[0270] Vinyl ester resin: the vinyl ester resin of Synthesis Example 3, styrene content 40% by mass
[0271] Saturated polyester resin: low shrinkage agent, saturated polyester resin of Synthesis Example 4, styrene content 40% by mass
[0272] Styrene-based thermoplastic elastomer solution: low shrinkage agent, G1701, manufactured by Kraton Polymers
[0273] Polyvinyl acetate solution: low shrinkage agent, polyvinyl acetate (number average molecular weight 30,000) styrene content 65% by mass
[0274] Polystyrene solution: low shrinkage agent, polystyrene (number average molecular weight about 110,000) with a styrene content of 65% by mass
[0275] Polyethylene powder: low shrinkage agent
[0276] Copolymer with acid groups: BYK-W9010, manufactured by BYK-CHEMIE
[0277] Alkyl ammonium salt of high molecular weight copolymer: BYK-9076, manufactured by BYK-CHEMIE
[0278] 9510045: Expanded graphite, average particle size 70 μm, Ito Graphite Industries, Ltd.
[0279] OP1230: phosphorus-containing flame retardant, aluminum tris(diethylphosphonate), phosphorus content 24% by mass, trade name "Exolit OP1230", manufactured by Clariant Chemicals
[0280] MC-4000: Nitrogen-containing flame retardant, melamine cyanurate, nitrogen content 49% by mass, trade name "MC-4000", manufactured by Nissan Chemical Co., Ltd.
[0281] Aluminum hydroxide: average particle size 8μm
[0282] <Preparation of unsaturated polyester resin>
[0283] Synthesis example 1
[0284] In a flask equipped with a thermometer, a nitrogen inlet tube, a reflux cooler, and a stirrer, 10.0 mol of maleic anhydride, 6.5 mol of propylene glycol, and 4.0 mol of neopentyl glycol were added. Then, a polycondensation reaction was carried out at 200°C to 210°C while stirring under a nitrogen atmosphere. Thus, an unsaturated polyester having an acid value of 26.5 mgKOH / g was obtained. In addition, the method for determining the acid value was in accordance with JIS K6901 (2008). Next, 0.02 parts by mass of hydroquinone and 66.7 parts by mass of styrene as a polymerization inhibitor were added to 100 parts by mass of the unsaturated polyester, and the mixture was uniformly mixed. Thus, an unsaturated polyester resin (styrene content 40% by mass) was obtained.
[0285] Synthesis example 2
[0286] In a flask equipped with a thermometer, a nitrogen inlet tube, a reflux cooler, and a stirrer, 3.3 mol of isophthalic acid and 10.5 mol of propylene glycol were added. Then, a polycondensation reaction was carried out at 200°C to 210°C while stirring under a nitrogen atmosphere. Then, the reaction product was cooled to 150°C when the acid value reached 20 mgKOH / g. Next, 6.7 mol of maleic anhydride was added, and the reaction was again carried out at 210°C to 220°C. An unsaturated polyester with an acid value of 27.5 mgKOH / g was obtained. 0.01 parts by mass of hydroquinone and 66.7 parts by mass of styrene as a polymerization inhibitor were added to 100 parts by mass of the unsaturated polyester, and they were uniformly mixed. Thus, an unsaturated polyester resin (styrene content 40% by mass) was obtained.
[0287] <Preparation of Vinyl Ester Resin>
[0288] Synthesis example 3
[0289] In a flask equipped with a stirrer, a reflux cooler, and a gas inlet tube, 1850 parts by mass (10.0 equivalents) of a bisphenol A-type epoxy compound (epoxy equivalent 185 g / eq), 317 parts by mass (2.78 equivalents) of bisphenol A, and 1.0 part by mass of triethylbenzylammonium chloride as a catalyst were added. Subsequently, the mixture was reacted at 170°C for 5 hours while blowing nitrogen gas. This yielded an epoxy resin (bisphenol-type epoxy resin) with an epoxy equivalent of 298 g / eq. The mixture was then cooled to 120°C, and 1.0 part by mass of hydroquinone (polymerization inhibitor), 5.0 parts by mass of triethylbenzylammonium chloride (catalyst), and 636 parts by mass (7.40 equivalents) of methacrylic acid were added. Subsequently, the mixture was reacted at 110°C for 8 hours while blowing air. This yielded a vinyl ester with an acid value of 8.0 mgKOH / g. Next, 1869 parts by mass of styrene (66.7 parts by mass relative to 100 parts by mass of vinyl ester) was added to the vinyl ester to obtain a vinyl ester resin (styrene content: 40% by mass).
[0290] <Preparation of saturated polyester resin>
[0291] Synthesis example 4
[0292] In a flask equipped with a thermometer, a nitrogen inlet tube, a reflux cooler, and a stirrer, 4.0 mol of isophthalic acid and 10.5 mol of neopentyl glycol were added. A polycondensation reaction was then carried out at 200°C to 210°C while stirring under a nitrogen atmosphere. The reaction product was then cooled to 150°C when its acid value reached 10 mgKOH / g. Subsequently, 6.0 mol of adipic acid was added, and the reaction was again carried out at 210°C to 220°C. Thus, a saturated polyester having an acid value of 9.5 mgKOH / g was obtained. To 100 parts by mass of this saturated polyester, 0.015 parts by mass of hydroquinone and 66.7 parts by mass of styrene were added as polymerization inhibitors and uniformly mixed. Thus, a saturated polyester resin (styrene content 40% by mass) was obtained.
[0293] <Manufacturing of Resin Composition, Molding Material, and Molded Article>
[0294] Examples 1 to 12 and Comparative Examples 1 to 13
[0295] [Manufacturing of resin composition]
[0296] Resin compositions were prepared by blending the components according to the descriptions in Tables 1 to 4. The thickener was blended immediately before impregnating the reinforcing fibers with the resin composition.
[0297] [Manufacturing of molding materials]
[0298] Using a known sheet molding compound (SMC) impregnation machine, glass roving was continuously cut into 25 mm pieces onto the resin composition applied to a carrier film using a doctor blade. This was then added to a glass fiber content of 35% by mass (25.5% by volume). This impregnation process yielded a molding material (sheet molding compound (SMC)). This molding material was then aged at 40°C for 48 hours to increase its viscosity until it reached a state suitable for heat compression molding.
[0299] [Manufacturing of molded products]
[0300] The molding material was heated and compression molded using a 300 mm × 300 mm flat metal plate to produce flat molded products with a thickness of 2.5 mm and a thickness of 2.3 mm, respectively.
[0301] Molding was performed under the following conditions: a mold temperature of 140°C on both the product surface and back, a molding pressure of 10 MPa, and a mold hold time of 300 seconds. The molded product was then released from the mold and immediately sandwiched between iron plates for cooling. This produced a flat plate-shaped molded product.
[0302] <Evaluation>
[0303] [Thermal insulation]
[0304] (Combustion test)
[0305] Test pieces (85 mm x 25 mm) were cut from the molded products (thickness 2.5 mm) of each Example and Comparative Example. The test pieces were then placed in a crucible and treated in an electric furnace at 600°C for 1 hour. After cooling to room temperature, the pieces were removed from the furnace and the state of the test pieces was confirmed. The post-combustion strength was evaluated based on the following criteria. The results are shown in Tables 1 to 4.
[0306] {Benchmark}
[0307] ○: The test piece can be grasped with fingers.
[0308] ×: I tried to grab the test piece with my fingers, but it collapsed.
[0309] (Flame resistance test)
[0310] Test pieces (150 mm x 150 mm) were cut from the molded products (thickness 2.3 mm) of each embodiment and each comparative example. Next, a commercially available cooking burner (box-type gas cooking burner CJ2 manufactured by Iwatani Industry) was used to adjust the inner flame length of the burner to about 40 mm and the temperature at the front end of the inner flame to about 1000°C. Furthermore, the center of the test piece was fixed at a position 40 mm away from the front end of the burner and perpendicular to it. The burner was ignited and stopped after 5 minutes, and the state of the molded plate was visually observed. The above test was carried out 5 times. The post-combustion strength was evaluated based on the following criteria. The results are shown in Tables 1 to 4.
[0311] {Benchmark}
[0312] ○: The number of times the back surface of the test piece was scorched and discolored was 0 to 1.
[0313] △: The back surface of the test piece was burned and discolored twice.
[0314] ×: The back surface of the test piece was burned and discolored 3 to 5 times.
[0315] (Moldability)
[0316] The molding materials of each embodiment and each comparative example were cut into 15cm×15cm pieces and four pieces were overlapped. They were placed in the center of a 300mm×300mm flat metal plate, and the mold temperature was set to 140°C on both the product surface and the back surface. The mold was heated under the conditions of a molding pressure of 10MPa and a holding time in the mold of 300 seconds. Thus, a molded product was manufactured. The molded product was then demolded from the mold and immediately sandwiched between iron plates for cooling. The moldability was evaluated based on the following criteria. The results are shown in Tables 1 to 4.
[0317] {Benchmark}
[0318] ○: The resin composition is filled to the edge of the molded article.
[0319] ×: The resin composition was not filled to the edge of the molded article.
[0320] (Bending Strength)
[0321] The flexural strength of the molded articles (thickness 2.3 mm) of each Example and each Comparative Example was measured at 23° C. in accordance with JIS K 7017 (1999). The results are shown in Tables 1 to 4.
[0322] Table 1
[0323]
[0324] Table 2
[0325]
[0326] Table 3
[0327]
[0328] Table 4
[0329]
[0330] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but is merely an illustration and should not be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are also included in the scope of the claims.
[0331] Industrial applicability
[0332] The resin composition, molding material, and molded article of the present invention can be suitably used for producing a battery case, for example.
Claims
1. A resin composition comprising a resin component, aluminum hydroxide, expanded graphite and a flame retardant, The flame retardant comprises a phosphorus-containing flame retardant and a nitrogen-containing flame retardant, The content of the expanded graphite is 1.0 part by mass or more and less than 5.0 parts by mass relative to 100 parts by mass of the resin component. The phosphorus content of the phosphorus-containing flame retardant is 1.5 parts by mass or more and 4.5 parts by mass or less relative to 100 parts by mass of the resin component. The mass ratio of the content of nitrogen in the nitrogen-containing flame retardant relative to 100 parts by mass of the resin component to the content of phosphorus in the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component is 0.5 or more and 3.0 or less, A mass ratio of the content of the expanded graphite relative to 100 parts by mass of the resin component to the content of phosphorus in the phosphorus-containing flame retardant relative to 100 parts by mass of the resin component is 0.5 or more and 2.0 or less.
2. The resin composition according to claim 1, in, The nitrogen content of the nitrogen-containing flame retardant is 2.0 parts by mass or more and 3.0 parts by mass or less relative to 100 parts by mass of the resin component.
3. A molding material comprising the resin composition according to claim 1 and reinforcing fibers.
4. A molded article comprising a cured product of the molding material according to claim 3.