Aqueous dispersion of biocide-free organic opaque pigment particles

By combining a multi-stage polymer particle aqueous dispersion with specific concentrations of hydrogen peroxide and chelating agents, the health and regulatory issues of biocides in coating preservation are solved, achieving effective inhibition of microorganisms at low pH, and ensuring the safety and sustainability of the coating.

CN118891330APending Publication Date: 2024-11-01ROHM & HAAS CO
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202380027259.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing technology, the biocides used in the preservation of coatings face challenges due to health, safety and regulatory issues, and the high pH adjustment method poses safety hazards. There is a need for safer and more sustainable preservation methods.

Method used

An aqueous dispersion of multi-stage polymer particles, comprising a water-absorbing core and a polymer shell, combined with a specific concentration of t-C4-C10-alkyl hydrogen peroxide or hydrogen peroxide with a chelating agent, forms a composition that effectively prevents microbial contamination at low pH.

Benefits of technology

It achieves effective inhibition of microorganisms without the use of biocides, prevents coating degradation and spoilage, avoids safety issues caused by high pH, ​​and meets regulatory requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005040310100000031
    Figure BDA0005040310100000031
Patent Text Reader

Abstract

The present invention relates to a composition comprising: an aqueous dispersion of multi-stage polymer particles, the aqueous dispersion of multi-stage polymer particles comprising a water-occluding core and a polymer shell, the polymer shell having a Tg in the range of 60 DEG C to 120 DEG C; t-C4-C10-alkyl hydrogen peroxide or hydrogen peroxide with an anti-corrosion amount; and less than 1000 ppm of residual monomer. The present invention addresses the need in the art by providing a way to preserve opaque polymers to prevent microbial contamination without the use of biocides.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The present invention relates to aqueous dispersions of organic opacifying pigment particles that exhibit resistance to microbial growth in the absence of a biocide.

[0002] Aqueous intermediates used in the coating industry are preserved with biocides to inhibit the formation and growth of biological organisms (such as bacteria, yeasts and molds) while in storage. Inhibition of these organisms prevents product degradation and spoilage, as well as the outgassing of volatile products and subsequent pressure buildup in closed containers. Preservation is therefore necessary for health, safety and performance reasons.

[0003] Can preservatives such as isothiazolinones are facing intense regulatory scrutiny for their real or perceived adverse effects on health, safety and the environment; in fact, a total ban on these biocides appears imminent in many parts of the world. To the extent that the development of new biocides is not possible due to cost reasons and the widespread perception (whether justified or not) of the inherent dangers of these biocides, there is a need to replace biocides with alternative non-biocidal preservatives that are safer and more sustainable.

[0004] In EP 3 456 787 B1, can be found for the preservation of coatings to prevent the recent example of non-biocidal methods of microbial contamination, the document discloses pH adjustment to the aqueous coating formulations in the range of 10 to 12.5. Although effective on the surface, these formulations of very high pH have produced other safety and sanitation issues, making this method impractical. Other non-traditional methods such as adding silver or zinc ions may adversely affect the characteristics of coatings, and also face regulatory review. Due to these reasons, it is necessary to be used to preserve other safer and more sustainable methods of coatings and coating additives. Summary of the invention

[0005] The present invention solves the need in the art by providing a composition comprising:

[0006] a) an aqueous dispersion of multistage polymer particles, the aqueous dispersion of multistage polymer particles comprising:

[0007] 1) a water absorbing core comprising 20 to 60% by weight of structural units of a salt of a carboxylic acid monomer and 40 to 80% by weight of structural units of a nonionic monoethylenically unsaturated monomer; and

[0008] 2) a polymer shell having a T g In the range of 60°C to 120°C;

[0009] b1) 500 ppm to 5,000 ppm, based on the weight of the composition, of t-C4-C10-alkyl hydroperoxide; or

[0010] b2) from 1000 ppm to 10000 ppm of hydrogen peroxide and from 50 ppm to 1000 ppm of a chelating agent not complexed with a polyvalent metal cation, based on the weight of the composition; and

[0011] c) less than 1000 ppm residual monomers based on the weight of the composition;

[0012] The z-average particle size of the polymer particles is in the range of 300 nm to 2000 nm.

[0013] The present invention addresses the need in the art by providing a way to preserve opaque polymers from microbial contamination without the use of biocides. DETAILED DESCRIPTION

[0014] The present invention is a composition comprising:

[0015] a) an aqueous dispersion of multistage polymer particles, the aqueous dispersion of multistage polymer particles comprising:

[0016] 1) a water absorbing core comprising 20 to 60% by weight of structural units of a salt of a carboxylic acid monomer and 40 to 80% by weight of structural units of a nonionic monoethylenically unsaturated monomer;

[0017] 2) a polymer shell having a T g In the range of 60°C to 120°C;

[0018] b1) 500 ppm to 5,000 ppm, based on the weight of the composition, of t-C4-C10-alkyl hydroperoxide; or

[0019] b2) from 1000 ppm to 10000 ppm of hydrogen peroxide and from 50 ppm to 1000 ppm of a chelating agent not complexed with a polyvalent metal cation, based on the weight of the composition; and

[0020] c) less than 1000 ppm residual monomers based on the weight of the composition;

[0021] The z-average particle size of the polymer particles is in the range of 300 nm to 2000 nm.

[0022] The water-retaining core comprises from 20 wt %, preferably from 25 wt %, more preferably from 30 wt %, and most preferably from 32 wt % to 60 wt %, preferably to 50 wt %, more preferably to 40 wt %, and most preferably to 36 wt % of structural units of salts of carboxylic acid monomers, based on the weight of the structural units of the monomers in the core.

[0023] As used herein, the term "structural unit" refers to the residue of the monomer after polymerization. For example, the structural unit of methacrylate, wherein M + is a counterion, preferably a lithium, sodium or potassium counterion, as shown:

[0024]

[0025] Examples of suitable carboxylic acid monomers include acrylic acid, methacrylic acid, itaconic acid, and maleic acid.

[0026] As used herein, "residual monomer" refers to monomer used to prepare the polymer particles that remains unreacted.

[0027] The water-retaining core also comprises from 40 wt %, preferably from 50 wt %, more preferably from 55 wt %, more preferably from 60 wt %, and most preferably from 64 wt % to 80 wt %, preferably to 75 wt %, more preferably to 70 wt %, and most preferably to 68 wt % of the structural unit of the nonionic monoethylenically unsaturated monomer, based on the weight of the structural unit of the monomer in the core. Examples of nonionic monoethylenically unsaturated monomers include one or more acrylates and / or methacrylates, such as methyl acrylate, ethyl acrylate, n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, isobornyl methacrylate, lauryl methacrylate, and cyclohexyl methacrylate; and one or more monoethylenically unsaturated aromatic compounds, such as styrene, α-methylstyrene, and 4-tert-butylstyrene. A preferred nonionic monoethylenically unsaturated monomer is methyl methacrylate.

[0028] The Tg of the polymer shell of the polymer particles is preferably in the range of not less than 60°C, or not less than 80°C, or not less than 90°C, or not less than 95°C and not more than 115°C, or not more than 110°C. As used herein, Tg g refers to the homopolymer T as reported in the Polymer Handbook, 4th edition (1999, John Wiley & Sons, Inc.). g Data, glass transition temperature calculated by Fox equation.

[0029] Preferably, the shell of the polymer particles comprises structural units of methyl methacrylate, styrene, α-methylstyrene, isobornyl methacrylate, lauryl methacrylate or cyclohexyl methacrylate. In one embodiment, the shell comprises structural units of at least 80 wt%, at least 90 wt% or at least 95 wt% of styrene. In another embodiment, the shell comprises structural units of styrene in an amount of 89 to 93 wt% and structural units of any one or all of methyl methacrylate (4 to 5 wt%), cyclohexyl methacrylate (0.9 to 2 wt%), methacrylic acid (2 to 3 wt%) and the multiethylenically unsaturated monomer allyl methacrylate (ALMA, 0.1 to 0.5 wt%).

[0030] The polymer shell may further comprise structural units of other polyethylenically unsaturated monomers, such as divinylbenzene (DVB), trimethylolpropane trimethacrylate (TMPTMA) or trimethylolpropane triacrylate (TMPTA). The solids content of the multistage polymer particles is preferably in the range of 10 to 40 wt % based on the weight of the composition.

[0031] In one aspect, the z-average particle size of the polymer particles is preferably in the range of 950 nm to 2000 nm; in another aspect, the z-average particle size of the polymer particles is in the range of 200 nm, preferably 350 nm, and more preferably 375 nm to preferably 600 nm, more preferably to 500 nm, and most preferably to 425 nm. As used herein, the z-average particle size refers to the particle size determined by dynamic light scattering, for example by a BI-90 Plus particle size analyzer (Brookhaven). The multi-stage polymer particles preferably constitute 10% to 35% by weight of the composition.

[0032] The composition also contains C4-C 10 -t-alkyl hydroperoxide or hydrogen peroxide. Preferably, t-C4-C 10 -alkyl hydroperoxide is t-C4-C8-alkyl hydroperoxide, more preferably tert-butyl hydroperoxide or tert-amyl hydroperoxide or a combination thereof, their concentration is in the range of 500 ppm, or 600 ppm, or 700 ppm or 1000 ppm to 10000 ppm, or to 5000 ppm or to 3000 ppm. When the composition comprises only hydrogen peroxide, the composition further comprises a chelating agent which is not complexed with a multivalent metal (such as iron).

[0033] Examples of suitable chelating agents include diaminocarboxylates, such as tetrasodium ethylenediaminetetraacetic acid (EDTA tetrasodium salt), which is available as VERSENE TMChelating agents are commercially available as DeQuest® (trademark of The Dow Chemical Company or its affiliates), and hydroxyethylidene diphosphonates, such as tetrasodium salt of 1-hydroxyethylidene-1,1-diphosphonic acid, are commercially available as DeQuest® 2016 chelating agent.

[0034] Aqueous dispersions of multi-stage polymer particles can be prepared, for example, by the methods disclosed in US 6,020,435 and US 2020 / 0071439A1. Examples of commercially available dispersions of first multi-stage polymer particles include ROPAQUE TM Ultra-Opaque Polymer, AQUACell HIDE 6299 Opaque Polymer and ROPAQUE TM TH-2000 hollow sphere pigment. (ROPAQUE is a trademark of The Dow Chemical Company or its affiliates).

[0035] As disclosed in US 6,020,435, dispersions of multi-stage polymer particles are prepared by sequential emulsion polymerization. In this process, an aqueous dispersion of core polymer particles is first contacted with a monomer under emulsion polymerization conditions to form an aqueous dispersion of core / shell or core / intermediate polymer particles, the calculated T of the homopolymer of the first monomer being 1:1. g In the range of 60°C, or 80°C, or 90°C, or 95°C to 115°C, or to 110°C.

[0036] In the second step, a free radical chaser is added to the reaction mixture to inhibit the polymerization of the subsequently added swelling monomer. Examples of suitable free radical chasers include oxidizable metal salts (such as FeSO4) that become water soluble at high pH by forming a water soluble complex with a chelating agent (such as EDTA tetrasodium salt). The chelating agent is used as a limiting agent in this step.

[0037] After adding the free radical chaser, the T g A swelling monomer in the range of 60° C., or 80° C., or 90° C. to 120° C., or to 110° C. and a polymerization inhibitor are added to the reaction mixture. In one aspect, the swelling monomer comprises at least 80 wt % or at least, or at least 90 wt % or at least 95 wt % styrene.

[0038] On the other hand, the swelling monomer comprises 89 to 93 wt% styrene and 7 to 11 wt% of any one or all of methyl methacrylate (4 to 5 wt%), cyclohexyl methacrylate (0.9 to 2 wt%), methacrylic acid (2 to 3 wt%), and a polyethylenically unsaturated monomer allyl methacrylate (ALMA, 0.1 to 0.5 wt%). Examples of polymerization inhibitors include 4-hydroxy-2,2,6,6, tetramethylpiperidinyloxy, free radical (4-hydroxy-TEMPO), hydroquinone, p-methoxyhydroquinone, tert-butyl-p-hydroquinone, and 4-tert-butylcatechol.

[0039] After the addition of the swelling monomer and the polymerization inhibitor is complete, a swelling agent is added to the aqueous dispersion of the multi-stage polymer particles to penetrate the shell or the middle layer and induce swelling of the core with water. The swelling agent is a base such as ammonium hydroxide, LiOH, NaOH and KOH. Next, in a key step of one aspect of the method of the present invention, C4-C 10 -t-Alkyl hydroperoxide, preferably C4-C 10 -t-alkyl hydroperoxide, more preferably tert-butyl hydroperoxide or tert-amyl hydroperoxide and a reducing agent such as isoascorbic acid in a C4-C4 ratio in the range of 5:1, or 7.5:1, or 12:1 to 50:1, or to 30:1 or to 20:1. 10 -t-alkyl hydroperoxide to reducing agent molar ratio is added to the aqueous dispersion. This ratio is significantly higher than previously reported ratios in the range of 2.0:1 to 3.0:1, and is therefore significantly higher than the ratio required to chase residual monomer. Clearly, there is no obvious reason to add more oxidant than the amount taught to be sufficient to chase residual monomer.

[0040] Preferably, the t-alkyl hydroperoxide is added all at once, followed by gradual addition of the reducing agent. It may also be advantageous to add a portion of the t-C4-C4-alkyl hydroperoxide all at once before adding the reducing agent. 10 -alkyl hydroperoxide, and then add the remaining portion of the t-C4-C 10 -alkyl hydroperoxide. For example, 1235 ppm of tert-butyl hydroperoxide may be added to the dispersion at once, followed by gradual addition of 305 ppm of isoascorbic acid; alternatively, 412 ppm of tert-butyl hydroperoxide may be added to the dispersion at once, followed by gradual addition of 305 ppm of isoascorbic acid, followed by 823 ppm of tert-butyl hydroperoxide. After the addition of isoascorbic acid is complete, 823 ppm of tert-butyl hydroperoxide may be added.

[0041] When hydrogen peroxide and a chelating agent are used, the redox coupling agent is added at a ratio ranging from 2.0:1 to 3.0:1, and the hydrogen peroxide and the chelating agent that are not combined with the metal ion (such as Fe) are added later.+2 ) complexed chelating agent. In this regard, the amount of hydrogen peroxide added is in the range of 0.1 wt % to 1 wt % based on the weight of the composition, and the amount of chelating agent not complexed with the metal cation is in the range of 50 ppm to 1000 ppm based on the weight of the composition.

[0042] In addition to achieving the goal of reinitiating polymerization and chemically converting the amount of unreacted monomer from a level typically in the range of 8% to 20% by weight based on the weight of the multi-stage polymer particles and unreacted monomer to a level below 1000 ppm, preferably below 500 ppm, the presence of a significant excess of an oxidizing agent of the type described herein produces an opaque polymer composition that resists microbial attack. In contrast, when conventional amounts of tert-butyl hydroperoxide described in the prior art are used (in the range of 2.0:1 to 3.0:1 molar ratios relative to isoascorbic acid without post-addition of hydrogen peroxide and chelating agents), the resulting concentration of tert-butyl hydroperoxide (about 350 ppm) is insufficient to act as a preservative when the final concentration of unreacted monomer is less than 1000 ppm.

[0043] It has been found that adding t-C4-C4 in a large excess over that which is conventionally added to chemically convert the monomers into part of the shell of the multi-stage polymer particle is effective. 10 -Alkyl hydroperoxides preserve the substantially monomer-free dispersion of the multi-stage polymer particles to prevent microbial attack. More specifically, tert-butyl hydroperoxide or tert-amyl hydroperoxide is added after the swelling step at a molar ratio of oxidant to reductant of at least 5:1, or at least 7.5:1, or at least 12:1, and preferably not more than 50:1, or 30:1, or 20:1, which gives excellent preservative properties without the need for biocides. As previously described, there is no need to add excess oxidant at one time. It is also possible to add approximately the same amount of oxidant as was used in the post-swelling monomer chase step, followed by a preservative amount of oxidant after the chase is complete.

[0044] Provides corrosion protection (where H2O2 is the oxidant) or improved corrosion protection (in t-C4-C 10 -alkyl hydroperoxide is the oxidizing agent) in an amount above that required to complex with any free (non-complexed) metal cations. Preferably, the non-complexed chelating agent concentration is in the range of 100 ppm to 2000 ppm based on the weight of the composition.

[0045] It has been found that preservation of aqueous dispersions of opaque polymers can be achieved at relatively low pH, typically 7.5 or 8.0 to 9.5 or to 9.0; it has also been found that preservation comparable to that achieved with biocides can be achieved at relatively low pH without the need for any biocides. Thus, in another aspect, the compositions of the invention do not contain any biocides.

[0046] The disclosed method describes the use of a stoichiometric excess of the metal salt, leaving no residual chelating agent that is not complexed with the metal salt. It has been found that when hydrogen peroxide is used, the presence of a sufficient amount of additional chelating agent is necessary to achieve the preservative effect, and when t-C4-C 10 -alkyl hydroperoxides are sometimes useful to improve corrosion protection.

[0047] Example

[0048] t-AHP or t-BHP in serum 1 H NMR spectroscopy

[0049] 3.0mL latex sample and 3.0mL Milli-Q water were loaded into approximately 10mL polycarbonate tubes and centrifuged at 100,000rpm for 15 minutes. The resulting clarified supernatant was carefully decanted and transferred to a 5-mm NMR tube. A flame-sealed capillary filled with an external standard (5.000wt% d4-trimethylsilyl propionate sodium in D2O) was added to the NMR tube. Careful attention was paid to the correct alignment of the external standard in the NMR tube. The NMR spectrum was obtained using a BrukerAVANCE III 600 spectrometer equipped with a 5-mm BroadBand CryoProbe. Each sample was individually tuned and shimmed, but the pulse width and receiver gain remained constant for the sample series. The concentration of free tert-amyl hydroperoxide or tert-butyl hydroperoxide was measured by using a zg pulse sequence with the following parameters: acquisition time (aq) = 2.5 seconds, recycle delay (d1) = 30 seconds, number of transients (ns) = 1024, receiver gain (rg) = 32, and pulse width (p1) = 11 milliseconds. All other parameters (time domain size, scan width, dwell time, prescan delay, and carrier frequency) were kept at default values. The concentration of free hydrogen peroxide was calculated by comparing the peak resonating around 1.2 ppm with the integral of the peak of an external standard at 0.0 ppm. The spectra were referenced to an external standard at 0.0 ppm on a trimethylsilyl chemical shift scale.

[0050] Hydrogen Peroxide 1 H NMR spectroscopy analysis

[0051] H2O2 1 H NMR spectroscopy can be performed as 1Quantitative analysis of hydrogen peroxide by H NMR spectroscopy was determined as described in Anal. Bioanal. Chem. (2005), 381: 1289-1293.

[0052] Preparation of samples for antimicrobial resistance

[0053] The samples were tested for antimicrobial properties "as is" (not heat aged) and after being subjected to 50°C for four weeks (heat aged). A 10-g aliquot was taken from each sample and heated to 10 6 -10 7 The samples were inoculated three times with a pool of standard bacteria, yeasts and molds (obtained from the American Type Culture Collection (ATCC) for common contaminants in coatings) with 7-day intervals. After inoculation, the samples were stored in a 25°C incubator. The microbial contamination of the test samples was monitored by agar plate inoculation using the standard streak plate method. The samples were inoculated on tryptic soy agar (TSA) and potato dextrose agar (PDA) plates on the 1st and 7th days after each microbial attack. All agar plates were checked daily until the 7th day after inoculation to determine the number of microorganisms that survived in the test samples. Between inspections, agar plates were stored in an incubator, at 30°C for TSA plates, and at 25°C for PDA plates. The degree of microbial contamination was determined by counting colonies, where the rating score was determined according to the number of microbial colonies observed on agar plates. The reported results are from the 7th day readings, and are summarized for both "as is" and heat aging samples. Table 1 illustrates the rating system used to estimate the level of microbial contamination on the planned production plates. Colony count refers to the number of colonies on the plate.

[0054] Table 1 - Rating system for estimating microbial contamination

[0055] Colony Rating score pollute result none 0 none qualified 1-9 Tr Trace qualified 10 to 99 1 Very slight Failure 100 to about 1000 2 slight Failure About 1000 to 10,000 3 Moderate Failure >10,000 4 Severe Failure

[0056] In Table 1, "pass" means less than ten colonies were detected on the plate on a specific day after inoculation (Day 1 (D1) or Day 7 (D7)). "Fail" means ten or more different colonies were detected on the plate on a specific day after inoculation.

[0057] Comparative Example 1 - Preparation of an aqueous dispersion of multi-stage polymer particles

[0058] In the following description, core #1 refers to an aqueous dispersion of polymer particles (66 MMA / 34 MAA, 32.0% solids, z-average particle size of 135 nm) prepared essentially as described in US 6,020,435.

[0059] A 5-L four-necked round bottom flask was equipped with a paddle stirrer, a thermometer, a N2 inlet, and a reflux condenser. DI water (730.64 g) and acetic acid (0.28 g in 1.64 g water) were added to the vessel and the contents were heated to 89 ° C under N2. Sodium persulfate (NaPS, 3.39 g in 24.55 g water) was immediately added to the vessel, followed by core # 1 (218.53 g). Then within 60 minutes, a monomer emulsion 1 (ME 1) prepared by mixing DI water (69.55 g), Polystep A-16-22 emulsifier (5.5 g), styrene (69.95 g), methacrylic acid (8.43 g), and methyl methacrylate (61.53 g) was added to the vessel. During the ME 1 feed, the temperature of the reaction mixture was kept constant at 78 ° C, after which a DI water rinse (32.73 g) was added. After the ME 1 feed was completed, monomer emulsion 2 (ME 2) prepared by mixing DI water (217.64 g), Polystep A-16-22 emulsifier (11.09 g), styrene (657 g), linseed oil fatty acid (4.17 g), allyl methacrylate (2.13 g) and methacrylic acid (12.6 g) was fed into the vessel over 60 minutes. The temperature of the reaction mixture was raised to 84° C. after 15 minutes and to 92° C. after 25 minutes. Simultaneously with the start of the ME 2 feed, a NaPS solution (0.93 g in 62.18 g water) was co-fed into the vessel over 65 minutes. After the ME 2 feed was completed, a DI water rinse (32.73 g) was added to the vessel followed by ferrous sulfate heptahydrate (16.36 g of 0.1 wt. % FeSO4·7H2O) and VERSENE TM An aqueous mixture of chelating agent (1.64 g of 1 wt.% EDTA tetrasodium salt) was added to the vessel followed by hot DI water (>60°C, 182.45 g).The contents of the reaction mixture were maintained at 90-92°C for 15 minutes.

[0060] ME 3 prepared by mixing DI water (57.27 g), Polystep A-16-22 emulsifier (2.05 g), styrene (167.73 g) and 4-hydroxy TEMPO (1.88 g) was fed into the container over 5 minutes, and the temperature of the reaction mixture was reduced to 85° C. Immediately after the ME 3 feed addition was completed, NaOH (29.45 g, 50 wt.% aqueous solution) mixed with hot DI water (572.73 g) was added to the container over 10 minutes. When the NaOH addition was complete, the batch was held for 5 minutes. After the holding was completed, a post-polymerization solution of t-BHP (2.12 g, 70 wt.% aqueous solution) in DI water (24.55 g) was added to the container, and a separate solution of isoascorbic acid (IAA, 1.1 g) in water (65.45 g) was fed into the container over 25 minutes. After the addition of the second co-feed was completed, DI water (94.11 g) was added to the vessel and the dispersion was cooled to room temperature and filtered to remove any coagulum. The solids content of the filtered dispersion was 31.0% and the pH was measured to be 8.3. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-BHP concentration of <300 ppm.

[0061] Comparative Example 2 - Preparation of an aqueous dispersion of multi-stage polymer particles

[0062] An aqueous dispersion of multistage polymer particles was prepared essentially as described in Example 1 of US 6,384,104, wherein the pH was adjusted to 8. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-BHP concentration of <350 ppm.

[0063] Example 1

[0064] The process was carried out essentially as described in the Comparative Example, except that upon completion of the hold after the NaOH addition, a post-polymerization solution of t-AHP (6.05 g, 85 wt.% aqueous solution) in DI water (24.55 g) was added to the vessel. The solids content of the filtered dispersion was 31.0%, and the pH was measured to be 8.3. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-AHP concentration of 740 ppm.

[0065] Example 2

[0066] The process was carried out essentially as described in the Comparative Example, except that upon completion of the post-NaOH addition hold, a post-polymerization solution of t-BHP (6.36 g, 70 wt.% aqueous solution) in DI water (24.55 g) was added to the vessel. The filtered dispersion had a solids content of 30.3% and a pH of 8.3 was measured. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-BHP concentration of 920 ppm.

[0067] Example 3

[0068] The process was carried out essentially as described in the Comparative Example, except that upon completion of the post-NaOH addition hold, a post-polymerization solution of t-AHP (10.05 g, 85 wt.% aqueous solution) in DI water (24.55 g) was added to the vessel. The filtered dispersion had a solids content of 29.7% and a pH of 8.3 was measured. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-AHP concentration of 1050 ppm.

[0069] Example 4

[0070] The method was carried out essentially as described in Example 2, except that Dequest 2016 chelating agent solution (7.2 g, 5 wt.% aqueous solution) was added and mixed for 5 minutes before filtration and after the dispersion was cooled to <50°C. The solids content of the filtered dispersion was 30.3%, and the pH was measured to be 8.3. Proton NMR spectroscopy analysis of the serum phase of the sample revealed a t-BHP concentration of 915 ppm.

[0071] Example 5

[0072] The method was performed essentially as described in the comparative example, except that a solution of Dequest 2016 chelating agent (1.8 g, 5 wt.% aqueous solution) in DI water (16.36 g) was added to the container over 5 minutes before filtering and after the dispersion was cooled to <50°C. A solution of hydrogen peroxide (48.48 g, 30 wt.% aqueous solution) in DI water (16.36 g) was then added to the container over 15 minutes. The dispersion was then filtered to remove any coagulum. The solids content of the filtered dispersion was 29.5%, and the pH was measured to be 8.5.

[0073] Table 1 shows the heat aging challenge test results for the Examples. The subscript "o" refers to the out of mill ("as is") challenge test, and the subscript "Δ" refers to the seven day heat aging challenge test.

[0074] Table 1 - Provocation test results

[0075] <![CDATA[C1 o ]]> <![CDATA[C2 o ]]> <![CDATA[C3 o ]]> <![CDATA[C1 Δ ]]> <![CDATA[C2 Δ ]]> <![CDATA[C3 Δ ]]> Comparison 1 Failure Failure Failure Failure Failure Failure Comparison 2 Failure Failure Failure Failure Failure Failure Example 1 qualified qualified qualified qualified qualified Failure Example 2 qualified qualified qualified qualified qualified Failure Example 3 qualified qualified qualified qualified qualified qualified Example 4 qualified qualified qualified qualified qualified qualified Example 5 qualified qualified qualified qualified qualified qualified

[0076] The data show that t-BHP and t-AHP are effective as preservatives for aqueous dispersions of opaque polymers. Chelating agents were used to achieve efficacy for the third heat aging challenge test (Example 3) at a concentration three times higher than that used under normal emulsion polymerization conditions (Comparative Example 1). Chelating agents were not required when the concentration of t-alkyl hydroperoxide was five times that of Comparative Example 1 (Example 4). In the presence of chelating agents, hydrogen peroxide was effective in all heat aging challenge tests.

Claims

1. A composition comprising: a) an aqueous dispersion of multistage polymer particles, the aqueous dispersion of multistage polymer particles comprising: 1) a water absorbing core comprising 20 to 60% by weight of structural units of a salt of a carboxylic acid monomer and 40 to 80% by weight of structural units of a nonionic monoethylenically unsaturated monomer; and 2) a polymer shell having a T g In the range of 60°C to 120°C; b1) 500 ppm to 5,000 ppm, based on the weight of the composition, of t-C4-C 10 - alkyl hydroperoxide; or b2) from 1000 ppm to 10000 ppm of hydrogen peroxide and from 50 ppm to 1000 ppm of a chelating agent not complexed with a polyvalent metal cation, based on the weight of the composition; and c) less than 1000 ppm residual monomers based on the weight of the composition; The z-average particle size of the polymer particles is in the range of 300 nm to 2000 nm.

2. The composition according to claim 1, wherein the t-C4-C 10 -Alkyl hydroperoxide is t-C4-C8-alkyl hydroperoxide in a concentration range of 600 ppm to 5000 ppm; wherein the water absorbing core comprises 30% to 50% by weight of structural units of salts of carboxylic acid monomers and 50% to 70% by weight of structural units of nonionic monoethylenically unsaturated monomers.

3. The composition according to claim 2, wherein the t-C4-C8-alkyl hydroperoxide is tert-butyl hydroperoxide or tert-amyl hydroperoxide or a combination thereof; wherein the nonionic monoethylenically unsaturated monomer is methyl methacrylate.

4. The composition of claim 3, wherein the composition comprises 700 ppm to 3000 ppm of tert-butyl hydroperoxide and less than 500 ppm of residual monomers.

5. The composition of claim 3, wherein the composition comprises 700 ppm to 3000 ppm of tert-amyl hydroperoxide and less than 500 ppm of residual monomers.

6. The composition of claim 2, further comprising a non-complexing chelating agent at a concentration ranging from 100 ppm to 2000 ppm based on the weight of the composition.

7. The composition of claim 1, wherein the composition comprises from 1000 ppm to 10000 ppm of hydrogen peroxide and from 50 ppm to 1000 ppm of the chelating agent not complexed with the metal cation, based on the weight of the composition.

8. The composition of claim 1, wherein the pH of the composition is in the range of 7.5 to 9.

5.

9. The composition of claim 1, wherein the pH of the composition is in the range of 8.0 to 9.

0.

10. The composition of claim 1, wherein the multi-stage polymer particles have a solids content in the range of 10 wt% to 40 wt% based on the weight of the composition.

11. The composition of claim 3, wherein the composition comprises 1000 ppm to 3000 ppm of tert-amyl hydroperoxide and less than 500 ppm of residual monomers.

12. The composition of claim 3, wherein the composition comprises 1000 ppm to 3000 ppm of tert-butyl hydroperoxide and less than 500 ppm of residual monomers.

Citation Information

Patent Citations

  • Water-borne coating formulation

    EP3456787B1

  • Method for preparing an aqueous dispersion of multistage polymer particles

    US20200071439A1

  • Process for preparing polymer core shell type emulsions and polymers formed therefrom

    US6020435A

  • Method for preparing ultraviolet radiation-absorbing compositions

    US6384104B1

  • Method for broad spectrum, low residue disinfection with a small droplet hydrogen peroxide-based aerosol