Nonwoven fabric and use thereof
By using polylactic acid-based polymer fiber layer in nonwoven fabrics and performing hot pressing treatment, the problems of insufficient pleating retention and environmental pollution in the prior art are solved, and non-biodegradability and high capture performance are achieved. Weaving fabrics are suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202380026960.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-01
AI Technical Summary
The existing nonwoven fabrics have shortcomings in pleating retention and are composed of non-biodegradable resins, resulting in environmental pollution problems.
The polylactic acid-based polymer fiber layer containing an average fiber diameter of more than 10μm or less than 30μm is used to adjust the Raman spectrum ratio of the fiber axis by polarization Raman spectroscopy, and combined with hot pressing technology, the biodegradability and good pleating retention are prepared. nonwoven fabrics.
It realizes nonwoven fabrics with good biodegradability and pleating retention, and is suitable for products such as filters, air filters and masks, reducing environmental pollution and improving product capture performance and dimensional stability.
Smart Images

Figure BDA0005038161650000091 
Figure BDA0005038161650000121 
Figure BDA0005038161650000131
Abstract
Description
Technical Field
[0001] The present invention relates to nonwoven fabrics and uses thereof. Background Art
[0002] Conventionally, nonwoven fabrics have been used as filter materials in products such as food filters, air filters, and masks. However, the resins constituting the nonwoven fabrics are generally non-biodegradable resins such as polyethylene, polypropylene, polyester, and polyamide, which have the problem of causing a large environmental burden due to incineration when discarded.
[0003] To address such a problem, for example, Patent Document 1 below proposes a sheet material for coffee extraction, which is formed of a melt-blown nonwoven fabric made of a biodegradable thermoplastic polymer and whose air permeability and water absorption rate are controlled by the average fiber diameter.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-336570 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, the coffee extraction sheet material described in Patent Document 1 is made of a melt-blown nonwoven fabric, and therefore has insufficient pleat retention.
[0009] In view of the above-mentioned prior art, the problem to be solved by the present invention is to provide a nonwoven fabric having biodegradability and good pleat retention and use thereof.
[0010] Solutions for solving problems
[0011] The present inventors conducted intensive research and repeated experiments to solve the above-mentioned problems, and unexpectedly found that the following nonwoven fabric can solve the above-mentioned problems. The nonwoven fabric comprises at least one fiber layer (I), wherein the fiber layer (I) comprises a polylactic acid (hereinafter also referred to as PLA) polymer having an average fiber diameter of 10 μm or more and 30 μm or less, and in the fiber layer (I), the Raman spectrum measured by polarized Raman spectroscopy using polarized light parallel to the fiber axis at 872 cm -1 The peak intensity I / / at 872 cm-1 of the Raman spectrum measured using polarized light perpendicular to the fiber axis -1 The present invention was completed by obtaining a ratio I∥ / I⊥ of the peak intensity I⊥ at 1.80 or less.
[0012] That is, the present invention is as follows.
[0013] [1] A nonwoven fabric comprising at least one fiber layer (I), wherein the fiber layer (I) comprises a polylactic acid polymer having an average fiber diameter of 10 μm or more and 30 μm or less, wherein in the fiber layer (I), a Raman spectrum at 872 cm-1 measured by polarized Raman spectroscopy using polarized light parallel to the fiber axis is -1 The peak intensity I / / at 872 cm-1 of the Raman spectrum measured using polarized light perpendicular to the fiber axis -1 The ratio I∥ / I⊥ of the peak intensity I⊥ at is less than 1.80.
[0014] [2] The nonwoven fabric according to [1], wherein I∥ / I⊥ is 1.40 or less.
[0015] [3] The nonwoven fabric according to [1] or [2], wherein I∥ / I⊥ is 1.08 or more.
[0016] [4] The nonwoven fabric according to any one of [1] to [3] above, wherein the fiber layer (I) has a crystallinity of 20% or more as determined by differential scanning calorimetry.
[0017] [5] The nonwoven fabric according to any one of [1] to [4], wherein the nonwoven fabric has a weight per unit area of 10 g / m 2 Above and 50g / m 2 the following.
[0018] [6] The nonwoven fabric according to any one of [1] to [5], wherein the nonwoven fabric is subjected to thermocompression bonding and a compression bonding area ratio is 5% to 40%.
[0019] [7] The nonwoven fabric according to any one of [1] to [6], further comprising at least one fiber layer (II), wherein the fiber layer (II) has an average fiber diameter of 0.3 μm or more and 7.0 μm or less.
[0020] [8] The nonwoven fabric according to any one of [1] to [7], wherein the air permeability of the nonwoven fabric is 400 cc / cm 2 / sec or less.
[0021] [9] A filter material comprising the nonwoven fabric according to any one of [1] to [8] above.
[0022]
[10] A food filter comprising the filter material described in [9].
[0023]
[11] An air filter comprising the filter material described in [9] above.
[0024]
[12] A mask comprising the filter material described in [9] above.
[0025] Effects of the Invention
[0026] The nonwoven fabric of the invention is biodegradable and has good pleat retention performance. DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the present invention will be described in detail.
[0028] The nonwoven fabric of the present embodiment is characterized in that it comprises at least one fiber layer (I), wherein the fiber layer (I) comprises a polylactic acid polymer having an average fiber diameter of 10 μm or more and 30 μm or less, and in the fiber layer (I), a Raman spectrum at 872 cm-1 measured by polarized Raman spectroscopy using polarized light parallel to the fiber axis is -1 The peak intensity I / / at 872 cm-1 of the Raman spectrum measured using polarized light perpendicular to the fiber axis -1 The ratio I∥ / I⊥ of the peak intensity I⊥ at is less than 1.80.
[0029] The fiber layer (I) may be composed of either short fibers or long fibers, and is preferably composed of long fibers from the viewpoint of strength. In the case of long fibers, it is preferably produced by a known spunbond method, and the filaments are preferably uniformly dispersed during spinning by friction charging, corona charging, etc.
[0030] The fiber layer (I) contains a polylactic acid polymer. When the total amount of the resin is 100% by mass, the content of the polylactic acid polymer in the fiber layer (I) is preferably 70 to 100% by mass.
[0031] As polylactic acid polymers, polymers of D-lactic acid, polymers of L-lactic acid, copolymers of D-lactic acid and L-lactic acid, copolymers of D-lactic acid and hydroxycarboxylic acid, copolymers of L-lactic acid and hydroxycarboxylic acid, copolymers of D-lactic acid and L-lactic acid and hydroxycarboxylic acid, and blends of two or more of these polymers can be listed. The D-body ratio in the total polylactic acid polymer mass can be set within the range that does not damage the spinnability and nonwoven fabric properties, preferably 0 to 15% by mass, more preferably 0.1 to 10% by mass, and further preferably 0.1 to 6% by mass. If the D-body ratio is 0 to 15% by mass, the spinnability is good, and nonwoven fabrics can be stably obtained. In addition, the melting point, crystallinity, etc. become appropriate ranges, and it is easy to obtain nonwoven fabrics with sufficient strength and excellent pleating retention.
[0032] The melt flow rate (MFR) of the polylactic acid polymer is preferably 20 to 120 g / 10 minutes, more preferably 30 to 70 g / 10 minutes. If the MFR is 20 g / 10 minutes or more, the melt viscosity is appropriate, and the fiber is easily thinned in the spinning process, so the spinnability becomes good. On the other hand, if the MFR is 120 g / 10 minutes or less, the melt viscosity is appropriate, so there is less occurrence of single filament breakage in the spinning process, and the spinnability becomes good.
[0033] The fiber layer (I) may further include a thermoplastic resin as a secondary component on the basis of the aforementioned polylactic acid polymer. When the total amount of the resin is set to 100% by mass, the content of the thermoplastic resin as the secondary component is preferably more than 0% by mass and less than 30% by mass, more preferably 0.5-30% by mass, further preferably 3-27% by mass, and most preferably 5-25% by mass. If the content of the thermoplastic resin as the secondary component is more than 0.5% by mass, the crystallization start temperature of the fiber layer (I) can be reduced, and crystallization can be promoted at a lower temperature. Therefore, when hot pressing is performed in the manufacture of the nonwoven fabric, it is not easy to fluff, for example, when the beverage is extracted as a filter for beverages, the fiber can be suppressed from falling off. On the other hand, if the addition amount is less than 30% by mass, crystallization is not suppressed and fully crystallized, so that sufficient strength and dimensional stability are easily obtained as a nonwoven fabric. The thermoplastic resin as the secondary component is preferably biodegradable.
[0034] As the thermoplastic resin of secondary component, homopolymer or copolymer of more than one monomer in the group consisting of aliphatic ester, aromatic ester or (methyl) acrylic acid monomer, olefin, caprolactone, hydroxyalkanoate, alkylene glycol, dibasic acid and glycol can be listed.And then, various polymers with biodegradability can be listed by selecting multiple these, and the material obtained by their blending.From the viewpoint of compatibility, spinnability with the polylactic acid polymer as principal component, aliphatic ester, aromatic ester are preferably used, specifically, polybutylene succinate (hereinafter also referred to as PBS), polybutylene adipate terephthalate, polybutylene succinate butylene adipate.
[0035] From the viewpoint of spinning stability, the average fiber diameter of the fiber layer (I) is 10 μm or more, preferably 12 μm or more, more preferably 13 μm or more, and from the viewpoint of strength and heat resistance, it is 30 μm or less, preferably 20 μm or less, more preferably 18 μm or less. In the present embodiment, regarding the fiber diameter of the fiber layer (I), the average fiber diameter is 10 μm or more and 30 μm or less, preferably 14 μm or more and 26 μm or less.
[0036] The cross-sectional shape of the fibers of the fiber layer (I) is not particularly limited, but is preferably a circular cross-sectional shape from the viewpoint of strength, and is preferably a yarn with an irregular cross-sectional shape such as a flat yarn from the viewpoint of forming fine voids.
[0037] In the fiber layer (I), the Raman spectrum at 872 cm-1 measured by polarized Raman spectroscopy using polarized light parallel to the fiber axis is -1 The peak intensity I / / at 872 cm-1 of the Raman spectrum measured using polarized light perpendicular to the fiber axis -1 The ratio of the peak intensity I⊥ at I∥ / I⊥ is less than 1.80, preferably less than 1.60, and more preferably less than 1.40. If I∥ / I⊥ is less than 1.80, excessive orientation is prevented and the shape can be maintained after pleating. If it is less than 1.40, the cutting property is further improved. From the viewpoint of pleating retention and cutting property, the lower I∥ / I⊥ is, the more preferred it is. For fibers containing polylactic acid polymers, it is usually greater than 1.08. The detailed measurement method of I∥ / I⊥ is described below.
[0038] There is no particular limitation on the method for controlling the aforementioned I∥ / I⊥. When using a known spunbonding method, the spinning speed of the filaments, the spinning temperature, the pulling force, the draft ratio, the intrinsic viscosity of the resin, the hot pressing temperature, the insulation length of the spinning section, etc. can be listed.
[0039] In particular, the aforementioned I∥ / I⊥ can be easily controlled by adjusting the traction force. As a method of controlling the traction force, when using the known spunbond method, a high-speed airflow traction device based on jet is usually used, and the traction force can be adjusted by the amount of air introduced into the traction device. Regarding the traction force, two nylon lines (fishing lines) with a length equal to the total length of the traction device and a diameter of 0.235 mm (the nylon line "Silver Scale (No. 2 / Natural / 50m roll monomer)" manufactured by Toray Industries, Ltd. is used in this specification) are put into the traction device, and the stress is measured using a spring balance connected to the nylon line, and divided by the length of the nylon line put in, thereby measuring the traction force (mN / m). The traction force is preferably 40 to 90 mN / m, more preferably 40 to 80 mN / m, and most preferably 50 to 70 mN / m. By controlling the traction force within an appropriate range, it is possible to fully suppress yarn breakage during spinning, and it is easy to set the aforementioned I∥ / I⊥ to a preferred range.
[0040] As a method for easily controlling the aforementioned I∥ / I⊥ in addition to the pulling force, the insulation length of the spinning section can be adjusted. The insulation length of the spinning section refers to the length from just below the spinning tube head to the cooling start part, and the insulation length of the spinning section is preferably 100 mm or more, and more preferably 120 to 250 mm. If the insulation length of the spinning section is within the above range, yarn breakage during spinning can be fully suppressed, and the aforementioned I∥ / I⊥ can be easily set to the preferred range.
[0041] The crystallinity of the fiber layer (I) measured by a differential scanning calorimeter is preferably 20% or more, more preferably 25% or more, and further preferably 30% or more. If the crystallinity of the fiber layer (I) is 20% or more, sufficient strength and dimensional stability can be obtained as a nonwoven fabric, and breakage during pleating can be prevented.
[0042] The nonwoven fabric of the present embodiment may further include at least one fiber layer (II) having an average fiber diameter of 0.3 μm or more and 7 μm or less. The fiber layer (II) may be produced by, for example, a melt-blowing method.
[0043] The average fiber diameter of the fiber layer (II) is 0.3 μm or more and 7 μm or less, preferably 0.4 μm or more and 5 μm or less, and more preferably 0.6 μm or more and 2 μm or less. If the fiber diameter is 0.3 μm or more, it is possible to obtain stable fibers by, for example, meltblowing and spinning under mild conditions. On the other hand, if the average fiber diameter of the fiber layer (II) is 7 μm or less, the fiber layer (II) enters the gap of the fiber layer (I) in the form of fine fibers, and the gap can be filled, presenting a dense structure, and therefore, the collection performance as a filter is improved.
[0044] As the raw material of the fiber layer (II), the raw materials that can be used for the above-mentioned fiber layer (I) can be used in the same manner.
[0045] The nonwoven fabric may have a laminated structure of one or more fiber layers (I) and one or more fiber layers (II). Examples of the laminated structure include layer structures such as I / II, I / II / I, I / II / II, I / II / II / I, I / II / I / II / I, and I / II / I / I / II / I.
[0046] The weight per unit area of the nonwoven fabric is preferably 10 g / m 2 Above and 50g / m 2 Below, more preferably 12g / m 2 Above and 47g / m 2 Below, more preferably 15g / m 2 Above and 45g / m 2 If the unit area weight of the nonwoven fabric is 10g / m 2 If the filter has a sufficient collection performance, it is easy to achieve the required strength during pleating, so the pleating process is excellent. 2 If the thickness is less than 100 μm, the structure can be prevented from becoming too dense, and the pressure loss will not increase. In addition, the softness, stretchability, and followability of the nonwoven fabric can be easily obtained, and the pleating processability is excellent.
[0047] When heat pressing is performed in the manufacture of nonwoven fabrics, the heat pressing can be heat pressing between an embossing roller and a smooth roller (hereinafter also referred to as a flat roller), heat pressing between a smooth roller and a smooth roller, or heat pressing between hot flat plates. From the viewpoint of improving strength, heat pressing is preferably performed between an embossing roller and a smooth roller.
[0048] When the embossing roller and the smooth roller are heat-pressed, the heat-pressed bonding is preferably performed in a manner that the area ratio of the press-bonded portion to the total area of the nonwoven fabric (press-bonded area ratio) is 5% or more and 40% or less, and more preferably 7% or more and 35% or less. If the press-bonded area ratio is 5% or more, a material with less fuzz and dimensional stability can be produced, and if it is 40% or less, the nonwoven fabric is not easy to become paper-like, and mechanical properties such as elongation at break and tear strength are not easy to decrease.
[0049] The thermocompression bonding temperature is preferably 30° C. or higher and 90° C. or lower than the melting point of the resin containing the polylactic acid polymer as the main component constituting the fiber, and more preferably 40° C. or higher and 70° C. or lower. If the difference between the thermocompression bonding temperature and the melting point of the resin constituting the fiber is within the above range, fuzzing is less likely to occur, fuzzing due to pleating can be suppressed, and fiber shedding can be suppressed during beverage extraction.
[0050] From the viewpoint of mechanical strength, rigidity, and dimensional stability, the thermal compression bonding pressure is preferably 10 N / mm or more and 100 N / mm or less, and more preferably 30 N / mm or more and 70 N / mm or less.
[0051] The shape of the heat-compression bonded portion is not particularly limited, and examples thereof include a texture pattern, IL pattern (rectangular pattern), needlepoint pattern, diamond pattern, square pattern, tortoise shell pattern, elliptical pattern, lattice pattern, water drop pattern, and circular pattern.
[0052] When hot pressing is performed between smooth rolls or between flat plates, heat is applied to the entire surface of the nonwoven fabric. Therefore, it is preferred to perform hot pressing at low pressure and low temperature so as not to cause excessive crystallinity of the nonwoven fabric as a whole and to avoid interlayer delamination.
[0053] The nonwoven fabric may contain black pigment, phosphorus-based flame retardant, water repellent within the range that does not impair the desired effect. In addition, known post-processing such as the addition of deodorant and / or antibacterial agent, dyeing, water repellent processing and water permeable processing may also be implemented.
[0054] The nonwoven fabric may further contain one or more flame retardants, inorganic fillers, softeners, plasticizers, pigments, antistatic agents, and the like, depending on the purpose.
[0055] The air permeability of the nonwoven fabric measured according to JIS L 1096 is preferably 200 cc / cm 2 / sec or less, more preferably 170cc / cm 2 / sec or less, more preferably 150cc / cm 2 / sec or less. If the air permeability of nonwoven fabric is 200cc / cm 2 / sec or less, sufficient collection performance can be obtained when used as a filter material.
[0056] Example
[0057] The present invention is specifically described below by way of examples and comparative examples, but the present invention is not limited thereto. In addition, the flow direction (machine direction) when manufacturing a nonwoven fabric is referred to as the MD direction, and the width direction perpendicular to the MD direction is referred to as the CD direction.
[0058] Each physical property in the following examples etc. is measured by the following methods. In addition, in the following examples etc., each physical property is measured by the following methods in principle. If it cannot be measured by the following methods, it can be measured by appropriate and reasonable alternative methods.
[0059] (1) Weight per unit area (g / m 2 )
[0060] The weight per unit area is measured in accordance with JIS L 1913.
[0061] (2) Average fiber diameter (μm)
[0062] A 500-fold magnification photograph was taken using a VHX-700F microscope manufactured by KEYENCE Corporation, and the average value of 10 fibers in focus in the observation field was calculated.
[0063] (3) The Raman spectrum at 872 cm was measured using polarized light parallel to the fiber axis. -1 The peak intensity at 872 cm (I / / ) is relative to the peak at 872 cm of the Raman spectrum measured using polarized light perpendicular to the fiber axis. -1 The ratio of the peak intensity (I⊥) at (I∥ / I⊥)
[0064] Using a Raman spectrophotometer InViaReflex manufactured by Renishaw, for any one fiber of the fiber layer (I) in the sample, the sample was set in a state where the polarization plane of the excitation light was parallel to the fiber axis, and the polarized light Raman spectrum obtained thereby was measured at 872 cm -1Next, the sample was rotated 90° and the polarization plane of the excitation light was perpendicular to the fiber axis. The polarized Raman spectrum at 872 cm was measured. -1 The peak intensity at (I⊥) is calculated. The ratio (I∥ / I⊥) of (I / / ) to (I⊥) is calculated as the average value of 10 fibers. The larger the value of (I∥ / I⊥), the higher the orientation of the molecular chain relative to the fiber axis. In addition, the measurement is performed in a manner that the optical axis of the polarizer on the detection side of the aforementioned polarized light Raman spectrum is parallel to the optical axis of the excitation light.
[0065] In addition, the measurement conditions using a Raman spectrophotometer are as follows.
[0066] (Measurement conditions)
[0067] Laser wavelength: 532nm
[0068] Excitation light intensity at the measurement position: 5mW
[0069] Objective lens: 20 times (NA0.40)
[0070] Diffraction grating: 1800gr / mm
[0071] Exposure time: 2 seconds
[0072] Cumulative times: 10 times
[0073] (4) Crystallinity of fiber layer (I) (%)
[0074] Using a differential scanning calorimeter DSC6000 manufactured by Perkin Elmer, 5 mg of a nonwoven fabric sample was placed in an aluminum pan manufactured by Perkin Elmer, and the temperature was raised from 30°C to the melting point of the fiber layer (I) + 50°C at a heating rate of 10°C / min. The exothermic peak heat and cold crystallization peak heat obtained from the differential curve of the obtained spectrum were calculated using the formula shown below.
[0075] [Mathematical formula 1]
[0076]
[0077] In addition, in this example, the following values were used as the heat of fusion of complete crystals.
[0078] Polylactic acid (PLA): 93.0 J / g
[0079] Polyethylene terephthalate (PET): 126.4 J / g
[0080] (5) Air permeability
[0081] The air permeability was measured in accordance with JIS L 1096 using an air permeability tester FX3340 manufactured by TEXTEST.
[0082] (6) Biodegradability
[0083] The nonwoven fabric samples were composted for a maximum of 12 weeks using the ISO 16929 (JIS K 6952) pilot-scale aerobic disintegration test. The samples were then passed through a 2 mm mesh sieve and evaluated based on the ratio of the mass remaining on the sieve to the mass before passing through the sieve according to the following evaluation criteria.
[0084] (Evaluation Criteria)
[0085] 0: The residue on the sieve is less than 5%
[0086] ×: Screen residue exceeds 5%
[0087] (7) Pleating retention
[0088] A rectangular nonwoven fabric sample with a width (CD direction) of 75 mm and a length (MD direction) of more than 75 mm was bent 180° at a position 20 mm long from one end in the MD direction, and a weight of 2 kg was placed on the sample so as to completely cover the bending line, and the sample was left to stand for 60 seconds. After that, the weight was removed and after 30 seconds, the angle at which the nonwoven fabric sample returned to the unfolded state was measured using a protractor, and the pleat retention was evaluated according to the following evaluation criteria.
[0089] (Evaluation Criteria)
[0090] ◎: Return expansion angle is less than 80°
[0091] ○: The return expansion angle exceeds 80° and is less than 100°
[0092] △: The return expansion angle is more than 100° and less than 120°
[0093] ×: The return expansion angle exceeds 120°.
[0094] (8) Cutting performance
[0095] A 47 mm diameter circular punching blade was placed at the center of a 100 mm square nonwoven fabric sample and pressed with a flat plate press at room temperature. The cutting properties were evaluated according to the following evaluation criteria.
[0096] (Evaluation Criteria)
[0097] ○: The nonwoven fabric sample was cut in the shape of a punching blade.
[0098] ×: The nonwoven fabric sample was not cut in the same manner as the shape of the punching blade.
[0099] [Example 1]
[0100] 10% by mass of polybutylene succinate (melting point: 110°C) was added to a polylactic acid (melting point: 160°C, MFR value at 210°C: 15 g / 10 min, D-body ratio: 2.0%) resin, and the mixture was supplied to a known melt spinning device, melted at 230°C, and ejected from a spinning tube head having a spinning hole with a circular cross section. The yarn was stretched using a high-speed airflow traction device based on an air jet under the conditions of a heat preservation length of 130 mm in the spinning section and a traction force of 60 mN / m, while the yarn was cooled, and a spunbond fiber web (weight per unit area: 40.0 g / m 2 , average fiber diameter of 17 μm), and formed on a net. The obtained fiber web was subjected to heat pressing using a textured pattern embossing roll and a flat roll with a pressing area rate of 15%, the surface temperature of the embossing roll was set to 130°C, the surface temperature of the flat roll was set to 130°C, and the calender line pressure of 30 N / mm, thereby obtaining a fiber web with a unit area weight of 40.0 g / m 2 Its properties are shown in the following Table 1.
[0101] [Examples 2 to 8]
[0102] A nonwoven fabric was obtained in the same manner as in Example 1 except that the pulling force was adjusted so that the average fiber diameter would be the value shown in Table 1. The properties thereof are shown in Table 1 below.
[0103] [Examples 9 to 12]
[0104] A nonwoven fabric was obtained in the same manner as in Example 1 except that the ejection amount and the line speed were adjusted so that the basis weight became the values shown in Tables 1 and 2. The properties thereof are shown in Tables 1 and 2 below.
[0105] [Example 13]
[0106] The weight per unit area is 11.7 g / m 2 The same operation as in Example 1 was performed except that the ejection amount and the line speed were adjusted in the same manner as in Example 1. The fiber web (weight per unit area: 11.7 g / m 2 , average fiber diameter of 17 μm), from the melt-blown nozzle at a spinning temperature of 230°C, heated air of 300°C and 1000Nm 3 / hr, polylactic acid (melting point 160°C, MFR value at 210°C 80 g / 10 min, D-body ratio 1.4%) was directly sprayed to form a melt-blown fiber web (weight per unit area 6.6 g / m 2, the average fiber diameter is 1.7 μm). At this time, the distance from the meltblowing nozzle to the spunbond fiber web is set to 110 mm, and the suction wind speed at the collecting surface just below the meltblowing nozzle is set to 7 m / sec. Then, a spunbond fiber web of polylactic acid identical to the aforementioned spunbond fiber web is formed on the obtained meltblown fiber web. The obtained laminated fiber web is heat-pressed in the same manner as in Example 1 to obtain a total unit area weight of 30.0 g / m 2 Its properties are shown in the following Table 2.
[0107] [Examples 14 and 15]
[0108] A nonwoven fabric was obtained in the same manner as in Example 12 except that the pulling force was adjusted so that the average fiber diameter of each spunbond fiber web would be the value described in Table 1. The properties thereof are shown in Table 2 below.
[0109] [Examples 16 and 17]
[0110] A nonwoven fabric was obtained in the same manner as in Example 12 except that the ejection rate and the line speed were adjusted so that the basis weight of the spunbond fiber web and the basis weight of the meltblown fiber web became the values shown in Table 1. The properties thereof are shown in Table 2 below.
[0111] [Table 1]
[0112]
[0113] [Table 2]
[0114]
[0115] [Comparative Example 1]
[0116] 10% by mass of polybutylene succinate (melting point: 110°C) was added to a polylactic acid (melting point: 160°C, MFR value at 210°C: 15 g / 10 min, D-body ratio: 2.0%) resin, and the mixture was supplied to a known melt spinning device, melted at 230°C, and ejected from a spinning tube head having a spinning hole with a circular cross-section. The yarn was stretched using a high-speed airflow traction device based on an air jet under the conditions of a heat preservation length of 80 mm in the spinning section and a traction force of 75 mN / m, while being cooled, and a spunbond fiber web (S1) (weight per unit area: 40.0 g / m 2 , average fiber diameter of 12 μm), and formed on a web. The obtained fiber web was subjected to heat pressing using a textured pattern embossing roll and a flat roll with a bonding area rate of 15%. The surface temperature of the embossing roll was set to 130°C, and the surface temperature of the flat roll was set to 130°C. The heat pressing was performed at a calender line pressure of 30 N / mm, thereby obtaining a fiber web with a unit area weight of 40.0 g / m 2Its properties are shown in the following Table 3.
[0117] [Comparative Example 2]
[0118] A polyethylene terephthalate resin (1% of o-chlorophenol, a solution viscosity ηsp / c of 0.77 at 25°C, and a melting point of 263°C) was supplied to a known melt spinning device, melted at 300°C, and ejected from a spinning tube head having a spinning hole with a circular cross-section. The yarn was cooled while being stretched at a pulling force of 69 mN / m using a high-speed airflow traction device based on an air jet, and a spunbond fiber web (weight per unit area of 14.0 g / m 2 , average fiber diameter of 14 μm) was formed on the web. The obtained fiber web was subjected to heat pressing using a textured pattern embossing roll and a flat roll with a pressing area rate of 15%. The surface temperature of the embossing roll was set to 220°C, and the surface temperature of the flat roll was set to 220°C. The calender line pressure was 30 N / mm, thereby obtaining a fiber web with a unit area weight of 30.0 g / m 2 Its properties are shown in the following Table 3.
[0119] [Comparative Example 3]
[0120] The weight per unit area is 11.7 g / m 2 The same operation as in Comparative Example 2 was performed except that the ejection amount and the line speed were adjusted in the same manner as in Comparative Example 2. The spunbonded fiber web (weight per unit area: 11.7 g / m 2 , average fiber diameter of 14 μm), from the melt-blown nozzle at a spinning temperature of 300°C, heated air at 320°C and 1000Nm 3 / hr, polyethylene terephthalate (similarly, solution viscosity ηsp / c: 0.50, melting point: 260°C) was directly sprayed to form a melt-blown fiber web (weight per unit area: 6.6 g / m 2 , average fiber diameter is 1.7 μm, D body ratio is 1.4%). At this time, the distance from the meltblowing nozzle to the spunbond layer is set to 110 mm, and the suction wind speed at the collecting surface just below the meltblowing nozzle is set to 7 m / sec. Furthermore, a spunbond fiber web of polyethylene terephthalate identical to the aforementioned spunbond fiber web is formed on the obtained meltblown fiber web. The obtained laminated fiber web is heat-pressed in the same manner as in Comparative Example 5 to obtain a total unit area weight of 30.0 g / m 2 Its properties are shown in the following Table 3.
[0121] [Comparative Example 4]
[0122] A spinning solution consisting of 11 parts by mass of polylactic acid (6060D) manufactured by NatureWorks, 44.5 parts by mass of dimethylformamide, and 44.5 parts by mass of dichloromethane was prepared. Then, the spinning solution was supplied to a nozzle having an inner diameter of 0.22 mm at 2.0 mL / hr using a syringe pump, and a voltage of 32.5 kV was applied to the nozzle to electrospin ultrafine fibers (weight per unit area of 0.9 g / m 2 , the average fiber diameter is 0.3 μm). The distance between the collector grounded to the nozzle is set to 22.5 cm. The feeding speed of the polyethylene terephthalate nonwoven fabric disposed between the nozzle and the collector is changed to obtain nonwoven fabrics with different unit area weights of the fiber structure of ultrafine fibers formed by polylactic acid. Its characteristics are shown in the following Table 3. In addition, in Table 3, the nonwoven fabric of Comparative Example 4 does not have a fiber layer equivalent to the fiber layer (I), so the measured value of the fiber layer equivalent to the fiber layer (II) is shown as the crystallinity.
[0123] [Comparative Example 5]
[0124] A polylactic acid resin having an MFR (230°C, 2160g load) of 190g / 10min and a D-body mixing ratio of 23.9% was used to form a fiber having an average fiber diameter of 8.2μm and a fiber weight of 50g / m 2 A meltblown fiber web formed of polylactic acid ultrafine fibers having a unit area weight of , and the constituent fibers of the fiber web are locally heat-fused by a hot embossing process to produce a meltblown nonwoven fabric. The pressing area at this time is 15%. The properties of the nonwoven fabric are shown in Table 3. In addition, in Table 3, the nonwoven fabric of Comparative Example 5 does not have a fiber layer equivalent to the fiber layer (I), and therefore, as the crystallinity, the measured value of the fiber layer equivalent to the fiber layer (II) is shown.
[0125] [Comparative Example 6]
[0126] A nonwoven fabric was obtained in the same manner as in Comparative Example 5 except that the ejection amount and the linear speed were adjusted so that the average fiber diameter and the weight per unit area became the values shown in Table 2. The properties thereof are shown in Table 3. In Table 3, since the nonwoven fabric of Comparative Example 5 does not have a fiber layer corresponding to the fiber layer (I), the measured value of the fiber layer corresponding to the fiber layer (II) is shown as the crystallinity.
[0127] [Table 3]
[0128]
[0129] Industrial Applicability
[0130] The nonwoven fabric of the present invention can provide a filter material with excellent pleating processability, a maintained pleated shape, high capture performance, and low pressure loss. In addition, since it is composed of a biodegradable resin, it is biodegraded in a natural environment after use, and has less burden on the environment. More specifically, the nonwoven fabric of the present invention can be suitably used as a filter for food such as a black tea filter and a coffee filter, an air filter for air conditioners or automobiles, and a mask.
Claims
1. A nonwoven fabric comprising at least one fiber layer (I), wherein the fiber layer (I) comprises a polylactic acid polymer having an average fiber diameter of 10 μm or more and 30 μm or less, wherein in the fiber layer (I), the Raman spectrum measured by polarized Raman spectroscopy using polarized light parallel to the fiber axis at 872 cm -1 The peak intensity I / / at 872 cm-1 of the Raman spectrum measured using polarized light perpendicular to the fiber axis -1 The ratio I∥ / I⊥ of the peak intensity I⊥ at is less than 1.
80.
2. The nonwoven fabric according to claim 1, in, The I∥ / I⊥ is less than 1.
40.
3. The nonwoven fabric according to claim 1 or 2, in, The I∥ / I⊥ is greater than 1.
08.
4. The nonwoven fabric according to claim 1 or 2, in, The fiber layer (I) has a crystallinity of 20% or more as determined by differential scanning calorimetry.
5. The nonwoven fabric according to claim 1 or 2, in, The nonwoven fabric has a unit area weight of 10 g / m 2 Above and 50g / m 2 the following.
6. The nonwoven fabric according to claim 1 or 2, in, The nonwoven fabric is thermally pressed and the pressing area ratio is 5% or more and 40% or less. 7 . The nonwoven fabric according to claim 1 , further comprising at least one fiber layer (II), wherein the fiber layer (II) has an average fiber diameter of 0.3 μm or more and 7.0 μm or less.
8. The nonwoven fabric according to claim 1 or 2, in, The air permeability of the nonwoven fabric is 400cc / cm 2 / sec or less.
9. A filter material comprising the nonwoven fabric according to claim 1 or 2. 10 . A food filter comprising the filter material according to claim 9 .
11. An air filter comprising the filter material according to claim 9.
12. A mask comprising the filter material according to claim 9.
Citation Information
Patent Citations
Nonwoven fabric and composite sound-absorbing material using same as skin material
CN111527253A
Manufacturing device of screen sheet consted of continuous fibre
CN1381623A
Air filter
JP2003260321A
Nonwoven fabric for simple mask and simple mask
JP2004263344A
Monolayer or multilayer polyester long fiber non-woven fabric and filter for food using the same
JP2020073751A