Adhesive film, and metal terminal and secondary battery using same

By using a resin laminate structure in the adhesive film, combining a modified polyolefin resin and a thermoplastic elastomer, the problem of low design freedom when bonding metals is solved, and firm bonding and high strength are achieved Performance of metal terminals and secondary battery sealing effect.

CN118891336APending Publication Date: 2024-11-01FUJIMORI KOGYO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380026277.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, acid-modified polyolefin resin has low design freedom when bonding to adhere to adhered metals, etc., and insufficient stress relief during peeling, resulting in poor bonding performance.

Method used

The adhesive film with a resin laminate structure includes a modified polyolefin resin layer and an adjacent layer modified with functional groups on at least one surface. The thickness of the adhesive resin layer is less than 10 μm and the tensile elastic modulus of the adjacent layer is 1000MPa. The following is the unsaturated carboxylic acid component in 100 parts by weight of the modified polyolefin resin, and the thermoplastic elastomer resin is combined to improve design freedom and bonding properties.

Benefits of technology

Firm bonding to the adherend is achieved, the design freedom is improved, and the water vapor permeability and cost are reduced, and the performance of the adhesive film is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891336A_ABST
    Figure CN118891336A_ABST
Patent Text Reader

Abstract

The invention provides an adhesive film (10), and a metal terminal and a secondary battery using the adhesive film. The adhesive film (10) is formed from a laminate of a resin. The adhesive film (10) contains, on at least one surface of the adhesive film (10), a modified polyolefin resin modified with a functional group that forms a chemical bond with an adherend. And an adjacent layer (12) that is adjacent to the adhesive resin layer (11) and contains a polyolefin resin, the adhesive resin layer (11) having a thickness of less than 10 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film, and a metal terminal and a secondary battery using the adhesive film.

[0002] This application claims priority based on Japanese Patent Application No. 2022-051603 filed in Japan on March 28, 2022, and the contents are incorporated herein by reference. Background Art

[0003] Conventionally, acid-modified polyolefin resins are known as materials having excellent adhesion to adherends such as metals.

[0004] Patent Document 1 describes a multilayer sealant film in which at least one of the skin layers on both sides of a core layer is composed of polypropylene modified with an unsaturated carboxylic acid or the like.

[0005] Patent Document 2 describes an adhesive film for a metal terminal in which at least one of the polyolefin resin layers on both surfaces of a substrate is formed of an acid-modified polyolefin.

[0006] Patent Document 3 describes an adhesive film for a metal terminal including at least one polypropylene layer and at least one acid-modified polypropylene layer.

[0007] Prior art literature Patent Literature Patent Document 1: International Publication No. 2021 / 100226 Patent Document 2: Japanese Patent Application Publication No. 2017-139120 Patent Document 3: International Publication No. 2018 / 110702 Summary of the invention

[0008] Technical issues Acid-modified polyolefin resins have functional groups that can form chemical bonds with adherends such as metals, so the adhesive resin needs to be in contact with and in close contact with the adherend. In order to provide sealing performance to the adherend and to relieve stress during peeling, the thickness of the adhesive resin needs to be sufficiently ensured, which results in a low degree of design freedom.

[0009] For example, in Examples 1 to 6 of Patent Document 1, the thickness of the acid-modified propylene random copolymer is set to 30 to 50 μm. In Examples 1 to 3 of Patent Document 2, the thickness of the maleic acid-modified polypropylene is set to 37.5 μm. In Examples 1 to 7 of Patent Document 3, the thickness of the acid-modified polypropylene is set to 16 to 36 μm. In addition, in paragraph 0054 of Patent Document 3, it is suggested that the thickness of the acid-modified polypropylene is preferably about 10 μm or more.

[0010] The present invention has been made in view of the above circumstances, and an object thereof is to provide an adhesive film that can form a chemical bond with an adherend to achieve strong adhesion and has a high degree of design freedom, and a metal terminal and a secondary battery using the adhesive film.

[0011] Technical Solution The first embodiment of the present invention is an adhesive film, which is an adhesive film formed by a resin stack, and the adhesive film has: an adhesive resin layer, which contains a modified polyolefin resin modified with a functional group that forms a chemical bond with an adherend on at least one surface of the adhesive film; and an adjacent layer, which is adjacent to the adhesive resin layer and contains a polyolefin resin, and the thickness of the adhesive resin layer is less than 10μm.

[0012] A second aspect of the present invention is the first aspect, wherein the adjacent layer has a tensile elastic modulus of 1000 MPa or less.

[0013] A third aspect of the present invention is the first aspect or the second aspect, wherein a ratio B / A of a thickness A of the adhesive resin layer to a thickness B of the adjacent layer is 1-20.

[0014] A fourth aspect of the present invention is any one of the first to third aspects, wherein the modified polyolefin resin is an acid-modified polyolefin resin.

[0015] A fifth aspect of the present invention is the fourth aspect, wherein the acid-modified polyolefin resin is a resin obtained by modifying a random copolymer of polypropylene or polyethylene.

[0016] A sixth aspect of the present invention is any one of the first to fifth aspects, wherein the polyolefin resin of the adjacent layer is a random copolymer of unmodified polypropylene or unmodified polyethylene.

[0017] A seventh aspect of the present invention is any one of the first to sixth aspects, wherein the modified polyolefin resin is modified with an unsaturated carboxylic acid component, and the unsaturated carboxylic acid component is contained in an amount of 0.01 to 2 parts by weight per 100 parts by weight of the modified polyolefin resin.

[0018] An eighth aspect of the present invention is any one of the first to seventh aspects, wherein the adhesive resin layer contains a thermoplastic elastomer resin in an amount ranging from 5 to 30 parts by weight per 100 parts by weight.

[0019] A ninth aspect of the present invention is a metal terminal for a secondary battery, and includes the adhesive film according to any one of the first to eighth aspects.

[0020] A tenth aspect of the present invention is a secondary battery including the metal terminal according to the ninth aspect.

[0021] Technical Effects According to the present invention, it is possible to provide an adhesive film that can form a chemical bond with an adherend to achieve strong adhesion and has a high degree of design freedom, and a metal terminal and a secondary battery using the adhesive film. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a cross-sectional view showing the adhesive film according to the first embodiment.

[0023] Figure 2 It is a cross-sectional view showing an adhesive film according to a second embodiment.

[0024] Figure 3 It is a cross-sectional view showing an adhesive film according to a third embodiment.

[0025] Figure 4 It is a cross-sectional view showing an adhesive film according to a fourth embodiment.

[0026] Explanation of symbols 10, 20, 30, 40 ... adhesive film, 11 ... adhesive resin layer, 12 ... adjacent layer, 13 ... core layer. DETAILED DESCRIPTION

[0027] Hereinafter, the present invention will be described based on preferred embodiments.

[0028] The adhesive film of the embodiment is formed of a resin laminate, and has an adhesive resin layer and an adjacent layer on at least one surface, wherein the adhesive resin layer includes a modified polyolefin resin modified with a functional group that forms a chemical bond with an adherend, and the adjacent layer is adjacent to the adhesive resin layer and includes a polyolefin resin. Moreover, the thickness of the adhesive resin layer is less than 10 μm.

[0029] The adhesive film of the embodiment may also be a laminate composed of an adhesive resin layer and an adjacent layer. Figure 1 The adhesive film 10 shown has an adhesive resin layer 11 on one side of an adjacent layer 12 . Figure 2 The adhesive film 20 shown has adhesive resin layers 11 on both sides of the adjacent layer 12 .

[0030] The adhesive film of the embodiment may be a laminate having a core layer in addition to the adhesive resin layer and the adjacent layer. Figure 3 The adhesive film 30 shown has an adhesive resin layer 11 on one surface of a core layer 13 via an adjacent layer 12 . Figure 4 The adhesive film 40 shown has adhesive resin layers 11 on both surfaces of a core layer 13 via adjacent layers 12 .

[0031] The adhesive resin layer 11 is disposed on at least one surface of the adhesive film 10, 20, 30, 40 and is a layer in contact with and in close contact with an adherend (not shown). The adhesive resin layer 11 includes a modified polyolefin resin modified with a functional group that forms a chemical bond with the adherend. Since the modified polyolefin resin has high adhesiveness, it is an essential component for imparting adhesiveness to the adhesive resin layer 11.

[0032] Examples of the modified polyolefin resin used for the adhesive resin layer 11 include one or two or more of acid-modified polyolefin resins, hydroxy-modified polyolefin resins, chlorinated polyolefin resins, and epoxy-modified polyolefin resins.

[0033] Among the modified polyolefin resins, acid-modified polyolefin resins modified with unsaturated carboxylic acid components are preferred. The modified polyolefin resin of the adhesive resin layer 11 preferably contains 0.01 to 2 parts by weight of the unsaturated carboxylic acid component per 100 parts by weight of the modified polyolefin resin.

[0034] The content of the unsaturated carboxylic acid component contained in the modified polyolefin resin can be obtained from the amount of the acid functional group-containing monomer used in the production process of the acid-modified polyolefin resin, or from the amount of the acid contained in the modified polyolefin resin. The method for determining the amount of the acid contained in the modified polyolefin resin is not particularly limited, and for example, it may be titration using a base such as potassium hydroxide (KOH), or the acid functional group may be methylated and quantified using NMR or the like.

[0035] As a use 1 The method of quantitatively measuring the content of the acid component contained in the resin by H-NMR includes, for example, the following method: using a sample of a modified resin such as modified PP to perform 1 H-NMR measurement, and methyl esterification of unsaturated carboxylic acid sites such as maleic acid 1 H-NMR determination, and according to 1 The grafting rate was calculated in mass % from the difference in the H peak area.

[0036] The unsaturated carboxylic acid component may be a carboxyl group-containing monomer having a free carboxyl group, or may be an acid anhydride group-containing monomer having a latent carboxyl group. Examples of carboxyl group-containing monomers include acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, tetrahydrophthalic acid, endo-bicyclo[2.2.1]-5-heptene-2,3-dicarboxylic acid (nadic acid), and other α,β-unsaturated carboxylic acid monomers. Examples of acid anhydride group-containing monomers include unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, nadic anhydride, itaconic anhydride, citraconic anhydride, and nadic anhydride. The modified polyolefin resin may be a resin obtained by copolymerizing one unsaturated carboxylic acid component, or may be a resin obtained by copolymerizing two or more unsaturated carboxylic acid components.

[0037] Examples of the method for producing the modified polyolefin resin include a method of graft-modifying an unmodified polyolefin resin with a monomer having a functional group by melt kneading, and a method of copolymerizing an olefin monomer with a monomer having a functional group.

[0038] Functional group-containing monomers are monomers having polar functional groups other than olefins, and specific examples thereof include unsaturated carboxylic acid components, hydroxyl group-containing olefins, chlorinated olefins, epoxy group-containing olefins, etc. These functional group-containing olefins may be (meth) alkyl acrylate monomers having functional groups.

[0039] Examples of the polar functional group of the functional group-containing monomer include a carboxylic acid group, a carboxylic anhydride group, a hydroxyl group, a chlorine atom, an epoxy group, etc. These functional groups can serve as functional groups that form a chemical bond with an adherend.

[0040] As at least a part of the modified polyolefin resin, an acid-modified polyolefin resin obtained by graft-modification of an unsaturated carboxylic acid component using a radical polymerization initiator can be used. Examples of the radical polymerization initiator include organic peroxides and aliphatic azo compounds.

[0041] Examples of the olefin monomer used in the modified polyolefin resin include one or more of ethylene, propylene, 1-butene, isobutylene, 1-hexene, 1-octene, α-olefins, etc. The modified polyolefin resin may be a metallocene-based resin polymerized using a metallocene catalyst.

[0042] The modified polyolefin resin may be a modified polyethylene resin, a modified polypropylene resin, a modified poly-1-butene resin, a modified polyisobutylene resin, etc. As unmodified polyolefin resins used in the graft modification of modified polyolefins, polyethylene, polypropylene, poly-1-butene, polyisobutylene, random copolymers of propylene and ethylene or α-olefins, block copolymers of propylene and ethylene or α-olefins, etc. may be cited.

[0043] The modified polyethylene resin preferably used for the adhesive resin layer 11 is a resin obtained by copolymerizing 50 parts by weight or more of ethylene in 100 parts by weight of the modified polyethylene resin. The modified polyethylene resin is copolymerized with a functional group-containing monomer such as an unsaturated carboxylic acid component. In addition, in the modified polyethylene resin, as an olefin monomer other than ethylene, propylene, 1-butene, 1-hexene, 1-octene, etc. can be copolymerized.

[0044] The modified polypropylene resin preferably used for the adhesive resin layer 11 is a resin obtained by copolymerizing 50 parts by weight or more of propylene in 100 parts by weight of the modified polypropylene resin. The modified polypropylene resin is copolymerized with a functional group-containing monomer such as an unsaturated carboxylic acid component. In addition, in the modified polypropylene resin, as an olefin monomer other than propylene, ethylene, 1-butene, 1-hexene, 1-octene, etc. can be copolymerized.

[0045] In the adhesive films 10, 20, 30, and 40 of the embodiments, the thickness of the adhesive resin layer 11 is less than 10 μm. This allows the physical properties of the adjacent layer 12 to affect the adherend, thereby increasing the degree of freedom in design.

[0046] In addition, although modified polyolefin resins such as acid-modified polyolefin resins used for the adhesive resin layer 11 are more expensive than polyolefin resins, cost reduction can be achieved by reducing the amount of modified polyolefin resin used.

[0047] Furthermore, by reducing the proportion of the acid-modified polyolefin resin (resin with high polarity) used in the adhesive resin layer 11 and lowering the water vapor permeability of the adhesive films 10 , 20 , 30 , and 40 , the water vapor barrier properties can be improved.

[0048] The adjacent layer 12 is a resin layer adjacent to the adhesive resin layer 11 and contains a polyolefin resin. The polyolefin resin of the adjacent layer 12 is preferably a polyolefin resin that is not modified with a polar functional group such as a carboxylic acid (unmodified polyolefin resin).

[0049] The polyolefin resin of the adjacent layer 12 can be polyethylene resin, polypropylene resin, poly-1-butene resin, polyisobutylene resin, etc. Specifically, as the polyolefin resin, polyethylene, polypropylene, poly-1-butene, polyisobutylene, random copolymers of propylene and ethylene or α-olefin, block copolymers of propylene and ethylene or α-olefin, etc. can be listed. From the viewpoint of low cost, polyethylene resin, polypropylene resin, etc. are also preferred.

[0050] Examples of the olefin monomer of the polyolefin resin used in the adjacent layer 12 include one or more of ethylene, propylene, 1-butene, isobutylene, 1-hexene, 1-octene, α-olefins, etc. The polyolefin resin may be a metallocene-based resin polymerized using a metallocene catalyst.

[0051] Adjacent layer 12 preferably relaxes stress and suppresses the reduction of bonding strength from the state of having adherend pasted adhesive film 10,20,30,40 to the direction action external force of peeling adhesive film 10,20,30,40.Therefore, preferably adjacent layer 12 contains soft polyolefin resin.Specifically, the tensile elastic modulus of adjacent layer 12 is preferably below 1000MPa.In order to reduce the tensile elastic modulus of adjacent layer 12, preferably use the polyolefin resin with low tensile elastic modulus of resin monomer.

[0052] The adjacent layer 12 preferably has a thickness greater than that of the adhesive resin layer 11. When the thickness of the adhesive resin layer 11 is represented by A and the thickness of the adjacent layer 12 is represented by B, the ratio B / A is preferably 1-20.

[0053] The acid-modified polyolefin resin of the adhesive resin layer 11 is preferably a resin obtained by modifying a random copolymer of polypropylene or polyethylene. In addition, the polyolefin resin of the adjacent layer 12 is preferably a random copolymer of unmodified polypropylene or unmodified polyethylene. The random copolymer of polypropylene (random polypropylene) has a large amount of amorphous parts due to copolymerization of comonomers such as ethylene, and has excellent flexibility like polyethylene.

[0054] Random polypropylene may be used in both the adhesive resin layer 11 and the adjacent layer 12. In addition, polyethylene may be used in both the adhesive resin layer 11 and the adjacent layer 12. In addition, random polypropylene may be used in either the adhesive resin layer 11 or the adjacent layer 12, and polyethylene may be used in the other. In these cases, a modified resin may be used in the adhesive resin layer 11, and an unmodified resin may be used in the adjacent layer 12. Random polypropylene may be a metallocene-based resin or a resin using a catalyst other than metallocene.

[0055] The adhesive resin layer 11 preferably contains 70 parts by weight or more of the modified polyolefin resin based on 100 parts by weight of the total amount thereof. The adhesive resin layer 11 may contain 5 to 30 parts by weight of the thermoplastic elastomer resin based on 100 parts by weight of the total amount thereof.

[0056] The thermoplastic elastomer resin used for the adhesive resin layer 11 is preferably an elastomer mainly composed of a hydrocarbon monomer having high compatibility with the modified polyolefin resin, and specific examples thereof include styrene elastomers and olefin elastomers. The thermoplastic elastomer resin may be a modified elastomer resin such as an acid-modified elastomer resin.

[0057] Examples of the styrene-based elastomer include one or more of styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), styrene-isoprene-butadiene-styrene block copolymers (SIBS), styrene-ethylene-butylene-olefin crystalline block copolymers (SEBC), and hydrogenated styrene-butadiene rubber (HSBR).

[0058] Examples of olefin copolymers that can be used for the olefin elastomer include aliphatic olefin copolymers such as propylene-ethylene copolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, propylene-ethylene-1-butene copolymers, and propylene-1-butene copolymers.

[0059] The adjacent layer 12 preferably contains 70 parts by weight or more of the polyolefin resin based on 100 parts by weight of the total amount. The adjacent layer 12 may contain 5 to 30 parts by weight of the thermoplastic elastomer resin based on 100 parts by weight of the total amount.

[0060] As the thermoplastic elastomer resin used for the adjacent layer 12, an elastomer mainly composed of a hydrocarbon monomer having high compatibility with the polyolefin resin is preferred, and specific examples thereof include styrene elastomers and olefin elastomers.

[0061] When the adhesive film 30, 40 has a core layer 13, the core layer 13 is not particularly limited, but is preferably a resin layer containing a polyolefin resin. The thickness of the core layer 13 is not particularly limited, and can be designed within a range of, for example, 50 to 500 μm for the total thickness of the adhesive film 30, 40. If the core layer 13 is formed of a resin having a higher melting point than the melting points of the adhesive resin layer 11 and the adjacent layer 12, the heat resistance of the adhesive film 30, 40 is improved, which is preferred.

[0062] As the polyolefin resin of the core layer 13, polyethylene, polypropylene, poly-1-butene, polyisobutylene, random copolymers of propylene and ethylene or α-olefin, block copolymers of propylene and ethylene or α-olefin, etc. can be listed. From the viewpoint of low cost, polyethylene, polypropylene, etc. are also preferred. Among them, polypropylene is preferred because of its excellent flexibility.

[0063] Although not particularly shown, when the adhesive film 10, 30 has the adhesive resin layer 11 containing a modified polyolefin resin on one side, the adhesive film 10, 30 may have another adhesive layer on the surface opposite to the adhesive resin layer 11. The adhesive resin used for the adhesive layer other than the adhesive resin layer 11 is not particularly limited, but examples thereof include acid-modified polyolefins, epoxy-based adhesives, and olefin-based heat sealants.

[0064] For the desired purpose, each layer constituting the adhesive film 10, 20, 30, 40, i.e., the adhesive resin layer 11, the adjacent layer 12, the core layer 13, etc., may contain various additives such as antioxidants, ultraviolet absorbers, antistatic agents, lubricants, anti-blocking agents, epoxy resins, etc. Any of the adhesive resin layer 11, the adjacent layer 12, the core layer 13, etc. may be a composition that does not contain any one or more of these additives or does not contain all of them.

[0065] The method for producing the adhesive films 10 , 20 , 30 , and 40 is not particularly limited, and examples thereof include a method of forming each layer by extrusion molding, inflation molding, heat lamination, extrusion lamination, dry lamination, or the like, or a method of laminating each layer.

[0066] For example, when manufacturing an adhesive film 10 or 20 composed of an adhesive resin layer 11 and an adjacent layer 12, the adhesive resin layer 11 may be formed first, the adjacent layer 12 may be formed first, or the adhesive resin layer 11 and the adjacent layer 12 may be formed simultaneously. The method of laminating the adhesive resin layer 11 and the adjacent layer 12 in a manner adjacent to each other is not particularly limited, and for example, the adhesive resin layer 11 and the adjacent layer 12 may be adjacent to each other by coextrusion molding. The relationship between the adhesive resin layer 11 and the adjacent layer 12 when manufacturing an adhesive film 30 or 40 having a core layer 13 is also the same.

[0067] When manufacturing the adhesive film 30, 40 with the core layer 13, the layers of the adhesive resin layer 11, the adjacent layer 12, and the core layer 13 can be molded in any order, or the adhesive resin layer 11, the adjacent layer 12, and the core layer 13 can be molded simultaneously. The core layer 13 can be laminated after the adhesive resin layer 11 and the adjacent layer 12 are molded simultaneously, or the adhesive resin layer 11, the adjacent layer 12, and the core layer 13 can be laminated by coextrusion molding. It is also possible to laminate in a manner that the core layer 13 is adjacent to the adjacent layer 12. It is also possible to sandwich other layers between the core layer 13 and the adjacent layer.

[0068] When manufacturing the adhesive films 20 and 40 having the adhesive resin layers 11 on both sides, the adhesive resin layers 11 on each side may be laminated by the same method or by different methods. The adhesive resin layers 11 on both sides may be resin layers having different compositions or thicknesses or resin layers having the same composition or thickness.

[0069] The adherend of the adhesive films 10, 20, 30, 40 is not particularly limited, and various materials such as resin, rubber, metal, glass, and ceramic can be listed. Since the adhesive resin layer 11 has a modified polyolefin resin as an essential component, even if the adherend is a metal, it can be properly bonded. As metal, there is no particular limitation, and iron, copper, aluminum, stainless steel, chromium, nickel, etc. can be listed. The surface of the adherend can also be a processed surface that has been subjected to surface processing such as concave-convex processing and chemical conversion processing. The adherend can have a plane shape different from that of the adhesive films 10, 20, 30, 40.

[0070] The adherend of the adhesive films 10, 20, 30, 40 may be a metal terminal. The adhesive films 10, 20, 30, 40 may be used for sealing metal terminals. For example, in a secondary battery, the adhesive films 10, 20, 30, 40 may be used as a sealing film between a battery container and a metal terminal. The sealing film may also be formed into a long and thin strip so that its length direction is arranged along the periphery of the battery container. The metal terminal may also protrude in a direction intersecting the periphery of the battery container. The two ends of the length direction of the metal terminal are respectively arranged outside and inside the battery container.

[0071] The metal terminal has a main body made of a known metal such as aluminum, copper, nickel, iron, gold, platinum, or various alloys. The metal terminal may also have a plating layer made of a metal different from the main body on its surface. The metal terminal may have a surface treatment layer based on a chemical conversion treatment of the metal, or may have a coating layer based on a coating of a resin or the like.

[0072] As the surface treatment layer, for example, an acid-resistant coating formed using any one or more of phosphate, chromate, fluoride, triazine thiol compound, etc. can be cited. Phosphate, chromate, and fluoride can be metal salts. As the coating layer, a coating layer containing a coating agent of a resin such as a polyvinyl alcohol resin and a polyvinyl ether resin can be cited.

[0073] Examples of battery containers for secondary batteries include outer packaging containers using a laminate such as a resin film or a laminate film. The outer packaging laminate may have one or more layers of a resin substrate, a metal foil, and a sealant resin layer.

[0074] As the resin substrate of the outer packaging laminate, polyamide resins such as nylon, polyester resins such as polyethylene terephthalate (PET), polyolefin resins such as polypropylene, phenolic resins, and the like are preferable.

[0075] The metal foil of the outer packaging laminate is not particularly limited, but aluminum foil, stainless steel foil, copper foil, iron foil, and the like are preferred.

[0076] The sealant resin layer of the outer packaging laminate can be heat-fused with the sealing film. As the sealant resin of the outer packaging laminate, for example, polypropylene resins and polyethylene resins can be listed. As the polypropylene resin, homopolymers of polypropylene, copolymers of propylene and ethylene, etc. can be listed. As the polyethylene resin, low-density polyethylene, linear low-density polyethylene, etc. can be listed.

[0077] When the adhesive films 10, 20, 30, and 40 of the embodiments are used as sealing films for secondary batteries, the adhesive resin layer 11 including the modified polyolefin resin can be thermally fused to the surface of the metal terminal. When the adhesive resin layer 11 is formed on both sides of the sealing film, the adhesive resin layer 11 can also be thermally fused to the sealant resin layer of the outer packaging laminate. When the adhesive resin layer 11 is formed on one side of the sealing film and another adhesive layer is formed on the opposite side, the other adhesive layer can also be thermally fused to the sealant resin layer of the outer packaging laminate.

[0078] As mentioned above, although this invention was demonstrated based on the preferred embodiment, this invention is not limited to the said embodiment, Various changes are possible within the range which does not deviate from the summary of this invention.

[0079] Example Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples.

[0080] In the production of the adhesive film, a method was used in which the adhesive resin layer, the adjacent layer, and the core layer were formed into films by coextrusion molding using a multilayer casting machine so as to have the thickness shown in Table 1. In the production of the adhesive film, the following resins were used. Here, PP represents polypropylene, PE represents polyethylene, and LLDPE represents linear low-density polyethylene.

[0081] (A)-1: Acid-modified PP (random copolymer, melting point 130~140℃, tensile elastic modulus 1000MPa, unsaturated carboxylic acid modification degree 0.08wt%) (A)-2: Acid-modified PP (metallocene-based, random copolymer, melting point 120-130°C, tensile modulus 750 MPa, unsaturated carboxylic acid acid modification degree 0.07 wt%) (A)-3: Acid-modified PE (LLDPE, melting point 125°C, tensile modulus 45 MPa, unsaturated carboxylic acid modification degree 0.15 wt%) (B)-1: PP (random copolymer, melting point 130~140℃, tensile modulus 1000MPa) (B)-2: PP (metallocene-based, random copolymer, melting point 120~130℃, tensile modulus 750MPa) (B)-3: Thermoplastic elastomer (metallocene-based, tensile modulus 320 MPa) (B)-4: PE (LLDPE, melting point 125°C, tensile modulus 300 MPa) (C)-1: PP (block copolymer, melting point 160~165℃, tensile modulus 1070MPa) In the column of core layer, "-" indicates that the adhesive film does not have a core layer. In the column of structure, "single-sided" indicates that the adhesive film has an adhesive resin layer only on one side. Figure 2 (without core layer) or Figure 4 In the case where the adhesive film is provided with a core layer, “double-sided” means that the adhesive film has an adhesive resin layer on both sides.

[0082] [Table 1]

[0083] (Evaluation method of bonding strength) The adhesive film was cut into 10 mm wide and sandwiched with an aluminum plate (400 μm thickness × 50 × 50 mm) of the adherend so that the adhesive resin layer of the adhesive film was on the adherend side. The sample was produced by thermal compression bonding at a temperature of 170°C, a pressure of 0.1 MPa, and a time of 10 seconds. The adhesive film with a width of 10 mm was peeled off from the adherend by a 180° peeling method at a tensile speed of 300 mm / min using a tensile tester (Autograph (registered trademark) AG-X20kN, Shimadzu Corporation), and the adhesive strength was measured. If the adhesive strength is high, the adhesiveness is good (○), and if the adhesive strength is low, the adhesiveness is poor (×).

[0084] (Evaluation method of shape following property) For the samples prepared by the bonding strength evaluation method, the edge of the aluminum plate of the adherend is magnified and observed to determine whether there is any lifting between the aluminum plate and the adhesive film. If there is no lifting, the shape following property is good (○), and if there is lifting, the shape following property is poor (×).

[0085] (Evaluation method of water vapor transmission rate) The water vapor permeability was evaluated by the following procedure using the API-MS method (atmospheric pressure ionization mass spectrometry) shown in the URL (https: / / www.scas.co.jp / scas-news / sn-back-issues / pdf / 45 / SCASNEWS2017-1_web_p15-18.pdf).

[0086] (1) Install the sample in the permeation unit and pass high-purity nitrogen to the supply side and the permeation side.

[0087] (2) The gas exhausted from the permeation cell on the permeation side was measured by API-MS to confirm that water vapor, the target component, could be removed.

[0088] (3) Nitrogen containing a known amount of water vapor is introduced into the permeation cell on the supply side, and the amount of water vapor exhausted from the permeation cell on the permeation side is measured.

[0089] (4) A state in which the amount of permeation per unit time is constant is defined as a steady state, and the water vapor permeability is evaluated based on the amount of water vapor detected in the steady state.

[0090] If the water vapor permeability is low, the water vapor barrier properties are good (○), and if the water vapor permeability is high, the water vapor barrier properties are poor (×).

[0091] (Cost evaluation method) Since the acid-modified polyolefin is expensive, when the amount of the acid-modified polyolefin used per adhesive resin layer corresponds to a thickness of less than 10 μm, the cost is considered good (○), and when the amount of the acid-modified polyolefin used per adhesive resin layer corresponds to a thickness of 10 μm or more, the cost is considered bad (×).

[0092] [Table 2]

[0093] Table 2 shows the evaluation results.

[0094] The adhesive films of Examples 1 to 11 were evaluated as good (○) in all the items in Table 2.

[0095] In the adhesive film of Comparative Example 1 in which the thickness of the adhesive resin layer was thick, the water vapor barrier properties and the cost were poor (×).

[0096] In the adhesive film of Comparative Example 2 in which unmodified PP was used for the adhesive resin layer, the adhesiveness and shape-conforming property were poor (×).

Claims

1. An adhesive film, It is characterized in that It is formed by a laminate of resins, The adhesive film has: an adhesive resin layer comprising, on at least one surface of the adhesive film, a modified polyolefin resin modified with a functional group that forms a chemical bond with an adherend; as well as an adjacent layer, which is adjacent to the adhesive resin layer and contains a polyolefin resin, The adhesive resin layer has a thickness of less than 10 μm.

2. The adhesive film according to claim 1, It is characterized in that The tensile elastic modulus of the adjacent layer is 1000 MPa or less.

3. The adhesive film according to claim 1 or 2, It is characterized in that A ratio B / A of a thickness A of the adhesive resin layer to a thickness B of the adjacent layer is 1-20.

4. The adhesive film according to any one of claims 1 to 3, It is characterized in that The modified polyolefin resin is an acid-modified polyolefin resin.

5. The adhesive film according to claim 4, It is characterized in that The acid-modified polyolefin resin is a resin obtained by modifying a random copolymer of polypropylene or polyethylene.

6. The adhesive film according to any one of claims 1 to 5, It is characterized in that The polyolefin resin of the adjacent layer is a random copolymer of unmodified polypropylene or unmodified polyethylene.

7. The adhesive film according to any one of claims 1 to 6, It is characterized in that The modified polyolefin resin is modified with an unsaturated carboxylic acid component, and contains 0.01 to 2 parts by weight of the unsaturated carboxylic acid component in 100 parts by weight of the modified polyolefin resin.

8. The adhesive film according to any one of claims 1 to 7, It is characterized in that The adhesive resin layer contains a thermoplastic elastomer resin in an amount within a range of 5 to 30 parts by weight based on 100 parts by weight of the adhesive resin layer.

9. A metal terminal, It is characterized in that The invention is used for a secondary battery and comprises the adhesive film according to any one of claims 1 to 8.

10. A secondary battery, It is characterized in that A metal terminal according to claim 9 is provided.

Citation Information

Patent Citations

  • Adhesive film for metal terminal

    JP2017139120A

  • Sealing film, and tab lead and secondary battery which use same

    WO2021100226A1