Aluminum alloy and method for producing aluminum alloy
By controlling the content of specific elements in aluminum alloys and the rapid cooling and solidification process, the problem of contaminant formation in aluminum alloy surface treatment was solved, mechanical strength and surface treatability were improved, and lightweight, high-strength aluminum alloy products were achieved.
Patent Information
- Application Number
- CN202280093814.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-11-01
Smart Images

Figure CN118891385A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an aluminum alloy having high strength and high surface treatability. Background Art
[0002] Light alloy materials meet various needs and are widely used in industry. If considered as mechanical materials and structural materials, light alloy materials are being used in applications such as automobiles, high-speed rail vehicles, and aerospace. Among light alloys, aluminum alloys are low-priced and easy to process materials, so they are used in almost all major fields of the country. Hereinafter, aluminum alloys will be referred to as Al alloys. Material manufacturers are conducting research on improving the mechanical strength of Al alloys. However, compared with steel, Ti-based alloys, Ni-based alloys, etc., Al alloys have low strength. Even A7075-T6 (JIS standard), which is a high-strength commercially available Al alloy, is considered to have insufficient mechanical strength depending on the application. Therefore, research on the optimal metal composition of Al alloys continues.
[0003] For example, Patent Document 1 states that in order to obtain a high-strength Al alloy, the Al alloy composition needs to include 5-12 mass % Zn, 2-4 mass % Mg, 1-2 mass % Cu, and further 0.01-0.1 mass % Ag.
[0004] In addition, in Patent Document 2, in order to obtain a high-strength Al alloy, the following composition is required: containing Zn: 3.2-8.0 mass%, Mg: 1.2-4.5 mass%, Cu: 0.2-1.5 mass%, Mn: 0.1-1.2 mass%, Cr: 0.1-0.5 mass%, B: 0.005-0.2 mass%, Be: 0.02-1.0 mass%, Ni and / or Co: 0.1-1.2 mass%, Zr and / or Hf: 0.05-1.2 mass%, and Ag: 0.05-2.0 mass%.
[0005] In Patent Document 3, in order to obtain a high-strength Al alloy, the composition is set to include 5-11 mass % Zn, 2-4.5 mass % Mg, 0.5-2.0 mass % Cu, 2-6 mass % Mn, and 0.01-0.5 mass % Ag.
[0006] Al alloy is a base metal second only to Mg alloy among practical metals and is known to be a metal that is easily corroded. Therefore, Al alloy products need to be subjected to surface treatment such as plating or painting to impart corrosion resistance. In particular, a plastic deformation layer called Bayer layer is formed on the surface of a machined metal. Therefore, the plastic deformation layer is generally etched away with an alkali or acid before surface treatment.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2008-240141
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 63-83251
[0011] Patent Document 3: Japanese Patent Application Publication No. 2006-274435
[0012] When Al alloy is etched with acid or alkali, black deposits called stains are generated on the surface.
[0013] Contamination requires a surface treatment process and has problems such as hindering the adhesion of plating and painting. Summary of the invention
[0014] Problems to be solved by the invention
[0015] An object of the present disclosure is to provide an Al alloy having high strength and suppressing generation of contaminants during a surface treatment process.
[0016] Means for solving problems
[0017] With respect to the aluminum alloy of the present disclosure,
[0018] Contains Zn: 5.0-6.5 mass%, Mg: 2.0-3.0 mass%, Cu: 1.2-2.0 mass%,
[0019] Contains at least one element selected from the following three elements: Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, and Li: 0.1-0.4 mass %,
[0020] The Si content is 0.25 mass % or less, the Mn content is 0.5 mass % or less, and the balance is Al and inevitable impurities.
[0021] The tensile strength is 650 MPa or more.
[0022] Effects of the Invention
[0023] According to the Al alloy disclosed in the present invention, a high-strength Al alloy with excellent surface treatability can be provided. The improvement of the high strength of the Al alloy can make the product lighter. In addition, the improvement of the surface treatability can achieve stable impartment of corrosion resistance and shorten the lead time of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The figure of Embodiment 1 is a flowchart showing the production process of the Al alloy.
[0025] Figure 2 The diagram of Embodiment 1 shows a cross-sectional SEM image of an Al alloy after solidification by slow cooling and rapid cooling.
[0026] Figure 3 This is a diagram of Embodiment 1, showing evaluation results of the composition, tensile strength, and stain formation of Al alloys.
[0027] Figure 4 The figure of Embodiment 1 is a flowchart of a method for producing an Al alloy using a layered molding method using a 3D printer.
[0028] Figure 5 This is a diagram of the first embodiment, and is a diagram for explaining the stacking molding method. DETAILED DESCRIPTION Implementation method 1.
[0029] The Al alloy of Embodiment 1 is described below. In the following description, there are Al alloys of raw material alloys and Al alloys finally generated from the raw material alloys. In order to distinguish between the two, these Al alloys are sometimes referred to as raw material alloys, and the Al alloys manufactured from the raw material alloys are referred to as final alloys. In addition, the final alloy is sometimes referred to as "Al alloy (final alloy)". The final alloy is the Al alloy in which the powder is solidified in the solidification step described later.
[0030] The Al alloy (final alloy) of Embodiment 1 is manufactured by cold solidification. The tensile strength of the Al alloy (final alloy) of Embodiment 1 is 650 MPa or more. When the Al alloy (final alloy) of Embodiment 1 is immersed in 10 mass % or more of alkali or 10 mass % or more of acid, the contamination film is 1 μm or less.
[0031] <S10: Melting process>
[0032] Figure 1 Indicates the manufacturing process of the final alloy. Figure 1 , the method for preparing the final alloy is described. Step S10 is a melting process. In the melting process, the raw material alloy shown below is placed in a melting furnace, melted at a temperature of 800-1200°C, and taken out of the furnace. Then, the raw material alloy in a molten state is led out to the molten metal outlet of the atomizing nozzle. The raw material alloy is an Al alloy.
[0033] The aluminum alloy of the raw material alloy has the following composition.
[0034] Contains Zn: 5.0-6.5 mass%, Mg: 2.0-3.0 mass%, and Cu: 1.2-2.0 mass%.
[0035] and
[0036] Contains at least one element selected from the following three elements: Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, and Li: 0.1-0.4 mass %,
[0037] As other inevitable metal elements, the present invention contains 1.0 mass % or less of Ti, 1.0 mass % or less of Fe, and 1.0 mass % or less of Zr.
[0038] The balance is composed of Al.
[0039] In addition, the elements contained in the raw material alloy will be described further later.
[0040] <S20: Powder generation step>
[0041] Step S20 is a powder production step. In step S20, an inert gas such as nitrogen, argon, or helium is injected at high pressure from a nozzle hole to produce a rapidly solidified Al alloy powder.
[0042] <Mass % of Zn, Mg, and Cu in raw alloy>
[0043] The relationship between the mass % of Zn, Mg, and Cu in the raw material alloy and the diameter of the crystal particles of the powder is described below. Powders with a particle size exceeding 300 μm are not used because they do not solidify by rapid cooling.
[0044] Since Zn, Mg, and Cu form a coarse intermetallic compound, the content of Zn is set to 6.5 mass % or less, the content of Mg is set to 3.0 mass % or less, and the content of Cu is set to 2.0 mass % or less.
[0045] On the other hand, when the content of Zn is less than 5.0 mass %, the content of Mg is less than 2.0 mass %, and the content of Cu is less than 1.2 mass %, high tensile strength cannot be obtained.
[0046] Therefore, the concentration ranges of Zn, Mg, and Cu are 5.0-6.5 mass % for Zn, 2.0-3.0 mass % for Mg, and 1.2-2.0 mass % for Cu.
[0047] In addition, the expression "5.0-6.5 mass %" in Zn means "5.0 mass % or more and 6.5 mass % or less". Moreover, the expressions such as Mg: 2.0-3.0 mass % and Cu: 1.2-2.0 mass % have the same meaning.
[0048] <Concentrations of Ni, Ag, and Li added to raw alloy>
[0049] When the addition concentration of Ni, Ag and Li is low, a tensile strength of 650 MPa or more is not generated. On the other hand, when the addition concentration of Ni, Ag and Li is high, coarse intermetallic compounds are easily generated, and hot cracks are easily generated during solidification.
[0050] Therefore, the raw material alloy contains at least one element in the respective mass % ranges of three elements, namely, Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, and Li: 0.1-0.4 mass %.
[0051] For example, when only Ni is included, the content is Ni: 2.0-5.0 mass%. When both Ni and Ag are included, the content is Ni: 2.0-5.0 mass% and Ag: 0.5-3.5 mass%. When three elements, Ni, Ag, and Li, are included, each element is within the three ranges shown above. When two or more elements among Ni, Ag, and Li are included, one of the elements may be the lower limit of the permissible mass% range.
[0052] <Contents of Si and Mn in Raw Material Alloy>
[0053] In addition, the raw material alloy contains 0.25 mass % or less of Si and 0.5 mass % or less of Mn. The contents of Si and Mn will be described later in relation to contaminants.
[0054] <S30: Curing process>
[0055] Step S30 is a solidification process. The rapidly solidified powder of the raw alloy produced in the powder generation process is subjected to hot extrusion processing to be densified and solidified. Then, the solidified rapidly solidified powder is subjected to solution treatment and aging treatment under the tempering condition equivalent to T6 of A7075 in the JIS standard. Thus, a high-strength Al alloy is obtained as the final alloy.
[0056] <Intermetallic compounds>
[0057] At once Figure 2 For the adoption of Figure 1 The Al alloy (final alloy) obtained by the production method of the flowchart described above was subjected to cross-sectional SEM observation and the obtained SEM image was binarized. Figure 2 The black color in the slow cooling and rapid cooling SEM images indicates the precipitation of intermetallic compounds. Figure 2 In FIG, a length of 100 μm is shown.
[0058] exist Figure 2In the Al alloy using the slowly cooled raw alloy powder, coarsened intermetallic compounds were confirmed. The appearance rate of the intermetallic compounds during the slow cooling was 10% or more in a 300 μm×300 μm field of view as a result of cross-section observation using SEM.
[0059] On the other hand, Figure 2 As shown in Figure 1, intermetallic compounds hardly appear in the Al alloy using the rapidly cooled raw alloy powder. During rapid cooling, the appearance rate of intermetallic compounds is less than 1% in a field of view of 300μm×300μm. If the intermetallic compounds are coarsened, a high tensile strength of 650MPa or more cannot be obtained.
[0060] exist Figure 2 The occurrence rate of intermetallic compounds is less than 1% in a field of view of 300μm×300μm.
[0061] To obtain a tensile strength of 650 MPa or more, the total appearance area representing the area of intermetallic compounds appearing in the Al alloy (final alloy) is preferably 2% or less, more preferably 1% or less, when observed in a field of view of 300 μm×300 μm under a scanning electron microscope.
[0062] <S40: Cleaning process>
[0063] Step S40 is a cleaning step. The Al alloy (final alloy) produced is subjected to degreasing cleaning to remove organic matter such as oil and then to alkaline cleaning.
[0064] <Alkaline cleaning>
[0065] In the alkali cleaning, an aqueous solution of sodium hydroxide or potassium hydroxide at 10 mass % or more and 20 mass % or less is used, and the surface is etched by immersion at a temperature of 50° C. or more for 10 to 30 seconds to expose the clean surface.
[0066] For the alkali cleaning, in addition to sodium hydroxide, a strong alkaline aqueous solution such as potassium hydroxide may be used.
[0067] <Dirty matter>
[0068] The thickness of dirt formed during alkaline cleaning is measured by spectroscopic ellipsometer. When the dirt is thin and the reflected light from the base metal can be measured, the dirt thickness can be measured. When it can be measured, the dirt thickness is less than 1μm. On the other hand, when the dirt is thick and appears black, it is difficult to measure. When it is difficult to measure, the dirt thickness becomes more than 1μm. The so-called poor surface treatment means that the black color changes due to the thick dirt, which can be judged by visual inspection.
[0069] <Acid cleaning>
[0070] In the acid cleaning, the final alloy after degreasing cleaning is immersed in an aqueous solution of 10 mass % or more and 20 mass % or less of nitric acid. By immersing at a temperature of 50°C or more for 10-30 seconds, the dirt is examined by the same method as the alkaline cleaning. The surface treatment property is judged by the dirt film thickness and blackening. It should be noted that for acid cleaning, in addition to nitric acid, strong acids such as sulfuric acid and hydrochloric acid can also be used, and mixed acids can also be used. In addition, the mixed acid can be a mixture of weak acids such as phosphoric acid and carbonic acid and strong acids. In particular, mixed acids of phosphoric acid and nitric acid and mixed acids of phosphoric acid and sulfuric acid are known as chemical polishing liquids. They are used to improve surface smoothness.
[0071] <Relationship between dirt, Si, and Mn>
[0072] The amount of Si and Mn has a great influence on the thickness of the stain and the blackening.
[0073] The results of the investigation show that Si is preferably less than 0.25 mass % and Mn is preferably less than 0.25 mass %. Si lowers the melting point of the Al alloy and increases the amount of solid solution of other metal elements. When the amount of Si added is reduced, other metal elements are difficult to solid-dissolve in the Al alloy, so intermetallic compounds are easily precipitated. Therefore, the solidification of the Al alloy needs to be carried out by rapid cooling. The conditions for rapid solidification are preferably a cooling rate of more than 100°C / second.
[0074] Figure 3 Indicates that Figure 1 The surface treatment properties and tensile strength of the Al alloy (final alloy) produced by the method. Figure 3 In the table, Al alloys of Examples 1 to 11, Comparative Examples 1 to 4, and A7075 are shown. Examples 1 to 11 are final alloys, and Comparative Examples 1 to 4 and A7075 are equivalent to the final alloys. In Examples 1 to 11, Zn, Mg, and Cu are: 5.5 mass% Zn, 2.5 mass% Mg, and 1.5 mass% Cu. For Si and Mn, Si is: 0.2 mass% and Mn is: 0.1-0.2 mass%. For Ni, Ag, and Li, Ni is: 2.0-5.0 mass%, Ag is: 0.5-3.5 mass%, and Li is: 0.1-0.4 mass%. Figure 3 On the left side, the tensile strength (MPa) of the Al alloy (final alloy), the presence of black after alkali cleaning, and the thickness (μm) of the dirt are shown.
[0075] **Description of the effects of Embodiment 1**
[0076] Using the raw material alloy of the composition described above, Figure 1The method described in the above can produce a high-strength Al alloy with excellent surface treatment properties. Therefore, by improving the high strength of the Al alloy, the product can be made lighter.
[0077] In addition, by improving the surface treatment property, it is possible to stably impart corrosion resistance and shorten the lead time of products. Supplement to implementation mode 1.
[0078] In order to suppress the generation of dirt caused by alkali or acid and improve the surface treatment property, the dirt thickness needs to be less than 1 μm. Therefore, it is necessary to make the Si content in the Al alloy less than 0.25 mass% and the Mn content less than 0.5 mass%. As for Patent Documents 1 and 2, it is confirmed that the Si content reaches more than 0.25 mass%, and Patent Document 3 confirms that the Mn content reaches 2-6 mass%. Therefore, in Patent Documents 1 and 2, the dirt thickness cannot be made less than 1 μm.
[0079] On the other hand, it is necessary to determine the optimum composition ratio of the additive elements in the Al alloy by limiting the addition amounts of Si and Mn.
[0080] In order to obtain a high-strength Al alloy with a tensile strength of 650 MPa or more, it is necessary to make Zn: 5.0-6.5 mass%, Mg: 2.0-3.0 mass%, Cu: 1.2-2.0 mass%, and contain at least one element among Ni: 2.0-5.0 mass%, Ag: 0.5-3.5 mass%, and Li: 0.1-0.4 mass%.
[0081] It is preferred that the added elements be dissolved in the Al matrix as much as possible. In addition, the less the precipitates as coarse intermetallic compounds are generated, the higher the tensile strength can be obtained, so the aluminum alloy is produced by rapid cooling and solidification.
[0082] <Variation example: Application to 3D printer>
[0083] As a modification of the first embodiment, application to a 3D printer 40 will be described. Figure 4 , Figure 5 , a method for directly manufacturing a product by using the layered modeling method using the 3D printer 40 using the powder produced in step S20 is described.
[0084] Figure 4 A flow chart showing a method for producing an Al alloy (final alloy) using the layer stacking method. Figure 4 middle, Figure 1 The difference is that steps S30 and S40 become steps S30-1 and S40-1.
[0085] Figure 5 This is a diagram illustrating the cascading modeling method. Figure 5In FIG. 4 , a conceptual stereogram of the 3D printer 40 in the XYZ coordinate is shown on the upper left side, an XY plane is shown on the upper right side, a YZ plane is shown on the lower left side, and a ZX plane is shown on the lower right side. In the 3D printer 40 in the XYZ coordinate, the powder generated in step S20 is arranged on the bottom plate 32. The powder is hereinafter referred to as powder 31.
[0086] In the XY plane and the ZX plane, diameter φd of crystal particle 20 is shown. The diameter of crystal particle 20 is sometimes also referred to as a particle size.
[0087] The powder particle size distribution of the atomized powder produced in the powder generating step of step S20 is adjusted as follows.
[0088] D10: Particle size 10 μm or more and 50 μm or less,
[0089] D50: Particle size 20μm or more and 70μm or less,
[0090] D90: Particle size is 40 μm or more and 100 μm or less.
[0091] By adjusting the particle size, in the solidification process of step S30 - 1 , a product of the Al alloy (final alloy) can be directly manufactured by additive manufacturing using the 3D printer 40 .
[0092] Reference Figure 5 , explain step S30-1. Figure 5 The Z direction is set as the height direction. Preferably, by irradiating the laser 11 of the laser device 10, the stacking formation is performed at a pitch P of 100 μm or less in the Z direction, and more preferably at a pitch P of 30 μm or less. In the YZ plane, layers #1 to #4 are shown. In the YZ plane, the pitch P between the layers is shown. By performing such stacking formation in the YZ plane, a product can be produced by rapid solidification at more than 100°C / second.
[0093] <Concentrations of oxygen and nitrogen>
[0094] By irradiating the laser 11, the temperature can be raised and lowered in a short time, so the powder 31 generated in step S20 is easily oxidized and nitrided. Therefore, it is important to manage the concentration of oxygen and nitrogen. In particular, oxidation becomes the root cause of brittle failure, so it is appropriate to use a 3D printer 40 in a non-oxygen atmosphere, preferably a product in an Ar gas atmosphere. As for the oxygen contained in the product made by using a 3D printer 40 in a non-oxygen atmosphere, it is preferably 0.1% by mass or less, and more preferably 0.05% by mass or less.
[0095] Furthermore, the nitrogen content in the object formed by the 3D printer 40 is preferably 0.01 mass % or less, and more preferably 0.001 mass % or less.
[0096] <Laser wavelength>
[0097] As for the laser wavelength of the laser 11 used in the melting of the powder 31 produced in step S20, the light absorption rate generated by Al decreases when it is below 700nm. Therefore, the range of the laser wavelength is preferably above 700nm and below 1100nm. In the powder 31 produced in step S20, the Si content is small, so the melting temperature rises. Therefore, it is more preferable to irradiate with a laser wavelength of 800nm or more and 1100nm or less, which is a wavelength region that is easy to absorb light.
[0098] <Diameter φd of Crystal Particle 20 After Irradiation with Laser Light 11>
[0099] The smaller the diameter φd of the crystal particles 20 of the rapidly solidified powder 31, the higher the tensile strength. When a product is manufactured using a 3D printer 40, the manufactured product has anisotropy in the diameter φd of the crystal particles 20 due to the properties of the 3D printer 40. If the laser 11 as a heat source is irradiated from the Z direction, the diameter φd of the crystal particles 20 becomes longer in the Z direction. The Z direction is set as the height direction.
[0100] After irradiation with the laser 11, Figure 5 As shown in the XY plane of FIG. 1 , the diameter φd of the crystal particle 20 is preferably 100 μm or less, and more preferably 30 μm or less, in the XY direction which is the plane direction of the laser 11 as the heat source. The particle size is the particle size directly produced by the 3D printer 40 and related to the product after production. In the XY direction, it means: in the direction of the two arrows shown as φd in the XY plane, the entire direction of 360 degrees on the XY plane.
[0101] After irradiation with the laser 11, Figure 5 As shown in the ZX plane of FIG. 1 , the diameter φd of the crystal particle 20 in the Z direction is preferably 400 μm or less, and more preferably 200 μm or less. This particle size is directly produced by the 3D printer 40 and is related to the product after production.
[0102] like Figure 5 As shown in the three-dimensional diagram of the XYZ coordinates of FIG. 3 , the object of the 3D printer 40 is formed on the aluminum base plate 32. The temperature of the base plate 32 can be below 200°C.
[0103] After the molding using the 3D printer 40, the product is not subjected to a solution treatment, but is subjected to either or both of an aging treatment and a stress relaxation heat treatment, thereby obtaining a high-strength Al alloy product.
[0104] In step S40-1 as the surface treatment, Figure 1 The cleaning was performed with an alkali and an acid under the same conditions. Through these cleanings, it was confirmed that the thickness of the dirt was 1 μm or less and that the appearance was not blackened.
[0105] As described above, in the Al alloy (final alloy) manufactured by solidification, the heat source is irradiated from the direction along the Z axis in the solidification process, and the diameter φd of the crystal particle 20 has anisotropy with respect to the laser 11 as the heat source. The diameter φd is 30 μm or less in the cross section parallel to the XY plane and 200 μm or less in the cross section parallel to the ZX plane. In addition, in the Al alloy (final alloy) manufactured by solidification, the oxygen contained is 0.1 mass % or less, and the nitrogen contained is 0.01 mass % or less.
[0106] **Description of the effects of Embodiment 1**
[0107] according to Figure 4 , Figure 5 The production of products using the 3D printer 40 described in the above can produce products that are precise, high-strength, and have excellent surface treatment properties.
[0108] The Al alloy (final alloy) described in the above first embodiment is as follows.
[0109] As for Al alloy (final alloy),
[0110] Contains Zn: 5.0-6.5 mass%, Mg: 2.0-3.0 mass%, Cu: 1.2-2.0 mass%,
[0111] Contains at least one element selected from the following three elements: Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, and Li: 0.1-0.4 mass %,
[0112] The Si content is 0.25 mass % or less, the Mn content is 0.25 mass % or less,
[0113] The balance consists of Al and inevitable impurities.
[0114] The tensile strength is 650 MPa or more.
[0115] Furthermore, the total appearance area, which represents the area of intermetallic compounds appearing in the Al alloy (final alloy), was 2% or less when observed in a field of view of 300 μm×300 μm using a scanning electron microscope. Description of Reference Numerals
[0116] 10 laser device, 11 laser, 20 particles, 31 powder, 32 base plate, 40 3D printer.
Claims
1. An aluminum alloy, in, Contains Zn: 5.0-6.5 mass%, Mg: 2.0-3.0 mass%, Cu: 1.2-2.0 mass%, Contains at least one element selected from the following three elements: Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, and Li: 0.1-0.4 mass %, The Si content is 0.25 mass % or less, The Mn content is 0.25 mass % or less, The balance consists of Al and inevitable impurities. The tensile strength is 650 MPa or more.
2. The aluminum alloy according to claim 1, in, The total appearance area, which represents the area of intermetallic compounds appearing in the aluminum alloy, is 2% or less when observed in a 300 μm×300 μm visual field of a scanning electron microscope.
3. A method for producing an aluminum alloy, comprising: A melting step of melting a raw material alloy, wherein the raw material alloy comprises Zn: 5.0-6.5 mass %, Mg: 2.0-3.0 mass %, Cu: 1.2-2.0 mass %; comprises at least one element selected from Ni: 2.0-5.0 mass %, Ag: 0.5-3.5 mass %, Li: 0.1-0.4 mass %, contains Si at most 0.25 mass %, contains Mn at most 0.25 mass %, and the balance is Al and unavoidable impurities; a powder generating step of rapidly solidifying the molten raw material alloy at a cooling rate of 100° C. / sec or more to generate powder; and a solidification step of producing an aluminum alloy by solidifying the powder, The aluminum alloy produced by solidification has a tensile strength of 650 MPa or more.
4. The method for producing an aluminum alloy according to claim 3, in, As for the aluminum alloy manufactured by solidification, in the solidification process, a heat source is irradiated from a direction along the Z axis, and the grain size is anisotropic with respect to the heat source, being less than 30 μm in a section parallel to the XY plane and less than 200 μm in a section parallel to the ZX plane. The oxygen content is less than 0.1 mass %, and the nitrogen content is less than 0.01 mass %.