Composite particles, method for producing composite particles, and cosmetic

By attaching rubber particles to the surface of organic resin particles and using silica binders, composite particles with a soft touch, smooth feel, and natural makeup finish are prepared. This solves the problems of hardness of organic resin particles and microplastic hazards, and improves the environmental friendliness and user experience of cosmetics.

CN118891326APending Publication Date: 2024-11-01SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032402.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-03-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing organic resin particles used in cosmetics have problems such as being hard to the touch, having poor extensibility, and being difficult to biodegrade. Furthermore, microplastics pose a potential hazard to the ecosystem.

Method used

By attaching rubber particles to the surface of organic resin particles and using silica as a binder to form composite particles, and then combining cationic and alkaline substances to carry out hydrolysis and condensation reactions, composite particles that can impart a soft touch, smooth feel, and natural makeup look are prepared.

Benefits of technology

It achieves the effects of a soft touch, smooth application, and natural makeup finish in cosmetics, while reducing the environmental hazards of microplastics and improving the biodegradability of particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891326A_ABST
    Figure CN118891326A_ABST
Patent Text Reader

Abstract

The present invention provides composite particles in which rubber particles are adhered to the surfaces of spherical organic resin particles, the composite particles being characterized in that the rubber particles are adhered to the organic resin particles using silica as a binder. Consequently, provided are: composite particles which are obtained by adhering rubber particles to the surfaces of organic resin particles, and which are capable of imparting a soft texture, a smooth feeling in use, ductility, and a natural makeup feeling due to light scattering properties; a method for producing the composite particles; and a cosmetic containing the composite particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to composite particles, and more particularly to composite particles in which rubber particles are attached to the surface of organic resin particles, a method for producing the composite particles, and a cosmetic containing the composite particles. Background Art

[0002] Spherical particles of organic resins (plastics) such as polyamide resins, polyacrylic resins, polystyrene resins, silicone resins (polyorganosilisesquioxanes), etc. are used in cosmetics such as foundations to give a smooth feel and ductility. In addition, since they scatter light, they can also give a natural makeup effect without unnatural gloss (oily sheen). Since these particles are resins (plastics), they have the disadvantage of being hard to the touch.

[0003] Microplastics, which are water-insoluble solids with a diameter of less than 5 mm, and chemical substances contained or adsorbed thereon, may be brought into the food chain, etc., and their impact on the ecosystem is worrying. It is also a high-profile issue worldwide, and even some national authorities are considering restricting it. This kind of microplastic made into particles is very small in size and difficult to recycle when it flows into rivers, oceans, ponds, etc. In addition, the aforementioned organic resin particles decompose very slowly in the natural environment. Therefore, it is proposed to use cellulose particles from natural substances in cosmetics (Patent Document 1). However, although cellulose particles are biodegradable, they have the disadvantages of low smoothness and hard touch.

[0004] Patent document 2 proposes a cosmetic that uses composite particles formed by attaching a silicone elastomer to the surface of particles (mother particles). The light diffusion property of the silicone elastomer enhances the natural makeup feel and obtains a soft and moist touch. A specific example is given: using silicone resin (polysilsesquioxane) as a binder to adhere the silicone elastomer to the surface of the particles. When the mother particle of the composite particle is an organic resin, the smoothness is poorer than that of an inorganic particle, and sometimes further leads to poor ductility and the generation of floating powder. It is believed that the reason is that the organic resin of the mother particle and the silicone resin of the binder are not hard like inorganic particles.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. WO2020 / 004604

[0008] Patent Document 2: Japanese Patent Application Publication No. 2011-1332 Summary of the invention

[0009] 1. Technical issues to be resolved

[0010] The present invention has been made in view of the above circumstances, and its object is to provide composite particles formed by attaching rubber particles to the surface of organic resin particles, which can impart soft touch and smooth feeling during use, ductility, and a natural makeup effect due to light scattering, and a method for producing the same, as well as a cosmetic containing the composite particles.

[0011] (II) Technical solution

[0012] In order to solve the above technical problems, the present invention provides a composite particle, which is a composite particle in which rubber particles are attached to the surface of spherical organic resin particles, and the rubber particles are fixed to the organic resin particles using silicon dioxide as a binder.

[0013] Such composite particles can provide a soft touch, a smooth feel during use, spreadability, and a natural makeup effect due to light scattering properties.

[0014] Furthermore, it is preferred that the amount of the rubber particles is in the range of 0.1 to 100 parts by mass relative to 100 parts by mass of the organic resin particles.

[0015] When the amount of the rubber particles is such, the cosmetic can be provided with a more pronounced soft touch and smooth feeling during use, spreadability, and light scattering property, and can also be made to have low cohesion.

[0016] Furthermore, it is preferred that the amount of the silica is in the range of 10 to 1,000 parts by mass relative to 100 parts by mass of the rubber particles.

[0017] When the amount of silica is within this range, the rubber particles can be more reliably fixed to the surface of the organic resin particles, and a soft touch can be imparted to the cosmetic.

[0018] Furthermore, it is preferred that the rubber particles are silicone rubber particles.

[0019] In the present invention, such rubber particles can be preferably used.

[0020] Furthermore, it is preferred that the organic resin particles are cellulose particles.

[0021] In the present invention, such organic resin particles can be preferably used.

[0022] In addition, the present invention provides a method for producing composite particles, which is the method for producing the above-mentioned composite particles, wherein:

[0023] A tetraalkoxysilane is added to a mixed solution of the organic resin particles, the rubber particles, a cationic substance, an alkaline substance and water to perform a hydrolysis and condensation reaction, wherein:

[0024] The cationic substance is a cationic surfactant and / or a cationic water-soluble polymer.

[0025] In this way, the composite particles of the present invention can be produced.

[0026] Furthermore, it is preferable that the cationic substance be a cationic surfactant or a cationic water-soluble polymer.

[0027] Thereby, the composite particles of the present invention can be produced more reliably.

[0028] Furthermore, it is preferred that the amount of the cationic substance blended is within a range of 0.0001 to 2.0 parts by mass relative to 100 parts by mass of water in the mixed liquid.

[0029] As a result, the rubber particles adhere to the surfaces of the organic resin particles, and the adhesion by silica is sufficient.

[0030] Furthermore, it is preferred that the amount of the cationic surfactant blended is in the range of 0.001 to 1.9 parts by mass relative to 100 parts by mass of water in the mixed solution, and the amount of the cationic water-soluble polymer blended is in the range of 0.0001 to 1.0 parts by mass relative to 100 parts by mass of water in the mixed solution.

[0031] In this way, the rubber particles are more reliably attached to the surfaces of the organic resin particles, and the adhesion by silica is sufficient.

[0032] Furthermore, the present invention provides a cosmetic containing the above-mentioned composite particles.

[0033] The cosmetic of the present invention is a cosmetic having a soft touch, a smooth feeling during use, spreadability, and a natural makeup feel due to light scattering properties.

[0034] (III) Beneficial effects

[0035] According to the present invention, composite particles capable of imparting soft touch, smooth feel during use, spreadability, and a natural makeup effect due to light scattering, a method for producing the same, and a cosmetic containing the composite particles can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is an electron microscope photograph of the composite particles obtained in Example 1.

[0037] Figure 2 This is an electron microscope photograph of the composite particles obtained in Example 2.

[0038] Figure 3 This is an electron microscope photograph of the composite particles obtained in Example 3.

[0039] Figure 4 These are electron microscope photographs of cellulose particles used in Examples and Comparative Examples.

[0040] Figure 5 The figures show the results of measuring the oil absorption of the composite particles of Examples and the cellulose particles of Comparative Examples. DETAILED DESCRIPTION

[0041] As described above, it is necessary to develop composite particles formed by attaching rubber particles to the surface of organic resin particles, which can provide soft touch and smooth feeling during use, spreadability, and a natural makeup effect due to light scattering, and a production method thereof, as well as a cosmetic containing the composite particles.

[0042] The inventors of the present invention have repeatedly conducted in-depth studies on the above-mentioned problems and found that composite particles in which rubber particles are bonded to the surface of spherical organic resin particles using silica as a binder can give cosmetics a soft touch and smooth feel, ductility, and a natural makeup effect due to light scattering, thereby completing the present invention.

[0043] That is, the present invention provides composite particles in which rubber particles are attached to the surface of spherical organic resin particles, and the rubber particles are fixed to the organic resin particles using silica as a binder.

[0044] In addition, the present invention is a method for producing composite particles, which is the method for producing the above-mentioned composite particles, wherein tetraalkoxysilane is added to a mixed solution formed by blending the organic resin particles, the rubber particles, a cationic substance, an alkaline substance and water, thereby performing hydrolysis and condensation reactions, wherein the cationic substance is set to a cationic surfactant and / or a cationic water-soluble polymer.

[0045] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following contents.

[0046] [Composite particles]

[0047] The composite particles of the present invention are composite particles in which rubber particles are attached to the surface of spherical organic resin particles, and the rubber particles are fixed to the organic resin particles using silica as a binder.

[0048] The volume average particle size can be measured by the Coulter counter method (electrical resistance method). The particle size is determined by the particle size of the organic resin particles, the particle size of the rubber particles, and the amount of rubber particles attached to the surface of the organic resin particles.

[0049] [Organic resin particles]

[0050] The organic resin particles used in the present invention are particles that become the core of the composite particles. The organic resin particles can be used alone or in combination of two or more, and as long as they are spherical, they can be powders that can be used in cosmetics and particles of all particle sizes.

[0051] The shape of the organic resin particles is spherical. In this specification, "spherical" refers not only to the shape of the particles being a true sphere, but also to a deformed sphere in which the length of the longest axis / the length of the shortest axis (aspect ratio) is generally 1.0 to 4.0, preferably 1.0 to 2.0, more preferably 1.0 to 1.6, and further preferably 1.0 to 1.4 on average. The shape of the particles can be confirmed by observing the particles using an optical microscope, an electron microscope, etc. The structure of the particles can be either non-porous or porous.

[0052] The volume average particle size is preferably in the range of 0.5 to 50 μm, more preferably 1 to 30 μm. If the particle size is 0.5 μm or more, the effect of imparting a refreshing feeling, smoothness, and ductility can be fully obtained, and if it is 50 μm or less, the roughness can be reduced. In addition, the volume average particle size is measured by the Coulter counter method (resistance method).

[0053] Examples of organic resin particles include polyethylene, polypropylene, polystyrene, divinylbenzene resin, polyvinyl chloride, methacrylic acid resin, polytetrafluoroethylene, methacrylic acid-styrene copolymer, polyamide, polycarbonate, polyesters such as polyethylene terephthalate, polybutylene succinate, polyhydroxybutyrate, and polycaprolactone, cellulose, cellulose derivatives, calcium alginate, phenolic resin, melamine resin, benzoguanamine resin, epoxy resin, and polyurethane particles.

[0054] When biodegradable properties are required, examples include particles of polybutylene succinate, polyhydroxybutyrate, polycaprolactone, cellulose, and cellulose derivatives such as cellulose acetate and cellulose acetate propionate. Furthermore, when natural substances are required, cellulose particles are included.

[0055] [Rubber particles]

[0056] The rubber particles used in the present invention are particles attached to the surface of organic resin particles as the core of the composite particles. The rubber particles can be used alone or in combination of two or more, and can be applied to powders that can be used in cosmetics and particles of all particle sizes. In addition, the geometric form can be any shape commonly used in cosmetics, and can be any shape of sphere, polyhedron, spindle, needle, plate, etc., and can be any of non-porous and porous.

[0057] The volume average particle size of the rubber particles is preferably smaller than that of the organic resin particles. If the volume average particle size is smaller than that of the organic resin particles as the core powder, the soft touch and smooth feel, ductility, light scattering and other characteristics of the powder will be fully exhibited. The volume average particle size is preferably in the range of 0.05 to 5 μm, more preferably 0.1 to 1 μm. In addition, the volume average particle size is measured by a laser diffraction / scattering method.

[0058] The rubber constituting the rubber particles is preferably non-sticky, and its rubber hardness is preferably in the range of 5 to 95 when measured using a type A durometer specified in JIS K6253, and more preferably 10 to 70. If the rubber hardness is 5 or more, the cohesion becomes low, and good smoothness and ductility can be given to the cosmetics, so that floating powder will not be generated. If the rubber hardness is 95 or less, a soft touch can be obtained. In addition, the rubber hardness refers to the value measured by making a test piece of the shape and size specified in JIS K6253 according to the composition of the particles.

[0059] Examples of the rubber particles include particles of polybutadiene rubber, acrylic rubber, urethane rubber, silicone rubber, fluororubber, etc. Silicone rubber particles are preferred because they can easily provide a soft touch.

[0060] Silicone rubber can be made of 2 / 2 )a-represented by a cured product of a linear organosiloxane block. Here, R in the formula is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms. a is a positive integer of 5 to 5,000.

[0061] The number of carbon atoms of R is 1 to 30, preferably 1 to 22, and more preferably 1 to 18. Examples of R include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, decyl, undecyl, dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, triacontyl; aryl groups such as phenyl, tolyl, naphthyl; aralkyl groups such as benzyl and phenethyl; alkenyl groups such as vinyl and allyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; and hydrocarbon groups in which some or all of the hydrogen atoms bonded to carbon atoms of these groups are substituted with atoms such as halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms) and / or substituents such as acryloyloxy, methacryloyloxy, epoxy, glycidyloxy, and carboxyl. Preferably, it is an alkyl group having 1 to 18 carbon atoms or a phenyl group, and preferably 50 mol% or more of all R are methyl groups.

[0062] Silicone rubber can be obtained from a curable liquid silicone composition, and the curing can be exemplified by curing by addition reaction, condensation reaction, free radical reaction, etc. The curable liquid silicone composition refers to a composition containing a component having a reactive group for the above curing reaction (a substance having both reactive groups, a component having one reactive group and a component having the other reactive group), a curing catalyst, and a free radical generator.

[0063] When the silicone rubber is cured by addition reaction, the curable liquid silicone composition may include (A) an organopolysiloxane having an alkenyl group, (B) an organohydrogenpolysiloxane having a hydrogen atom bonded to a silicon atom, and an addition reaction catalyst.

[0064] The component (A) is an organopolysiloxane having at least two alkenyl groups in one molecule and represented by the following average composition formula (1). 1 Each of R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms and not having an alkenyl group. 2 Each of them is independently an alkenyl group having a carbon number of 2 to 6. b and c are positive numbers satisfying 0<b<3, 0<c≤3, and 0.1≤b+c≤3.

[0065] R 1 b R 2 c SiO (4-b-c) / 2 (1)

[0066] The organopolysiloxane represented by the average composition formula (1) may be used alone or in combination of two or more.

[0067] R 1 The number of carbon atoms in R is 1 to 30, preferably 1 to 22, and more preferably 1 to 18. 1 Among the groups listed for R above, monovalent hydrocarbon groups other than alkenyl groups can be mentioned. 1 Preferably, 50 mol % or more of the groups are methyl groups. 2 Examples thereof include vinyl, allyl, propenyl, butenyl, pentenyl, and hexenyl, and vinyl is preferred. b and c are preferably positive numbers satisfying 0<b≤2.295, 0.005≤c≤2.3, and 0.5≤b+c≤2.3.

[0068] The viscosity of the component (A) at 25°C is preferably 100,000 mm 2 / s or less, more preferably 10,000 mm 2 / s or less. If the viscosity is 100,000mm 2 / s or less, it is particularly easy to obtain silicone microparticles with a narrow particle size distribution in the preparation of the aqueous dispersion of silicone rubber particles described later. The lower limit of the viscosity is not particularly limited, but is 0.7 mm 2 / s or more, especially 2mm 2 In the present invention, the value of the kinematic viscosity may be a value measured at 25° C. using a capillary viscometer.

[0069] In addition, the structure of component (A) may be any of linear, cyclic and branched, preferably linear or branched with fewer branch units. The bonding site of the alkenyl group is not particularly limited, and it may be bonded to any silicon atom on the side chain and the terminal of the molecule, and is particularly preferably bonded to the silicon atoms at both terminals of the linear organopolysiloxane.

[0070] Examples of the linear structure include a structure represented by the following general formula (2).

[0071] [Chemical formula 1]

[0072]

[0073] (Where R 1 , R 2 Same as above, d is a positive number, e is 0 or a positive number, and f is 0, 1, 2, or 3, where e and f are numbers that satisfy e+2×f≥2. )

[0074] Examples of the branched structure include: 1 SiO 3 / 2 The units form a branched structure represented by the following general formula (3).

[0075] [Chemical formula 2]

[0076]

[0077] (Where R 1 , R 2 Same as above, g is a positive number, h is 0 or a positive number, i is a positive number, j is 0, 1, 2 or 3, where h and j are numbers that satisfy h+j≥1. )

[0078] As SiO 4 / 2 The structure in which the unit forms a branch includes, for example, a structure represented by the following general formula (4).

[0079] [Chemical formula 3]

[0080]

[0081] (Where R 1 , R 2Same as above, k is a positive number, l is 0 or a positive number, m is a positive number, and n is 0, 1, 2 or 3, where l and n are numbers that satisfy 1+n≥1. )

[0082] Furthermore, a structure having two or more alkenyl groups per molecule represented by the following unit formula (5) can be exemplified.

[0083] [R 1 3SiO 1 / 2 ] o [R 2 (R 1 )2SiO 1 / 2 ] p [SiO 4 / 2 ] q [(OR 3 )SiO 3 / 2 ] r (5)

[0084] (Where R 1 , R 2 Same as above, R 3 is a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, o is 0 or a positive number, p is a positive number, q is a positive number, and r is 0 or a positive number.)

[0085] Component (B) is an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms (referred to as SiH groups) in one molecule and represented by the following average composition formula (6). 4 Each is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 30 carbon atoms and not having an alkenyl group. s and t are numbers satisfying 0<s<3, 0<t≤3, and 0.1≤s+t≤3.

[0086] R 4 s H t SiO (4-s-t) / 2 (6)

[0087] The organopolysiloxane represented by the average composition formula (6) may be used alone or in combination of two or more.

[0088] R 4 The number of carbon atoms in R is 1 to 30, preferably 1 to 22, and more preferably 1 to 18. 4 We can list the 1 The same monovalent hydrocarbon group preferably has methyl groups in an amount of 80 mol% or more, and more preferably 95 mol% or more. s and t are preferably positive numbers satisfying 0<s≤2.295, 0.005≤t≤2.3, and 0.5≤s+t≤2.3.

[0089] The viscosity of the component (B) at 25°C is preferably 100,000 mm 2 / s or less, more preferably 10,000 mm 2 / s or less. If the viscosity is 100,000mm 2 / s or less, it is particularly easy to obtain silicone microparticles with a narrow particle size distribution in the preparation of the aqueous dispersion of silicone rubber particles described later. The lower limit of the viscosity is not particularly limited, but is 0.4 mm 2 / s or more, especially 2mm 2 / s or above.

[0090] In addition, the structure of component (B) may be any of linear, cyclic, and branched, preferably linear or branched. In addition, the bonding site of the hydrogen atom bonded to the silicon atom is not particularly limited, and the hydrogen atom may be bonded to the silicon atom at any of the side chains and ends of the molecule.

[0091] Examples of the linear structure include a structure represented by the following general formula (7).

[0092] [Chemical formula 4]

[0093]

[0094] (Where R 4 Same as above, u is a positive number, v is 0 or a positive number, and w is 0, 1, 2, or 3, where v and w are numbers that satisfy v+2×w≥2. )

[0095] Examples of the branched structure include: 4 SiO 3 / 2 The units form a branched structure represented by the following general formula (8).

[0096] [Chemical formula 5]

[0097]

[0098] (Where R 4 Same as above, x is a positive number, y is 0 or a positive number, z is a positive number, a1 is 0, 1, 2 or 3, where y and a1 are numbers that satisfy y+a1≥1. )

[0099] As SiO 4 / 2 The unit forms a branched structure, and an example thereof is a structure represented by the following general formula (9).

[0100] [Chemical formula 6]

[0101]

[0102] (Where R 4Same as above, b1 is a positive number, c1 is 0 or a positive number, d1 is a positive number, e1 is 0, 1, 2 or 3, where c1 and e1 are numbers that satisfy c1+e1≥1. )

[0103] In addition, there can be mentioned a structure represented by the following unit formula (10) having two or more hydrogen atoms bonded to silicon atoms per molecule.

[0104] [R 4 3SiO 1 / 2 ] f1 [H(R 4 )2SiO 1 / 3 ] g1 [SiO 4 / 2 ] h1 [(OR 5 )SiO 3 / 2 ] i1 (10)

[0105] In the formula, R 4 Same as above, R 5 is a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, f1 is 0 or a positive number, g1 is a positive number, h1 is a positive number, and i1 is 0 or a positive number.

[0106] As described above, component (A) is an organopolysiloxane having two or more alkenyl groups in one molecule, and component (B) is an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule. However, the combination of an organopolysiloxane (A) having only two alkenyl groups and an organohydrogenpolysiloxane (B) having only two SiH groups is excluded. The reason is that the combination of an organopolysiloxane having two alkenyl groups as component (A) and an organohydrogensiloxane having two SiH groups as component (B) will cause the cured product to be sticky, and silicone rubber cannot be obtained. That is, when component (A) has two alkenyl groups, at least one of components (B) is an organohydrogensiloxane having three or more SiH groups, and when component (B) has two SiH groups, at least one of components (A) is an organosiloxane having three or more alkenyl groups.

[0107] The amount of component (B) relative to component (A) is preferably such that the number ratio of SiH groups in component (B) to monovalent olefin groups in component (A) is 0.5 to 2, and more preferably such that the number ratio is 0.7 to 1.5. When component (B) is blended in an amount in which the number ratio of SiH groups is within the above range, the obtained silicone rubber cured product is not sticky and has moderate reactivity.

[0108] Examples of the addition reaction catalyst include platinum group metal catalysts used in hydrosilylation reactions. For example, the present invention can include: platinum (including platinum black), rhodium, palladium and other platinum group metal single substances; platinum chloride, chloroplatinic acid and chloroplatinates such as H2PtCl4·XH2O, H2PtCl6·XH2O, NaHPtCl6·XH2O, KHPtCl6·XH2O, Na2PtCl6·XH2O, K2PtCl4·XH2O, PtCl4·XH2O, PtCl2, Na2HPtCl4·XH2O (wherein, X is an integer of 0 to 6, preferably 0 or 6); alcohol-modified chloroplatinic acid; complexes of platinum chloride, chloroplatinic acid and olefins, complexes of chloroplatinic acid and vinyl-containing siloxanes, and complexes of platinum and vinyl-containing siloxanes; compounds in which platinum group metals such as platinum black and palladium are supported on carriers such as alumina, silica, and carbon; rhodium-olefin complexes; tris(triphenylphosphine)rhodium chloride (Wilkinson catalyst), etc. One type may be used alone, or two or more types may be used simultaneously.

[0109] The amount of the platinum group metal catalyst to be added may be an effective amount as a hydrosilylation reaction catalyst. The amount of the platinum group metal in the platinum group metal catalyst is generally about 0.1 to 500 ppm, preferably about 0.5 to 200 ppm, and more preferably about 1 to 100 ppm, calculated on a mass basis, relative to the total amount of the components (A) and (B).

[0110] Silicone rubber may also contain silicone oil, organic silane, inorganic powder, organic powder, antioxidant and the like.

[0111] In the present invention, the density of the rubber particles attached to the surface of the organic resin particles is not particularly limited. That is, the rubber particles may be sparsely attached to the surface of the organic resin particles, or may cover and attach to the surface of the organic resin particles without gaps. In addition, the rubber particles may be attached in a state of being agglomerated with each other, or may be a structure in which rubber particles are further attached to the rubber particles that cover and attach to the surface of the organic resin particles without gaps. The attachment density or state of the rubber particles can be confirmed using an electron microscope.

[0112] The amount of rubber particles is not particularly limited. When more pronounced soft touch and smooth feel, ductility, and light scattering are required, the amount is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, further preferably 0.5 parts by mass or more, and further preferably 0.8 parts by mass or more, relative to 100 parts by mass of organic resin particles. In addition, from the perspective of obtaining low cohesion, smooth feel, and ductility, the amount is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, further preferably 20 parts by mass or less, and further preferably 10 parts by mass or less, relative to 100 parts by mass of organic resin particles.

[0113] [Silicon dioxide]

[0114] The silicon dioxide used in the present invention is a binder for the organic resin particles and the rubber particles. By making composite particles in which the rubber particles are attached to the surface of the organic resin particles using silicon dioxide as a binder, the rubber particles are fixed to the surface of the organic resin particles and are not easily detached from the surface of the organic resin particles, which can provide a better feeling of use.

[0115] The shape of the silica may be film-like or particle-like, and the silica may be attached to the entire or a part of the surface of the organic resin particles and / or the entire or a part of the surface of the rubber particles.

[0116] Silica has a structure composed of SiO2 units. The method for producing the silicon dioxide is not particularly limited, but the silicon dioxide is preferably obtained by hydrolysis and condensation reaction of tetraalkoxysilane according to the production method described below.

[0117] The amount of silica is not particularly limited, but in order to make the rubber particles adhere to the surface of the organic resin particles, it is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, further preferably 30 parts by mass or more, and further preferably 50 parts by mass or more, relative to 100 parts by mass of the rubber particles. In addition, from the perspective of obtaining a soft touch, it is preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, further preferably 500 parts by mass or less, and further preferably 350 parts by mass or less, relative to 100 parts by mass of the rubber particles.

[0118] [Surface treatment agent]

[0119] The composite particles of the present invention may be surface treated with silylating agents, silicone oils, waxes, paraffins, organic fluorine compounds, surfactants, etc. to impart or enhance water repellency and improve dispersibility in oils.

[0120] [Method for producing composite particles]

[0121] The composite particles of the present invention, in which rubber particles are attached to the surface of organic resin particles using silica as a binder, can be obtained by adding tetraalkoxysilane to a mixed solution of organic resin particles, rubber particles, a cationic substance (cationic surfactant and / or a cationic water-soluble polymer), an alkaline substance and water to carry out hydrolysis and condensation reactions.

[0122] [Organic resin particles and rubber particles]

[0123] The organic resin particles and rubber particles used are those described in the section of composite particles, but those prepared in advance as aqueous dispersions or aqueous dispersions synthesized in water may also be used.

[0124] In order to disperse the organic resin particles and rubber particles in water, a surfactant and a water-soluble polymer may be added to the aqueous dispersion. In addition, when an aqueous dispersion synthesized in water is used, the surfactant and water-soluble polymer used during the synthesis may also be included in the aqueous dispersion.

[0125] The surfactant is not particularly limited, but is preferably a nonionic surfactant, a cationic surfactant and / or an amphoteric surfactant.

[0126] Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerol fatty acid esters, polyoxyethylene glycerol fatty acid esters, polyglycerol fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene hydrogenated castor oil fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene modified organopolysiloxanes, and polyoxyethylene polyoxypropylene modified organopolysiloxanes.

[0127] The cationic surfactant is not particularly limited, and examples thereof include alkyltrimethylammonium salts, dialkyldimethylammonium salts, polyoxyethylene alkyldimethylammonium salts, dimeroxyethylene alkylmethylammonium salts, trimeroxyethylene alkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, and monoalkylamidoamine salts.

[0128] Examples of the amphoteric surfactant include alkyl dimethyl amine oxide, alkyl dimethyl carboxy betaine, alkyl amidopropyl dimethyl carboxy betaine, alkyl hydroxysulfonate betaine, and alkyl carboxymethyl hydroxyethyl imidazolinium betaine.

[0129] The water-soluble polymer is not particularly limited, but is preferably a nonionic water-soluble polymer and / or a cationic water-soluble polymer.

[0130] Examples of the nonionic water-soluble polymer include polyvinyl alcohol, polyacrylamide, polyvinyl pyrrolidone, polyethylene oxide, polymethyl vinyl ether, polyisopropylacrylamide, methylcellulose, hydroxypropylmethylcellulose, starch, guar gum, and xanthan gum.

[0131] Examples of the cationic water-soluble polymer include polymers of dimethyldiallylammonium chloride, polymers of vinylimidazoline, polymers of methylvinylimidazolium chloride, polymers of ethyltrimethylammonium chloride of acrylate, polymers of ethyltrimethylammonium chloride of methacrylate, polymers of acrylamidopropyltrimethylammonium chloride, polymers of methacrylamidopropyltrimethylammonium chloride, epichlorohydrin / dimethylamine polymers, polymers of ethyleneimine, quaternary products of polymers of ethyleneimine, polymers of allylamine hydrochloride, polylysine, cationic starch, cationized cellulose, chitosan, and derivatives of the above compounds obtained by copolymerizing the above compounds with monomers having nonionic groups or anionic groups.

[0132] When silicone rubber particles are used for the rubber particles, it is preferred to use a substance prepared as an aqueous dispersion of silicone rubber particles.

[0133] The method for preparing the aqueous dispersion of silicone rubber particles is not particularly limited, and a known method for preparing the aqueous dispersion of silicone rubber particles can be used. For example, it can be prepared by emulsifying the curable liquid silicone composition described in the composite particle section in water using the above-mentioned surfactant and / or the above-mentioned water-soluble polymer, and then performing a curing reaction.

[0134] When curing is performed by addition reaction to prepare an aqueous dispersion of silicone rubber particles, the following method can be cited: a method in which the above-mentioned surfactant and / or the above-mentioned water-soluble polymer and water are added to a curable liquid silicone composition to emulsify, and after preparing an emulsion, a platinum-based catalyst is added to perform addition polymerization, wherein the curable liquid silicone composition is composed of an organopolysiloxane (A) having an alkenyl group and an organohydrogenpolysiloxane (B) having a hydrogen atom bonded to a silicon atom as described in the section on composite particles. Alternatively, a platinum-group metal-based catalyst may be pre-blended into the curable liquid silicone composition, in which case the reaction is prevented from proceeding before the end of the emulsification by adjusting the temperature, adjusting the amount of the catalyst, or blending a control agent.

[0135] In a mixed solution formed by blending organic resin particles, rubber particles, cationic substances, alkaline substances and water, the organic resin particles are preferably 3 to 150 parts by mass, more preferably 5 to 50 parts by mass, relative to 100 parts by mass of water blended. If it is 3 parts by mass or more, the manufacturing efficiency becomes high, and if it is 150 parts by mass or less, the kinematic viscosity of the aqueous dispersion (mixed solution) will not become too high, and the rubber particles are easy to adhere. The amount of rubber particles is set to the amount that adheres to the surface of the organic resin particles.

[0136] [Cationic substances]

[0137] The cationic surfactant and / or cationic water-soluble polymer added when producing the composite particles has the function of promoting the condensation reaction of the hydrolyzed tetraalkoxysilane and generating silica. In addition, it is presumed that it has the function of causing the generated silica to be adsorbed on the surface of the organic resin particles and rubber particles and causing the organic resin particles and rubber particles to be adsorbed.

[0138] The cationic surfactant and the cationic water-soluble polymer may be used alone or in combination of two or more thereof. It is preferred to use both of the cationic surfactant and the cationic water-soluble polymer in order to allow more rubber particles to adhere to the surface of the organic resin particles.

[0139] Examples of the cationic surfactant include the compounds described in the description of the method for producing the composite particles, and alkyl trimethylammonium salts are preferred, and among them, lauryl trimethylammonium salt and cetyl trimethylammonium salt are more preferred.

[0140] Examples of the cationic water-soluble polymer include the compounds described in the explanation of the method for producing the composite particles. Among them, a polymer that does not use a monomer having a nonionic group is preferred, and a polymer of dimethyldiallylammonium chloride is more preferred.

[0141] The cationic substance (cationic surfactant and / or cationic water-soluble polymer) is preferably in the range of 0.0001 to 2.0 parts by mass, more preferably in the range of 0.001 to 1.0 parts by mass, relative to 100 parts by mass of water added to the mixed solution. When the amount is 0.0001 to 2.0 parts by mass, the rubber particles adhere to the surface of the organic resin particles and the fixation by silica is sufficient.

[0142] Furthermore, it is preferred that the cationic surfactant is 0.001 to 1.9 parts by mass and the cationic water-soluble polymer is 0.0001 to 1.0 parts by mass, based on 100 parts by mass of water added to the mixed solution. It is more preferred that the cationic surfactant is 0.01 to 1.0 parts by mass and the cationic water-soluble polymer is 0.001 to 0.5 parts by mass. It is further preferred that the cationic surfactant is 0.05 to 0.5 parts by mass and the cationic water-soluble polymer is 0.01 to 0.2 parts by mass.

[0143] In addition, as described above, when a cationic surfactant and / or a cationic water-soluble polymer is used to disperse organic resin particles and rubber particles in water in advance to prepare an aqueous dispersion, if the cationic surfactant and / or a cationic water-soluble polymer are not of the required type and amount, they are additionally added; if they are of the required type and amount, there is no need to add them additionally.

[0144] The cationic surfactant and / or cationic water-soluble polymer may be blended in advance in the mixed solution of organic resin particles, rubber particles, alkaline substance and water, or may be added simultaneously with the addition of the tetraalkoxysilane described below.

[0145] [Alkaline substances]

[0146] The alkaline substance is a catalyst for the hydrolysis and condensation reaction of tetraalkoxysilane.

[0147] The alkaline substance is not particularly limited, and examples thereof include alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, and lithium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide and barium hydroxide; alkali metal carbonates such as potassium carbonate and sodium carbonate; ammonia; tetraalkylammonium hydroxides such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; or amines such as monomethylamine, monoethylamine, monopropylamine, monobutylamine, monopentylamine, dimethylamine, diethylamine, trimethylamine, triethanolamine, and ethylenediamine. Among them, ammonia is most suitable in that it can be easily removed from the powder of the obtained composite particles by volatilization. As ammonia, a commercially available ammonia solution can be used.

[0148] The amount of the alkaline substance added is preferably an amount such that the pH of the mixed solution obtained by mixing the alkaline substance, organic resin particles, rubber particles, cationic surfactant and / or cationic water-soluble polymer, and water is at least 9.0 to 12.0, and more preferably an amount such that the pH is 9.5 to 11.5. When the alkaline substance is added in an amount such that the pH is 9.0 to 12.0, the hydrolysis and condensation reaction of the tetraalkoxysilane proceeds and the rubber particles are sufficiently fixed to the surface of the organic resin particles.

[0149] [Tetraalkoxysilane]

[0150] In the method for producing composite particles of the present invention, tetraalkoxysilane is added to a mixed solution of organic resin particles, rubber particles, a cationic surfactant and / or a cationic water-soluble polymer, an alkaline substance, and water.

[0151] Tetraalkoxysilane undergoes hydrolysis and condensation reaction under the catalytic action of alkaline substances, and further becomes silicon dioxide. After the addition of tetraalkoxysilane, silicon dioxide generated by the hydrolysis and condensation reaction of tetraalkoxysilane is formed on the surface of organic resin particles and / or the surface of rubber particles, and at the same time, the rubber particles are adsorbed on the surface of the organic resin particles, thereby forming a state in which the rubber particles are fixed to the surface of the organic resin particles through the silicon dioxide.

[0152] Tetraalkoxysilane is composed of Si(OR 6 )4 represents. R in the formula 6The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms. Specifically, methyl, ethyl, propyl, butyl, pentyl, hexyl, etc. can be cited, and methyl and ethyl are more preferred in terms of reactivity. That is, tetramethoxysilane and tetraethoxysilane are more preferred, and tetramethoxysilane is further preferred. Tetraalkoxysilane can also be a compound obtained by hydrolyzing part or all of the alkoxy groups. Further, a compound obtained by partially condensing can also be used.

[0153] The amount of tetraalkoxysilane added is not particularly limited as long as the amount of silica after the hydrolysis and condensation reaction is the above-mentioned amount relative to the amount of the rubber particles.

[0154] [Hydrolysis and condensation reaction]

[0155] While stirring and blending the mixed solution of organic resin particles, rubber particles, cationic surfactant and / or cationic water-soluble polymer, alkaline substance and water, tetraalkoxysilane is added to carry out hydrolysis and condensation reaction. The tetraalkoxysilane can be added dropwise gradually, or can be added in the form of being dissolved in water or dispersed in water, or can be added as a solution blended with a water-soluble organic solvent such as alcohol.

[0156] From the perspective of preventing the aggregation of organic resin particles and rubber particles, it is preferably set to slow stirring using paddle wings, propeller wings, swept wings, anchor wings, etc., and the stirring intensity is required to be such that the organic resin particles, rubber particles and tetraalkoxysilane are dispersed in the mixed liquid.

[0157] The temperature when adding tetraalkoxysilane to the mixed solution is preferably 0 to 60° C., more preferably 0 to 39° C. If the temperature is 0° C. or higher, there is no concern that the mixed solution will solidify, and if the temperature is 60° C. or lower, there is no concern that the obtained particles will aggregate.

[0158] A water-soluble organic solvent such as alcohol may be added to the mixed liquid for the purpose of improving the dispersibility of the organic resin particles and the rubber particles in water and for the purpose of making the rubber particles uniformly adhere to the surface of the organic resin particles.

[0159] When the particles are surface treated with a silylating agent, the finished composite particles may be treated, or the silylating agent may be added to the mixed solution after adding tetraalkoxysilane. Examples of the silylating agent include trimethylmethoxysilane, trimethylsilanol, hexamethyldisilazane, methyltrimethoxysilane, and phenyltrimethoxysilane.

[0160] After the tetraalkoxysilane is added, stirring is preferably continued for a period of time until the hydrolysis and condensation reactions are completed. In order to promote the reaction, heating may be performed at 40 to 100°C, and an alkaline substance may be added. Then, if necessary, an acidic substance may be added for neutralization.

[0161] After the hydrolysis and condensation reactions, water is removed. The removal of water can be carried out, for example, by heating the mixed solution after the reaction under normal pressure or reduced pressure. Specifically, there are methods of removing water by leaving the mixed solution to stand under heating; methods of removing water while stirring the mixed solution under heating to make it flow; methods of spraying the mixed solution in a hot air flow in the form of a spray dryer; methods of using a flowing heat medium, etc. In addition, as a pretreatment for this operation, the mixed solution can be concentrated by methods such as heating dehydration, filtration separation such as pressure filtration, centrifugal separation, decantation, etc., and the mixed solution can also be washed with water or alcohol as needed.

[0162] When the powder obtained by removing water from the mixed liquid after the reaction is agglomerated, it is preferably pulverized or classified by a pulverizer such as a jet mill, a ball mill, or a hammer mill.

[0163] [Cosmetics containing composite particles]

[0164] The cosmetic of the present invention is characterized by containing the composite particles. The cosmetic of the present invention is described in detail below. In addition, in the present invention, the name of the ingredient may be described in the cosmetic name or the International Nomenclature of Cosmetic Ingredient (INCI). When the cosmetic name corresponds to INCI, the English description may be omitted.

[0165] The present invention is applicable to various cosmetics, preferably cosmetics for external use on the skin such as skin care cosmetics, color makeup cosmetics, antiperspirant cosmetics, and anti-ultraviolet cosmetics, and cosmetics for external use on hair such as hair cosmetics. As skin care cosmetics, for example, lotions, emulsions, face creams, cleansing milks, facial masks, oils, massage materials, beauty essences, beauty oils, cleansers, deodorants, hand creams, lip balms, wrinkle-covering creams, etc. can be listed. As color makeup cosmetics, for example, primers, concealers, loose powders, pressed powders, eye makeup (eye color), eye shadows (eye shadows), mascara, eyeliners, eyebrow pencils, lipsticks, etc. can be listed. As antiperspirant cosmetics, for example, antiperspirant cosmetics such as roller ball type, cream type, solution type, and stick type can be listed. As anti-ultraviolet cosmetics, for example, sunscreen oils, sunscreen emulsions, and sunscreen creams can be listed. As hair cosmetics, for example, shampoos, conditioners, hair toners, and styling agents can be listed.

[0166] The form of the cosmetic of the present invention may be, for example, any of powder, oily liquid, water-in-oil emulsion, oil-in-water emulsion, non-aqueous emulsion, W / O / W type, O / W / O type, and other multiple emulsions. In addition, as the properties of the cosmetic of the present invention, various properties may be selected, such as liquid, emulsion, cream, solid, paste, gel, powder, cake, multi-layer, mousse, spray, stick, pencil, and the like.

[0167] There are no particular limitations on the cosmetics as long as they contain essential ingredients, and the cosmetics can be applied to, for example, skin care products, liquid foundations, pressed powders, concealers, lipsticks, and various products that impart sunscreen functions to these products.

[0168] The cosmetics of the present invention may contain various ingredients used in conventional cosmetics. For example, they may include (1) oil, (2) aqueous components, (3) surfactants, (4) powders other than those of the present invention, (5) a composition consisting of a crosslinked organopolysiloxane and an oil that is liquid at room temperature, (6) a film-forming agent, (7) an ultraviolet light absorbing and scattering agent, and (8) other additives. These ingredients may be used alone or in combination of two or more.

[0169] (1) Oil

[0170] The oil agent may be volatile or non-volatile, and may be any of solid, semi-solid, or liquid at room temperature (25° C.); examples thereof include silicone oil, silicone wax, natural animal and plant oils and fats and semi-synthetic oils, hydrocarbon oils, higher alcohols, fatty acids, ester oils, fluorine-based oils, and ultraviolet absorbers.

[0171] The composite particles of the present invention have high oil absorption for various liquid oils on the surface of the rubber particles. By absorbing the liquid oil, the stickiness and glare of the oil can be suppressed, and the effect of improving the feeling of use is high. In addition, the viscosity of the oil can be adjusted, or various properties such as a mousse can be obtained. The composite particles used in the present invention can be directly contained as a cosmetic ingredient, or an oily gel composition containing the composite particles and the oily component can be separately prepared for the purpose of showing the desired feeling of use of the cosmetic, and a cosmetic containing the composite particles and the oily component can be prepared in the form of the oily gel composition.

[0172] Silicone oil

[0173] Examples of the silicone oil include alkyl-modified silicones such as dimethicone (INCI), trisiloxane (INCI), methyl trimethicone (INCI), ethyl trisiloxane (INCI), ethyl methicone (INCI), and hexyl dimethicone (INCI), long-chain alkyl-modified silicones such as octyl methicone (INCI), phenyl trimethicone (INCI), diphenyl dimethicone (INCI), diphenylsiloxyphenyl trimethicone (INCI), tetraphenyl dimethyl disiloxane (INCI), and methyl hydrogen polysiloxane, and low-viscosity to high-viscosity linear or branched organopolysiloxanes, cyclic Cyclic organopolysiloxanes such as tetrasiloxane (INCI), cyclopentasiloxane (INCI), and cyclohexasiloxane (INCI), amino-modified organopolysiloxanes such as amodimethicone (INCI) and aminopropyldimethicone (INCI), pyrrolidone-modified organopolysiloxanes such as PCA dimethicone (INCI), pyrrolidonecarboxylic acid-modified organopolysiloxane, high-polymerization colloidal dimethylpolysiloxane, colloidal amino-modified organopolysiloxane, silicone rubber such as colloidal dimethylsiloxane-methylphenylsiloxane copolymer, and low-viscosity organopolysiloxane solutions of silicone or rubber, amino acid-modified silicone, fluorine-modified silicone, silicone resin, and silicone resin dissolutions, etc.

[0174] Examples of commercially available silicone oils include KF-96L-1cs, KF-96L-1.5cs, KF-96L-2cs, KF-96A-6cs, KF-4422, KF-54, KF-54HV, KF-56A, and KF-995 manufactured by Shin-Etsu Chemical Co., Ltd.

[0175] Solid oily ingredients

[0176] In the present invention, when the cosmetic is to be solidified, it is preferably blended with an oily component that is solid at 25° C. Examples of the oily component that is solid at 25° C. include waxes, hydrocarbons, esters, higher alcohols, and higher fatty acids that preferably have a melting point of 40° C. or higher, more preferably 60 to 110° C., and are not particularly limited as long as they are raw materials that can be generally blended in cosmetics.

[0177] Specific examples include carnauba wax (INCI: Copernicia Cerifera (Carnauba) Wax), sugar cane wax, candelilla wax (INCI: Euphorbia Cerifera (Candelilla) Wax), purified candelilla wax, rice wax, vegetable wax, jojoba seed wax, kapok wax, rice bran wax, bayberry fruit wax, shea butter, cocoa butter, Rhus Succedanea Fruit Wax (INCI: Rhus Succedanea Fruit Wax), montan wax (INCI: Montan Wax), vegetable waxes such as hydrogenated castor oil isostearate, beeswax, beef tallow, beef bone fat, pig fat (INCI: Lard), horse fat (INCI: Horse fat) and the like. Fat), lanolin, wool fat (INCI: Lanolin), animal wax such as flax, shellac wax, spermaceti, lanolin esters, lanolin fatty acid esters, semi-synthetic waxes such as beeswax acid esters, hydrogenated oils such as hydrogenated castor oil and hydrogenated coconut oil, paraffin wax, polyethylene, ceresin, ozokerite, microcrystalline wax and other hydrocarbon waxes, synthetic beeswax and other wax esters, amino acid stearyl esters such as dioctyldodecyl lauroyl glutamate, dioctyldodecyl lauroyl glutamate, dioctyldodecyl lauroyl glutamate, fatty acids such as stearic acid and behenic acid, and silicone waxes such as acrylic acid silicone resins of acrylic acid-organic silicon graft or block copolymers (acrylic acid-organic silicon graft copolymers manufactured by Shin-Etsu Chemical Co., Ltd.: KP-561P, 562P, etc.), or derivatives thereof, preferably one or more selected from the above substances.

[0178] Natural animal and plant oils and semi-synthetic oils

[0179] Examples of natural animal and plant oils and semi-synthetic oils include avocado oil (: Indicative name (INCI: Perseus Very grateful (Avocado) Oil)), linseed oil (: indicates the name (INCI: Common Linen (Linseed) Seed Oil)), Almond Oil (: Indicates the name (INCI: Prunus Sweet Almond (SweetAlmond) Oil)), Perilla Oil (Indicated Name), Olive Oil (Indicated Name (INCI: European Olive (Olive) Fruit Oil)), California Torreya Oil (: Indicates the name (INCI: Torreya Californica (California Nutmeg) Oil)), Citronella Oil (: indicates the name (INCI: Cymbopogon Nardus Citronella Oil)), Torreya grandis seed oil (: Indicated name (INCI: Torreya NuciferaSeed Oil)), almond oil (: indicates the name (INCI: KyouninYu)), wheat germ oil (: indicates the name (INCI: Common Wheat (Wheat) Germ Oil)), Sesame Seed Oil (: Indicated Name (INCI: Indian sesame (Sesame) Seed Oil)), wheat germ oil (: indicates the name (INCI: Common Wheat (Wheat) Germ Oil)), Rice Germ Oil (: Indicates the name (INCI: Rice (Rice) Germ Oil)), Rice Bran Oil (: Indicates the name (INCI: Rice (Rice) Bran Oil)), Camellia Oil (: Indicated Name (INCI: Camellia Kissi Seed Oil)), Safflower Oil (: Indicates the name (INCI: We are playing cards Dyer (Safflower) Seed Oil)), soybean oil (: indicates the name (INCI: Glycine Soja (Soybean) Oil)), Tea Seed Oil (: Indicates the name (INCI: Chinese Camellia Seed Oil)), Camellia Oil (: Indicates the name (INCI: Camellia Japonica Seed Oil)), Evening Primrose Oil (: Indicates the name (INCI: Evening Primrose (Evening Primrose) Oil)), Rapeseed Oil (denoted by name), Corn Germ Oil (denoted by name (INCI; Zea Mays (Corn) Germ Oil)), wheat germ oil (: indicates the name (INCI: Common Wheat (Wheat) Germ Oil)) and other germ oils, peach kernel oil (indicated name), palm oil (: indicated name (INCI: Guinean Olive (Palm)Oil)), Palm Kernel Oil (: indicates the name (INCI: Guinean Olive (Palm) Kernel Oil)), Castor Oil (: Indicates the name (INCI: Castor oil (Castor) Seed Oil)), Sunflower Oil (: Indicates the name (INCI: Helianthus Annuus (Sunflower) Seed Oil)), Grape Seed Oil (: Indicates the name (INCI: Vine Wine-growing (Grape) Seed Oil)), Jojoba Seed Oil (: Indicates the name (INCI: Simmondsia chinensis (Jojoba) Seed Oil)), Macadamia Seed Oil (: Indicated Name (INCI: Macadamia Ternifolia Seed Oil)), Limnanthes Alba Seed Oil (: Indicates the name (INCI: White Limnanthes (Meadowfoam) Seed Oil)), Cottonseed Oil (: Indicates the name (INCI: Gossypium Herbaceous (Cotton) Seed Oil)), Coconut Oil (: indicates the name (INCI: Cocos Nucifera (Coconut) Oil)), peanut oil (: indicates the name (INCI: Peanut Natural plant oils such as shark liver oil (INCI: Shark Liver oil), cod liver oil (INCI: Cod Liver Oil), cod liver oil (INCI: Fish Liver Oil), turtle oil (INCI: Turtle Oil), mink oil (INCI: Mink Oil), egg yolk oil (INCI: Egg Oil), and other natural animal oils; semi-synthetic oils such as hydrogenated coconut oil (INCI: Hydrogenated Coconut Oil) and liquid lanolin (INCI: Lanolin Oil).

[0180] Hydrocarbon oil

[0181] Examples of the hydrocarbon oil include linear or branched hydrocarbon oils, and may be volatile or non-volatile hydrocarbon oils. Specifically, examples include olefin oligomers (INCI), isoparaffins such as (C13,14) isoparaffin (INCI), isododecane (INCI), undecane (INCI), dodecane (INCI), isohexadecane (INCI), hydrogenated polyisobutene (INCI: Hydrogenated Polyisobutene), squalane (INCI), mineral oil (INCI), coconut alkane (INCI), and alkanes such as (C13-15) alkane (INCI).

[0182] ·Higher alcohols

[0183] Examples of the higher alcohols include alcohols having preferably 6 or more carbon atoms, and more preferably 10 to 30 carbon atoms. Specific examples of the higher alcohols include lauryl alcohol (INCI), myristyl alcohol (INCI), palmityl alcohol (INCI), stearyl alcohol (INCI), behenyl alcohol (INCI), oleyl alcohol (INCI), isostearyl alcohol (INCI), octyldodecanol (INCI), cholesterol (INCI), phytosterols (INCI), and batyl alcohol (INCI).

[0184] · Oil

[0185] Examples of the ester oil include diisobutyl adipate (INCI: Diisobutyl Adipate), dihexyldecyl adipate (INCI: Diheptylundecyl Adipate), isostearyl isostearate (INCI: Isostearyl Isostearate), and other n-alkyl glycol monoisostearate, isocetyl isostearate (INCI: Isocetyl Isostearate), trimethylolpropane triisostearate (INCI: Trimethylolpropane Triisostearate), glycol diethylhexanoate (INCI: Glycol Diethylhexanoate), cetyl ethylhexanoate (INCI: Cetyl Ethylhexanoate), trimethylolpropane triethylhexanoate (INCI: Trimethylolpropane Triethylhexanoate), Pentaerythrityl Tetraethylhexanoate, Cetyl Ethylhexanoate, Octyldodecyl Stearoyl Stearate, Oleyl Oleate, Octyldodecyl Oleate, Decyl Oleate, Neopentyl Glycol Diethylhexanoate, Neopentyl Glycol Dicaprate, etc. Dicaprate), diisostearyl malate (INCI: Diisostearyl Malate), triethyl citrate (INCI: Triethyl Citrate), diethylhexyl succinate (INCI: Diethylhexyl Succinate), amyl acetate (INCI: AmylAcetate), ethyl acetate (INCI: EtylAcetate), Butyl Acetate, Isocetyl Stearate, Butyl Stearate, Diisopropyl Sebacate, Diethylhexyl Sebacate, Cetyl Lactate, Myristyl Lactate, Isononyl Isononanoate, Isononyl Isononanoate, Isotridecyl Isononanoate, Isopropyl Palmitate Palmitate), ethylhexyl palmitate (INCI: EthylhexylIsopalmitate), isocetyl palmitate (INCI: Isocetyl Palmitate, HexyldecylPalmitate), palmitic acid esters such as cholesteryl hydroxystearate (INCI: CholesterylHydroxystearate), isopropyl myristate (INCI: Isopropyl Myristate), octyldodecyl myristate (INCI: Octyldodecyl Myristate), myristyl myristate (INCI: Myristyl Myristate), ethylhexyl laurate (INCI: Ethylhexyl Laurate), hexyl laurate (INCI: Hexyl Laurate), Dioctyldodecyl Lauroyl Glutamate (INCI: Dioctyldodecyl Lauroyl Glutamate), Isopropyl Lauroyl Sarcosinate (INCI: Isopropyl Lauroyl Sarcosinate), Coco-Caprylate / Caprate (INCI: Coco-Caprylate・Caprate), etc.

[0186] Among the ester oils, examples of the glyceride oil include triethylhexanoin (INCI), caprylic / capric triglyceride (INCI: Caprylic / Capric Triglyceride), cocoglyceryl (INCI), caprylic / capric / succinic triglyceride (INCI: Caprylic / Capric / succinic Triglyceride), and caprylic / capric glycerides (INCI: Caprylic / Capric Glycerides).

[0187] Fluorine oil

[0188] Examples of the fluorine-based oil include perfluorodecalin (INCI), perfluorononyl dimethicone (INCI), and perfluoromethylcyclopentane (INCI).

[0189] UV absorber

[0190] Examples of the ultraviolet absorber include benzophenone-1 (INCI: Benzophenone-1), benzophenone-2 (INCI: Benzophenone-2), benzophenone-3 (INCI: Benzophenone-3), benzophenone-4 (INCI: Benzophenone-4), benzophenone-5 (INCI: Benzophenone-5), benzophenone-6 (INCI: Benzophenone-6), benzophenone-9 (INCI: Benzophenone-9), homosalate (INCI), octocrylene (INCI), butyl methoxydibenzoylmethane (INCI: Butyl Methoxydibenzoylmethane), ethylhexyl salicylate (INCI: Ethylhexyl salicylate) and succinate. Salicylate), Diethylamino Hydroxybenzoyl Hexyl Benzoate (INCI), Polysilicone-15 (INCI), Ethylhexyl Dimethoxybenzylidene Dioxoimidazolidine Propionate (INCI), Terephthalylidene Dicamphor Sulfonic Acid (INCI), Ethylhexyl Triazone (INCI), Isopentyl Trimethoxycinnamate Trisiloxane (INCI), Drometrizole Trisiloxane (INCI), Ethylhexyl Dimethyl PABA (INCI), PABA)), Isopropyl Methoxycinnamate (: Indication Name (INCI: IsopropylMethoxycinnamate)), Ethylhexyl Methoxycinnamate (: Indication Name (INCI: EthylhexylMethoxycinnamate)), Bis-Ethylhexyloxyphenol Methoxyphenyl Triazine (INCI), Phenylbenzimidazole Sulfonic Acid (: Indication Name (INCI: Phenylbenzimidazole SulfonicAcid)), Methylene Bis-Benzotriazolyl Tetramethylbutylphenol (INCI), Glyceryl Ethylhexanoate Dimethoxycinnamate (INCI: Glyceryl Ethylhexanoate Dimethoxycinnamate), Glyceryl Hexyl PABA (INCI), Methyl Diisopropyl Cinnamate (INCI: Diisopropyl Methyl Cinnamate), Cinoxate (INCI), Ethylhexyl Dimethoxybenzylidene Dioxoimidazolidine Propionate (INCI: Ethylhexyl Dimethoxybenzylidene Dioxoimidazolidine Propionate), etc.

[0191] (2) Water-based ingredients

[0192] The aqueous component is not particularly limited as long as it is an aqueous component that can be generally incorporated into cosmetics. Specifically, water, lower alcohols preferably having 2 to 5 carbon atoms such as ethanol (INCI: Alcohol) and isopropyl alcohol (INCI: Isopropyl Alcohol), and sugar alcohols such as sorbitol (INCI), maltose (INCI), and xylitol (INCI) can be cited. In addition, polyols such as butylene glycol (INCI: Butylene Glycol), propylene glycol (INCI: Propylene Glycol), dipropylene glycol (INCI: Dipropylene Glycol), pentylene glycol (INCI), 1,10-decanediol (INCI), caprylyl glycol (INCI), 1,2-hexanediol (INCI), erythritol (INCI), glycerol (INCI), diglycerol (INCI), and polyethylene glycol; glucose (INCI), glyceryl glucoside (INCI), betaine (INCI), sodium chondroitin sulfate (INCI: Sodium Chondroitin Sulfate), PCA-Na (INCI: Sodium PCA)), methyl gluceth-10 (INCI), methyl gluceth-20 (INCI), hyaluronic acid, egg yolk lecithin, soy lecithin, phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidylglycerol, phosphatidylinositol, sphingomyelin and other moisturizers.

[0193] (3) Surfactants

[0194] As surfactants, there are nonionic, anionic, cationic and amphoteric active agents, and there are no special restrictions. As long as it is an active agent commonly used in cosmetics, any surfactant can be used. Among these surfactants, one or more selected from non-crosslinked silicone surfactants or crosslinked silicone surfactants are preferred because stable cosmetics can be obtained. In any case, the amount of surfactant blended is preferably 0.1~20% by mass of the entire cosmetic. If it is more than 0.1%, the functions of dispersion and emulsification can be fully exerted; if it is less than 20% by mass, there is no need to worry about the use of cosmetics becoming sticky, so it is preferred. The hydrophilic lipophile balance (HLB) of the surfactant is not limited, but from the purpose of maintaining the water resistance of cosmetics, it is preferably 2~14.5.

[0195] As the non-crosslinked silicone surfactant, preferably, a silicone surfactant in which part of the methyl groups of the linear or branched silicone main chain are substituted with a hydrophilic group such as polyethylene glycol or polyglycerol, specifically, a linear or branched polyoxyethylene-modified organopolysiloxane, a linear or branched polyoxyethylene-polyoxypropylene-modified organopolysiloxane, a linear or branched polyoxyethylene-alkyl co-modified organopolysiloxane, a linear or branched polyoxyethylene-polyoxypropylene-alkyl co-modified organopolysiloxane, a linear or branched polyoxyethylene-polyoxypropylene-alkyl co-modified organopolysiloxane, a linear or branched polyglycerol-modified organopolysiloxane, a linear or branched polyglycerol-alkyl co-modified organopolysiloxane, or a linear or branched pyrrolidone-modified organopolysiloxane.

[0196] Examples thereof include PEG-11 methyl ether dimethicone (INCI), PEG / PPG-20 / 22 butyl ether dimethicone (INCI), PEG-3 dimethicone (INCI), PEG-10 dimethicone (INCI), PEG-9 polydimethylsiloxyethyl dimethicone (INCI), lauryl PEG-9 polydimethylsiloxyethyl dimethicone (INCI), cetyl PEG / PPG-10 / 1 dimethicone (INCI), polyglyceryl-3 disiloxane dimethicone (INCI), polyglyceryl-3 polydimethylsiloxyethyl dimethicone (INCI), and lauryl polyglyceryl-3 polydimethylsiloxyethyl dimethicone (INCI).

[0197] Examples of commercially available non-cross-linked silicone surfactants include KF-6011, KF-6011P, KF-6012, KF-6015, KF-6017, KF-6043, KF-6028, KF-6038, KF-6048, KF-6100, KF-6104, KF-6106, KF-6105, KF-6115, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0198] Examples of the cross-linked silicone surfactant include (dimethicone / (PEG-10 / 15)) crosspolymer (INCI), (PEG-15 / lauryl dimethicone) crosspolymer (INCI), (PEG-10 / lauryl dimethicone) crosspolymer (INCI), (PEG-15 / lauryl dimethicone ethyl dimethicone) crosspolymer (INCI), (dimethicone / polyglyceryl-3) crosspolymer (INCI), (lauryl dimethicone / polyglyceryl-3) crosspolymer (INCI), and (polyglyceryl-3 / lauryl dimethicone ethyl dimethicone) crosspolymer (INCI).

[0199] When a crosslinked silicone surfactant is used, in a composition comprising the crosslinked silicone surfactant and an oil agent that is liquid at room temperature, the crosslinked silicone surfactant is preferably swollen by containing the liquid oil agent in an amount greater than its own weight.

[0200] As the liquid oil, liquid silicone oil, hydrocarbon oil, ester oil, natural animal and plant oil, semi-synthetic oil, and fluorine-based oil in the oil of the antioxidant component (1) can be used. Examples thereof include cyclopentasiloxane (INCI), dimethicone (INCI), mineral oil (INCI), isododecane (INCI), isohexadecane (INCI), triethylhexanoin (INCI), isotridecanol isononanoate (INCI: Isotridecyl Isononanoate), and squalane (INCI).

[0201] Examples of commercially available cross-linked silicone surfactants that are swollen by containing a liquid oil agent include KSG-210, KSG-240, KSG-270, KSG-310, KSG-320, KSG-330, KSG-340, KSG-320Z, KSG-350Z, KSG-710, KSG-810, KSG-820, KSG-830, KSG-840, KSG-820Z, and KSG-850Z manufactured by Shin-Etsu Chemical Co., Ltd.

[0202] (4) Powder

[0203] Examples of the powder include coloring pigments, inorganic powders, metal powders, organic powders, inorganic-organic composite powders, etc. The specific examples are as follows.

[0204] Coloring Pigments

[0205] The coloring pigment is not particularly limited as long as it is a pigment used for the purpose of coloring cosmetics. Examples of the coloring pigment include red iron oxide (INCI: Iron Oxides), yellow iron oxide (INCI: Iron Oxides), white titanium dioxide (INCI: Titanium Dioxide), black iron oxide (INCI: Iron Oxides), ultramarine (INCI: Ultramarines), ferric ferrocyanide (INCI: Ferric Ferrocyanide, Ferric Ammonium Ferrocyanide), manganese violet (INCI: Manganese Violet), cobalt titanium oxide (INCI: Cobalt Titanium Oxide), chromium hydroxide green (INCI: Chromium Hydroxide Green), chromium oxide greens (INCI: Chromium Oxide Greens), cobalt aluminum oxide (INCI: Cobalt Aluminum Oxide), and chromium hydroxide green (INCI: Chromium Hydroxide Green). Any coloring pigment selected from the group consisting of inorganic brown pigments such as ferrous oxide, cobalt titanium oxide (INCI: Cobalt Titanium Oxide), (titanium / titanium dioxide) sintered product (INCI: Titanium / Titanium Dioxide), lithium cobalt titanate (INCI: Lithium Cobalt Titanate), cobalt titanium oxide (INCI: Cobalt Titanium Oxide), (iron oxide / titanium dioxide) sintered product (INCI:), iron oxide-doped titanium dioxide (INCI: Iron Oxides, Titanium Dioxide), and the like, inorganic brown pigments such as titanium nitride (INCI: Titanium Nitride), ferrous hydroxide (INCI: Iron Hydroxide), and γ-iron oxide, inorganic yellow pigments such as yellow ochre, pigments obtained by laking tar pigments, and pigments obtained by laking natural pigments.

[0206] The shape of the pigment may be any of spherical, substantially spherical, rod-shaped, spindle-shaped, petal-shaped, short strip-shaped, irregular, etc., and the geometric form is not particularly limited as long as it can impart color to the cosmetic.

[0207] Inorganic powder

[0208] Examples of the inorganic powder include zirconium oxide (INCI: Zirconium Dioxide), zinc oxide (INCI: Zinc Oxide), cerium oxide (INCI: Cerium Oxide), magnesium oxide (INCI: Magnesium Oxide), barium sulfate (INCI: Barium Sulfate), calcium sulfate (INCI: Calcium Carbonate), magnesium sulfate (INCI: Magnesium Sulfate), calcium carbonate (INCI: Calcium Carbonate), magnesium carbonate (INCI: Magnesium Carbonate), talc (INCI), mica (INCI), kaolin (INCI), synthetic fluorphlogopite (INCI: Synthetic Fluorphlogopite), synthetic phlogopite iron (Indicative name), biotite (Indicative name (INCI: Biotite)), potassium silicate (Indicative name (INCI: Potassium Silicate)), silicon dioxide (INCI), aluminum silicate (Indicative name (INCI: Aluminum Silicate)), magnesium silicate (Indicative name (INCI: Magnesium Silicate)), magnesium aluminum silicate (Indicative name (INCI: Magnesium Aluminum Silicate)), calcium silicate (Indicative name (INCI: Calcium Silicate)), calcium sodium aluminum silicate (Indicative name (INCI: Aluminum CalciumSodium Silicate)), sodium magnesium silicate (Indicative name (INCI: Lithium Magnesium Sodium Silicate)), sodium magnesium silicate (Indicative name (INCI: Sodium Magnesium Silicate)), calcium aluminum borosilicate (Indicative name (INCI: Calcium Aluminum Borosilicate)), calcium sodium borosilicate (Indicative name (INCI: CalciumSodium Borosilicate), hydroxyapatite (INCI), bentonite (INCI), montmorillonite (INCI), laponite (INCI), zeolite (INCI), alumina (INCI), aluminum hydroxide (INCI: Aluminum Hydroxide), boron nitride (INCI: BoronMicroparticles composed of Nitride) and glass (: indicates the name (INCI: Glass)).

[0209] Inorganic colored pearlescent pigments include pearlescent agents such as mica coated with titanium dioxide (INCI: Titanium Dioxide), synthetic fluorphlogopite coated with titanium dioxide (INCI: Titanium Dioxide), bismuth oxychloride (INCI: Bisniuth Oxychloride), bismuth oxychloride coated with titanium dioxide (INCI: Titanium Dioxide), talc coated with titanium dioxide (INCI: Titanium Dioxide), fish scale foil (INCI), and colored mica coated with titanium dioxide (INCI: Titanium Dioxide). The pearlescent pigments are not particularly limited and may be untreated or subjected to a known surface treatment generally used in cosmetics.

[0210] Metal powder

[0211] Examples of the metal powder include metal fine particles made of aluminum (INCI: Aluminum, Aluminum Powder), copper (INCI: Copper Powder), silver (INCI: Silver Powder), and gold (INCI: Gold).

[0212] Organic powder

[0213] Examples of the organic powder include powders composed of silicone, polyamide, polyacrylic acid-acrylate, polyester, polyethylene (INCI), polypropylene (INCI), polystyrene (INCI), styrene-acrylic acid copolymer, divinylbenzene-styrene copolymer, polyurethane, vinyl resin, urea resin, melamine resin, benzoguanamine, polymethylbenzoguanamine, tetrafluoroethylene, polymethyl methacrylate, cellulose (INCI), silk (INCI), nylon (indicative name), phenolic resin, epoxy resin, polycarbonate, and the like.

[0214] In particular, examples of the silicone include silicone resin particles; polymethylsilsesquioxane (INCI), silicone rubber powder, silicone resin-coated silicone rubber powder; vinyl dimethicone / polymethylsiloxane silsesquioxane crosspolymer (INCI), (diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane crosspolymer (INCI), polysilicone-1 crosspolymer (INCI), polysilicone-22 (INCI), and the like.

[0215] Examples of commercially available powders composed of silicone include KMP-590, KMP-591, KMP-592, KMP-597, KMP-598, KSP-100, KSP-101, KSP-102, KSP-105, KSP-300, KSP-411, KSP-441, KM-9729, and KM-440 manufactured by Shin-Etsu Chemical Co., Ltd.

[0216] In addition, metal soaps and the like can be mentioned. Specific examples include powders consisting of zinc stearate (INCI: Zinc Stearate), aluminum stearate (INCI: Aluminum Stearate), calcium stearate (INCI: Calcium Stearate), magnesium stearate (INCI: Magnesium Stearate), zinc myristate (INCI: Zinc Myristate), magnesium myristate (INCI: Magnesium Myristate), sodium zinc cetyl phosphate (INCI: Sodium Zinc Cetyl Phosphate), and potassium cetyl phosphate (INCI: Potassium Cetyl Phosphate).

[0217] Furthermore, organic pigments and the like can be mentioned. Specific examples thereof include CI 45430, Red 28 (lake) (: Indicative name (INCI: Red 28, Red 28 Lake)), CI 45100, Red 6 (: Indicative name (INCI: Red 6)), Red 7 (: Indicative name (INCI: Red 7)), CI 15585, CI 15630, Red 34 (: Indicative name (INCI: Red 34)), Red 30 (: Indicative name (INCI: Red 30)), Red 33 (lake) (: Indicative name (INCI: Red 33, RED 33 Lake); Red 36 (: Indicative name (INCI: Red 36)), Red 22 (lake) (: Indicative name (INCI: Red 22, Red 22 Lake)), CI 45380 (Indicative name), CI 45190 (Indicative name), CI 12140 (Indicative Name), Yellow 5 (Indicative Name (INCI: Yellow 5)), Yellow 6 (Lake) (Indicative Name (INCI: Yellow 6, Yellow 6 Lake)), Yellow 8 (Indicative Name (INCI: Yellow 8)), Yellow 10 (Lake) (Indicative Name (INCI: Yellow 10, Yellow 10 Lake)), Yellow 11 (Indicative Name (INCI: Yellow 11)), CI 11680, Blue 1 (Lake) (Indicative Name (INCI: Blue 1, Blue 1 Lake)), CI 73015, CI 73000, Blue 4 (Indicative Name (INCI: Blue 4)), CI 74160 (Indicative Name), Green 3 (Lake) (Indicative Name (INCI: Green 3, Green 3 Lake)), Green 5 (Indicative Name (INCI: Green 5)), Green 6 (Indicative Name (INCI: Green 6)), Green 8 (: Indicative name (INCI: Green 8)), CI 42095 (Indicative name), Orange 5 (: Indicative name (INCI: Orange 5)), Pigment Orange 5 (: Indicative name (INCI: Pigment Orange 5)), Pigment Orange 13 (Indicative name), Orange 4 (lake) (: Indicative name (INCI: Orange 4, Orange 4 Lake)), Orange 10 (: Indicative name (INCI: Orange 10)), Orange 11 (: Indicative name (INCI: Orange 11)) and other tar pigments, cochineal (INCI), lac acid (: Indicative name (INCI: Laccaic Acid)), Carthamus tinctorius flower extract (: Indicative name (INCI: We are playing cards Dyer(Safflower) Flower Extract)), Ginkgo Biloba Root Extract (: Indicated Name (INCI: Lithospermum Officinale Natural pigments such as Gardenia Florida Root Extract), Gardenia Yellow (Indication Name), Hydrolyzed Gardenia Florida Extract (: Indication Name (INCI: Hydrolyzed Gardenia Florida Extract)).

[0218] Inorganic-organic composite powder

[0219] Examples of the inorganic-organic composite powder include composite powders obtained by coating the surface of an inorganic powder with an organic powder by a known and commonly used method.

[0220] In addition, the powders may be those in which the particle surfaces are treated. In addition, from the viewpoint of water resistance of the cosmetic, it is preferred that the surface treatment agent imparts hydrophobicity, and the treatment agent imparting hydrophobicity is not particularly limited, and examples thereof include silicone treatment agents, waxes, paraffins, organic fluorine compounds such as perfluoroalkanes and phosphates, surfactants, amino acids such as N-acylglutamic acid, and metal soaps such as aluminum stearate and magnesium myristate.

[0221] More preferred silicone treatment agents include silanes such as triethoxycaprylylsilane (INCI) or silylating agents, dimethicone (INCI), methylsiloxane (INCI), hydrogenated dimethicone (INCI), triethoxysilylethyl dimethicone ethyl dimethicone (INCI), triethoxysilylethyl dimethicone ethylhexyl dimethicone (INCI), and (Acrylates / Tridecyl Acrylate / Triethoxysilylpropyl Methacrylate / Dimethicone Methacrylate Copolymer).

[0222] Specific examples of the silicone treatment agent include AES-3083, KF-99P, KF-9901, KF-9908, KF-9909, KP-574, and KP-541 manufactured by Shin-Etsu Chemical Co., Ltd.

[0223] Furthermore, the above-mentioned surface hydrophobizing agents may be used alone or in combination of two or more.

[0224] Specific examples of the surface-treated coloring pigment include KTP-09 series manufactured by Shin-Etsu Chemical Co., Ltd., particularly KTP-09W, 09R, 09Y, and 09B.

[0225] (5) Composition of a cross-linked organopolysiloxane and an oil agent that is liquid at room temperature

[0226] In the composition composed of the crosslinked organopolysiloxane and the oil agent that is liquid at room temperature, the crosslinked organopolysiloxane preferably swells in the liquid oil by containing the liquid oil agent in an amount greater than its own weight. As the liquid oil agent, liquid silicone oil, hydrocarbon oil, ester oil, natural animal and plant oil, semi-synthetic oil, and fluorine-based oil in the oil agent of the optional component (1) can be used, for example, cyclopentasiloxane (INCI), dimethicone (INCI), mineral oil (INCI), isododecane (INCI), isohexadecane (INCI), triethylhexanoin (INCI), isotridecyl isononanoate (INCI: Isotridecyl Isononanoate), squalane (INCI), and the like can be cited.

[0227] The component (5) is different from the cross-linked silicone surfactant of the component (3) described above, and is a compound that does not have a polyether or polyglycerol structure in its molecular structure. Specific examples thereof include dimethicone / vinyl dimethicone crosspolymer (INCI), dimethicone / phenyl vinyl dimethicone crosspolymer (INCI), vinyl dimethicone / lauryl dimethicone crosspolymer (INCI), and lauryl dimethylsiloxyethyl dimethicone / bisvinyl dimethicone crosspolymer (INCI).

[0228] Examples of commercially available compositions consisting of a cross-linked organopolysiloxane and an oil agent that is liquid at room temperature include KSG-15, KSG-1510, KSG-16, KSG-1610, KSG-19, KSG-016F, KSG-18A, KSG-41A, KSG-42A, KSG-43, KSG-44, KSG-042Z, KSG-045Z, KSG-048Z, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0229] (6) Film-forming agent

[0230] The film-forming agent is mainly blended for the purpose of further maintaining the effect durability of the cosmetic. Although not particularly limited, from the perspective of imparting water repellency, a silicone composition is preferred. Specifically, trimethylsiloxysilicate, acrylic acid-silicone film-forming agent, silicone-modified norbornene, silicone-modified pullulan, silicone-modified polyvinyl alcohol, etc. can be used.

[0231] Examples of film-forming agents for silicone compositions include trimethylsiloxysilicate (INCI: Trimethylsiloxysilicate), acrylate / dimethylsiloxane copolymer (INCI), norbornene / tris(trimethylsiloxy)silylnorbornene copolymer (INCI), and trimethylsiloxysilylcarbamoyl pullulan (INCI: Trimethylsiloxysilylcarbamoyl Pullulan).

[0232] The film-forming agent may be dissolved in an oily agent that is liquid at room temperature and then blended into the cosmetic. As the liquid oily agent, liquid silicone oil, hydrocarbon oil, ester oil, natural animal and plant oil, semi-synthetic oil, etc., or fluorine-based oil in the oily agent of any component (1) may be used.

[0233] Specific examples of commercially available silicone film-forming agents include KF-7312J, KP-545, KP-549, KP-543, NBN-30-ID, TSPL-30-ID, and TSPL-30-D5 manufactured by Shin-Etsu Chemical Co., Ltd.

[0234] (7) Ultraviolet light absorbing and scattering agent

[0235] As the ultraviolet absorbing and scattering agent, particles that absorb and scatter ultraviolet light, such as microparticle titanium dioxide, microparticle iron-containing titanium dioxide, microparticle zinc oxide, microparticle cerium oxide, and composites thereof, can be listed. A dispersion prepared by preliminarily dispersing the above-mentioned ultraviolet absorbing and scattering particles in an oil can also be used.

[0236] As the oil agent, liquid silicone oil, hydrocarbon oil, ester oil, natural animal and plant oil, semi-synthetic oil, or fluorine-based oil in the optional component (1) of the oil agent can be used.

[0237] Specific examples of dispersions in which particles that absorb and scatter ultraviolet rays are dispersed in an oil in advance include the SPD series (trade name) manufactured by Shin-Etsu Chemical Co., Ltd., especially SPD-T5, Z5, T6, Z6, T7, etc.

[0238] (8) Other additives

[0239] Other additives include oil-soluble gelling agents, preservatives / bactericides, antiperspirants, fragrances, salts, antioxidants, pH adjusters, chelating agents, cooling agents, anti-inflammatory agents, skin beautifying ingredients (whitening agents, cell activators, rough skin improvers, blood circulation promoters, skin astringents, anti-seborrheic agents, etc.), vitamins, amino acids, nucleic acids, hormones, inclusion compounds, etc.

[0240] Oil-soluble gelling agent

[0241] Examples of the oil-soluble gelling agent include metal soaps such as aluminum stearate, magnesium stearate, and zinc myristate; amino acid derivatives such as lauroyl glutamic acid (INCI: Lauroyl Glutamic Acid) and α,γ-di-n-butylamine; dextrin palmitate (INCI: Dextrin Palmitate), dextrin isostearate (INCI: Dextrin Isostearate), dextrin myristate (INCI: Dextrin Myristate), stearoyl inulin (INCI: Stearoyl Inulin), dextrin palmitate / ethylhexanoate (INCI: Dextrin Palmitate / Ethylhexanoate) and other dextrin fatty acid esters; sucrose fatty acid esters such as sucrose palmitate and sucrose stearate; oligofructose fatty acid esters such as oligofructose stearate and oligofructose 2-ethylhexanoate; benzyl derivatives of sorbitol such as monobenzylidene sorbitol and dibenzylidene sorbitol; organically modified clay minerals of disteardimethylammonium hectorite (INCI), stearalkonium hectorite (INCI), and montmorillonite; stearalkonium bentonite (INCI), etc.

[0242] Preservatives / fungicides

[0243] Examples of the preservative / bactericide include alkyl parabens, benzoic acid, sodium benzoate, sorbic acid, potassium sorbate, phenoxyethanol, imidazolidinyl urea, salicylic acid, isopropyl methylphenol, phenol, p-chloro-meta-cresol, hexachlorophene, benzalkonium chloride, chlorhexidine, trichlorocarbamide, iodopropynyl butylcarbamate, polylysine, photosensitizers, silver, and plant extracts.

[0244] Antiperspirant

[0245] Examples of antiperspirants include aluminum hydroxyhalides such as aluminum chlorohydrate, aluminum halides such as aluminum chloride, aluminum salts of allantoin, tannic acid, persimmon tannin, potassium aluminum sulfate, zinc oxide, zinc p-phenolsulfonate, burnt alum, aluminum zirconium tetrachlorohydrate, aluminum zirconium trichlorohydrate GLY complex, etc. As components showing particularly high effects, aluminum hydroxyhalides, aluminum halides, and complexes or mixtures thereof with zirconium oxyhalides and zirconium hydroxyhalides (e.g., aluminum zirconium tetrachlorohydrate, aluminum zirconium trichlorohydrate GLY complex), etc. are preferred.

[0246] ·spices

[0247] As fragrances, there are natural fragrances and synthetic fragrances. As natural fragrances, there are plant fragrances separated from flowers, leaves, wood, peels, etc.; animal fragrances such as musk and civet. As synthetic fragrances, there are hydrocarbons such as monoterpenes, alcohols such as aliphatic alcohols and aromatic alcohols; aldehydes such as terpene aldehydes and aromatic aldehydes; ketones such as alicyclic ketones; esters such as terpene esters; lactones; phenols; oxides; nitrogen-containing compounds; acetals, etc.

[0248] Salts

[0249] As salts, inorganic salts, organic acid salts, amine salts and amino acid salts can be listed. As inorganic salts, for example, sodium salts, potassium salts, magnesium salts, calcium salts, aluminum salts, zirconium salts, zinc salts, etc. of inorganic acids such as hydrochloric acid, sulfuric acid, carbonic acid, and nitric acid can be listed; as organic acid salts, for example, salts of organic acids such as acetic acid, dehydroacetic acid, citric acid, malic acid, succinic acid, ascorbic acid, and stearic acid can be listed; as amine salts and amino acid salts, for example, salts of amines such as triethanolamine, and salts of amino acids such as glutamic acid can be listed. In addition, salts of hyaluronic acid, chondroitin sulfate, aluminum zirconium glycine complexes, and acid-base neutralization salts used in cosmetic formulations can also be used.

[0250] Antioxidants

[0251] The antioxidant is not particularly limited, and examples thereof include carotenoids, ascorbic acid and salts thereof, ascorbyl stearate, tocopherol, tocopherol acetate, tocopherol, p-tert-butylphenol, butylated hydroxyanisole, butylated hydroxytoluene, phytic acid, ferulic acid, thiotaurine, hypotaurine, sulfites, isoascorbic acid and salts thereof, chlorogenic acid, epicatechin, epigallocatechin, epigallocatechin gallate, apigenin, kaempferol, myricetin, quercetin, etc. The antioxidant may be used alone or in combination of two or more.

[0252] PH regulator

[0253] Examples of the pH adjuster include lactic acid, citric acid, glycolic acid, succinic acid, tartaric acid, dl-malic acid, potassium carbonate, sodium bicarbonate, and ammonium bicarbonate.

[0254] Chelating agents

[0255] Examples of the chelating agent include alanine, edetate sodium salt, sodium polyphosphate, sodium metaphosphate, phosphoric acid, and the like.

[0256] · Cooling agent

[0257] Examples of the cooling agent include L-menthol, camphor, and menthol lactate.

[0258] Anti-inflammatory agents

[0259] Examples of the anti-inflammatory agent include allantoin, glycyrrhizic acid and its salts, glycyrrhetinic acid and glycyrrhetinic acid stearyl ester, tranexamic acid, and azulene.

[0260] Skin-beautifying ingredients

[0261] Examples of skin beautifying ingredients include whitening agents such as placenta extract, arbutin, glutathione, and saxifrage extract; cell activators such as royal jelly, photosensitizers, cholesterol derivatives, and calf blood extract; rough skin improving agents, nonanoic acid vanillamide, benzyl nicotinate, β-butoxyethyl nicotinate, capsaicin, zingerone, cantharidestincture, ichthyol, caffeine, tannic acid, α-borneol, tocopherol nicotinate, inositol nicotinate, cycloamycin, cinnarizine, tolazoline, acetylcholine, verapamil, cepharanthin, γ-oryzanol, and other blood circulation promoters; skin astringents such as zinc oxide and tannic acid; and anti-seborrheic agents such as sulfur and dimethylthianthrene.

[0262] Vitamins

[0263] Examples of vitamins include vitamin A oil, retinol, vitamin A acetate, vitamin A palmitate and other vitamins, riboflavin, riboflavin butyrate and the like. butyrate), flavin adenine nucleotide and other vitamin B2, pyridoxine hydrochloride, pyridoxine dioctanoate, pyridoxine tripalmitate and other vitamin B6, vitamin B12 and its derivatives, vitamin B15 and its derivatives and other vitamin B, L-ascorbic acid, L-ascorbyl dipalmitate, sodium L-ascorbic acid-2-sulfate, L-ascorbyl phosphate dipotassium and other vitamin C, ergocalciferol, cholecalciferol and other vitamin D, α-tocopherol, β-tocopherol, γ-tocopherol, dl-α-tocopherol acetate, dl-α-tocopherol nicotinate, dl-α-tocopherol succinate and other vitamin E; niacin, benzyl nicotinate, niacinamide and other niacin, vitamin H, vitamin P, pantothenic acid calcium, D-panthenol, pantothenic acid ethyl ether, acetyl pantothenic acid ethyl ether and other pantothenic acid, biotin and the like.

[0264] Amino Acids

[0265] Examples of the amino acids include glycine, valine, leucine, isoleucine, serine, threonine, phenylalanine, arginine, lysine, aspartic acid, glutamic acid, cystine, cysteine, methionine, and tryptophan.

[0266] Nucleic Acids

[0267] Examples of nucleic acids include deoxyribonucleic acid and the like.

[0268] ·hormone

[0269] Examples of the hormone include estradiol and vinyl estradiol.

[0270] Inclusion complex

[0271] Examples of the inclusion compound include cyclodextrin and the like.

[0272] Example

[0273] The present invention is described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. In each example, the kinematic viscosity is a value measured at 25° C. using a capillary viscometer, and “%” indicating the concentration and content rate indicates “mass %”.

[0274] [Production Example 1]

[0275] (Manufacturing of Aqueous Dispersion of Silicone Rubber Particles)

[0276] The kinematic viscosity of 344 g expressed by the following formula (11) is 55 mm 2 / s, 56 g of a vinyl-containing dimethylpolysiloxane (A1) (the amount of which is 1.15 hydrosilyl groups per vinyl group), and a kinematic viscosity represented by the following formula (12) of 30 mm 2 / s of methyl hydrogen polysiloxane (B1) and 0.1g of d1-a-tocopherol (antioxidant) were added to a glass beaker with a capacity of 1 liter, and mixed and dissolved using a homogenizer. 30g of lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) and 40g of water were added, and stirred using a homogenizer until the viscosity was increased to a state where it could not be stirred. The viscosity-increasing material was kneaded for 15 minutes using a homogenizer. Next, 528g of water was added and mixed using a homogenizer to obtain a uniform white emulsion. The emulsion was transferred to a 1-liter glass flask equipped with a stirring device using an anchor-type stirring wing, and the temperature was adjusted to 20-25°C. Then, a mixed solution of 1 g of a platinum-vinyl disiloxane complex-containing isododecane solution (platinum content 0.5%) and 1 g of lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) was added under stirring, and stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber particles.

[0277] The volume average particle size of the silicone rubber particles was measured using a “laser diffraction / scattering particle size distribution analyzer LA-960” (manufactured by HORIBA, Ltd.) and found to be 300 nm.

[0278] The kinematic viscosity represented by the following formula (11) is 55 mm 2 / s, and the kinetic viscosity represented by the following formula (12) is 30 mm 2 / s methyl hydrogen polysiloxane (B1) and isododecane solution of platinum-containing vinyl disiloxane complex (platinum content 0.5%) were mixed in the above blending ratio, poured into an aluminum dish in a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a constant temperature bath at 50°C for 1 hour. The obtained cured product was a non-sticky rubber elastic body, and the hardness was 50 when measured by a type A durometer specified in JIS K6253.

[0279] (A1): Vinyl-containing dimethyl polysiloxane

[0280] [Chemical formula 7]

[0281]

[0282] (B1): Methyl hydrogen polysiloxane

[0283] [Chemical formula 8]

[0284]

[0285] [Production Example 2]

[0286] (Manufacturing of Aqueous Dispersion of Silicone Rubber Particles)

[0287] The kinematic viscosity of 393 g represented by the following formula (13) is 5,060 mm 2 / s, 7 g of a vinyl-containing dimethylpolysiloxane (A2) (the amount of the hydrosilyl group is 1.19 per vinyl group), and the kinematic viscosity represented by the above formula (12) is 30 mm 2 / s of methyl hydrogen polysiloxane and 0.1g of d1-a-tocopherol (antioxidant) were added to a glass beaker with a capacity of 1 liter, and mixed and dissolved using a homogenizer. 42g of lauryl alcohol polyoxyethylene ether (trade name: EMULGEN109P, manufactured by Kao Corporation) and 35g of water were added, and stirred using a homogenizer until the viscosity was increased to a state where it could not be stirred. The viscosity-increasing material was kneaded for 15 minutes using a homogenizer. Next, 521g of water was added, and mixed using a homogenizer to obtain a uniform white emulsion. The emulsion was transferred to a 1-liter glass flask equipped with a stirring device using an anchor-type stirring wing, and the temperature was adjusted to 20-25°C. Then, a mixed solution of 0.6 g of a platinum-vinyl disiloxane complex-containing isododecane solution (platinum content 0.5%) and 1 g of lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) was added under stirring, and stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber particles.

[0288] The volume average particle size of the silicone rubber particles was measured using a “laser diffraction / scattering particle size distribution analyzer LA-960” (manufactured by HORIBA, Ltd.) and found to be 300 nm.

[0289] The kinematic viscosity represented by the following formula (13) is 5,060 mm 2 / s of vinyl-containing dimethylpolysiloxane, the kinematic viscosity represented by the above formula (12) is 30 mm 2 / s methyl hydrogen polysiloxane and isododecane solution of platinum-containing vinyl disiloxane complex (platinum content 0.5%) were mixed according to the above blending ratio, poured into an aluminum dish in a thickness of 10 mm, left at 25°C for 6 hours, and then heated in a constant temperature bath at 50°C for 1 hour. The obtained cured product was a non-sticky rubber elastic body, and the hardness was measured by a type A durometer, and the result was 20.

[0290] (A2): Vinyl-containing dimethyl polysiloxane

[0291] [Chemical formula 9]

[0292]

[0293] [Example 1]

[0294] 150 g of cellulose particles (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm, electron microscope photograph: Figure 4 ), 20 g (5.3 parts by mass of silicone rubber particles relative to 100 parts by mass of cellulose particles) of the silicone rubber particle aqueous dispersion obtained in the above-mentioned Preparation Example 1, 5.5 g (0.2 parts by mass of lauryltrimethylammonium chloride relative to 100 parts by mass of water) of a 30% aqueous solution of lauryltrimethylammonium chloride (trade name: CATION BB, manufactured by NOF CORPORATION), 0.62 g (0.03 parts by mass of a polymer of dimethyldiallylammonium chloride relative to 100 parts by mass of water) of a 40% aqueous solution of a polymer of dimethyldiallylammonium chloride (trade name: ME Polymer H40W, manufactured by TOHO Chemical Industry Co., Ltd.), 1.6 g of 2.8% ammonia water, and 800 g of water. The pH of the liquid at this time was 10.8. After adjusting the temperature to 5-10°C, 22g (the amount of silica after hydrolysis and condensation reaction is 8.69g, and the amount of silica after hydrolysis and condensation reaction is 109 parts by mass relative to 100 parts by mass of silicone rubber particles) of tetramethoxysilane is added dropwise over 20 minutes, and the liquid temperature during this period is maintained at 5-10°C, and stirring is further performed for 1 hour. Next, heat to 75-80°C, maintain this temperature and stir for 1 hour to terminate the hydrolysis and condensation reaction of tetramethoxysilane. Dehydrate the obtained suspension using a pressure filter. Transfer the dehydrated product to a 2-liter glass flask with a stirring device using an anchor-type stirring wing, add 1,000g of water, stir for 30 minutes, and then dehydrate using a pressure filter. Repeat this operation twice. The obtained dehydrated product is dried at a temperature of 105°C in a hot air flow dryer, and the dried product is crushed using a jet mill to obtain particles.

[0295] The volume average particle size of the obtained silicone particles was measured using a resistance-based particle size distribution analyzer (Multisizer 3, manufactured by Beckman Coulter Inc.) and found to be 12 μm.

[0296] The obtained particles were observed using an electron microscope, and it was confirmed that spherical particles of about 300 nm in size were attached to the surface of the spherical particles without gaps, and that they had become composite particles in which silicone rubber particles were attached to the surface of cellulose particles. The electron microscope photograph is shown in Figure 1.

[0297] 5 g of the obtained particles were added to a 100 mL beaker containing 80 g of an aqueous solution in which 1% lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) was dissolved, and the particles were dispersed in the aqueous solution by stirring with a glass rod. After standing for 24 hours, the ups and downs of the particles were observed. As a result, all the particles settled. Since the specific gravity of the silicone rubber particles was less than that of water, they gradually floated up. Based on this result, it was judged that the silicone rubber particles did not fall off from the surface of the cellulose particles, and the silicon dioxide became a binder, suggesting that the silicone rubber particles were fixed to the surface of the cellulose particles.

[0298] [Example 2]

[0299] Into a 150 g glass flask with a capacity of 2 liters and a stirring device using an anchor-type stirring blade, cellulose particles (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm), 20 g (5.3 parts by mass of silicone rubber particles per 100 parts by mass of cellulose particles) of the silicone rubber particle aqueous dispersion obtained in the above-mentioned Production Example 2, 5.5 g (0.2 parts by mass of lauryltrimethylammonium chloride per 100 parts by mass of water) of a 30% lauryltrimethylammonium chloride aqueous solution (trade name: CATION BB, manufactured by NOFCORPORATION), and 0.62 g (0.03 parts by mass of a polymer of dimethyldiallylammonium chloride per 100 parts by mass of water) of a 40% aqueous solution of a polymer of dimethyldiallylammonium chloride (trade name: ME Polymer H40W, manufactured by TOHO Chemical Industry Co., Ltd.) were added. Co., Ltd.), 1.6g of 2.8% ammonia water, and 811g of water. The pH of the liquid at this time is 10.8. After adjusting the temperature to 5~10°C, it takes 10 minutes to drip 11g (the amount of silica after hydrolysis and condensation reaction is 4.34g, and the amount of silica after hydrolysis and condensation reaction is 54 parts by mass relative to 100 parts by mass of silicone rubber particles) tetramethoxysilane, and the liquid temperature during this period is maintained at 5~10°C, and further stirred for 1 hour. Then, heat to 75~80°C, maintain this temperature and stir for 1 hour to end the hydrolysis and condensation reaction of tetramethoxysilane. Dehydrate the obtained suspension using a pressure filter. Transfer the dehydrated material to a 2-liter glass flask with a stirring device using an anchor-type stirring wing, add 1,000g of water, stir for 30 minutes, and then dehydrate using a pressure filter. Repeat this operation twice. The obtained dehydrated product was dried at 105° C. in a hot air flow dryer, and the dried product was pulverized by a jet mill to obtain granules.

[0300] The volume average particle size of the obtained silicone particles was measured using a resistance-based particle size distribution analyzer (Multisizer 3, manufactured by Beckman Coulter Inc.) and found to be 12 μm.

[0301] The obtained particles were observed using an electron microscope, and it was confirmed that 80% to 90% of the spherical particles and their aggregates with a size of about 300 nm were attached to the surface of the spherical particles, and they had become composite particles formed by silicone rubber particles attached to the surface of cellulose particles. The electron microscope photo is shown in Figure 2 .

[0302] 5 g of the obtained particles were added to a 100 mL beaker containing 80 g of an aqueous solution in which 1% lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) was dissolved, and the particles were dispersed in the aqueous solution by stirring with a glass rod. After standing for 24 hours, the ups and downs of the particles were observed. As a result, all the particles settled. Since the specific gravity of the silicone rubber particles is less than that of water, they float. Based on this result, it is judged that the silicone rubber particles have not fallen off from the surface of the cellulose particles, and the silicon dioxide has become a binder, suggesting that the silicone rubber particles are fixed to the surface of the cellulose particles.

[0303] [Example 3]

[0304] Into a 2-liter glass flask equipped with a stirring device using an anchor-type stirring blade, 150 g of cellulose particles (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm), 3.5 g (0.9 parts by mass of silicone rubber particles per 100 parts by mass of cellulose particles) of the silicone rubber particle aqueous dispersion obtained in the above-mentioned Production Example 2, 5.6 g (0.2 parts by mass of lauryltrimethylammonium chloride per 100 parts by mass of water) of a 30% lauryltrimethylammonium chloride aqueous solution (trade name: CATION BB, manufactured by NOFCORPORATION), and 0.63 g (0.03 parts by mass of a polymer of dimethyldiallylammonium chloride per 100 parts by mass of water) of a 40% dimethyldiallylammonium chloride polymer aqueous solution (trade name: ME Polymer H40W, manufactured by TOHO Chemical Industry Co., Ltd.) were added. Co., Ltd.), 1.6g of 2.8% ammonia water, and 828g of water. The pH of the liquid at this time is 10.8. After adjusting the temperature to 5~10°C, it takes 10 minutes to drip 11g (the amount of silica after hydrolysis and condensation reaction is 4.34g, and the amount of silica after hydrolysis and condensation reaction is 310 parts by mass relative to 100 parts by mass of silicone rubber particles) tetramethoxysilane, and the liquid temperature during this period is maintained at 5~10°C, and stirring is performed for another hour. Next, heat to 75~80°C, maintain this temperature and stir for 1 hour to end the hydrolysis and condensation reaction of tetramethoxysilane. Dehydrate the obtained suspension using a pressure filter. Transfer the dehydrated material to a 2-liter glass flask with a stirring device using an anchor-type stirring wing, add 1,000g of water, stir for 30 minutes, and then dehydrate using a pressure filter. Repeat this operation twice. The obtained dehydrated product was dried at 105° C. in a hot air flow dryer, and the dried product was pulverized by a jet mill to obtain granules.

[0305] The volume average particle size of the obtained silicone particles was measured using a resistance-based particle size distribution analyzer (Multisizer 3, manufactured by Beckman Coulter Inc.) and found to be 12 μm.

[0306] The obtained particles were observed using an electron microscope, and it was confirmed that spherical particles of about 300 nm in size were sparsely attached to the surface of the spherical particles, which had become composite particles formed by silicone rubber particles attached to the surface of cellulose particles. Particles of less than 100 nm were observed to be attached to the surface where silicone rubber particles were not attached, and it was determined that they were silicon dioxide. The electron microscope photo is shown in Figure 3 .

[0307] 5 g of the obtained particles were added to a 100 mL beaker containing 80 g of an aqueous solution in which 1% lauryl alcohol polyoxyethylene ether (trade name: EMULGEN 109P, manufactured by Kao Corporation) was dissolved, and the particles were dispersed in the aqueous solution by stirring with a glass rod. After standing for 24 hours, the ups and downs of the particles were observed, and all the particles settled. Since the specific gravity of the silicone rubber particles is less than that of water, they float. Based on this result, it is judged that the silicone rubber particles have not fallen off from the surface of the cellulose particles, and the silicon dioxide has become a binder, suggesting that the silicone rubber particles are fixed to the surface of the cellulose particles.

[0308] [Comparative Example 1]

[0309] In a 2-liter glass flask equipped with a stirring device using an anchor-type stirring blade, 150 g of cellulose particles (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm), 20 g (5.3 parts by mass of silicone rubber particles relative to 100 parts by mass of cellulose particles) of the silicone rubber particle aqueous dispersion obtained in the above-mentioned Production Example 1, 1.6 g of 2.8% ammonia water, and 806 g of water were added. The pH of the liquid at this time was 10.8. After adjusting the temperature to 5 to 10°C, 22 g (8.69 g of silica after hydrolysis and condensation reaction, and 109 parts by mass of silica after hydrolysis and condensation reaction relative to 100 parts by mass of silicone rubber particles) of tetramethoxysilane were added dropwise over 20 minutes, and the liquid temperature during this period was maintained at 5 to 10°C, and stirring was further performed for 1 hour. Next, heat to 75-80°C, maintain the temperature and stir for 1 hour to terminate the hydrolysis and condensation reaction of tetramethoxysilane. Dehydrate the obtained suspension using a pressure filter. Transfer the dehydrated product to a 2-liter glass flask with a stirring device using an anchor-type stirring wing, add 1,000 g of water, stir for 30 minutes, and then dehydrate using a pressure filter. Repeat this operation twice. Dry the obtained dehydrated product at a temperature of 105°C in a hot air flow dryer, and crush the dried product using a jet mill to obtain particles.

[0310] The obtained particles were observed using an electron microscope, and no particles were observed to be attached to the surface of the cellulose particles.

[0311] In the step of adding tetraalkoxysilane to a mixed solution of cellulose particles, silicone rubber particles, ammonia water and water to carry out hydrolysis and condensation reaction, when a cationic substance (cationic surfactant and / or cationic water-soluble polymer) is not added, the silicone rubber particles do not adhere to the surface of the cellulose particles.

[0312] [Determination of oil absorption of composite particles]

[0313] The composite particles and cellulose particles (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm) prepared in the above examples were measured for oils used for cosmetic applications with reference to JIS K 5101-13-1 Part 13: Oil absorption - Section 1: Purified linseed oil method (JIS K 5101-13-1 Part 13: Oil absorption - Section 1: Purified linseed oil method). The results are recorded together in the following Tables 1 and Figure 5 middle.

[0314] [Table 1]

[0315]

[0316] (Note 1) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 6 mm 2 / s Dimethicone (INCI)

[0317] * In Comparative Example 1, rubber particles and silica were not attached to the organic resin particles.

[0318] According to the above Table 1 and Figure 5 The results show that Examples 1 to 3 have higher oil absorption performance for various oil agents than cellulose particles. In particular, it is known that in Example 3, although the amount of silicone rubber particles is 1.0 part by mass or less relative to 100 parts by mass of organic resin particles, the oil absorption performance for various oil agents is higher.

[0319] [Examples 4 to 6, Comparative Example 2: Evaluation of the usability of composite particles]

[0320] Skin care cosmetics having the formulations shown in Table 3 below were prepared by the following method, and the following property evaluations were performed.

[0321] (1) Usability evaluation

[0322] For skin care cosmetics blended with composite particles and cellulose particles prepared in the above example (trade name: CELLULOBEADS D5, manufactured by DAITO KASEI KOGYO CO., LTD., shape = spherical, volume average particle size = 12 μm), the usability during application (extensibility, skin compatibility) and the usability after application (degree of non-stickiness, concealment, smoothness) were evaluated. Ten expert panelists were asked to evaluate the degree of usability. The evaluation was performed according to the evaluation criteria shown in Table 2, and the results were judged based on the average value of the ten members and the following judgment criteria. The results are recorded in Table 3 below.

[0323] [Table 2]

[0324]

[0325] (2) Criteria for determining usability

[0326] ◎: Average score is 4.0 or above

[0327] 0: The average score is 3.0 or more and less than 4.0

[0328] △: Average score is 2.0 or more and less than 3.0

[0329] ×: Average score is less than 2.0

[0330] [Table 3]

[0331]

[0332] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 70-80% + (dimethicone / (PEG-10 / 15)) cross-polymer 20-30%)

[0333] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 80-90% + (dimethicone / vinyl dimethicone) crosspolymer 10-20%)

[0334] (Note 3) Shin-Etsu Chemical Co., Ltd.: PEG-10 dimethicone

[0335] (Note 4) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 6 mm 2 / s polydimethylsiloxane

[0336] According to the results in Table 3, the oil absorption performance of Examples 1 to 3 is higher than that of cellulose particles, and they are composite particles with silicone rubber particles attached to the surface. Examples 4 to 6, which are cosmetics containing Examples 1 to 3, have excellent skin compatibility when applied, and the usability after application is smooth and the blemish-covering effect is evaluated as higher than that of Comparative Example 2.

[0337] Example 7: Water-in-oil facial cream

[0338]

[0339] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (mineral oil 65-75% + (PEG-15 / lauryl dimethicone) crosspolymer 25-35%)

[0340] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: Mixture of (squalane 65-75% + (vinyl dimethicone / lauryl dimethicone) crosspolymer 25-35%)

[0341] (Note 3) Shin-Etsu Chemical Co., Ltd.: Cetyl PEG / PPG-10 / 1 dimethicone

[0342] (Manufacturing method)

[0343] A: Mix ingredients 1 to 5.

[0344] B: Mix ingredients 6 to 10.

[0345] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0346] D: The mixture obtained in the above step C is defoamed and then filled into a container to obtain a water-in-oil type facial cream.

[0347] The water-in-oil type facial cream of the present invention obtained in the above manner has excellent smoothness when applied, is non-sticky, is lightly spread, has excellent adhesion, and has a natural makeup feel with suppressed oiliness.

[0348] Example 8: Liquid emulsified foundation

[0349]

[0350] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 70-80% + (dimethicone / polyglyceryl-3) crosspolymer 20-30%)

[0351] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: Mixture of (cyclopentasiloxane 90-96% + (dimethicone / vinyl dimethicone) crosspolymer 4-10%)

[0352] (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone

[0353] (Note 4) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 6 mm 2 / s polydimethylsiloxane

[0354] (Note 5) Shin-Etsu Chemical Co., Ltd.: Trimethylsiloxysilicate 50% dissolved in cyclopentasiloxane

[0355] (Note 6) Shin-Etsu Chemical Co., Ltd.: Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone

[0356] (Note 7) Shin-Etsu Chemical Co., Ltd.: Triethoxysilylethyl polydimethylsiloxyethylhexyl polydimethylsiloxane treated coloring inorganic pigment, W: white, R: red, Y: yellow, B: black

[0357] (Manufacturing method)

[0358] A: Mix ingredients 1 to 7.

[0359] B: Components 8 to 13 are mixed and rolled.

[0360] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0361] D: Mix ingredients 14 to 18.

[0362] E: The mixture obtained in the above step D is added to the mixture obtained in the above step C, and mixed uniformly.

[0363] F: The mixture obtained in the above E was defoamed and then filled into a container to obtain a liquid emulsified foundation.

[0364] The liquid emulsion foundation of the present invention obtained in the above manner has excellent smoothness and moisturizing properties when applied, is non-sticky, is lightly spread, has excellent adhesion, and has a natural makeup feel with reduced oiliness.

[0365] Example 9: Pressed Powder

[0366]

[0367] (Note 1) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone

[0368] (Note 2) Shin-Etsu Chemical Co., Ltd.: Polymethylsilsesquioxane

[0369] (Note 3) Shin-Etsu Chemical Co., Ltd.: Methylsiloxane treatment

[0370] (Note 4) Shin-Etsu Chemical Co., Ltd.: Triethoxyoctylsilane treatment

[0371] (Manufacturing method)

[0372] A: Mix ingredients 1 to 4 evenly.

[0373] B: Mix ingredients 5 to 14 evenly.

[0374] C: The mixture obtained in the above step A is added to the mixture obtained in the above step B, and mixed.

[0375] D: The mixture obtained in the above step C is sieved and then pressed into a metal plate using a die to obtain a pressed powder.

[0376] The powder cake of the present invention obtained in the above manner has excellent smoothness and adhesion when applied, a long-lasting makeup effect, and a good makeup feel.

[0377] Example 10: Water-in-oil concealer

[0378]

[0379] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 70-80% + (dimethicone / (PEG-10 / 15)) cross-polymer 20-30%)

[0380] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: Mixture of (cyclopentasiloxane 90-96% + (dimethicone / vinyl dimethicone) crosspolymer 4-10%)

[0381] (Note 3) Shin-Etsu Chemical Co., Ltd.: PEG-9 polydimethylsiloxyethyl dimethicone

[0382] (Note 4) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 2 mm 2 / s polydimethylsiloxane

[0383] (Note 5) Shin-Etsu Chemical Co., Ltd.: Acrylate / polydimethylsiloxane copolymer 30% cyclopentasiloxane solution

[0384] (Note 6) Shin-Etsu Chemical Co., Ltd.: Acrylates / Ethylhexyl Acrylate / Dimethylsiloxane Methacrylate Copolymer

[0385] (Note 7) Shin-Etsu Chemical Co., Ltd.: Triethoxysilylethyl polydimethylsiloxyethylhexyl polydimethylsiloxane treated coloring inorganic pigment, W: white, R: red, Y: yellow, B: black

[0386] (Manufacturing method)

[0387] A: Mix ingredients 1 to 6.

[0388] B: Components 7 to 12 are mixed and rolled.

[0389] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0390] D: Mix ingredients 13 to 17.

[0391] E: The mixture obtained in the above step D is added to the mixture obtained in the above step C, and mixed uniformly.

[0392] F: The mixture obtained in the above E was defoamed and then filled into a container to obtain a water-in-oil concealer.

[0393] The water-in-oil concealer of the present invention obtained in the above manner has excellent smoothness when applied, is non-sticky, has excellent adherence, has suppressed oiliness, has a long-lasting makeup effect, and has a good makeup feel.

[0394] Example 11: Lipstick

[0395]

[0396] (Note 1) Shin-Etsu Chemical Co., Ltd.: Acrylates / stearyl acrylate / dimethicone methacrylate copolymer

[0397] (Note 2) Shin-Etsu Chemical Co., Ltd.: Acrylates / Ethylhexyl Acrylate / Dimethylsiloxane Methacrylate Copolymer

[0398] (Note 3) Shin-Etsu Chemical Co., Ltd.: Acrylates / Tridecyl Acrylate / Triethoxysilylpropanol Methacrylate / Polydimethylsiloxane Methacrylate Copolymer Treatment

[0399] (Manufacturing method)

[0400] A: Heat and dissolve ingredients 1 to 10.

[0401] B: Components 11 to 18 are mixed uniformly and subjected to roller compaction.

[0402] C: The mixture obtained in the above step B and component 19 are added to the mixture obtained in the above step A, and mixed uniformly.

[0403] D: The mixture obtained in the above step C is defoamed and then filled into a container to obtain a lipstick.

[0404] The lipstick of the present invention obtained in the above manner has excellent smoothness when applied, is non-sticky, is lightly spread, has excellent adhesion, is excellent in fit, and has a matte finish with reduced oiliness.

[0405] Example 12: Oil-in-water base cream

[0406]

[0407] (Manufacturing method)

[0408] A: Mix ingredients 1 to 6 evenly.

[0409] B: Heat and dissolve ingredients 7 to 11, and add ingredient 12 to make it uniform.

[0410] C: Components 13 to 19 are mixed and rolled.

[0411] D: The mixture obtained in the above step C is added to the mixture obtained in the above step B, and mixed uniformly.

[0412] E: The heated mixture obtained in the above step D is added to the heated mixture obtained in the above step A, and the mixture is mixed uniformly.

[0413] F: After the mixture obtained in the above step E is cooled to room temperature, components 20 and 21 are added and mixed uniformly.

[0414] G: The mixture obtained in the above step F is defoamed and then filled into a container to obtain an oil-in-water type base cream.

[0415] The oil-in-water base cream of the present invention obtained in the above manner has excellent moisturizing properties when applied, is non-sticky, is lightly spread, has excellent adhesion, and has a matte makeup feel with suppressed oiliness.

[0416] Example 13: Aqueous Gel

[0417]

[0418] (Note 1) Shin-Etsu Chemical Co., Ltd.: Polyglyceryl-3 Disiloxane Dimethicone

[0419] (Manufacturing method)

[0420] A: Mix ingredients 1 to 3 evenly.

[0421] B: Mix ingredients 4 to 10 evenly.

[0422] C: The mixture obtained in the above step A is added to the mixture obtained in the above step B, and mixed uniformly.

[0423] D: The mixture obtained in the above step C is defoamed and then filled into a container to obtain an aqueous gel.

[0424] The aqueous gel of the present invention obtained in the above manner has excellent moisturizing properties when applied, is non-sticky, is lightly spread, has excellent adhesion, and has a matte makeup feel with reduced oiliness.

[0425] Example 14: Oily Gel

[0426]

[0427] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 70-80% + (dimethicone / vinyl dimethicone) crosspolymer 20-30%)

[0428] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: Mixture of (cyclopentasiloxane 90-96% + (dimethicone / vinyl dimethicone) crosspolymer 4-10%)

[0429] (Note 3) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone

[0430] (Note 4) Shin-Etsu Chemical Co., Ltd.: Cyclopentasiloxane

[0431] (Manufacturing method)

[0432] A: Mix ingredients 1 to 5 evenly.

[0433] B: The mixture obtained in the above step A is defoamed and then filled into a container to obtain an oily gel.

[0434] The oily gel of the present invention obtained in the above manner has excellent smoothness when applied, is non-sticky, is lightly spread, has excellent adhesion, is excellent in fit, and has a matte makeup feel with reduced oiliness.

[0435] Example 15: Oily solid foundation

[0436]

[0437] (Note 1) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone

[0438] (Note 2) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 2 mm 2 / s polydimethylsiloxane

[0439] (Note 3) Shin-Etsu Chemical Co., Ltd.: Polymethylsilsesquioxane

[0440] (Note 4) Shin-Etsu Chemical Co., Ltd.: Lauryl Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone

[0441] (Note 5) Shin-Etsu Chemical Co., Ltd.: Methylsiloxane treatment

[0442] (Note 6) Shin-Etsu Chemical Co., Ltd.: Triethoxysilylethyl polydimethylsiloxyethylhexyl polydimethylsiloxane treated coloring inorganic pigment, W: white, R: red, Y: yellow, B: black

[0443] (Manufacturing method)

[0444] A: Heat and dissolve ingredients 1 to 9.

[0445] B: Mix ingredients 12 to 18 evenly and perform roller compaction.

[0446] C: The mixture obtained in the above step B and components 10 to 11 are added to the heated mixture obtained in the above step A, and mixed uniformly.

[0447] D: The mixture obtained in the above step C is defoamed, filled into a container in a heated state, and cooled to room temperature to obtain an oil-based solid foundation.

[0448] The oil-based solid foundation of the present invention obtained in the above manner spreads lightly, fits the skin closely, and has a moisturizing makeup feel. A makeup film with reduced shine and tension can be obtained, and the makeup effect is long-lasting and very excellent.

[0449] Example 16: Oily foundation

[0450]

[0451] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (75-85% isododecane + 15-25% (vinyl dimethicone / lauryl dimethicone) crosspolymer)

[0452] (Note 2) Shin-Etsu Chemical Co., Ltd.: Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone

[0453] (Note 3) Shin-Etsu Chemical Co., Ltd.: 30% trimethylsiloxysilylcarbamoyl pullulan dissolved in isododecane

[0454] (Note 4) Manufactured by Shin-Etsu Chemical Co., Ltd.: Kinematic viscosity at 25°C: 6 mm 2 / s polydimethylsiloxane

[0455] (Note 5) Shin-Etsu Chemical Co., Ltd.: Acrylates / Ethylhexyl Acrylate / Dimethylsiloxane Methacrylate Copolymer

[0456] (Note 6) Shin-Etsu Chemical Co., Ltd.: Hydrogenated polydimethylsiloxane treatment

[0457] (Note 7) Shin-Etsu Chemical Co., Ltd.: Triethoxyoctylsilane treatment

[0458] (Manufacturing method)

[0459] A: Mix ingredients 1 to 9 evenly.

[0460] B: Mix ingredients 10 to 17 evenly and perform roller compaction.

[0461] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0462] D: The mixture obtained in the above step C is defoamed and then filled into a container to obtain an oil-based foundation.

[0463] The oil-based foundation of the present invention obtained in the above manner has light spreadability, fits the skin well, has a moist makeup feel, and can obtain a makeup film that suppresses oiliness and has tension, and has a long-lasting makeup effect, which is very excellent.

[0464] Example 17: Oily Mascara

[0465]

[0466] (Note 1) Shin-Etsu Chemical Co., Ltd.: PEG-9 polydimethylsiloxyethyl dimethicone

[0467] (Note 2) Shin-Etsu Chemical Co., Ltd.: (Norbornene / tris(trimethylsiloxy)silylnorbornene) copolymer 30% dissolved in isododecane

[0468] (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone

[0469] (Note 4) Shin-Etsu Chemical Co., Ltd.: Triethoxysilylethyl polydimethylsiloxyethylhexyl polydimethylsiloxane treated coloring inorganic pigment, W: white, B: black

[0470] (Manufacturing method)

[0471] A: Heat and dissolve ingredients 1 to 8.

[0472] B: Mix components 10 to 13 evenly and perform roller compaction.

[0473] C: The mixture obtained in the above step B and component 9 are added to the heated mixture obtained in the above step A, and mixed uniformly.

[0474] D: The mixture obtained in the above step C was defoamed, cooled to room temperature, and then filled into a container to obtain an oily mascara.

[0475] It can be seen that the oily mascara of the present invention obtained in the above manner has excellent smoothness when applied, no stickiness, is light when spread, has excellent adhesion, is excellent in fit, has a makeup feel with suppressed oiliness, does not stick to the makeup, and has a long-lasting makeup effect, which is very excellent.

[0476] Example 18: Loose powder

[0477]

[0478] (Note 1) Shin-Etsu Chemical Co., Ltd.: Hydrogenated polydimethylsiloxane treatment

[0479] (Note 2) Shin-Etsu Chemical Co., Ltd.: Triethoxyoctylsilane treatment

[0480] (Manufacturing method)

[0481] A: Mix ingredients 1 to 10 evenly.

[0482] B: Mix ingredients 11 and 12 evenly.

[0483] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0484] D: The mixture obtained in the above step C is sieved and filled into a container to obtain loose powder.

[0485] It is found that the loose powder of the present invention obtained in the above manner is excellent in smoothness when applied, has a makeup feel with reduced oiliness, and has a very excellent long-lasting makeup effect.

[0486] Example 19: Sunscreen Lotion

[0487]

[0488] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (diphenylsiloxyphenyl trimethicone 75-85% + (dimethicone / (PEG-10 / 15)) crosspolymer 15-25%)

[0489] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (diphenylsiloxyphenyl trimethicone 80-90% + (dimethicone / phenyl vinyl dimethicone) crosspolymer 10-20%)

[0490] (Note 3) Shin-Etsu Chemical Co., Ltd.: Cetyl PEG / PPG-10 / 1 dimethicone

[0491] (Note 4) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone

[0492] (Note 5) Shin-Etsu Chemical Co., Ltd.: Ethyl trimethicone

[0493] (Note 6) Shin-Etsu Chemical Co., Ltd.: 40% cyclopentasiloxane dispersion of titanium dioxide fine particles

[0494] (Note 7) Shin-Etsu Chemical Co., Ltd.: Micronized zinc oxide 60% cyclopentasiloxane dispersion

[0495] (Manufacturing method)

[0496] A: Mix ingredients 1 to 10 evenly.

[0497] B: Mix ingredients 13 to 17 evenly.

[0498] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0499] D: Add components 11 and 12 to the mixture obtained in step C above and mix well.

[0500] E: The mixture obtained in the above step D is defoamed and then filled into a container to obtain a sunscreen emulsion.

[0501] It can be seen that the sunscreen emulsion of the present invention obtained in the above manner is excellent in smoothness when applied, has a makeup feel with reduced oiliness, and has a very excellent long-lasting makeup effect.

[0502] Example 20: Sunscreen Lotion

[0503]

[0504] (Note 1) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (dimethicone 70-80% + (dimethicone / (PEG-10 / 15)) cross-polymer 20-30%)

[0505] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: A mixture of (diphenylsiloxyphenyl trimethicone 80-90% + (dimethicone / phenyl vinyl dimethicone) crosspolymer 10-20%)

[0506] (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl PEG-9 Polydimethylsiloxyethyl Dimethicone

[0507] (Note 4) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone

[0508] (Note 5) Shin-Etsu Chemical Co., Ltd.: Cyclopentasiloxane

[0509] (Manufacturing method)

[0510] A: Mix ingredients 1 to 7 evenly.

[0511] B: Mix ingredients 8 to 11 evenly.

[0512] C: The mixture obtained in the above step B is added to the mixture obtained in the above step A, and mixed uniformly.

[0513] D: The mixture obtained in the above step C is defoamed and then filled into a container to obtain a sunscreen emulsion.

[0514] It can be seen that the sunscreen emulsion of the present invention obtained in the above manner is excellent in smoothness when applied, has a makeup feel with reduced oiliness, and has a very excellent long-lasting makeup effect.

[0515] Example 21: Non-aqueous deodorant cream

[0516]

[0517] (Note 1) Shin-Etsu Chemical Co., Ltd.: Ethyl trimethicone

[0518] (Note 2) Made by Shin-Etsu Chemical Co., Ltd.: Mixture of (cyclopentasiloxane 90-96% + (dimethicone / vinyl dimethicone) crosspolymer 4-10%)

[0519] (Manufacturing method)

[0520] A: Heat ingredients 2, 3, 5, 7, 9, 11, and 12 and mix well.

[0521] B: Component 10 is added to the mixture obtained in the above step A, and the mixture is uniformly dispersed and mixed using a mixer.

[0522] C: Add components 1, 4, and 8 to the mixture obtained in step B above and mix well.

[0523] D: Component 6 is added to the mixture obtained in the above step C, mixed evenly, and then filled into a container.

[0524] The deodorant cream obtained in the above manner can be spread very smoothly, has excellent ductility, does not have excessive dryness and stickiness, and has excellent durability of the deodorizing effect.

[0525] As described above, according to the present invention, composite particles formed by attaching rubber particles to the surface of organic resin particles, which can impart soft touch and smooth feeling during use, spreadability, and a natural makeup effect due to light scattering, a method for producing the same, and a cosmetic containing the composite particles can be provided.

[0526] This specification includes the following inventions.

[0527] [1] A composite particle comprising a spherical organic resin particle and a rubber particle attached to the surface of the spherical organic resin particle, wherein the rubber particle is fixed to the organic resin particle using silica as a binder.

[0528] [2]: The composite particles according to [1] above, wherein the amount of the rubber particles is in the range of 0.1 to 100 parts by mass per 100 parts by mass of the organic resin particles.

[0529] [3]: The composite particles according to [1] or [2] above, wherein the amount of the silica is in the range of 10 to 1,000 parts by mass per 100 parts by mass of the rubber particles.

[0530] [4]: The composite particles according to [1], [2] or [3] above, wherein the rubber particles are silicone rubber particles.

[0531] [5]: The composite particles according to [1], [2], [3] or [4] above, wherein the organic resin particles are cellulose particles.

[0532] [6]: A method for producing composite particles, which is the method for producing composite particles described in [1], [2], [3], [4] or [5] above, characterized in that tetraalkoxysilane is added to a mixed solution formed by blending the organic resin particles, the rubber particles, a cationic substance, an alkaline substance and water to carry out hydrolysis and condensation reactions, wherein the cationic substance is set to a cationic surfactant and / or a cationic water-soluble polymer.

[0533] [7]: The method for producing composite particles according to [6] above, wherein the cationic substance is a cationic surfactant and a cationic water-soluble polymer.

[0534] [8]: The method for producing composite particles according to [6] or [7] above, characterized in that the amount of the cationic substance added is set to a range of 0.0001 to 2.0 parts by mass relative to 100 parts by mass of water in the mixed solution.

[0535] [9]: The method for producing composite particles according to the above [6], [7] or [8] is characterized in that the blending amount of the cationic surfactant is set to: a range of 0.001 to 1.9 parts by mass relative to 100 parts by mass of water in the mixed solution, and the blending amount of the cationic water-soluble polymer is set to: a range of 0.0001 to 1.0 parts by mass relative to 100 parts by mass of water in the mixed solution.

[0536]

[10] : A cosmetic comprising the composite particles described in [1], [2], [3], [4] or [5] above.

[0537] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are examples, and any technical solution having substantially the same configuration as the technical concept described in the claims of the present invention and having the same technical effect is included in the technical scope of the present invention.

Claims

1. A composite particle comprising a spherical organic resin particle and a rubber particle attached to the surface of the spherical organic resin particle, characterized in that: The rubber particles are fixed to the organic resin particles by using silicon dioxide as a binder.

2. The composite particles according to claim 1, characterized in that The amount of the rubber particles is in the range of 0.1 to 100 parts by mass relative to 100 parts by mass of the organic resin particles.

3. The composite particles according to claim 1, characterized in that The amount of the silica is in the range of 10 to 1,000 parts by mass relative to 100 parts by mass of the rubber particles.

4. The composite particles according to claim 1, characterized in that The rubber particles are silicone rubber particles.

5. The composite particles according to any one of claims 1 to 4, characterized in that The organic resin particles are cellulose particles.

6. A method for producing composite particles, which is the method for producing composite particles according to claim 1, characterized in that: Tetraalkoxysilane is added to a mixed solution of the organic resin particles, the rubber particles, a cationic substance, an alkaline substance and water to carry out hydrolysis and condensation reactions, wherein the cationic substance is a cationic surfactant and / or a cationic water-soluble polymer.

7. The method for producing composite particles according to claim 6, characterized in that: The cationic substances are cationic surfactants and cationic water-soluble polymers.

8. The method for producing composite particles according to claim 6, characterized in that: The amount of the cationic substance added is set to be in the range of 0.0001 to 2.0 parts by mass relative to 100 parts by mass of water in the mixed liquid.

9. The method for producing composite particles according to any one of claims 6 to 8, characterized in that: The amount of the cationic surfactant blended is set to be in the range of 0.001 to 1.9 parts by mass relative to 100 parts by mass of water in the mixed solution, and the amount of the cationic water-soluble polymer blended is set to be in the range of 0.0001 to 1.0 parts by mass relative to 100 parts by mass of water in the mixed solution.