Pigment dispersion liquid, photosensitive resin composition, cured product, black matrix, image display device, and method for producing pigment dispersion liquid

By controlling the particle size distribution and gloss of pigment dispersions in a specific dispersion state, the problem of insufficient surface roughness of BM is solved, thereby improving the display performance and yield of color filters.

CN118891333APending Publication Date: 2024-11-01MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380028204.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the black matrix (BM) of the color filter has insufficient surface roughness during the thin-film process, which leads to uneven gaps between liquid crystal cells and disordered liquid crystal orientation, affecting display performance. Furthermore, high pigment concentration results in a reduced yield.

Method used

By using a pigment dispersion in a specific dispersion state, containing pigments, dispersants, sulfonic acid compounds, and solvents, particle size distribution and gloss are controlled to form a cured film with low surface roughness.

Benefits of technology

This resulted in low surface roughness of the BM, improved the flatness and yield of the display device, and ensured high light-blocking performance and dispersion stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005046510700000241
    Figure BDA0005046510700000241
  • Figure BDA0005046510700000242
    Figure BDA0005046510700000242
  • Figure BDA0005046510700000281
    Figure BDA0005046510700000281
Patent Text Reader

Abstract

The invention provides a pigment dispersion liquid and a photosensitive resin composition which can form a cured film with small surface roughness. According to one embodiment of the present invention, a pigment dispersion liquid contains (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound, and a solvent, and the pigment (A) and the sulfonic acid group-containing compound (C) are present in the form of particles. The ratio (D90 / D50) of 90% cumulative particle diameter (D90) to 50% cumulative particle diameter (D50) in a volume-based particle diameter distribution measurement result obtained by dynamic scattering measurement and cumulative analysis is 1.4 or less. The photosensitive resin composition according to the present invention contains the pigment dispersion liquid according to the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pigment dispersion, a photosensitive resin composition, a cured product, a black matrix (hereinafter sometimes referred to as "BM"), an image display device, and a method for producing the pigment dispersion.

[0002] This application claims priority based on Japanese Patent Application No. 2022-049781 filed in Japan on March 25, 2022, and the contents are incorporated herein by reference. Background Art

[0003] Color filters usually form a black matrix on the surface of a transparent substrate such as glass or plastic, and then form pixels of three or more different colors such as red, green, and blue in a grid, stripe, or mosaic pattern. The pattern size varies depending on the purpose of the color filter and the color of each color, but is usually around 5 to 700 μm.

[0004] As a representative method for manufacturing color filters, the pigment dispersion method is currently known. When manufacturing a color filter by the pigment dispersion method, first, a photosensitive resin composition containing a black pigment such as carbon black is coated on a transparent substrate, and then reduced-pressure drying is performed using a vacuum drying device, and then heating and drying is performed using a hot plate, and then image exposure and development are performed, and then it is cured by high-temperature treatment at 200°C or above to form a BM, which is repeated in each color such as red, green, and blue to form pixels, thereby forming a color filter having a BM and pixels.

[0005] BM is usually arranged in a grid, stripe or mosaic shape between pixels such as red, green and blue, and has the effect of improving contrast or preventing light leakage by suppressing color mixing between pixels. Therefore, high light-shielding properties are required for BM. In addition, the edge of the red, green and blue pixels formed after the BM is formed overlaps with a part of the BM, so a height difference is formed in the overlapping part due to the influence of the BM film thickness. In the overlapping part, the flatness of the pixel is impaired, and the liquid crystal unit gap becomes uneven or the liquid crystal orientation is disturbed, which becomes a cause of reduced display capability. Therefore, in recent years, it is particularly required to make the BM film thinner and thinner. In order to show sufficient light-shielding properties even when thinning, the pigment concentration in the BM tends to increase, but the surface roughness of the BM increases as a result, which becomes the cause of various problems such as reduced yield.

[0006] Under such background, improvements in pigment dispersions and photosensitive resin compositions that can form BMs with small surface roughness have been advanced.

[0007] For example, Patent Document 1 describes a photosensitive resin composition for color filter obtained by blending a dispersed pigment using a dispersing aid having an acid value of 0 to 30 into a specific alkali-soluble resin.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2008-164937 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] The present inventors evaluated BM using the photosensitive resin composition described in Patent Document 1. As a result, it was found that the surface roughness of BM formed from the photosensitive resin composition described in Patent Document 1 was insufficient.

[0013] Therefore, an object of the present invention is to provide a pigment dispersion and a photosensitive resin composition capable of forming a cured film having a small surface roughness.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by making the pigment dispersion liquid into a specific dispersion state. That is, the gist of the present invention is as follows.

[0016] [1] A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent,

[0017] In the pigment dispersion, the pigment (A) and the sulfonic acid group-containing compound (C) are present in the form of particles.

[0018] The ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement results measured by a dynamic scattering method and cumulatively analyzed is 1.4 or less.

[0019] [2] A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent,

[0020] In a dry coating film having a thickness of 1.2 μm obtained by applying the pigment dispersion, the glossiness Gs defined by ISO 2813 in the ranges of 18.2±0.9° and 21.8±0.9° with respect to incident light at -20° is 100 or less.

[0021] [3] A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent,

[0022] In a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion, the glossiness Gd defined by ISO 2813 in the range of 20±0.9° with respect to incident light at -20° is 170 or more.

[0023] [4] The pigment dispersion according to any one of [1] to [3], wherein the sulfonic acid group-containing compound (C) is at least one selected from the group consisting of sulfonic acid derivatives of phthalocyanine, sulfonic acid derivatives of quinophthalone, sulfonic acid derivatives of anthraquinone, sulfonic acid derivatives of quinacridone, sulfonic acid derivatives of diketopyrrolopyrrole and sulfonic acid derivatives of dioxazine.

[0024] [5] The pigment dispersion according to any one of [1] to [3], wherein the (C) sulfonic acid group-containing compound is a copper phthalocyanine sulfonate derivative.

[0025] [6] The pigment dispersion according to any one of [1] to [5], wherein the acid value of the sulfonic acid group-containing compound (C) is 80 mgKOH / g or more.

[0026] [7] The pigment dispersion according to any one of [1] to [6], wherein the content ratio of the (A) pigment to the (C) sulfonic acid group-containing compound ((A) pigment / (C) sulfonic acid group-containing compound) on a mass basis is 10 or more.

[0027] [8] The pigment dispersion according to any one of [1] to [7], wherein the content ratio of the (A) pigment to the (B) dispersant ((A) pigment / (B) dispersant) on a mass basis is 4 or more.

[0028] [9] The pigment dispersion according to any one of [1] to [8], wherein the pigment (A) contains carbon black.

[0029]

[10] A photosensitive resin composition comprising the pigment dispersion according to any one of [1] to [9].

[0030]

[11] A cured product obtained by curing the photosensitive resin composition described in

[10] .

[0031]

[12] A black matrix comprising the cured product described in

[11] .

[0032]

[13] An image display device comprising the cured product described in

[11] .

[0033]

[14] A method for producing a pigment dispersion, the pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent,

[0034] The production method comprises the following steps (1) and (2).

[0035] Step (1): A step of mixing and dispersing the aforementioned (C) sulfonic acid group-containing compound with a solvent.

[0036] Step (2): A step of mixing and dispersing the (C) sulfonic acid group-containing compound dispersion obtained in step (1), the (A) pigment and the (B) dispersant.

[0037] Effects of the Invention

[0038] According to the present invention, it is possible to provide a pigment dispersion and a photosensitive resin composition that can form a cured film having a small surface roughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic cross-sectional view showing an example of an organic EL element having the color filter of the present invention. DETAILED DESCRIPTION

[0040] Hereinafter, although embodiment of the present invention is described concretely, the present invention is not limited to the following embodiment, and various modifications can be implemented within the scope of the gist thereof.

[0041] In the present invention, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", and the same applies to "(meth)acrylate" and "(meth)acryloyl".

[0042] In the present invention, "total solid content" refers to all components other than the solvent contained in the photosensitive resin composition or the pigment dispersion. Even if the components other than the solvent are liquid at room temperature, the components are not contained in the solvent but are contained in the total solid content.

[0043] In the present invention, the weight average molecular weight refers to a polystyrene-equivalent weight average molecular weight (Mw) based on GPC (gel permeation chromatography).

[0044] In the present invention, "amine value" means the amine value converted to effective solid content unless otherwise specified, and is a value represented by the mass of KOH equivalent to the amount of alkali per 1g of solid content of the dispersant. The measurement method will be described later.

[0045] In the present invention, the acid value means an acid value calculated as effective solid content, and is calculated by neutralization titration.

[0046] [Pigment dispersion]

[0047] The pigment dispersion of the present invention contains (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound, and a solvent.

[0048] The pigment dispersion of the present invention may further contain other components as required. For example, the pigment dispersion of the present invention may contain an alkali-soluble resin.

[0049] As the alkali-soluble resin, an alkali-soluble resin used in the photosensitive resin composition of the present invention described later can be preferably used.

[0050] In the first embodiment of the pigment dispersion of the present invention, (A) the pigment and (C) the sulfonic acid group-containing compound are present in particulate form, and the ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement results measured by a dynamic scattering method and cumulatively analyzed is 1.4 or less.

[0051] The pigment dispersion of the second embodiment of the present invention has a glossiness Gs defined by ISO2813 of 100 or less in the range of 18.2±0.9° and 21.8±0.9° with respect to incident light at -20° in a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion.

[0052] The pigment dispersion of the third aspect of the present invention has a glossiness Gd defined by ISO 2813 of 170 or more in the range of 20±0.9° with respect to -20° incident light in a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion.

[0053] Hereinafter, unless otherwise specified, the "pigment dispersion of the present invention" means all of the pigment dispersions of the first to third aspects of the present invention.

[0054] <(A) Pigments>

[0055] The pigment dispersion of the present invention contains (A) a pigment. (A) The pigment is a substance that colors the pigment dispersion or the photosensitive resin composition of the present invention.

[0056] As the pigment (A), pigments of various colors such as blue pigments, green pigments, red pigments, yellow pigments, purple pigments, orange pigments, brown pigments, black pigments, etc. In addition, as for its structure, in addition to organic pigments such as azo, phthalocyanine, quinacridone, benzimidazolone, isoindolinone, dioxazine, indanthrene, and perylene, various inorganic pigments can also be used.

[0057] Specific examples of the (A) pigment that can be used in the present invention are shown below using pigment numbers. It should be noted that the terms "CI Pigment Red 2" and the like listed below refer to the Color Index (CI).

[0058] Examples of the red pigment include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, 53:2, 53: 3, 57, 57:1, 57:2, 58:4, 60, 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 1 49, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179, 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 216, 220, 221, 224, 230, 231, 232 2, 233, 235, 236, 237, 238, 239, 242, 243, 245, 247, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276. Preferred examples include CI Pigment Red 48:1, 122, 168, 177, 202, 206, 207, 209, 224, 242, and 254, and more preferred examples include CI Pigment Red 177, 209, 224, and 254.

[0059] Examples of the blue pigment include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79. Preferably, CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, and 60 are included, and more preferably, CI Pigment Blue 15:6 and 60 are included.

[0060] Examples of the green pigment include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, 58, and 59. Preferably, CI Pigment Green 7, 36, 58, and 59 are mentioned.

[0061] Examples of yellow pigments include CI Pigment Yellow 1, 1:1, 2, 3, 4, 5, 6, 9, 10, 12, 13, 14, 16, 17, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 53, 55, 61, 62, 62:1, 63, 65, 73, 74, 75, 81, 83, 87, 93, 94, 95, 97, 100, 101, 104, 105, 108, 109, 110, 111, 116, 117, 119, 120, 126, 127, 127:1, 128, 129, 133, 1 34, 136, 138, 139, 142, 147, 148, 150, 151, 153, 154, 155, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 172, 173, 174, 175, 176, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191: 1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208. Preferred examples include CI Pigment Yellow 83, 117, 129, 138, 139, 150, 154, 155, 180, and 185, and more preferred examples include CI Pigment Yellow 83, 138, 139, 150, 180, and 185.

[0062] Examples of the orange pigment include CI Pigment Orange 1, 2, 5, 13, 16, 17, 19, 20, 21, 22, 23, 24, 34, 36, 38, 39, 43, 46, 48, 49, 61, 62, 64, 65, 67, 68, 69, 70, 71, 72, 73, 74, 75, 77, 78, and 79. Preferably, CI Pigment Orange 38, 64, and 71 are used.

[0063] Examples of the violet pigment include CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, and 50. Preferably, CI Pigment Violet 19, 23, and 29 are used, and more preferably, CI Pigment Violet 23 and 29 are used.

[0064] When the photosensitive resin composition of the pigment dispersion of the present invention is a photosensitive resin composition for a black matrix of a color filter, a black pigment can be used as (A) pigment. The black pigment can be a single black pigment or a mixture of red, green, blue, etc. In addition, these pigments can be appropriately selected from inorganic or organic pigments.

[0065] Examples of pigments that can be used in combination to prepare black pigments include Victoria Pure Blue (42595), Auramine O (41000), Cation Brilliant Flavin (Basic 13), Rhodamine 6GCP (45160), Rhodamine B (45170), Safranine OK 70:100 (50240), Wool Red X (42080), No. 120 / Lionol Yellow (21090), Lionol Yellow GRO (21090), SYMULER Fast Yellow 8GF (21105), Benzidine Yellow 4T-564D (21095), SYMULER FastRed 4015 (12355), Lionol Red 7B4401 (15850), Fastogen Blue TGR-L (74160), Leonor Blue SM (26150), Leonor Blue ES (Pigment Blue 15:6), LIONOGEN RED GD (Pigment Red 168), Leonor Green 2YS (Pigment Green 36) (It should be noted that the numbers in parentheses above refer to the Color Index (CI)).

[0066] Other pigments that can be mixed and used are represented by CI numbers, for example, CI yellow pigments 20, 24, 86, 93, 109, 110, 117, 125, 137, 138, 147, 148, 153, 154, 166; CI orange pigments 36, 43, 51, 55, 59, 61, 64; CI red pigments 9, 97, 122, 123, 149, 168, 177, 180, 192, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, 254; CI violet pigments 19, 23, 29, 30, 37, 40, 50; CI blue pigments 15, 15:1, 15:4, 22, 60, 64; CI green pigment 7; CI brown pigments 23, 25, 26.

[0067] Examples of the black pigment that can be used alone include carbon black, acetylene black, lamp black, bone black, graphite, iron black, aniline black, cyanine black, titanium black, perylene black, and lactam black.

[0068] When a black pigment is used, the above-mentioned black pigments that can be used alone are preferred from the viewpoint of light shielding rate and image characteristics, and carbon black is particularly preferred. Examples of carbon black include the following carbon blacks.

[0069] Made by Mitsubishi Chemical Corporation: MA7, MA77, MA8, MA11, MA100, MA100R, MD120, MD130, MA600, #5, #10, # 20, #25, #30, #32, #33, #40, #44, #45, #47, #50, #52, #55, #650, #750, #850, #950, # 960, #970, #980, #990, #1000, #2200, #2300, #2350, #2400, #2600, #3050, #3150, #3250, #3600, #3750, #3950, #4000, #4010, OIL7B, OIL9B, OIL11B, OIL30B, OIL31B

[0070] Made by Degussa: Printex (registered trademark. Same below) 3, Printex3OP, Printex30, Printex30OP, Printex40, Printex45, Printex55, Printex60, Printex75, Printex80, Printex85, Printex90, Printex A, Printex L, Printex G, Printex P, Printex U, PrintexV, PrintexG, SpecialBlack550, SpecialBlack350, SpecialBlack250, SpecialBlack100, SpecialBlack6, SpecialBlack5, SpecialBlack4, Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW200, Color Black S160, Color Black S170

[0071] Made by Cabot Corporation: Monarch (registered trademark. Same as below) 120, Monarch 280, Monarch 460, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, Monarch 4630, REGAL (registered trademark. Same as below) 99, REGAL 99R, REGAL 415, REGAL 415R, REGAL 250, REGAL 250R, REGAL 330, REGAL 400R, REGAL 550R, REGAL 660R, BLACK PEARLS 480, PEARLS 130, VULCAN (registered trademark) XC72R, ELFTEX (registered trademark) -8

[0072] Birla Made by Carbon: RAVEN11, RAVEN14, RAVEN15, RAVEN16, RAVEN22, RAVEN30, RAVEN35, RAVEN40, RAVEN410, RAVEN420, RAVEN450, RAVEN500, RAVEN780, RAVEN850, RAVEN890H, RAVEN1000, RA VEN1020, RAVEN1040, RAVEN1060U, RAVEN1080U, RAVEN1170, RAVEN1190U, RAVEN1250, RAVEN1500, RAVEN2000, RAVEN2500U, RAVEN3500, RAVEN5000, RAVEN5250, RAVEN5750, RAVEN7000

[0073] As the (A) pigment, for example, barium sulfate, lead sulfate, titanium oxide, yellow lead, red iron, and chromium oxide can also be used.

[0074] Pigments may be used in combination of multiple types. For example, in order to adjust the chromaticity, a green pigment and a yellow pigment may be used in combination, or a blue pigment and a violet pigment may be used in combination.

[0075] The average particle size of the pigment (A) used in the present invention is not particularly limited as long as the desired color development can be performed, for example, in the case of forming a black matrix of a color filter, and varies depending on the type of pigment used, but is preferably within the range of 10 to 100 nm, and more preferably within the range of 10 to 70 nm. By making the average particle size of the pigment within the above range, there is a tendency to make the color characteristics of the liquid crystal display device manufactured using the pigment dispersion of the present invention high quality.

[0076] When carbon black is used as the pigment (A), the average particle diameter is preferably 60 nm or less, more preferably 50 nm or less, and preferably 20 nm or more. For example, it is preferably 20 to 60 nm, and more preferably 20 to 50 nm. By setting the average particle diameter to be below the upper limit, there is a tendency that scattering becomes smaller and the color characteristics such as light shielding and contrast can be suppressed from being reduced. In addition, by setting the average particle diameter to be above the lower limit, the amount of dispersant is not too much, and there is a tendency that the dispersibility becomes good.

[0077] The average particle size of the pigment can be obtained by directly measuring the size of the primary particles according to the electron microscope photograph. Specifically, the minor axis diameter and major axis diameter of each primary particle are measured, and the average is used as the particle size of the particle. For more than 100 particles, the volume (mass) of each particle is approximated to a rectangular parallelepiped of the obtained particle size, and the volume average particle size is obtained, which is used as the average particle size. It should be noted that the same result can be obtained using any of a transmission electron microscope (TEM) or a scanning electron microscope (SEM).

[0078] The pigment dispersion of the present invention may also be used in combination with dyes in the range that does not affect the effect of the present invention, except for the pigment (A). As dyes that can be used in combination, for example, azo dyes, anthraquinone dyes, phthalocyanine dyes, quinoneimine dyes, quinoline dyes, nitro dyes, carbonyl dyes, and methylene dyes may be cited.

[0079] Examples of the azo dye include CI Acid Yellow 11, CI Acid Orange 7, CI Acid Red 37, CI Acid Red 180, CI Acid Blue 29, CI Direct Red 28, CI Direct Red 83, CI Direct Yellow 12, CI Direct Orange 26, CI Direct Green 28, CI Direct Green 59, CI Reactive Yellow 2, CI Reactive Red 17, CI Reactive Red 120, CI Reactive Black 5, CI Disperse Orange 5, CI Disperse Red 58, CI Disperse Blue 165, CI Basic Blue 41, CI Basic Red 18, CI Mordant Red 7, CI Mordant Yellow 5, and CI Mordant Black 7.

[0080] Examples of the anthraquinone dye include CI Vat Blue 4, CI Acid Blue 40, CI Acid Green 25, CI Reactive Blue 19, CI Reactive Blue 49, CI Disperse Red 60, CI Disperse Blue 56, and CI Disperse Blue 60.

[0081] As a phthalocyanine dye, CI Vat Blue 5 is mentioned, for example.

[0082] Examples of the quinoneimine dye include CI Basic Blue 3 and CI Basic Blue 9.

[0083] As quinoline dyes, CI Solvent Yellow 33, CI Acid Yellow 3, and CI Disperse Yellow 64 are mentioned, for example.

[0084] Examples of the nitro dye include CI Acid Yellow 1, CI Acid Orange 3, and CI Disperse Yellow 42.

[0085] The photosensitive resin composition using the pigment dispersion of the present invention can be used for various purposes described below, and the excellent image forming property is particularly effective when used for the formation of a black matrix for a color filter. When the pigment dispersion of the present invention is used for the formation of a black matrix, as the pigment (A), a black pigment such as the above-mentioned carbon black, titanium black, etc. can be used, or a plurality of pigments other than black can be mixed to adjust to black and used.

[0086] Among them, carbon black is particularly preferably used from the viewpoint of dispersion stability and light shielding properties.

[0087] In the photosensitive resin composition of the present invention described later, when the light shielding degree is increased, the pigment concentration needs to be increased. The content ratio of (A) the pigment is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, and particularly preferably 52% by mass or more relative to the total solid content of the photosensitive resin composition. In addition, from the viewpoint of image forming performance, it is preferably 70% by mass or less, more preferably 65% ​​by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 30 to 70% by mass, more preferably 40 to 70% by mass, further preferably 50 to 65% by mass, and particularly preferably 52 to 65% by mass.

[0088] In the photosensitive resin composition of the present invention described later, by making the content ratio of the pigment within the above range, a photosensitive resin composition with high light-shielding properties (optical concentration, OD value) can be obtained. Specifically, by making the content ratio of (A) pigment relative to the total solid content of the photosensitive resin composition be 50% by mass or more, the optical concentration when a black matrix with a thickness of 1 μm is formed using the photosensitive resin composition of the present invention can be a value of 4.0 or more. The optical concentration is more preferably 4.1 or more, and more preferably 4.2 or more. The upper limit is not particularly limited, and is preferably 6.0 or less. For example, preferably 4.0 to 6.0, more preferably 4.1 to 6.0, and more preferably 4.2 to 6.0.

[0089] In the photosensitive resin composition of the present invention described later, the content ratio of the pigment (A) is not particularly limited. It is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, further preferably 100 parts by mass or more, further preferably 120 parts by mass or more, further preferably 150 parts by mass or more, and particularly preferably 180 parts by mass or more, relative to 100 parts by mass of the alkali-soluble resin. In addition, it is preferably 500 parts by mass or less, more preferably 300 parts by mass or less, and further preferably 250 parts by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 20 to 500 parts by mass, more preferably 50 to 500 parts by mass, further preferably 100 to 300 parts by mass, further preferably 120 to 300 parts by mass, further preferably 150 to 250 parts by mass, and particularly preferably 180 to 250 parts by mass. When the content ratio of the pigment (A) is at least the above lower limit, a decrease in solubility of the unexposed portion in the developer tends to be easily suppressed, and when it is at most the above upper limit, fine line adhesion during development tends to be improved.

[0090] <(B) Dispersant>

[0091] Since it is important to finely disperse the (A) pigment and stabilize the dispersion state in order to ensure the stability of quality, the pigment dispersion of the present invention contains the (B) dispersant.

[0092] As the (B) dispersant, a polymer dispersant having a functional group is preferred, and from the perspective of dispersion stability, a polymer dispersant having, for example, a carboxyl group; a phosphoric acid group; a sulfonic acid group; or a salt thereof; a primary, secondary or tertiary amino group; a quaternary ammonium salt group; or a group derived from a nitrogen-containing heterocyclic ring such as pyridine, pyrimidine, or pyrazine as a functional group is more preferred, and a polymer dispersant having a primary, secondary or tertiary amino group; a quaternary ammonium salt group; or a group derived from a nitrogen-containing heterocyclic ring such as pyridine, pyrimidine, or pyrazine as a basic functional group is further preferred. By using a polymer dispersant having a basic functional group, there is a tendency that the dispersibility of the pigment etc. can be improved and high light-shielding properties can be achieved.

[0093] Examples of the polymer dispersant include urethane dispersants, acrylic acid dispersants, polyethyleneimine dispersants, polyallylamine dispersants, dispersants containing monomers and macromonomers having an amino group, polyoxyethylene alkyl ether dispersants, polyoxyethylene diester dispersants, polyether phosphate dispersants, polyester phosphate dispersants, sorbitan aliphatic ester dispersants, and aliphatic modified polyester dispersants.

[0094] Examples of such dispersants include EFKA (registered trademark, manufactured by EFKA Chemicals (EFKA)), Disperbyk (registered trademark, manufactured by BYK-Chemie), DISPARLON (registered trademark, manufactured by Kusumoto Chemicals Co., Ltd.), SOLSPERSE (registered trademark, manufactured by Lubrizol Corporation), KP (manufactured by Shin-Etsu Chemical Co., Ltd.), POLYFLOW or FLOWLEN (registered trademark, manufactured by Kyoeisha Chemical Co., Ltd.), and AJISPER (registered trademark, manufactured by Ajinomoto Fine-Techno Co., Inc.).

[0095] The polymer dispersants may be used alone or in combination of two or more.

[0096] From the viewpoint of fine line adhesion and linearity, the dispersant (B) is preferably a urethane polymer dispersant and / or an acrylic polymer dispersant having a basic functional group. From the viewpoint of fine line adhesion, a urethane polymer dispersant having a basic functional group is more preferred.

[0097] As another embodiment, from the viewpoint of dispersibility and storage stability, the dispersant (B) is preferably a polyester having a basic functional group and / or a polymer dispersant having a polyether bond.

[0098] The weight average molecular weight (Mw) of the polymer dispersant is preferably 700 or more, more preferably 1000 or more, and preferably 100000 or less, more preferably 50000 or less, and further preferably 30000 or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 700 to 100000, more preferably 700 to 50000, and further preferably 1000 to 30000. By setting it below the above upper limit, there is a tendency that the alkali developability becomes good even when the pigment concentration is high. In addition, by setting it above the above lower limit, there is a tendency that the dispersion stability of the pigment becomes good.

[0099] Examples of urethane-based and acrylic-based polymer dispersants include Disperbyk 160 to 167 and 182 series (all urethane-based) and Disperbyk 2000 and 2001 (all acrylic-based) (all manufactured by BYK-Chemie).

[0100] Examples of polyester having a basic functional group and / or urethane-based polymer dispersants having a polyether bond and having a weight average molecular weight of 30,000 or less include Disperbyk 167 and 182.

[0101] <Urethane polymer dispersant>

[0102] Examples of the urethane polymer dispersant include dispersion resins having a weight average molecular weight of 1,000 to 200,000 obtained by reacting a polyisocyanate compound with a compound having one or two hydroxyl groups in the molecule and having a number average molecular weight of 300 to 10,000 and a compound having active hydrogen and a tertiary amino group in the same molecule.

[0103] Examples of the polyisocyanate compound include aromatic diisocyanates such as p-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, naphthalene-1,5-diisocyanate, and dimethylbiphenyl diisocyanate; aliphatic diisocyanates such as hexamethylene diisocyanate, lysine methyl ester diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and dimer acid diisocyanate; isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), ω,ω'-diisocyanate, and bis(cyclohexyl isocyanate). alicyclic diisocyanates such as ester dimethylcyclohexane; aliphatic diisocyanates having aromatic rings such as xylylene diisocyanate, α,α,α',α'-tetramethylxylylene diisocyanate; triisocyanates such as lysine ester triisocyanate, 1,6,11-undecane triisocyanate, 1,8-diisocyanate-4-isocyanate methyloctane, 1,3,6-hexamethylene triisocyanate, dicycloheptane triisocyanate, tris(isocyanate phenylmethane), tris(isocyanate phenyl)thiophosphate; and trimers thereof, water adducts thereof, and polyol adducts thereof. As the polyisocyanate compound, a trimer of an organic diisocyanate is preferred, and a trimer of toluene diisocyanate and a trimer of isophorone diisocyanate are more preferred.

[0104] The polyisocyanate compound may be used alone or in combination of two or more.

[0105] As a method for producing a trimer of isocyanate, the following method can be cited: a polyisocyanate compound is subjected to partial trimerization of isocyanate groups using a suitable trimerization catalyst, such as tertiary amines, phosphines, alkoxides, metal oxides, and carboxylates; the trimerization is stopped by adding a catalyst poison; and the unreacted polyisocyanate is removed by solvent extraction or thin film distillation to obtain the target polyisocyanate containing isocyanurate groups.

[0106] Examples of the compound having one or two hydroxyl groups in the same molecule and having a number average molecular weight of 300 to 10,000 include polyether diols, polyester diols, polycarbonate diols, polyolefin diols, and compounds in which one terminal hydroxyl group of these compounds is alkoxylated with an alkyl group having 1 to 25 carbon atoms.

[0107] Examples of the polyether diol include polyether diol and polyether ester diol.

[0108] Examples of the polyether diol include compounds obtained by using an alkylene oxide alone or in a copolymer, such as polyethylene glycol, polypropylene glycol, polyethylene glycol-propylene glycol, polyoxytetramethylene glycol, polyoxyhexamethylene glycol, and polyoxyoctamethylene glycol.

[0109] Examples of the polyetherester diol include compounds obtained by reacting an ether group-containing diol or a mixture with other diols with dicarboxylic acids or anhydrides thereof, or reacting a polyester diol with an alkylene oxide, such as poly(polyoxytetramethylene) adipate.

[0110] As the polyether diol, polyethylene glycol, polypropylene glycol, polyoxytetramethylene glycol, or a compound in which one terminal hydroxyl group of these compounds is alkoxylated with an alkyl group having 1 to 25 carbon atoms.

[0111] Examples of the polyester diol include those obtained by reacting dicarboxylic acids (e.g., succinic acid, glutaric acid, adipic acid, sebacic acid, fumaric acid, maleic acid, and phthalic acid), anhydrides thereof, and diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, aliphatic diols such as 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,8-octamethylene glycol, 2-methyl-1,8-octamethylene glycol, 1,9-nonanediol; alicyclic diols such as bishydroxymethylcyclohexane; aromatic diols such as benzyl alcohol and bishydroxyethoxybenzene; N-alkyldialkanolamines such as N-methyldiethanolamine) are obtained by polycondensation, for example, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polyethylene / propylene adipate, or polylactone diols or polylactone monools obtained by using a diol or a monohydric alcohol having 1 to 25 carbon atoms as an initiator, for example, polycaprolactone diol and polymethylvalerolactone.

[0112] As the polyester diol, polycaprolactone diol and polycaprolactone obtained by using an alcohol having 1 to 25 carbon atoms as an initiator are preferred.

[0113] Examples of the polycarbonate diol include poly(1,6-hexamethylene) carbonate and poly(3-methyl-1,5-pentamethylene) carbonate.

[0114] Examples of the polyolefin diol include polybutadiene diol, hydrogenated polybutadiene diol, and hydrogenated polyisoprene diol.

[0115] The compound having one or two hydroxyl groups in the same molecule and having a number average molecular weight of 300 to 10,000 may be used alone or in combination of two or more.

[0116] The number average molecular weight of the compound having one or two hydroxyl groups in the same molecule and having a number average molecular weight of 300 to 10,000 is preferably 500 to 6,000, more preferably 1,000 to 4,000.

[0117] Examples of active hydrogen in a compound having active hydrogen and a tertiary amino group in the same molecule, i.e., a hydrogen atom directly bonded to an oxygen atom, a nitrogen atom or a sulfur atom include hydrogen atoms in functional groups such as hydroxyl groups, amino groups and thiol groups, among which hydrogen atoms in amino groups, particularly primary amino groups, are preferred.

[0118] Examples of the tertiary amino group in the compound having active hydrogen and a tertiary amino group in the same molecule include an amino group having an alkyl group having 1 to 4 carbon atoms, and a heterocyclic structure such as an imidazole ring and a triazole ring.

[0119] Examples of the compound having active hydrogen and a tertiary amino group in the same molecule include N,N-dimethyl-1,3-propylenediamine, N,N-diethyl-1,3-propylenediamine, N,N-dipropyl-1,3-propylenediamine, N,N-dibutyl-1,3-propylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dipropylethylenediamine, N,N-dibutylethylenediamine, N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dipropyl-1,4-butanediamine, and N,N-dibutyl-1,4-butanediamine.

[0120] When the tertiary amino group is a nitrogen-containing heterocyclic structure, for example, there can be listed nitrogen-containing five-membered heterocyclic rings such as pyrazole ring, imidazole ring, triazole ring, tetrazole ring, indole ring, carbazole ring, indazole ring, benzimidazole ring, benzotriazole ring, benzoxazole ring, benzothiazole ring, and benzothiadiazole ring; and nitrogen-containing six-membered heterocyclic rings such as pyridine ring, pyridazine ring, pyrimidine ring, triazine ring, quinoline ring, acridine ring, and isoquinoline ring, preferably imidazole ring and triazole ring.

[0121] Examples of the compound having an imidazole ring and an amino group include 1-(3-aminopropyl)imidazole, histidine, 2-aminoimidazole, and 1-(2-aminoethyl)imidazole.

[0122] Examples of the compound having a triazole ring and an amino group include 3-amino-1,2,4-triazole, 5-(2-amino-5-chlorophenyl)-3-phenyl-1H-1,2,4-triazole, 4-amino-4H-1,2,4-triazole-3,5-diol, 3-amino-5-phenyl-1H-1,3,4-triazole, 5-amino-1,4-diphenyl-1,2,3-triazole, and 3-amino-1-benzyl-1H-2,4-triazole.

[0123] As the compound having active hydrogen and a tertiary amino group in the same molecule, N,N-dimethyl-1,3-propylenediamine, N,N-diethyl-1,3-propylenediamine, 1-(3-aminopropyl)imidazole, and 3-amino-1,2,4-triazole are preferred.

[0124] The compound having active hydrogen and a tertiary amino group in the same molecule may be used alone or in combination of two or more.

[0125] The preferred blending ratio of the raw materials when manufacturing the carbamate polymer dispersant is: relative to 100 parts by mass of the polyisocyanate compound, the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule is 10 to 200 parts by mass, preferably 20 to 190 parts by mass, and more preferably 30 to 180 parts by mass, and the compound having active hydrogen and tertiary amino groups in the same molecule is 0.2 to 25 parts by mass, preferably 0.3 to 24 parts by mass. The above blending ratios can be combined arbitrarily. For example, preferably, the amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule is 10 to 200 parts by mass, and the amount of the compound having active hydrogen and a tertiary amino group in the same molecule is 0.2 to 25 parts by mass, based on 100 parts by mass of the polyisocyanate compound. More preferably, the amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule is 20 to 190 parts by mass, and the amount of the compound having active hydrogen and a tertiary amino group in the same molecule is 0.2 to 25 parts by mass, based on 100 parts by mass of the polyisocyanate compound. Further preferably, the amount of the compound having a number average molecular weight of 300 to 10,000 and having one or two hydroxyl groups in the same molecule is 30 to 180 parts by mass, and the amount of the compound having active hydrogen and a tertiary amino group in the same molecule is 0.3 to 24 parts by mass, based on 100 parts by mass of the polyisocyanate compound.

[0126] The production of the urethane polymer dispersant is carried out according to the known method for producing polyurethane resin. As the solvent used in the production, for example, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, isophorone, esters such as ethyl acetate, butyl acetate, and cellosolve, hydrocarbons such as benzene, toluene, xylene, and hexane, some alcohols such as diacetone alcohol, isopropanol, sec-butyl alcohol, and tert-butyl alcohol, chlorides such as dichloromethane and chloroform, ethers such as tetrahydrofuran and diethyl ether, and aprotic polar solvents such as dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide can be used.

[0127] The solvent may be used alone or in combination of two or more.

[0128] When the urethane-based polymer dispersant is produced, a urethanization reaction catalyst may be used. Examples of the urethanization reaction catalyst include tin-based catalysts such as dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctoate, and stannous octoate; iron-based catalysts such as ferric acetylacetonate and ferric chloride; and tertiary amine-based catalysts such as triethylamine and triethylenediamine.

[0129] The urethanization reaction catalyst may be used alone or in combination of two or more.

[0130] <Measurement method of amine value>

[0131] (B) The amine value of the dispersant is represented by the mass of KOH equivalent to the amount of alkali per 1 g of solid content in the dispersant sample excluding the solvent, and can be measured by the following method.

[0132] In a 100mL beaker, accurately weigh 0.5-1.5g of the dispersant sample and dissolve it in 50mL of acetic acid. Use an automatic titrator equipped with a pH electrode to neutralize and titrate the solution with 0.1mol / L HClO4 (perchloric acid) acetic acid solution. The inflection point of the titration pH curve is taken as the titration endpoint, and the amine value is calculated by the following formula.

[0133] Amine value [mgKOH / g] = (561×V) / (W×S)

[0134] [W: represents the amount of the dispersant sample weighed [g], V: represents the titration amount at the titration endpoint [mL], and S: represents the solid content concentration of the dispersant sample [mass %].]

[0135] The amount of the compound having active hydrogen and a tertiary amino group in the same molecule to be introduced is preferably controlled within the range of 1 to 100 mgKOH / g, more preferably 5 to 95 mgKOH / g, in terms of amine value after the reaction.

[0136] The amine value is a value obtained by neutralizing and titrating a basic amino group with an acid and expressed as mg of KOH corresponding to the acid value. When the amine value is set to be equal to or greater than the lower limit, dispersibility tends to be improved, and when the amine value is set to be equal to or less than the upper limit, developability tends to be improved.

[0137] When an isocyanate group remains in the polymer dispersant, it is preferred to further use an alcohol or an amino compound to deactivate the isocyanate group because the temporal stability of the product is improved.

[0138] The weight average molecular weight (Mw) of the carbamate polymer dispersant is preferably 1000 to 200000, more preferably 2000 to 100000, and further preferably 3000 to 50000. As the upper limit, it is particularly preferably 30000 or less, and it can be combined with the above lower limit arbitrarily. For example, it is preferably 1000 to 30000, more preferably 2000 to 30000, and further preferably 3000 to 30000. By setting it above the above lower limit, there is a tendency for dispersibility and dispersion stability to become better, and by setting it below the above upper limit, there is a tendency for solubility to become better. If the molecular weight is 30000 or less, there is a tendency that alkali developability becomes good even when the pigment concentration is high. As such commercially available carbamate dispersants, for example, Disperbyk167 and 182 (manufactured by BYK-Chemie) can be cited.

[0139] In the pigment dispersion of the present invention, the content ratio of (A) pigment to (B) dispersant on a mass basis ((A) pigment / (B) dispersant) is preferably 1 or more, more preferably 3 or more, further preferably 4 or more, and particularly preferably 5 or more. In addition, it is preferably 50 or less, further preferably 30 or less, and particularly preferably 15 or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 1 to 50, more preferably 3 to 50, further preferably 4 to 30, and particularly preferably 5 to 15. By setting it to be above the aforementioned lower limit, there is a tendency for the developing solubility to become good. In addition, by setting it to be below the aforementioned upper limit, there is a tendency for the dispersion stability to be improved.

[0140] The content ratio of the (B) dispersant in the photosensitive resin composition of the present invention described later is not particularly limited. In the total solid content of the photosensitive resin composition, it is preferably 50% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less. In addition, it is preferably 1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, further preferably 7% by mass or more, and particularly preferably 10% by mass or more. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 1 to 50% by mass, more preferably 3 to 50% by mass, further preferably 5 to 30% by mass, further preferably 7 to 30% by mass, and particularly preferably 10 to 20% by mass. By setting it to above the above lower limit, there is a tendency to suppress the aggregation of the pigment. In addition, by setting it to below the above upper limit, the development and dissolution morphology is optimized, and in addition, there is a tendency for the curability of the composition to be improved.

[0141] The content ratio of the (B) dispersant in the photosensitive resin composition of the present invention described later is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 15 parts by mass or more relative to 100 parts by mass of the (A) pigment, and is preferably 200 parts by mass or less, more preferably 80 parts by mass or less, and further preferably 50 parts by mass or less. By setting it to be above the aforementioned lower limit, there is a tendency to easily ensure sufficient dispersibility. In addition, by setting it to be below the aforementioned upper limit, there is a tendency to easily make color density, sensitivity, film-forming properties, etc. sufficient without reducing the proportion of other components.

[0142] <(C) Sulfonic acid group-containing compound>

[0143] The pigment dispersion of the present invention contains (C) a sulfonic acid group-containing compound in order to improve dispersibility and storage stability.

[0144] Examples of the sulfonic acid group-containing compound (C) include derivatives of azo, phthalocyanine, quinacridone, benzimidazolone, quinophthalone, isoindolinone, dioxazine, anthraquinone, indanthrene, perylene, perinone, diketopyrrolopyrrole and dioxazine compounds, preferably derivatives of phthalocyanine, quinophthalone, anthraquinone, quinacridone, diketopyrrolopyrrole and dioxazine compounds, and more preferably derivatives of phthalocyanine and quinophthalone compounds.

[0145] The derivatives of the compound (C) which is the sulfonic acid group-containing compound include compounds obtained by introducing a substituent into the skeleton of each compound directly or via, for example, an alkyl group, an aryl group, or a heterocyclic group.

[0146] Examples of the introduced substituent include sulfonic acid group, sulfonamide group and quaternary salts thereof, phthalimidomethyl group, dialkylaminoalkyl group, hydroxyl group, carboxyl group and amide group, preferably sulfonic acid group. Multiple substituents may be substituted on the skeleton of one compound.

[0147] The (C) sulfonic acid group-containing compound is preferably a sulfonic acid derivative of phthalocyanine, a sulfonic acid derivative of quinophthalone, a sulfonic acid derivative of anthraquinone, a sulfonic acid derivative of quinacridone, a sulfonic acid derivative of diketopyrrolopyrrole, or a sulfonic acid derivative of dioxazine, more preferably a sulfonic acid derivative of phthalocyanine, and still more preferably a copper phthalocyanine sulfonate derivative.

[0148] (C) The sulfonic acid group-containing compound may be used alone or in combination of two or more.

[0149] The content ratio of the sulfonic acid group-containing compound (C) contained in the pigment dispersion of the present invention is not particularly limited. In the total solid content of the pigment dispersion, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1% by mass or more. In addition, it is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, and further preferably 1 to 5% by mass. By setting it above the above lower limit, there is a tendency to improve dispersion stability. In addition, by setting it below the above upper limit, there is a tendency to suppress the aggregation of pigments and make the coating surface uniform.

[0150] In the pigment dispersion of the present invention, the content ratio of (A) pigment to (C) sulfonic acid group-containing compound on a mass basis ((A) pigment / (C) sulfonic acid group-containing compound) is preferably 10 or more, more preferably 20 or more, and particularly preferably 25 or more. In addition, it is preferably 200 or less, more preferably 150 or less, further preferably 100 or less, and particularly preferably 50 or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 10 to 200, more preferably 10 to 150, further preferably 20 to 100, and particularly preferably 25 to 50. By setting it to be above the aforementioned lower limit, there is a tendency for the substrate adhesion to be improved. In addition, by setting it to be below the aforementioned upper limit, there is a tendency for the dispersion stability to be improved.

[0151] The content ratio of the sulfonic acid group-containing compound (C) contained in the photosensitive resin composition of the present invention described later is not particularly limited. It is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1% by mass or more relative to the total solid content of the photosensitive resin composition. In addition, it is preferably 10% by mass or less, and more preferably 5% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 0.1 to 10% by mass, more preferably 0.5 to 10% by mass, and further preferably 1 to 5% by mass. By setting it above the above lower limit, there is a tendency for the development solubility to be improved. In addition, by setting it below the above upper limit, there is a tendency for the development property to be stable and the patterning adhesion to be good.

[0152] (C) The conductivity of the sulfonic acid group-containing compound is preferably 2000 μS / cm or more, more preferably 2500 μS / cm or more, particularly preferably 3000 μS / cm or more, and preferably 9000 μS / cm or less, more preferably 8000 μS / cm or less, and particularly preferably 7000 μS / cm or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 2000 to 9000 μS / cm, more preferably 2500 to 8000 μS / cm, and particularly preferably 3000 to 7000 μS / cm. By setting it above the above lower limit, there is a tendency for dispersion stability to be improved. In addition, by setting it below the above upper limit, there is a tendency for undercutting to be suppressed and development adhesion to be good.

[0153] The conductivity of the sulfonic acid group-containing compound (C) is expressed as the conductivity when the sulfonic acid group-containing compound (C) is stirred in ultrapure water to form a 5% solution, and can be measured with a conductivity meter. The unit can be expressed in μS / cm.

[0154] (C) The acid value of the sulfonic acid group-containing compound is not particularly limited, but is preferably 80 mgKOH / g or more, more preferably 90 mgKOH / g or more, and further preferably 100 mgKOH / g or more. In addition, it is preferably 500 mgKOH / g or less, more preferably 300 mgKOH / g or less, further preferably 200 mgKOH / g or less, and particularly preferably 150 mgKOH / g or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 80 to 500 mgKOH / g, more preferably 80 to 300 mgKOH / g, further preferably 90 to 200 mgKOH / g, and particularly preferably 100 to 150 mgKOH / g. By setting it above the aforementioned lower limit, there is a tendency for the solubility to be improved. In addition, by setting it below the aforementioned upper limit, there is a tendency for undercutting to be suppressed and for the development adhesion to be good.

[0155] The pigment dispersion of the present invention is used in a state where (A) the pigment, (B) the dispersant, (C) the sulfonic acid group-containing compound, and various materials used as necessary are dissolved or dispersed in a solvent.

[0156] As the solvent, water or an organic solvent used in the photosensitive resin composition of the present invention described later can be preferably used.

[0157] The content ratio of the solvent in the pigment dispersion of the present invention is not particularly limited. From the viewpoint of ease of application and viscosity stability, the total solid content in the pigment dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 20% by mass or more. In addition, it is preferably 50% by mass or less, more preferably 45% by mass or less, further preferably 40% by mass or less, and particularly preferably 35% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 5 to 50% by mass, more preferably 5 to 45% by mass, further preferably 10 to 40% by mass, and particularly preferably 20 to 35% by mass. By setting it to above the aforementioned lower limit, there is a tendency that the tinting power is improved and the optical density (OD value) is easily increased. In addition, by setting it to below the aforementioned upper limit, there is a tendency that the dispersion stability becomes good.

[0158] In the first embodiment of the pigment dispersion of the present invention, (A) the pigment and (C) the sulfonic acid group-containing compound are present in particulate form, and the ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement results measured by a dynamic scattering method and cumulatively analyzed is 1.4 or less.

[0159] In a pigment dispersion in which (A) the pigment and (C) the sulfonic acid group-containing compound are present in particulate form, by setting the ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement result to 1.4 or less, the particle sizes tend to be uniform, and a BM having a small surface roughness can be formed using a photosensitive resin composition using the pigment dispersion.

[0160] The ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement results measured by dynamic scattering method and cumulatively analyzed is preferably 1.35 or less, more preferably 1.3 or less. In addition, it is particularly preferably 1.0 or more. For example, it is preferably 1.0 to 1.4, more preferably 1.0 to 1.35, further preferably 1.0 to 1.3, and particularly preferably 1.0. By setting it below the above upper limit, the particle size distribution becomes uniform, and there is a tendency for the surface roughness of the coating film to become smaller.

[0161] The volume-based particle size distribution in the pigment dispersion can be measured by a dynamic scattering method and obtained by cumulative analysis of the measurement data.

[0162] The pigment dispersion of the second embodiment of the present invention has a glossiness Gs defined by ISO2813 of 100 or less in the range of 18.2±0.9° and 21.8±0.9° with respect to incident light at -20° in a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion.

[0163] When the glossiness Gs defined by ISO 2813 in the range of 18.2±0.9° and 21.8±0.9° with respect to -20° incident light is 100 or less, dispersion stability becomes good, and a BM having a small surface roughness can be formed using the photosensitive resin composition using the pigment dispersion.

[0164] The glossiness Gs defined by ISO2813 in the range of 18.2±0.9° and 21.8±0.9° relative to -20° incident light is preferably 80 or less, more preferably 50 or less, further preferably 30 or less, and particularly preferably 10 or less. In addition, the lower limit is not particularly limited, but is preferably 1 or more. For example, it can be 1 to 100, preferably 1 to 80, more preferably 1 to 50, further preferably 1 to 30, and particularly preferably 1 to 10. By setting it below the above upper limit, the particle size distribution in the pigment dispersion is uniform and the dispersion stability is good, and there is a tendency for the surface roughness of the coating film to be reduced.

[0165] The glossiness Gs defined by ISO 2813 in the range of 18.2±0.9° and 21.8±0.9° with respect to incident light at -20° is measured in accordance with ISO 2813, for example, using a corresponding haze-gloss meter.

[0166] The pigment dispersion of the third aspect of the present invention has a glossiness Gd defined by ISO 2813 of 170 or more in the range of 20±0.9° with respect to -20° incident light in a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion.

[0167] When the glossiness Gd defined by ISO 2813 in the range of 20±0.9° with respect to -20° incident light is 170 or less, dispersion stability becomes good, and a BM having a small surface roughness can be formed using the photosensitive resin composition using the pigment dispersion.

[0168] The glossiness Gd defined by ISO2813 in the range of 20±0.9° with respect to -20° incident light is preferably 180 or more, more preferably 200 or more, and further preferably 220 or more. In addition, the lower limit is not particularly limited, but is preferably 300 or less. For example, it may be 170 to 300, preferably 180 to 300, more preferably 200 to 300, and further preferably 220 to 300. By setting it to be equal to or more than the above lower limit, the particle size distribution in the pigment dispersion is uniform and the dispersion stability is good, and there is a tendency that the surface roughness of the coating film becomes small.

[0169] The gloss Gd defined by ISO 2813 in the range of 20±0.9° with respect to incident light at -20° is measured in accordance with ISO 2813, and can be measured using, for example, a corresponding haze-gloss meter.

[0170] [Photosensitive resin composition]

[0171] The photosensitive resin composition of the present invention contains the pigment dispersion of the present invention.

[0172] Since the photosensitive resin composition of the present invention includes the pigment dispersion of the present invention, it contains (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent. As the (A) pigment, (B) dispersant, and (C) sulfonic acid group-containing compound contained in the photosensitive resin composition of the present invention, the (A) pigment, (B) dispersant, and (C) sulfonic acid group-containing compound listed in the description of the pigment dispersion of the present invention can be preferably used. The photosensitive resin composition of the present invention may further contain (D) an alkali-soluble resin, (E) a photopolymerizable compound, and (F) a photopolymerization initiator.

[0173] <(D) Alkali-soluble resin>

[0174] (D) alkali-soluble resin is not particularly limited as long as the solubility of the exposed part and the non-exposed part to alkali development changes after the coating film obtained by applying the photosensitive resin composition and drying is exposed, and alkali-soluble resins having carboxyl groups are preferred. In addition, alkali-soluble resins having ethylenically unsaturated groups are preferred, and alkali-soluble resins having ethylenically unsaturated groups and carboxyl groups are further preferred.

[0175] An example is shown below.

[0176] <Alkali-soluble resin (d1)>

[0177] The alkali-soluble resin (D) in the present invention preferably contains an alkali-soluble resin (d1) having a partial structure represented by the following general formula (d1-1). The inclusion of the alkali-soluble resin (d1) tends to improve adhesion.

[0178]

[0179] The benzene ring in formula (d1-1) may be further substituted by any substituent. 7 Each independently represents a hydrogen atom or a methyl group. Each independently represents O, S, CO, or a direct bond. Each independently represents a connecting bond. n represents an integer of 0 to 4.

[0180] In formula (d1-1), n ​​is preferably 0 to 3, more preferably 0 to 2, and even more preferably 0, from the viewpoint of sensitivity.

[0181] In formula (d1-1), from the perspective of sensitivity, R 7 Preferred is a hydrogen atom.

[0182] In formula (d1-1), from the viewpoint of sensitivity, X is preferably a direct bond.

[0183] The alkali-soluble resin (d1) having a partial structure represented by formula (d1-1) is preferably an alkali-soluble resin obtained by, for example, adding (meth)acrylic acid to an epoxy resin having a cardo skeleton represented by the following formula (d7-1), and further reacting a polybasic acid and / or its anhydride.

[0184]

[0185] The benzene ring in formula (d7-1) may be further substituted by any substituent. X's each independently represent O, S, CO, or a direct bond. n represents an integer of 0 to 4.

[0186] In formula (d7-1), n ​​is preferably 0 to 3, more preferably 0 to 2, and further preferably 0.

[0187] As a method for adding (meth)acrylic acid to an epoxy resin, a known method can be used. For example, the reaction can be carried out at a temperature of 50 to 150°C in the presence of an esterification catalyst.

[0188] As the esterification catalyst, for example, tertiary phosphines such as triethylphosphine, tributylphosphine, tricyclohexylphosphine, and triphenylphosphine; tertiary amines such as triethylamine, trimethylamine, benzyldimethylamine, and benzyldiethylamine; and quaternary ammonium salts such as tetramethylammonium chloride, tetraethylammonium chloride, and dodecyltrimethylammonium chloride can be used.

[0189] The amount of (meth)acrylic acid used is preferably 0.5 to 1.2 equivalents, more preferably 0.7 to 1.1 equivalents, based on 1 equivalent of the epoxy group of the epoxy resin.

[0190] By setting the amount of (meth)acrylic acid to be above the lower limit, the amount of unsaturated groups introduced becomes sufficient, the subsequent reaction with the polyacid and / or its anhydride is also sufficient, and there is a tendency to suppress a large amount of epoxy groups from remaining. On the other hand, by setting the amount to be below the upper limit, there is a tendency to suppress (meth)acrylic acid from remaining as an unreacted product.

[0191] Examples of the polybasic acid and / or its anhydride include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, pyromellitic acid, trimellitic acid, benzophenonetetracarboxylic acid, methylhexahydrophthalic acid, endomethylenetetrahydrophthalic acid, chlorendic acid, methyltetrahydrophthalic acid, biphenyltetracarboxylic acid, and anhydrides thereof.

[0192] As the addition reaction of the polybasic acid and / or its anhydride, a known method can be used, and the target product can be obtained by continuing the reaction under the same conditions as the addition reaction of (meth)acrylic acid.

[0193] A multi-branched structure may be introduced by adding a polyol such as trimethylolpropane, pentaerythritol, or dipentaerythritol during the synthesis of the alkali-soluble resin (d1) by addition reaction of the polybasic acid and / or its anhydride.

[0194] The alkali-soluble resin (d1) can be obtained, for example, by mixing a polybasic acid and / or its anhydride with a reactant of an epoxy resin and (meth) acrylic acid, or by mixing a polybasic acid and / or its anhydride and a polyol with a reactant of an epoxy resin and (meth) acrylic acid, followed by heating. In this case, the order of mixing the polybasic acid and / or its anhydride and the polyol is not particularly limited. By heating, the polybasic acid and / or its anhydride react with any hydroxyl group present in the mixture of the reactant with (meth) acrylic acid and the polyol.

[0195] The amount of the polyol used is preferably 0.01 to 0.5 times by mass, more preferably 0.02 to 0.2 times by mass, based on the reaction product of the epoxy resin and (meth)acrylic acid and the reaction product of the polybasic acid and / or its anhydride, from the viewpoint of suppressing thickening and gelation and exhibiting the effect.

[0196] The alkali-soluble resin (d1) may be used alone or in combination of two or more.

[0197] The acid value of the alkali-soluble resin (d1) is preferably 10 mgKOH / g or more, more preferably 50 mgKOH / g or more, further preferably 60 mgKOH / g or more, particularly preferably 80 mgKOH / g or more, and preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, and further preferably 120 mgKOH / g or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 10 to 200 mgKOH / g, more preferably 50 to 200 mgKOH / g, further preferably 60 to 150 mgKOH / g, and particularly preferably 80 to 120 mgKOH / g. By setting it above the aforementioned lower limit, there is a tendency for the residue to be reduced. In addition, by setting it below the aforementioned upper limit, there is a tendency to be able to make the fine line adhesion good.

[0198] The polystyrene-equivalent weight average molecular weight (Mw) of the alkali-soluble resin (d1) measured by gel permeation chromatography (GPC) is preferably 1000 or more, more preferably 2000 or more, further preferably 4000 or more, and particularly preferably 5000 or more. In addition, it is preferably 20000 or less, more preferably 15000 or less, further preferably 10000 or less, further preferably 8000 or less, and particularly preferably 7000 or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 1000 to 20000, more preferably 1000 to 15000, further preferably 2000 to 10000, further preferably 4000 to 8000, and particularly preferably 5000 to 7000. By setting it to the above lower limit value or more, there is a tendency that the fine line adhesion becomes good. In addition, by setting it to the above upper limit value or less, there is a tendency that the developing solubility and resolubility can be made good.

[0199] The photosensitive resin composition of the present invention may contain an alkali-soluble resin other than the alkali-soluble resin (d1) as (D) the alkali-soluble resin.

[0200] The alkali-soluble resin other than the alkali-soluble resin (d1) is not particularly limited as long as the solubility of the exposed portion and the non-exposed portion to alkali development changes after the coating film obtained by applying the photosensitive resin composition and drying is exposed, but is preferably an alkali-soluble resin having a carboxyl group. In addition, an alkali-soluble resin having an ethylenically unsaturated group is preferred, and an alkali-soluble resin having an ethylenically unsaturated group and a carboxyl group is further preferred.

[0201] Specifically, examples thereof include epoxy (meth)acrylate resins (d2) and acrylic copolymer resins (d3) having a carboxyl group other than the alkali-soluble resin (d1), and other resins (d4).

[0202] <Epoxy (meth)acrylate resin (d2) having a carboxyl group other than the alkali-soluble resin (d1)>

[0203] Examples of the epoxy (meth)acrylate resin (d2) having a carboxyl group other than the alkali-soluble resin (d1) include the following epoxy (meth)acrylate resins (d2-1) and epoxy (meth)acrylate resins (d2-2).

[0204] <Epoxy (meth)acrylate resin (d2-1)>

[0205] An alkali-soluble resin obtained by adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin and further reacting the epoxy resin with a polybasic acid and / or an anhydride thereof.

[0206] <Epoxy (meth)acrylate resin (d2-2)>

[0207] An alkali-soluble resin obtained by adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin and further reacting the epoxy resin with a polyol and a polybasic acid and / or an anhydride thereof.

[0208] <Epoxy (meth)acrylate resin (d2-1), epoxy (meth)acrylate resin (d2-2)>

[0209] As the epoxy resin as a raw material, for example, bisphenol A type epoxy resin (for example, "jER (registered trademark. The same applies hereinafter) 828", "jER1001", "jER1002", "jER1004", etc. manufactured by Mitsubishi Chemical Corporation), epoxy resin obtained by reaction of alcoholic hydroxyl group of bisphenol A type epoxy resin with epichlorohydrin (for example, "NER-1302" (epoxy equivalent 323, softening point 76°C) manufactured by Nippon Kayaku Co., Ltd.), bisphenol F type epoxy resin (for example, "jER807", "EP-4 001", "EP-4002", "EP-4004", etc."), epoxy resins obtained by the reaction of alcoholic hydroxyl groups of bisphenol F type epoxy resins with epichlorohydrin (e.g., "NER-7406" manufactured by Nippon Kayaku Co., Ltd. (epoxy equivalent 350, softening point 66°C)), bisphenol S type epoxy resins, biphenyl glycidyl ether (e.g., "YX-4000" manufactured by Mitsubishi Chemical Corporation), phenol novolac type epoxy resins (e.g., "EPPN-201" manufactured by Nippon Kayaku Co., Ltd., "EP-152", "EP-154" manufactured by Mitsubishi Chemical Corporation, Dow Chemical Company, "DEN-438"), (o,m,p-) cresol novolac type epoxy resin (for example, "EOCN (registered trademark. The same below) -102S", "EOCN-1020", "EOCN-104S" manufactured by Nippon Kayaku Co., Ltd.), triglycidyl isocyanurate (for example, "TEPIC (registered trademark)" manufactured by Nissan Chemical Co., Ltd.), trisphenol methane type epoxy resin (for example, "EPPN (registered trademark. The same below) -501", "EPPN-502", "EPPN-503" manufactured by Nippon Kayaku Co., Ltd.), alicyclic epoxy resin ("CELLOXIDE (registered trademark. The same below) 2021P", "CELLOXIDE EHPE”), epoxy resins obtained by glycidylating a phenolic resin obtained by the reaction of dicyclopentadiene and phenol (for example, “EXA-7200” manufactured by DIC Corporation, “NC-7300” manufactured by Nippon Kayaku Co., Ltd.), and epoxy resins represented by the following general formulas (d2-a) to (d2-e). Specifically, for example, as the epoxy resin represented by the following general formula (d2-a), “XD-1000” manufactured by Nippon Kayaku Co., Ltd. can be listed, and as the epoxy resin represented by the following general formula (d2-b), “NC-3000” manufactured by Nippon Kayaku Co., Ltd. can be listed.

[0210]

[0211] In formula (d2-a), b11 represents an average value and is a number from 0 to 10. 11represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a phenyl group, a naphthyl group, or a biphenyl group. 11 They are optionally the same as or different from each other.

[0212]

[0213] In formula (d2-b), b12 represents an average value and is a number from 0 to 10. 21 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a phenyl group, a naphthyl group, or a biphenyl group. 21 They are optionally the same as or different from each other.

[0214]

[0215] In formula (d2-c), X represents a linking group represented by the following general formula (d2-c-1) or (d2-c-2).

[0216] The molecular structure contains one or more adamantane structures. b13 represents an integer of 2 or 3.

[0217]

[0218] In formula (d2-c-1) and (d2-c-2), R 31 ~R 34 and R 35 ~R 37 Each independently represents an adamantyl group which may have a substituent, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or a phenyl group which may have a substituent. In addition, the * symbol in the formula represents a bonding site in (d2-c).

[0219]

[0220] In formula (d2-d), R 51 ~R 54 are each independently a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and R 55 are each independently an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and R 56 Each independently represents an alkylene group having 1 to 5 carbon atoms. k represents an integer of 1 to 5, l represents an integer of 0 to 13, and m represents an integer of 0 to 5.

[0221]

[0222] In formula (d2-e), n and o are each independently an integer of 1 to 9.

[0223] R 23 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a phenyl group, a naphthyl group, or a biphenyl group. 23 They are optionally the same as or different from each other.

[0224] Among these, the epoxy resin represented by any of formulas (d2-a) to (d2-e) is preferably used.

[0225] Examples of the α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group include: (meth)acrylic acid, crotonic acid, o-vinylbenzoic acid, m-vinylbenzoic acid, p-vinylbenzoic acid, monocarboxylic acids such as (meth)acrylic acid substituted with halogenated alkyl, alkoxy, halogen, nitro, and cyano groups at the α-position, 2-(meth)acryloyloxyethylsuccinic acid, 2-(meth)acryloyloxyethyladipic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxyethylhexahydro ... Acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl succinic acid, 2-(meth)acryloyloxypropyl adipic acid, 2-(meth)acryloyloxypropyl tetrahydrophthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxybutyl succinic acid, 2-(meth)acryloyloxybutyl adipic acid, 2-(meth)acryloyloxybutyl hydrophthalic acid, 2-(meth)acryloyloxybutyl phthalic acid, 2-(meth)acryloyloxybutyl maleic acid;

[0226] Examples of the (meth)acrylate include monomers obtained by adding (meth)acrylic acid to lactones such as ε-caprolactone, β-propiolactone, γ-butyrolactone, and δ-valerolactone, and having one hydroxyl group at the terminal;

[0227] Or a monomer having one hydroxyl group at the terminal such as hydroxyalkyl (meth)acrylate, a compound having one hydroxyl group at the terminal such as pentaerythritol tri(meth)acrylate and an acid (anhydride) such as succinic acid (anhydride), phthalic acid (anhydride), maleic acid (anhydride), etc., to have one or more ethylenically unsaturated groups and one carboxyl group at the terminal, and (meth)acrylic acid dimer can also be mentioned.

[0228] From the viewpoint of sensitivity, (meth)acrylic acid is preferred.

[0229] As a method for adding an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group to an epoxy resin, a known method can be used. For example, an α,β-unsaturated monocarboxylic acid or an α,β-unsaturated monocarboxylic acid ester having a carboxyl group and an epoxy resin can be reacted at a temperature of 50 to 150° C. in the presence of an esterification catalyst.

[0230] As the esterification catalyst, for example, tertiary phosphines such as triethylphosphine, tributylphosphine, tricyclohexylphosphine, and triphenylphosphine; tertiary amines such as triethylamine, trimethylamine, benzyldimethylamine, and benzyldiethylamine; and quaternary ammonium salts such as tetramethylammonium chloride, tetraethylammonium chloride, and dodecyltrimethylammonium chloride can be used.

[0231] The epoxy resin, the α,β-unsaturated monocarboxylic acid or the α,β-unsaturated monocarboxylic acid ester having a carboxyl group, and the esterification catalyst may be used alone or in combination of two or more.

[0232] The amount of the α,β-unsaturated monocarboxylic acid or the α,β-unsaturated monocarboxylic acid ester having a carboxyl group used is preferably 0.5 to 1.2 equivalents, more preferably 0.7 to 1.1 equivalents, based on 1 equivalent of the epoxy group of the epoxy resin.

[0233] By setting the amount of α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group to be above the aforementioned lower limit, the amount of unsaturated group introduced becomes sufficient, the subsequent reaction with polyacid and / or its anhydride is also sufficient, and there is a tendency to suppress a large amount of epoxy groups from remaining. On the other hand, by setting the aforementioned amount to be below the aforementioned upper limit, there is a tendency to suppress the α,β-unsaturated monocarboxylic acid or α,β-unsaturated monocarboxylic acid ester having a carboxyl group from remaining as an unreacted product.

[0234] As the polybasic acid and / or its anhydride and the polyol, the same compounds as those for the alkali-soluble resin (d1) can be used. Also, the same synthesis method as that for the alkali-soluble resin (d1) can be used for the synthesis method.

[0235] The acid value of the epoxy (meth) acrylate resin (d2-1, d2-2) thus obtained is preferably 10 mgKOH / g or more, more preferably 50 mgKOH / g or more, and further preferably 80 mgKOH / g or more. In addition, it is preferably 200 mgKOH / g or less, and more preferably 150 mgKOH / g or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 10 to 200 mgKOH / g, more preferably 50 to 200 mgKOH / g, and further preferably 80 to 150 mgKOH / g. By setting it to above the aforementioned lower limit, there is a tendency for fine line adhesion to become good. In addition, by setting it to below the aforementioned upper limit, there is a tendency for the developing solubility to be good.

[0236] The weight average molecular weight (Mw) of the epoxy (meth) acrylate resin (d2-1, d2-2) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1000 or more, more preferably 1500 or more, further preferably 2000 or more, and particularly preferably 2300 or more. In addition, it is preferably 20000 or less, more preferably 15000 or less, further preferably 10000 or less, further preferably 8000 or less, and particularly preferably 6000 or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 1000 to 20000, more preferably 1000 to 15000, further preferably 1500 to 10000, further preferably 2000 to 8000, and particularly preferably 2300 to 6000. By setting it to above the above lower limit, there is a tendency that sensitivity, coating film strength, and alkali resistance become good. In addition, by setting it to below the above upper limit, there is a tendency that developability and re-solubility can be made good.

[0237] <Acrylic copolymer resin (d3)>

[0238] As the acrylic copolymer resin (d3), for example, the polymer compounds described in Japanese Patent Laid-Open No. 7-207211, Japanese Patent Laid-Open No. 8-259876, Japanese Patent Laid-Open No. 10-300922, Japanese Patent Laid-Open No. 11-140144, Japanese Patent Laid-Open No. 11-174224, Japanese Patent Laid-Open No. 2000-56118, Japanese Patent Laid-Open No. 2003-233179, Japanese Patent Laid-Open No. 2007-270147, etc. can be used. Preferred examples include the following acrylic copolymer resins (d3-1) to (d3-4), and the acrylic copolymer resin (d3-1) is particularly preferred.

[0239] Acrylic copolymer resin (d3-1): A resin obtained by adding an unsaturated monobasic acid to at least a portion of the epoxy groups of a copolymer of epoxy (meth)acrylate and other free radical polymerizable monomers; or a resin obtained by adding a polyacid anhydride to at least a portion of the hydroxyl groups generated by the addition reaction.

[0240] Acrylic copolymer resin (d3-2): a straight-chain alkali-soluble resin having a carboxyl group in its main chain.

[0241] Acrylic copolymer resin (d3-3): a resin obtained by adding an epoxy group-containing unsaturated compound to the carboxyl portion of the acrylic copolymer resin (d3-2).

[0242] Acrylic copolymer resin (d3-4): (meth)acrylic resin.

[0243] <Other alkali-soluble resins (d4)>

[0244] The other alkali-soluble resin (d4) is not particularly limited as long as it is an alkali-soluble resin other than the alkali-soluble resin (d1), the epoxy (meth)acrylate resin (d2) having a carboxyl group other than the alkali-soluble resin (d1), and the acrylic copolymer resin (d3), and can be selected from resins commonly used in photosensitive resin compositions for color filters. For example, the alkali-soluble resins described in Japanese Patent Application Publication No. 2007-271727, Japanese Patent Application Publication No. 2007-316620, and Japanese Patent Application Publication No. 2007-334290 can be cited.

[0245] When the photosensitive resin composition of the present invention contains (D) an alkali-soluble resin, the content ratio of (D) the alkali-soluble resin is not particularly limited, but is preferably 5% by mass or more, more preferably 10% by mass or more, further preferably 15% by mass or more, and particularly preferably 20% by mass or more, relative to the total solid content of the photosensitive resin composition of the present invention, and is preferably 90% by mass or less, more preferably 70% by mass or less, further preferably 50% by mass or less, further preferably 30% by mass or less, and particularly preferably 25% by mass or less. The above upper and lower limits may be combined arbitrarily. For example, it is preferably 5 to 90% by mass, more preferably 5 to 70% by mass, further preferably 10 to 50% by mass, further preferably 15 to 30% by mass, and particularly preferably 20 to 25% by mass. By setting it to the above lower limit or more, there is a tendency that the solubility of the unexposed portion in the developer becomes better. In addition, by setting it to the above upper limit or less, it is possible to suppress the excessive penetration of the developer into the exposed portion, and there is a tendency that the sharpness of the image and the adhesion of fine lines become better.

[0246] When the photosensitive resin composition of the present invention contains (D) an alkali-soluble resin and (E) a photopolymerizable compound, the content of the (D) alkali-soluble resin is preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and further preferably 200 parts by mass or more, relative to 100 parts by mass of the (E) photopolymerizable compound. In addition, it is preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, further preferably 600 parts by mass or less, and particularly preferably 400 parts by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 100 to 1000 parts by mass, more preferably 100 to 800 parts by mass, further preferably 150 to 600 parts by mass, and particularly preferably 200 to 400 parts by mass. By being above the above lower limit, there is a tendency for the solubility of the unexposed portion in the developer to become good.

[0247] Moreover, by being below the above upper limit, the excessive penetration of the developer into the exposed portion can be suppressed, and the sharpness of the image and the adhesion of thin lines tend to be improved.

[0248] <(E) Photopolymerizable Compound>

[0249] The photosensitive resin composition of the present invention preferably contains (E) a photopolymerizable compound from the viewpoint of sensitivity and the like.

[0250] As the (E) photopolymerizable compound, a polyfunctional ethylenic monomer having two or more ethylenic unsaturated groups in one molecule is preferably used. The number of ethylenic unsaturated groups in the polyfunctional ethylenic monomer is preferably two or more, more preferably three or more, and further preferably four or more, and further preferably 10 or less, and further preferably 8 or less. The above upper and lower limits may be combined arbitrarily. For example, 2 to 10 are preferred, 3 to 10 are more preferred, and 4 to 8 are further preferred. By setting the number above the aforementioned lower limit, the photosensitive resin composition tends to have a high sensitivity, and by setting the number below the aforementioned upper limit, the curing shrinkage during polymerization tends to be reduced.

[0251] Examples of polyfunctional olefinic monomers include: esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids; esters of aromatic polyhydroxy compounds and unsaturated carboxylic acids; esters obtained by esterification of polyhydroxy compounds such as aliphatic polyhydroxy compounds and aromatic polyhydroxy compounds with unsaturated carboxylic acids and polycarboxylic acids, etc., preferably esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids.

[0252] Examples of the esters of aliphatic polyhydroxy compounds and unsaturated carboxylic acids include acrylates of aliphatic polyhydroxy compounds such as ethylene glycol diacrylate, triethylene glycol diacrylate, trimethylolpropane triacrylate, trimethylolethane triacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, and glycerol acrylate; methacrylates obtained by replacing these acrylates with methacrylates; itaconates obtained by replacing these acrylates with itaconates; crotonates obtained by replacing these acrylates with crotonates; and maleates obtained by replacing these acrylates with maleates. Preferred are acrylates of aliphatic polyhydroxy compounds and methacrylates of aliphatic polyhydroxy compounds.

[0253] Examples of the esters of an aromatic polyhydroxy compound and an unsaturated carboxylic acid include acrylates and methacrylates of aromatic polyhydroxy compounds such as hydroquinone diacrylate, hydroquinone dimethacrylate, resorcinol diacrylate, resorcinol dimethacrylate, and pyrogallol triacrylate.

[0254] The esters obtained by the esterification reaction of polycarboxylic acids and unsaturated carboxylic acids with polyhydroxy compounds are not necessarily single substances, and examples thereof include condensates of acrylic acid, phthalic acid and ethylene glycol; condensates of acrylic acid, maleic acid and diethylene glycol; condensates of methacrylic acid, terephthalic acid and pentaerythritol; and condensates of acrylic acid, adipic acid, butanediol and glycerol.

[0255] In addition, examples of the polyfunctional olefinic monomer used in the present invention include: urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a hydroxyl-containing (meth)acrylate or a polyisocyanate compound with a polyol and a hydroxyl-containing (meth)acrylate; epoxy acrylates such as addition reaction products of a polyvalent epoxy compound with a hydroxyl (meth)acrylate or (meth)acrylic acid; acrylamides such as ethylenebisacrylamide; allyl esters such as diallyl phthalate; and vinyl-containing compounds such as divinyl phthalate.

[0256] (E) The photopolymerizable compound may be used alone or in combination of two or more.

[0257] When the photosensitive resin composition of the present invention contains (E) a photopolymerizable compound, the content ratio of the (E) photopolymerizable compound is not particularly limited, and is preferably 90% by mass or less, more preferably 70% by mass or less, further preferably 50% by mass or less, further preferably 30% by mass or less, still further preferably 20% by mass or less, and particularly preferably 10% by mass or less relative to the total solid content of the photosensitive resin composition. By making the content of the photopolymerizable compound below the above upper limit, there is a tendency that the permeability of the developer to the exposed portion becomes moderate and a good image can be obtained. The lower limit of the content ratio of the (E) photopolymerizable compound is not particularly limited, and is preferably 1% by mass or more, and more preferably 5% by mass or more. By being above the above lower limit, there is a tendency that the photocuring based on ultraviolet irradiation is improved and the fine line adhesion is also improved.

[0258] The above upper and lower limits may be combined arbitrarily. For example, it is preferably 1 to 90% by mass, more preferably 1 to 70% by mass, further preferably 1 to 50% by mass, further preferably 5 to 30% by mass, further preferably 5 to 20% by mass, and particularly preferably 5 to 10% by mass.

[0259] <(F) Photopolymerization Initiator>

[0260] The photosensitive resin composition of the present invention may contain a photopolymerization initiator. (F) The photopolymerization initiator is a component that directly absorbs light and undergoes a decomposition reaction or a hydrogen abstraction reaction to generate polymerization-active free radicals. An additive such as a sensitizing dye may be added as needed.

[0261] (F) Photopolymerization initiator, for example, metallocene compounds including titanocene compounds described in Japanese Patent Application Laid-Open No. 59-152396 and Japanese Patent Application Laid-Open No. 61-151197; hexaarylbiimidazole derivatives described in Japanese Patent Application Laid-Open No. 2000-56118; halogenated methylated oxadiazole derivatives, halogenated methyl s-triazine derivatives, N-aryl-α-amino acids such as N-phenylglycine, N-aryl-α-amino acid salts, free radical activators such as N-aryl-α-amino acid esters, α-aminoalkylphenone derivatives described in Japanese Patent Application Laid-Open No. 10-39503; oxime ester derivatives described in Japanese Patent Application Laid-Open No. 2000-80068 and Japanese Patent Application Laid-Open No. 2006-36750.

[0262] Examples of the titanocene derivatives include dicyclopentadienyl titanium dichloride, dicyclopentadienyl bisphenyl titanium, dicyclopentadienyl bis(2,3,4,5,6-pentafluorophenyl-1-yl)titanium, dicyclopentadienyl bis(2,3,5,6-tetrafluorophenyl-1-yl)titanium, dicyclopentadienyl bis(2,4,6-trifluorophenyl-1-yl)titanium, dicyclopentadienyl bis(2,6-difluorophenyl-1-yl)titanium, dicyclopentadienyl bis(2,4-difluorophenyl-1-yl)titanium, di(methylcyclopentadienyl)bis(2,3,4,5,6-pentafluorophenyl-1-yl)titanium, di(methylcyclopentadienyl)bis(2,6-difluorophenyl-1-yl)titanium, and dicyclopentadienyl [2,6-difluoro-3-(pyrrol-1-yl)-phenyl-1-yl]titanium.

[0263] Examples of biimidazole derivatives include 2-(2'-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(2'-chlorophenyl)-4,5-bis(3'-methoxyphenyl)imidazole dimer, 2-(2'-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(2'-methoxyphenyl)-4,5-diphenylimidazole dimer, and (4'-methoxyphenyl)-4,5-diphenylimidazole dimer.

[0264] Examples of the halogenated methylated oxadiazole derivatives include 2-trichloromethyl-5-(2'-benzofuranyl)-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-benzofuranyl)vinyl]-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-(6"-benzofuranyl)vinyl)]-1,3,4-oxadiazole, and 2-trichloromethyl-5-furanyl-1,3,4-oxadiazole.

[0265] Examples of the halomethyl-s-triazine derivatives include 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-ethoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, and 2-(4-ethoxycarbonylnaphthyl)-4,6-bis(trichloromethyl)-s-triazine.

[0266] Examples of the α-aminoalkylphenone derivatives include 2-methyl-1〔4-(methylthio)phenyl〕-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane-1-one, 4-dimethylaminoethyl benzoate, 4-dimethylaminoisoamyl benzoate, 4-dimethylaminoacetophenone, 4-dimethylaminopropiophenone, 1,4-dimethylaminobenzoic acid 2-ethylhexyl ester, 2,5-bis(4-diethylaminobenzylidene)cyclohexanone, 7-diethylamino-3-(4-diethylaminobenzoyl)coumarin, and 4-(diethylamino)chalcone.

[0267] As (F) a photopolymerization initiator, oxime ester derivatives (oxime ester compounds and ketoxime ester compounds) are particularly effective in terms of sensitivity. When an alkali-soluble resin containing a phenolic hydroxyl group is used, the sensitivity may be disadvantageous. Therefore, oxime ester derivatives (oxime ester compounds and ketoxime ester compounds) having excellent sensitivity are particularly useful. Among oxime ester derivatives, oxime ester compounds are preferred from the viewpoint of adhesion to the substrate.

[0268] The photopolymerization initiator of the oxime ester compound has a structure for absorbing ultraviolet rays, a structure for transmitting light energy, and a structure for generating free radicals in its structure, so a small amount of high sensitivity can be obtained, and the thermal reaction is stable, and a small amount of high-sensitivity photosensitive resin composition can be designed. In particular, from the viewpoint of light absorption of the i-ray (365nm) of the exposure light source, in the case of an oxime ester compound containing an optionally substituted carbazole group (a group having an optionally substituted carbazole ring), the structural characteristics can be well expressed, which is more preferred. Now, in the market, high light-shielding degree and thin film BM are required, and the pigment concentration is also increasing. It is particularly effective under such conditions.

[0269] Examples of the oxime ester compound include compounds containing a structural portion represented by formula (22), and preferably include oxime ester compounds represented by general formula (23).

[0270]

[0271] In formula (22), R 22Each represents an optionally substituted alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, an alkoxycarbonylalkanoyl group having 3 to 20 carbon atoms, a phenoxycarbonylalkanoyl group having 8 to 20 carbon atoms, a heteroaryloxycarbonylalkanoyl group having 3 to 20 carbon atoms, an aminoalkylcarbonyl group having 2 to 10 carbon atoms, an aroyl group having 7 to 20 carbon atoms, a heteroaroyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, or an aryloxycarbonyl group having 7 to 20 carbon atoms.

[0272]

[0273] In formula (23), R 21a represents hydrogen, or optionally substituted, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 25 carbon atoms, heteroarylalkyl having 1 to 20 carbon atoms, alkoxycarbonylalkyl having 3 to 20 carbon atoms, phenoxycarbonylalkyl having 8 to 20 carbon atoms, heteroaryloxycarbonylalkyl or heteroarylsulfanyl having 1 to 20 carbon atoms, aminoalkyl having 1 to 20 carbon atoms, alkanoyl having 2 to 12 carbon atoms, alkenoyl having 3 to 25 carbon atoms, cycloalkanoyl having 3 to 8 carbon atoms, aroyl having 7 to 20 carbon atoms, heteroaroyl having 1 to 20 carbon atoms, alkoxycarbonyl having 2 to 10 carbon atoms, aryloxycarbonyl having 7 to 20 carbon atoms, or cycloalkylalkyl having 1 to 10 carbon atoms;

[0274] R 21b It represents an arbitrary substituent containing an aromatic ring or a heteroaromatic ring.

[0275] It should be noted that R 21a Can be used with R 21b Together they form a ring, and examples of the linking group include an alkylene group having 1 to 10 carbon atoms, a polyvinyl group (-(CH=CH) r -), polyethynyl (-(C≡C) r -) or a group formed by combining them (it should be noted that r is an integer of 0 to 3).

[0276] R 22a It is expressed as R in formula (22) 22 Same group.

[0277] As R in formula (22) 22 and R in formula (23) 22a Preferred examples include an alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, and a cycloalkanoyl group having 3 to 8 carbon atoms.

[0278] As R in formula (23) 21a Preferred examples include unsubstituted straight-chain alkyl or cycloalkylalkyl groups such as methyl, ethyl and propyl groups, and propyl groups substituted with N-acetyl-N-acetoxyamino groups.

[0279] As R in formula (23) 21b Preferred examples include an optionally substituted carbazolyl group, an optionally substituted thioxanthone group, and an optionally substituted phenyl sulfide group.

[0280] As the photopolymerization initiator of the oxime ester compound, R in the formula (23) 21b The photopolymerization initiator which is an optionally substituted carbazole group is more preferred for the above reasons. Furthermore, the carbazole group having at least one group selected from the group consisting of an optionally substituted aryl group having 6 to 25 carbon atoms, an optionally substituted arylcarbonyl group having 7 to 25 carbon atoms, an optionally substituted heteroaryl group having 5 to 25 carbon atoms, an optionally substituted heteroarylcarbonyl group having 6 to 25 carbon atoms, and a nitro group is preferred.

[0281] Particularly preferred are carbazolyl groups having at least one group selected from the group consisting of a benzoyl group, a toluoyl group, a naphthoyl group, a thienylcarbonyl group, and a nitro group. In addition, it is desirable that these groups are bonded to the 3-position of the carbazolyl group.

[0282] Examples of commercially available products of the photopolymerization initiator of the oxime ester compound include OXE-02 manufactured by BASF, and TR-PBG-304 and TR-PBG-314 manufactured by Changzhou Qiangli Electronics Co., Ltd.

[0283] Examples of the photopolymerization initiator of the oxime ester compound include the compounds exemplified below.

[0284]

[0285]

[0286]

[0287] Examples of the ketoxime ester compound include compounds containing a structural portion represented by formula (24), and preferably include a ketoxime ester compound represented by formula (25).

[0288]

[0289] In formula (24), R 24 With R in formula (22) 22 Same meaning.

[0290]

[0291] In formula (25), R 23arepresents an optionally substituted phenyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 25 carbon atoms, a heteroarylalkyl group having 1 to 20 carbon atoms, an alkoxycarbonylalkyl group having 3 to 20 carbon atoms, a phenoxycarbonylalkyl group having 8 to 20 carbon atoms, an alkylsulfanyl group having 2 to 20 carbon atoms, a heteroaryloxycarbonylalkyl group or a heteroarylsulfanyl group having 1 to 20 carbon atoms, an aminoalkyl group having 1 to 20 carbon atoms, an alkanoyl group having 2 to 12 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, an aroyl group having 7 to 20 carbon atoms, a heteroaroyl group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 20 carbon atoms, or a cycloalkylalkyl group having 1 to 10 carbon atoms.

[0292] R 23b represents any substituent containing an aromatic ring or a heteroaromatic ring. 23a Can be used with R 23b Together they form a ring, and examples of the linking group include an alkylene group having 1 to 10 carbon atoms, a polyvinyl group (-(CH=CH) r -), polyethynyl (-(C≡C) r -) or a group formed by combining them (it should be noted that r is an integer of 0 to 3).

[0293] R 24a represents an alkanoyl group having 2 to 12 carbon atoms, an alkenoyl group having 3 to 25 carbon atoms, a cycloalkanoyl group having 4 to 8 carbon atoms, a benzoyl group having 7 to 20 carbon atoms, a heteroaroyl group having 3 to 20 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an aryloxycarbonyl group having 7 to 20 carbon atoms, a heteroaryl group having 2 to 20 carbon atoms, or an alkylaminocarbonyl group having 2 to 20 carbon atoms, each of which is optionally substituted.

[0294] As R in formula (24) 24 and R in the above general formula (25) 24a Preferred examples include an alkanoyl group having 2 to 12 carbon atoms, a heteroarylalkanoyl group having 1 to 20 carbon atoms, a cycloalkanoyl group having 3 to 8 carbon atoms, and an aroyl group having 7 to 20 carbon atoms.

[0295] As R in formula (25) 23a Preferred examples include unsubstituted ethyl, propyl, butyl, and ethyl or propyl substituted with methoxycarbonyl.

[0296] As R in formula (25) 23b Preferably, an optionally substituted carbazolyl group and an optionally substituted phenyl sulfide group are mentioned.

[0297] Examples of the ketoxime ester-based compound include the compounds exemplified below.

[0298]

[0299]

[0300] Examples of the photopolymerization initiator of the ketoxime ester compound include OXE-01 manufactured by BASF and TR-PBG-305 manufactured by Changzhou Qiangli Electronics Co., Ltd.

[0301] Oxime ester compounds and ketoxime ester compounds are known compounds per se, and are described in, for example, Japanese Patent Application Laid-Open Nos. 2000-80068 and 2006-36750.

[0302] The photopolymerization initiator may be used alone or in combination of two or more.

[0303] In addition, for example, benzoin alkyl ethers such as benzoin methyl ether, benzoin phenyl ether, benzoin isobutyl ether, and benzoin isopropyl ether can be cited; anthraquinone derivatives such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 1-chloroanthraquinone; benzophenone derivatives such as benzophenone, Michler's ketone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2-chlorobenzophenone, 4-bromobenzophenone, and 2-carboxybenzophenone; 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, α-hydroxy-2-methylphenylacetone, 1-hydroxy-1-methylethyl-(p-isopropylphenyl)ketone, 1-hydroxy 1-(p-dodecylphenyl)ketone, 2-methyl-(4'-methylthiophenyl)-2-morpholinyl-1-propanone, 1,1,1-trichloromethyl-(p-butylphenyl)ketone and other acetophenone derivatives; thioxanthone derivatives such as 2-ethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone derivatives; benzoate derivatives such as ethyl p-dimethylaminobenzoate and ethyl p-diethylaminobenzoate; acridine derivatives such as 9-phenylacridine and 9-(p-methoxyphenyl)acridine; phenazine derivatives such as 9,10-dimethylbenzophenazine; anthrone derivatives such as benzanthrone.

[0304] <Sensitizing Pigment>

[0305] (F) The photopolymerization initiator may be used in combination with a sensitizing dye corresponding to the wavelength of the image exposure light source for the purpose of improving the sensitivity as required. Examples of the sensitizing dye include xanthene dyes described in Japanese Patent Laid-Open Nos. 4-221958 and 4-219756; coumarin dyes having a heterocyclic ring described in Japanese Patent Laid-Open Nos. 3-239703 and 5-289335; 3-coumarin keto compounds described in Japanese Patent Laid-Open Nos. 3-239703 and 5-289335; pyrromethene dyes described in Japanese Patent Laid-Open No. 6-19240; and pyrromethene dyes described in Japanese Patent Laid-Open Nos. 47-2528 and 54-54. -155292, Japanese Patent Publication No. 45-37377, Japanese Patent Application Laid-Open No. 48-84183, Japanese Patent Application Laid-Open No. 52-112681, Japanese Patent Application Laid-Open No. 58-15503, Japanese Patent Application Laid-Open No. 60-88005, Japanese Patent Application Laid-Open No. 59-56403, Japanese Patent Application Laid-Open No. 2-69, Japanese Patent Application Laid-Open No. 57-168088, Japanese Patent Application Laid-Open No. 5-107761, Japanese Patent Application Laid-Open No. 5-210240, and Japanese Patent Application Laid-Open No. 4-288818.

[0306] As the sensitizing dye, an amino group-containing sensitizing dye is preferred, and a compound having an amino group and a phenyl group in the same molecule is more preferred, and benzophenone compounds such as 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 2-aminobenzophenone, 4-aminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, and 3,4-diaminobenzophenone are further preferred; 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-diethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzo[4,5]benzoxazole, 2-(p-dimethylaminophenyl)benzo[6,7]benzoxazole, 2,5- Compounds containing a p-dialkylaminophenyl group such as bis(p-diethylaminophenyl)1,3,4-oxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-(p-diethylaminophenyl)benzothiazole, 2-(p-dimethylaminophenyl)benzimidazole, 2-(p-diethylaminophenyl)benzimidazole, 2,5-bis(p-diethylaminophenyl)1,3,4-thiadiazole, (p-dimethylaminophenyl)pyridine, (p-diethylaminophenyl)pyridine, (p-dimethylaminophenyl)quinoline, (p-diethylaminophenyl)quinoline, (p-dimethylaminophenyl)pyrimidine, and (p-diethylaminophenyl)pyrimidine are particularly preferred, and 4,4'-dialkylaminobenzophenone is particularly preferred.

[0307] The sensitizing dye may be used alone or in combination of two or more.

[0308] When the photosensitive resin composition of the present invention contains (F) a photopolymerization initiator, the content ratio of the (F) photopolymerization initiator is not particularly limited, and is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 3% by mass or more, and particularly preferably 4% by mass or more relative to the total solid content of the photosensitive resin composition of the present invention. In addition, it is preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 8% by mass or less. The above upper and lower limits can be combined arbitrarily. Preferably 1 to 30% by mass, more preferably 1 to 20% by mass, further preferably 2 to 15% by mass, further preferably 3 to 10% by mass, and particularly preferably 4 to 8% by mass. By setting it to above the aforementioned lower limit, there is a tendency for the sensitivity to be improved. In addition, by setting it to below the aforementioned upper limit, there is a tendency for the adhesion stress with the substrate to be improved.

[0309] When the photosensitive resin composition of the present invention contains an oxime ester compound as the (F) photopolymerization initiator, the content ratio of the oxime ester compound is not particularly limited, and is preferably 1% by mass or more, more preferably 2% by mass or more, further preferably 3% by mass or more, and particularly preferably 4% by mass or more relative to the total solid content of the photosensitive resin composition of the present invention. In addition, it is preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 8% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 1 to 30% by mass, more preferably 1 to 20% by mass, further preferably 2 to 15% by mass, further preferably 3 to 10% by mass, and particularly preferably 4 to 8% by mass. By setting it above the aforementioned lower limit, there is a tendency for the sensitivity to be improved, and the fine line adhesion becomes good. In addition, by setting it below the aforementioned upper limit, there is a tendency for the solubility of the unexposed portion in the developer to be improved.

[0310] When using a sensitizing dye, the content ratio of the sensitizing dye in the total solid content of the photosensitive resin composition is preferably more than 0 mass % and 20 mass % or less, more preferably more than 0 mass % and 15 mass % or less, and further preferably more than 0 mass % and 10 mass % or less.

[0311] <Surfactant>

[0312] The photosensitive resin composition of the present invention may contain a surfactant for the purpose of adjusting coating properties.

[0313] Examples of the surfactant include BYK-330 (manufactured by BYK-Chemie, surface tension 24.4 mN / m), F-475 (manufactured by DIC Corporation, surface tension 25.4 mN / m), and F-554 (manufactured by DIC Corporation, surface tension 23.3 mN / m).

[0314] The surfactant may be used alone or in combination of two or more.

[0315] When the photosensitive resin composition of the present invention contains a surfactant, the content ratio of the surfactant is not particularly limited, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly preferably 0.15% by mass or more in the total solid content of the photosensitive resin composition. In addition, it is preferably 1% by mass or less, more preferably 0.7% by mass or less, further preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 0.01 to 1% by mass, more preferably 0.05 to 0.7% by mass, further preferably 0.1 to 0.5% by mass, and particularly preferably 0.15 to 0.3% by mass. By setting it above the aforementioned lower limit, there is a tendency that the uniformity of the coating film is improved and the adhesion of the fine line can be improved. In addition, by setting it below the aforementioned upper limit, there is a tendency that the sensitivity is improved.

[0316] <Solvent>

[0317] The photosensitive resin composition of the present invention is used in a state where (D) an alkali-soluble resin, (E) a photopolymerizable compound, (F) a photopolymerization initiator, and various materials used as required are dissolved or dispersed in a solvent, preferably an organic solvent.

[0318] As the organic solvent, it is preferable to select an organic solvent having a boiling point (under a pressure of 1013.25 [hPa]; the same shall apply hereinafter) in the range of 100 to 300°C, preferably 120 to 280°C.

[0319] Examples of the organic solvent include the following organic solvents.

[0320] Glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-butyl ether, propylene glycol tert-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, methoxymethylpentanol, dipropylene glycol monoethyl ether, dipropylene glycol monomethyl ether, 3-methyl-3-methoxybutanol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and tripropylene glycol methyl ether;

[0321] Glycol dialkyl ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether;

[0322] Glycol alkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-butyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, methoxybutyl acetate, 3-methoxybutyl acetate, methoxypentyl acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol mono-n-butyl ether acetate, dipropylene glycol monomethyl ether acetate, triethylene glycol monomethyl ether acetate, triethylene glycol monoethyl ether acetate, and 3-methyl-3-methoxybutyl acetate;

[0323] Glycol diacetates such as ethylene glycol diacetate, 1,3-butylene glycol diacetate, and 1,6-hexanol diacetate;

[0324] Alkyl acetates such as cyclohexanol acetate;

[0325] Ethers such as amyl ether, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, diamyl ether, ethyl isobutyl ether, and dihexyl ether;

[0326] Ketones such as acetone, methyl ethyl ketone, methyl amyl ketone, methyl isopropyl ketone, methyl isoamyl ketone, diisopropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclohexanone, ethyl amyl ketone, methyl butyl ketone, methyl hexyl ketone, methyl nonyl ketone, and methoxymethyl amyl ketone;

[0327] Monohydric or polyhydric alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, methoxymethylpentanol, glycerol, and benzyl alcohol;

[0328] Aliphatic hydrocarbons such as n-pentane, n-octane, diisobutylene, n-hexane, hexene, isoprene, dipentene, and dodecane;

[0329] Alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, methylcyclohexene, and bicyclohexane;

[0330] Aromatic hydrocarbons such as benzene, toluene, xylene, and cumene;

[0331] Chain or cyclic esters such as amyl formate, ethyl formate, ethyl acetate, butyl acetate, propyl acetate, amyl acetate, methyl isobutyrate, ethylene glycol acetate, ethyl propionate, propyl propionate, butyl butyrate, isobutyl butyrate, methyl isobutyrate, ethyl octanoate, butyl stearate, ethyl benzoate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, and γ-butyrolactone;

[0332] Alkoxycarboxylic acids such as 3-methoxypropionic acid and 3-ethoxypropionic acid;

[0333] Halogenated hydrocarbons such as butyl chloride and amyl chloride;

[0334] Ether ketones such as methoxymethylpentyl ketone;

[0335] Nitriles such as acetonitrile and benzonitrile.

[0336] Examples of commercially available solvents include mineral spirit, Varsol #2, Apco #18 Solvent, Apco thinner, Sorcal solvent No. 1 and No. 2, Solvesso #150, Shell TS28 Solvent, carbitol, ethyl carbitol, butyl carbitol, methyl cellosolve (“Cellosolve” is a registered trademark. The same shall apply hereinafter), ethyl cellosolve, ethyl cellosolve acetate, methyl cellosolve acetate, and Diglyme (all trade names).

[0337] The organic solvent may be used alone or in combination of two or more.

[0338] When forming the pixels of the color filter or the black matrix by photolithography, it is preferable to select an organic solvent having a boiling point of 100 to 250° C., preferably 120 to 230° C. as the organic solvent.

[0339] Glycol alkyl ether acetates are preferred because they have a good balance between coating properties and surface tension and because the solubility of each component of the photosensitive resin composition is relatively high.

[0340] The glycol alkyl ether acetates may be used alone or in combination with other organic solvents.

[0341] As other organic solvents that can be used in combination, glycol monoalkyl ethers are preferred. Propylene glycol monomethyl ether is preferred from the viewpoint of solubility of the constituent components in the composition.

[0342] From the viewpoint of storage stability of the obtained photosensitive resin composition, the ratio of the glycol monoalkyl ether in the solvent is preferably 5 to 30% by mass, more preferably 5 to 20% by mass.

[0343] As an organic solvent, an organic solvent having a boiling point of 200° C. or more (hereinafter sometimes referred to as a “high boiling point solvent”) can be used in combination. By using a high boiling point solvent in combination, the photosensitive resin composition is not easy to dry, and there is an effect of preventing the uniform dispersion state of the pigment in the photosensitive resin composition from being destroyed by rapid drying. For example, there is an effect of preventing the generation of foreign matter defects caused by the precipitation / solidification of the coloring material at the front end of the slit nozzle. From such a viewpoint, dipropylene glycol methyl ether acetate, diethylene glycol mono-n-butyl ether acetate, diethylene glycol monoethyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, triacetin, and 1,6-hexanediol diacetate are preferred.

[0344] The content of the high boiling point solvent in the organic solvent is preferably 0 to 50% by mass, more preferably 0.5 to 40% by mass, and further preferably 1 to 30% by mass. By setting the content above the lower limit, for example, there is a tendency to suppress the precipitation / solidification of the coloring material at the front end of the slit nozzle to cause foreign matter defects, and by setting the content below the upper limit, there is a tendency to suppress the slow drying speed of the composition to cause problems such as poor rhythm of the reduced pressure drying process in the color filter manufacturing process and pin marks of pre-baking.

[0345] When the photosensitive resin composition of the present invention contains an organic solvent, the content ratio of the organic solvent is not particularly limited. From the viewpoint of ease of coating and viscosity stability, the total solid content in the photosensitive resin composition is preferably 5% by mass or more, more preferably 8% by mass or more, further preferably 10% by mass or more, and preferably 40% by mass or less, more preferably 30% by mass or less, further preferably 25% by mass or less, and particularly preferably 20% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, preferably 5 to 40% by mass, more preferably 5 to 30% by mass, further preferably 8 to 25% by mass, and particularly preferably 10 to 20% by mass.

[0346] <Other Compounding Components of the Photosensitive Resin Composition>

[0347] The photosensitive resin composition of the present invention may contain, in addition to the above-mentioned components, for example, thiols, additives, development improvers, ultraviolet absorbers, and antioxidants as appropriate.

[0348] <Mercaptans>

[0349] The photosensitive resin composition of the present invention may contain thiols for the purpose of increasing sensitivity and improving adhesion to a substrate. Examples of the thiols include hexanedithiol, decanedithiol, 1,4-dimethylmercaptobenzene, butanediol bisthiopropionate, butanediol bisthioglycolate, ethylene glycol bisthioglycolate, trimethylolpropane trimerthioglycolate, butanediol bisthiopropionate, trimethylolpropane trithiopropionate, trimethylolpropane trimerthioglycolate, pentaerythritol tetrathiopropionate, pentaerythritol tetrathioglycolate, trihydroxyethyl trithiopropionate, ethylene glycol bis(3-mercaptobutyrate), propylene glycol bis(3-mercaptobutyrate; PGMB), butanediol bis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane (trade name; Karenz MT BD1, manufactured by Showa Denko K.K.), butanediol trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptobutyrate) (trade name; Karenz MT PE1, manufactured by Showa Denko K.K.), pentaerythritol tris(3-mercaptobutyrate), ethylene glycol bis(3-mercaptoisobutyrate), butanediol bis(3-mercaptoisobutyrate), trimethylolpropane tris(3-mercaptoisobutyrate), trimethylolpropane tris(3-mercaptobutyrate; TPMB), trimethylolpropane tris(2-mercaptoisobutyrate; TPMIB), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (trade name; Karenz MT NR1, manufactured by Showa Denko K.K.), preferably polyfunctional thiols such as PGMB, TPMB, TPMIB, Karenz MT BD1, Karenz MTPE1, and Karenz MT NR1, more preferably Karenz MT BD1, Karenz MT PE1, and Karenz MTNR1, and particularly preferably Karenz MT PE1.

[0350] The thiols may be used alone or in combination of two or more.

[0351] When the photosensitive resin composition of the present invention contains thiols, the content ratio of thiols is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more relative to the total solid content of the photosensitive resin composition of the present invention. In addition, it is preferably 10% by mass or less, and more preferably 5% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 0.1 to 10% by mass, more preferably 0.3 to 10% by mass, and further preferably 0.5 to 5% by mass. By setting it to above the above lower limit, there is a tendency to suppress the decrease in sensitivity. In addition, by setting it to below the above upper limit, there is a tendency to easily make the storage stability good.

[0352] <Additives>

[0353] The photosensitive resin composition of the present invention may contain an additive in order to improve adhesion to a substrate. Examples of the additive include a silane coupling agent and a titanium coupling agent, and a silane coupling agent is preferred.

[0354] Examples of the silane coupling agent include KBM-402, KBM-403, KBM-502, KBM-5103, KBE-9007, X-12-1048, and X-12-1050 (manufactured by Shin-Etsu Silicones Co., Ltd.), and Z-6040, Z-6043, and Z-6062 (manufactured by Dow Corning Toray Co., Ltd.).

[0355] The silane coupling agents may be used alone or in combination of two or more.

[0356] The photosensitive resin composition of the present invention may contain additives other than the silane coupling agent. Examples of additives other than the silane coupling agent include phosphoric acid additives and other additives.

[0357] As the phosphoric acid-based additive, phosphoric acid esters containing a (meth)acryloyloxy group are preferred, and phosphoric acid-based additives represented by the following general formulas (g1), (g2), and (g3) are more preferred.

[0358]

[0359] In formula (g1), (g2), and (g3), R 51 Each independently represents a hydrogen atom or a methyl group, l and l' each independently represent an integer of 1 to 10, and m each independently represents 1, 2 or 3.

[0360] As other additives, TEGO*Add Bond LTH (produced by Evonik) can be mentioned, for example.

[0361] The phosphoric acid-based additive and other additives may be used alone or in combination of two or more.

[0362] When the photosensitive resin composition of the present invention includes an additive, the content ratio of the additive is not particularly limited, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 0.5% by mass or more in the total solid content of the photosensitive resin composition. In addition, it is preferably 5% by mass or less, more preferably 3% by mass or less, further preferably 2% by mass or less, and particularly preferably 1.5% by mass or less. The above upper and lower limits can be combined arbitrarily. For example, it is preferably 0.01 to 5% by mass, more preferably 0.01 to 3% by mass, further preferably 0.1 to 2% by mass, and particularly preferably 0.5 to 1.5% by mass. By setting it to above the aforementioned lower limit, there is a tendency for the adhesion to be improved. By setting it to below the aforementioned upper limit, there is a tendency for the developability to become good.

[0363] <Physical Properties of Photosensitive Resin Composition>

[0364] The photosensitive resin composition of the present invention can be suitably used for forming a black matrix, and from this viewpoint, it preferably exhibits black color.

[0365] The optical density (OD value) per 1.0 μm film thickness of the coating film formed by curing the photosensitive resin composition of the present invention is preferably 4.0 or more, more preferably 4.1 or more, further preferably 4.2 or more, and preferably 6.0 or less. For example, it is preferably 4.0 to 6.0, more preferably 4.1 to 6.0, and further preferably 4.2 to 6.0. By setting it to be above the above lower limit, there is a tendency to ensure sufficient light-shielding properties.

[0366] Optical density refers to the transmitted optical density expressed by ISO visual density in the ISO 5-3 standard, which is the spectral sensitivity characteristic of the light receiving unit. Usually, the A light source specified by CIE (International Commission on Illumination) is used as the light source. As a measuring instrument that can be used for the measurement of transmitted optical density, for example, X-Rite 361T (V) of SAKATAINX ENG.CO.,LTD. can be cited.

[0367] <Method for producing pigment dispersion>

[0368] The pigment dispersion of the present invention is manufactured by conventional methods. Usually, the (A) pigment is preferably pre-dispersed using a paint conditioner, a sand mill, a ball mill, a roller mill, a stone mill, a jet mill, a homogenizer, etc. By dispersing, the (A) pigment is micronized, and therefore, the coating characteristics of the photosensitive resin composition are improved. In addition, when a black pigment is used as the (A) pigment, it helps to improve the light-shielding ability.

[0369] The dispersion treatment is usually preferably carried out in a system using a combination of (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound, a solvent, and, if necessary, part or all of (D) an alkali-soluble resin (hereinafter, the mixture subjected to the dispersion treatment and the pigment dispersion obtained by the treatment are sometimes referred to as "ink"). In particular, when a polymer dispersant is used as the dispersant, the thickening of the obtained ink over time is suppressed, and the dispersion stability is excellent, so it is preferred.

[0370] When the (A) pigment is dispersed by a sand mill, glass beads, zircon beads, or zirconium oxide beads with a diameter of about 0.1 to 8 mm are preferably used. The temperature of the dispersion treatment condition is preferably in the range of 0°C to 100°C, more preferably in the range of room temperature to 80°C. As for the dispersion time, since the appropriate time varies depending on the composition of the dispersion liquid and the size of the dispersion treatment device, it is appropriately adjusted. The standard of dispersion is: the gloss of the ink is controlled so that the 20-degree specular gloss (JIS Z8741) of the photosensitive resin composition is in the range of 100 to 200. When the gloss of the photosensitive resin composition is low, most of the dispersion treatment is insufficient, and coarse pigment (coloring material) particles remain, and there is a possibility of insufficient developability, adhesion, resolution, etc. In addition, if the dispersion treatment is carried out until the gloss value exceeds the above range, the pigment is broken and a large number of ultrafine particles are produced, which tends to impair the dispersion stability.

[0371] From the viewpoint of the surface smoothness of the cured product, the pigment dispersion of the present invention is preferably prepared by preliminarily preparing a (C) sulfonic acid group-containing compound dispersion in which the (C) sulfonic acid group-containing compound is dispersed in a solvent, and then mixing the liquid with the (A) pigment and the (B) dispersant and performing a dispersion treatment. When preparing the (C) sulfonic acid group-containing compound dispersion, the content ratio of each component is adjusted so as to fall within the above-described ratio. In addition, it is also useful to adjust the treatment time and select the bead diameter as described above.

[0372] <Method for producing photosensitive resin composition>

[0373] The photosensitive resin composition of the present invention is manufactured by a conventional method, for example, by mixing the ink obtained by the above-mentioned dispersion treatment with other components contained in the photosensitive resin composition to prepare a uniform solution. In the manufacturing process of the photosensitive resin composition, fine garbage is often mixed into the liquid, so it is desirable to filter the obtained photosensitive resin composition using a filter or the like.

[0374] [cured material]

[0375] The cured product of the present invention is obtained by curing the photosensitive resin composition of the present invention. The cured product of the present invention can be suitably used as a member constituting a color filter such as a pixel, a black matrix, or a color spacer.

[0376] [Black Matrix]

[0377] The black matrix of the present invention includes the cured product of the present invention.

[0378] Hereinafter, the black matrix of the present invention will be described according to its production method.

[0379] (1) Support

[0380] As a support for forming a black matrix, as long as it has appropriate strength, its material is not particularly limited. A transparent substrate is mainly used, and as a material, for example, polyester resins such as polyethylene terephthalate, polyolefin resins such as polypropylene and polyethylene, thermoplastic resin films such as polycarbonate, polymethyl methacrylate, and polysulfone, epoxy resins, unsaturated polyester resins, poly (meth) acrylic resins, and other thermosetting resin sheets, or various glasses can be listed.

[0381] Among them, glass and heat-resistant resin are preferred from the viewpoint of heat resistance. In addition, transparent electrodes such as ITO and IZO are sometimes formed on the surface of the substrate. In addition to the transparent substrate, it can also be formed on the TFT array.

[0382] To improve surface properties such as adhesiveness, the support may be subjected to corona discharge treatment, ozone treatment, atmospheric pressure plasma treatment, or thin film formation treatment using a silane coupling agent, urethane resin, or other resin, as necessary.

[0383] The thickness of the transparent substrate is preferably 0.05 to 10 mm, more preferably 0.1 to 7 mm. When a thin film of various resins is formed, the film thickness is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm.

[0384] (2) Black Matrix

[0385] When forming a black matrix using the photosensitive resin composition of the present invention, the photosensitive resin composition is applied to a transparent substrate and dried, and then a photomask is placed on the sample to perform image exposure through the photomask, development, and, if necessary, thermal curing or photocuring to form a black matrix.

[0386] (3) Formation of black matrix

[0387] (3-1) Application of photosensitive resin composition

[0388] The photosensitive resin composition for black matrix can be applied to the transparent substrate by spin coating, wire bar coating, flow coating, die coating, roller coating, or spray coating, etc. Among them, die coating is preferred from the comprehensive viewpoints of greatly reducing the amount of coating liquid, completely eliminating the influence of mist attached in the case of spin coating, and suppressing the generation of foreign matter.

[0389] The thickness of the coating film is preferably 0.2 to 10 μm, more preferably 0.5 to 6 μm, and further preferably 1 to 4 μm in terms of the film thickness after drying. By setting the thickness below the upper limit, pattern development tends to be easier and gap adjustment in the liquid crystal cell process tends to be easier. By setting the thickness above the lower limit, desired color expression tends to be easier.

[0390] (3-2) Drying of coating film

[0391] The drying of the coating film after applying the photosensitive resin composition on the substrate is preferably carried out by a reduced pressure drying method using a vacuum drying device and a heating drying method using a hot plate, an IR oven, or a convection oven. In the case of a heating drying method using a hot plate, the back of the substrate is sometimes supported by pins. The conditions for heating and drying can be appropriately selected according to the type of the aforementioned solvent component, the performance of the dryer used, etc. The drying time is preferably 15 seconds to 5 minutes at a temperature of 40 to 200°C, and more preferably 30 seconds to 3 minutes at a temperature of 50 to 130°C, depending on the type of the solvent component, the performance of the dryer used, etc.

[0392] The higher the drying temperature, the more the adhesion of the coating to the transparent substrate improves. If it is below the above upper limit, it is not easy to cause the alkali-soluble resin to decompose and initiate the poor development caused by thermal polymerization. In addition, if the drying is carried out uniformly, the film thickness easily becomes uniform and is not easy to produce unevenness.

[0393] (3-3) Exposure

[0394] For image exposure, a negative mask pattern is superimposed on the coating of the photosensitive resin composition, and light of a wavelength from the ultraviolet region to the visible region is irradiated through the mask pattern. At this time, as required, in order to prevent the sensitivity of the photopolymerizable layer from being reduced due to oxygen, an oxygen blocking layer such as a polyvinyl alcohol layer can be formed on the photopolymerizable coating before exposure. The light source used in the above-mentioned image exposure is not particularly limited. As the light source, for example, a xenon lamp, a halogen lamp, a tungsten lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp, a carbon arc, and the like can be cited. When irradiating light of a specific wavelength and using it, a filter can also be used.

[0395] (3-4) Development

[0396] The black matrix of the present invention can be prepared as follows: after the coating film based on the photosensitive resin composition is image-exposed using the above-mentioned light source, an image is formed on the substrate by developing using an organic solvent or an aqueous solution containing a surfactant and an alkaline compound. The aqueous solution may further contain an organic solvent, a buffer, a complexing agent, a dye or a pigment.

[0397] Examples of the alkaline compound include inorganic alkaline compounds such as sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium silicate, potassium silicate, sodium metasilicate, sodium phosphate, potassium phosphate, sodium hydrogen phosphate, potassium hydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, and ammonium hydroxide; and organic alkaline compounds such as monoethanolamine, diethanolamine, or triethanolamine, monomethylamine, dimethylamine, or trimethylamine, monoethylamine, diethylamine, or triethylamine, monoisopropylamine, or diisopropylamine, n-butylamine, monoisopropanolamine, diisopropanolamine, or triisopropanolamine, ethyleneimine, ethylenediamine, tetramethylammonium hydroxide (TMAH), and choline.

[0398] The basic compound may be used alone or in combination of two or more.

[0399] Examples of the surfactant include nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl aryl ethers, polyoxyethylene alkyl esters, sorbitan alkyl esters, and monoglyceride alkyl esters; anionic surfactants such as alkylbenzene sulfonates, alkylnaphthalene sulfonates, alkyl sulfates, alkyl sulfonates, and sulfosuccinate salts; and amphoteric surfactants such as alkyl betaines and amino acids.

[0400] The surfactant may be used alone or in combination of two or more.

[0401] Examples of the organic solvent include isopropyl alcohol, benzyl alcohol, ethyl cellosolve, butyl cellosolve, phenyl cellosolve, propylene glycol, and diacetone alcohol. The organic solvent may be used in combination with an aqueous solution.

[0402] The organic solvent may be used alone or in combination of two or more.

[0403] The conditions for the development treatment are not particularly limited, but the development temperature is preferably 10 to 50° C., more preferably 15 to 45° C., and further preferably 20 to 40° C. The development method may be, for example, immersion development, spray development, brush development, or ultrasonic development.

[0404] (3-5) Thermal curing treatment

[0405] The developed substrate is subjected to a heat curing treatment or a photocuring treatment, preferably a heat curing treatment, wherein the heat curing treatment conditions are selected from a temperature in the range of 100 to 280° C., preferably 150 to 250° C., and a time in the range of 5 to 60 minutes.

[0406] The height of the black matrix formed in this way is preferably 0.5 to 5 μm, more preferably 0.8 to 4 μm.

[0407] [Formation of other color filters]

[0408] On a transparent substrate provided with a black matrix, a photosensitive resin composition containing a coloring material of one color among red, green, and blue is applied and dried by the same process as (3-1) to (3-5) above, and a photomask is overlapped on the coating film. Through the photomask, a pixel image is formed by image exposure, development, and thermal curing or photocuring as required to produce a coloring layer. The photosensitive resin compositions of the three colors of red, green, and blue are respectively subjected to this operation, thereby forming a color filter. Their order is not limited to the above.

[0409] [Coloring spacer]

[0410] The photosensitive resin composition of the present invention can be used as a photosensitive resin composition for coloring spacers in addition to the black matrix. When the spacer is used for a TFT-type LCD, sometimes the TFT as a switching element causes malfunction due to light incident on the TFT, and the coloring spacer is used to prevent this situation. For example, Japanese Patent Publication No. 8-234212 records that the spacer is light-shielding. The coloring spacer can be formed by the same method as the above-mentioned black matrix except that a mask for the coloring spacer is used.

[0411] (3-6) Formation of transparent electrode

[0412] The color filter can be used as a part of a component such as a color display or a liquid crystal display device by forming a transparent electrode such as ITO on the image in its original state. In order to improve the surface smoothness and durability, a top coating of polyamide, polyimide, etc. can also be provided on the image as needed. In addition, in some uses such as a planar alignment drive mode (IPS mode), a transparent electrode may not be formed.

[0413] [Image display device]

[0414] The image display device of the present invention comprises the cured product of the present invention. The image display device of the present invention is not particularly limited as long as it is a device that displays images or videos, and examples thereof include liquid crystal display devices and organic EL displays described below.

[0415] [Liquid crystal display device]

[0416] The liquid crystal display device of the present invention comprises the cured product of the present invention, particularly the black matrix of the present invention, and the formation order and formation position of the color pixels and the black matrix are not particularly limited.

[0417] Liquid crystal display devices are usually completed as follows: an alignment film is formed on a color filter, a spacer is dispersed on the alignment film, and then a liquid crystal cell is formed by bonding with an opposing substrate, and a liquid crystal is injected into the formed liquid crystal cell, and connected to an opposing electrode. As an alignment film, a resin film such as polyimide is suitable. In the formation of the alignment film, a gravure printing method and / or a flexible printing method are usually used, and the thickness of the alignment film is set to several 10nm. After the alignment film is cured by thermal sintering, a surface treatment is performed by irradiation of ultraviolet rays and a treatment based on a brushing cloth to be processed into a surface state that can adjust the tilt of the liquid crystal.

[0418] As a spacer, an object that matches the size of the gap with the opposing substrate is used, and a spacer of 2 to 8 μm is usually suitable. A photolithography spacer (PS) of a transparent resin film can also be formed on the color filter substrate by photolithography and used as a substitute for the spacer. As an opposing substrate, an array substrate is usually used, and a TFT (thin film transistor) substrate is particularly suitable.

[0419] The gap between the substrate and the opposing substrate varies depending on the purpose of the liquid crystal display device, and is preferably selected within the range of 2 to 8 μm. After bonding to the opposing substrate, the portion other than the liquid crystal injection port is sealed with a sealing material such as epoxy resin. The sealing material is cured by UV irradiation and / or heating to seal the periphery of the liquid crystal unit.

[0420] After the sealed liquid crystal cell is cut into unit panels, the vacuum chamber is set to a reduced pressure, the liquid crystal injection port is immersed in liquid crystal, and the cavity is leaked to inject liquid crystal into the liquid crystal cell. The reduced pressure in the liquid crystal cell is preferably 1×10 -7 ~1×10 -2 Pa, more preferably 1×10 -6 ~1×10 -3 Pa. In addition, the liquid crystal cell is preferably heated during decompression, and the heating temperature is preferably 30 to 100° C., more preferably 50 to 90° C. The heating during decompression is preferably maintained in the range of 10 to 60 minutes, and then immersed in liquid crystal. The liquid crystal cell injected with liquid crystal is sealed by curing the UV curable resin to complete the liquid crystal display device (panel).

[0421] The type of liquid crystal is not particularly limited, and may be any known liquid crystal such as aromatic, aliphatic, or polycyclic compounds, lyotropic, or thermotropic. Among thermotropic liquid crystals, nematic, smectic, and cholesteric liquid crystals are known, and any of them may be used.

[0422] [Organic EL display]

[0423] The organic EL display of the present invention is produced using the color filter of the present invention.

[0424] When an organic EL display is produced using the color filter of the present invention, for example Figure 1 As shown, first, a color filter is prepared by forming a pattern formed of a photosensitive resin composition on a transparent supporting substrate 10 (i.e., pixels 20 and a resin black matrix (not shown) provided between adjacent pixels 20), and an organic light emitting body 500 is stacked on the color filter via an organic protective layer 30 and an inorganic oxide film 40, thereby preparing an organic EL element 100. It should be noted that at least one of the pixels 20 and the resin black matrix is ​​prepared using the photosensitive resin composition of the present invention.

[0425] As a lamination method of the organic light emitting body 500, there are listed: a method of sequentially forming a transparent anode 50, a hole injection layer 51, a hole transport layer 52, a light emitting layer 53, an electron injection layer 54 and a cathode 55 on the upper surface of the color filter; a method of laminating the organic light emitting body 500 formed on another substrate on the inorganic oxide film 40, etc. Using the organic EL element 100 thus produced, an organic EL display can be produced, for example, by the method described in "Organic EL Display" (Ohmsha, Ltd., published on August 20, 2004, written by Shizuo Tokito, Chiba Ya Adachi, and Hideyuki Murata).

[0426] It should be noted that the color filter of the present invention can be applied to both passively driven organic EL displays and actively driven organic EL displays.

[0427] Example

[0428] Next, the present invention will be described in more detail with reference to synthesis examples, examples and comparative examples. However, the present invention is not limited to the following examples unless the gist of the invention is exceeded.

[0429] <Synthesis Example: Synthesis of Alkali-Soluble Resin>

[0430]

[0431] 240 parts by mass of the epoxy compound (epoxy equivalent 264) of the above structure, 81.6 parts by mass of methacrylic acid, 263.1 parts by mass of methoxybutyl acetate, 6.4 parts by mass of triphenylphosphine and 0.16 parts by mass of p-methoxyphenol were placed in a flask equipped with a thermometer, a stirrer and a condenser, and reacted at 90° C. for 12 hours while stirring until the acid value was 5 mgKOH / g or less.

[0432] Next, in a flask equipped with a thermometer, a stirrer and a condenser, 8.3 parts by mass of trimethylolpropane (TMP), 80.7 parts by mass of biphenyltetracarboxylic dianhydride (BPDA) and 51.6 parts by mass of tetrahydrophthalic anhydride (THPA) were added to the reaction solution obtained by the above reaction, and the temperature was slowly raised to 105°C while stirring to carry out a reaction, thereby obtaining an alkali-soluble resin having a solid acid value of 112 mgKOH / g and a weight average molecular weight (Mw) of 2500 in terms of polystyrene measured by GPC.

[0433] The constituent components of the pigment dispersion and the photosensitive resin composition used in the following Examples and Comparative Examples are as follows.

[0434] <Pigment-1>

[0435] R1060: Birla Carbon "RAVEN1060" (carbon black)

[0436] <Dispersant-1>

[0437] BYK167: BYK-Chemie "DISPERBYK-167" (urethane polymer dispersant)

[0438] <Sulfonic acid group-containing compound-1>

[0439] S12000-S: Lubrizol "S12000-S" (copper phthalocyanine sulfonate derivative)

[0440] <Sulfonic acid group-containing compound dispersion-1>

[0441] For a mixed solution in which sulfonic acid group-containing compound-1 is added to propylene glycol monomethyl ether acetate, use The zirconium oxide beads were dispersed using a paint stirrer, and the beads were separated from the dispersion using a filter to prepare a sulfonic acid group-containing compound dispersion-1.

[0442] <Alkali soluble resin-1>

[0443] Alkali-soluble resin-1: Resin obtained in the above synthesis example

[0444] <Photopolymerizable compound-1>

[0445] DPHA: "KAYARAD DPHA" (multifunctional acrylate) manufactured by Nippon Kayaku Co., Ltd.

[0446] <Photopolymerization Initiator-1>

[0447] TR-PBG-304: "TR-PBG-304" manufactured by Changzhou Qiangli Electronic New Materials Co., Ltd. (oxime ester compound with carbazole skeleton)

[0448] <Additive-1>

[0449] X-12-1048: Shin-Etsu Chemical Co., Ltd. "X-12-1048" (multifunctional acrylic silane)

[0450] <Surfactant-1>

[0451] F-554: DIC Corporation "MEGAFACE F554" (fluorine-based surfactant)

[0452] <Solvent>

[0453] PGMEA: Propylene glycol monomethyl ether acetate

[0454] <Preparation of Dispersions 1 to 3>

[0455] [Example 1, Comparative Example 1, Reference Example 1]

[0456] The pigment-1, dispersant-1, sulfonic acid group-containing compound dispersion-1, sulfonic acid group-containing compound-1 and solvent described in Table 1 were mixed at the mass ratio described in Table 1 to obtain a mixed solution.

[0457] Specifically, in dispersion 1, the sulfonic acid group-containing compound dispersion 1 prepared in advance, pigment 1, and solvent were mixed in the mass ratio described in Table 1 to obtain a mixed solution, and in dispersions 2 and 3, the sulfonic acid group-containing compound 1, pigment 1, and solvent were mixed in the mass ratio described in Table 1 to obtain a mixed solution.

[0458] In addition, the mixing ratio of the solvent in Table 1 also includes the amount of the solvent derived from the dispersant.

[0459] The obtained mixed solution was dispersed for 6 hours at 25 to 45°C using a paint shaker. Zirconia beads of 2.5 times the mass of the dispersion were added. After the dispersion was completed, the beads and the dispersion were separated by a filter to prepare dispersions 1 to 3.

[0460] The pigment dispersions (dispersion 1 to dispersion 3) had good initial dispersibility. However, when dispersion 3 was stored at room temperature for more than one week, a tendency to thicken was observed, indicating that the storage stability was inferior to that of dispersions 1 and 2.

[0461] It was confirmed that in the obtained dispersion liquids 1 and 2, the pigment and the sulfonic acid group-containing compound were present in the form of particles.

[0462] Evaluation was performed by the method described below using the dispersions obtained in Table 1. Table 2 shows the evaluation results.

[0463] [Table 1]

[0464]

[0465] (Evaluation of dispersion)

[0466] <Measurement of the ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50)>

[0467] The dispersion concentration was adjusted to 0.02% by mass, and a particle size analyzer (FPAR-1000 manufactured by Otsuka Electronics Co., Ltd.) was used to measure the volume-based particle size distribution by dynamic scattering method and cumulative analysis. It should be noted that the measurement results are the results of dynamic scattering method and cumulative analysis.

[0468] From the obtained measurement results, the ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) was calculated.

[0469] <Measurement of glossiness Gs>

[0470] The pigment dispersion was applied to a glass substrate by a spin coater so that the dry film thickness was 1.2 μm, and dried on a hot plate at 100° C. for 120 seconds. The glossiness Gs of the obtained coating film was measured using a HAZE-GLOSS meter manufactured by BYK Gardner.

[0471] <Measurement of Glossiness Gd>

[0472] The pigment dispersion was applied on a glass substrate by a spin coater so as to have a dry film thickness of 1.2 μm, and dried on a hot plate at 100° C. for 120 seconds. The glossiness Gd of the obtained coating film was measured using a HAZE-GLOSS meter manufactured by BYK Gardner.

[0473] [Table 2]

[0474]

[0475] <Preparation of Photosensitive Resin Composition>

[0476] [Example 2, Comparative Example 2, Reference Example 2]

[0477] Using the dispersions 1 to 3 prepared above, each component was added in such a manner that the solid content ratio of each component in the total solid content of the photosensitive resin composition became the blending ratio of Table 3, and propylene glycol monomethyl ether acetate (PGMEA), 3-methoxybutyl acetate (MBA) and diethylene glycol monoethyl ether acetate (DGMEA) were added in such a manner that the content ratio of the total solid content of the photosensitive resin composition became 14% by mass, and the ratio of PGMEA / MBA / DGMEA in the solvent became 68 / 30 / 2% by mass, and stirred and dissolved to prepare photosensitive resin compositions 1 to 3 (compositions 1 to 3). Using each of the obtained photosensitive resin compositions, evaluation was performed by the method described below.

[0478] [Table 3]

[0479]

[0480] (Evaluation of Photosensitive Resin Composition)

[0481] <Measurement of surface roughness (arithmetic mean surface roughness (Sa))>

[0482] The photosensitive resin composition was applied on a glass substrate by a spin coater so that the film thickness after heat curing was 1.2 μm, and dried under reduced pressure at 100 Pa for 60 seconds, and then dried on a hot plate at 100° C. for 120 seconds. The obtained coating film was heat cured at 230° C. for 25 minutes (post-baking) to prepare a substrate for surface roughness evaluation.

[0483] For the aforementioned substrate for surface roughness evaluation, a scanning white interference microscope (VS1530 manufactured by HITACHI Corporation) was used to measure the surface roughness (arithmetic mean surface roughness (Sa)). Specifically, the arithmetic mean surface roughness (Sa) of the surface in the range of 10 μm × 10 μm of the substrate obtained by measuring the above-mentioned scanning white interference microscope was evaluated according to the following benchmarks. It should be noted that the measurement mode is the Focus mode, the magnification of the objective lens is 50 times, and the central wavelength of the measurement light is 520 nm. Sa is the value obtained by dividing the volume of the portion surrounded by the surface shape curved surface and the average surface by the measurement area, and the smaller the value, the higher the smoothness.

[0484] If the surface roughness is 5 nm or less, there is no problem in practical use.

[0485] From the comparison between Example 2 and Comparative Example 2 in Table 3, it can be seen that when (D 90 / D 50) in the pigment dispersion is 1.4 or less, the glossiness Gs in the dried coating film of the dispersion is 100 or less, or the glossiness Gd in the dried coating film of the dispersion is 170 or more, the surface roughness of the cured film of the photosensitive resin composition obtained as a result is low.

[0486] In addition, from the comparison between Example 2 and Reference Example 2, it can be confirmed that when (D90 / D50) in the pigment dispersion is 1.4 or less, the glossiness Gs in the dried coating film of the dispersion is 100 or less, or the glossiness Gd in the dried coating film of the dispersion is 170 or more, the cured film of the obtained photosensitive resin composition can maintain the same surface smoothness as that of the cured film without compounding the sulfonic acid group-containing compound (C).

[0487] Description of Reference Numerals

[0488] 10 Transparent support substrate

[0489] 20 pixels

[0490] 30 Organic protective layer

[0491] 40 Inorganic oxide film

[0492] 50 Transparent Anode

[0493] 51 Hole injection layer

[0494] 52 Hole transport layer

[0495] 53 Luminous layer

[0496] 54 Electron injection layer

[0497] 55 cathode

[0498] 100 organic EL components

[0499] 500 organic light emitting bodies

Claims

1. A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent, In the pigment dispersion, the (A) pigment and the (C) sulfonic acid group-containing compound are present in the form of particles. The ratio (D90 / D50) of the 90% cumulative particle size (D90) to the 50% cumulative particle size (D50) in the volume-based particle size distribution measurement results measured by a dynamic scattering method and cumulatively analyzed is 1.4 or less.

2. A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent, In a dry coating film having a thickness of 1.2 μm obtained by applying the pigment dispersion, the glossiness Gs defined by ISO 2813 in the ranges of 18.2±0.9° and 21.8±0.9° with respect to incident light at -20° was 100 or less.

3. A pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent, In a dry coating film having a film thickness of 1.2 μm obtained by applying the pigment dispersion, the glossiness Gd defined by ISO 2813 in the range of 20±0.9° with respect to incident light at -20° is 170 or more.

4. The pigment dispersion according to any one of claims 1 to 3, wherein The (C) sulfonic acid group-containing compound is at least one selected from the group consisting of sulfonic acid derivatives of phthalocyanine, sulfonic acid derivatives of quinophthalone, sulfonic acid derivatives of anthraquinone, sulfonic acid derivatives of quinacridone, sulfonic acid derivatives of diketopyrrolopyrrole and sulfonic acid derivatives of dioxazine.

5. The pigment dispersion according to any one of claims 1 to 3, wherein The (C) sulfonic acid group-containing compound is a copper phthalocyanine sulfonate derivative.

6. The pigment dispersion according to any one of claims 1 to 5, wherein The (C) sulfonic acid group-containing compound has an acid value of 80 mgKOH / g or more.

7. The pigment dispersion according to any one of claims 1 to 6, wherein The content ratio of the (A) pigment to the (C) sulfonic acid group-containing compound ((A) pigment / (C) sulfonic acid group-containing compound) on a mass basis is 10 or more.

8. The pigment dispersion according to any one of claims 1 to 7, wherein The content ratio of the (A) pigment to the (B) dispersant ((A) pigment / (B) dispersant) on a mass basis is 4 or more.

9. The pigment dispersion according to any one of claims 1 to 8, wherein The (A) pigment contains carbon black. 10 . A photosensitive resin composition comprising the pigment dispersion according to claim 1 . 11 . A cured product obtained by curing the photosensitive resin composition according to claim 10 . 12 . A black matrix comprising the cured product according to claim 11 .

13. An image display device comprising the cured product according to claim 11.

14. A method for producing a pigment dispersion, the pigment dispersion comprising (A) a pigment, (B) a dispersant, (C) a sulfonic acid group-containing compound and a solvent, The manufacturing method comprises the following steps (1) and (2): Step (1): a step of mixing and dispersing the sulfonic acid group-containing compound (C) with a solvent; Step (2): A step of mixing and dispersing the (C) sulfonic acid group-containing compound dispersion obtained in step (1), the (A) pigment and the (B) dispersant.

Citation Information

Patent Citations

  • Toner, image forming method using said toner and processing cartridge

    CN1452021A

  • Makeup cosmetic

    JP2003012461A

  • Aqueous pigment dispersion for inkjet ink, and aqueous pigment ink for inkjet printer

    JP2012021120A

  • Ink, ink container, inkjet recording method and inkjet recording device

    JP2017165961A

  • Pigment dispersion, and coloring composition for film formation

    JP2020147632A