Method for manufacturing optical article

By using an ultraviolet cut-off filter and a photopolymerization initiator in the visible light range during the illumination process, the problem of molecular aggregation caused by ultraviolet-absorbing compounds in optical articles is solved, and a curing layer with excellent transparency is formed.

CN118891546APending Publication Date: 2024-11-01HOYA LENS THAILAND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028612.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In existing optical articles with cured layers formed by photopolymerization, the problem of reduced transparency is prone to occur. This is mainly due to the molecular aggregation caused by ultraviolet-absorbing compounds in the early stage of polymerization, which affects the polymerization of polymerizable compounds.

Method used

During illumination, ultraviolet (UV) cutoff filters are used to block UV rays, and polymerization is carried out using photopolymerization initiators in the visible light range. This ensures good reaction of polymerizable compounds and avoids molecular aggregation of UV-absorbing compounds.

Benefits of technology

The cured layer formed by this method has excellent transparency, reduces surface defects, and improves the transparency and polymerization efficiency of optical items.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049435170000071
    Figure BDA0005049435170000071
  • Figure BDA0005049435170000072
    Figure BDA0005049435170000072
  • Figure BDA0005049435170000151
    Figure BDA0005049435170000151
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an optical article, the method comprising: forming a coating layer by applying a polymerizable composition onto a substrate; and performing curing treatment on the coating layer by illuminating the coating layer with a light source that emits light in a wavelength range from ultraviolet light to visible light, the polymerizable composition contains one or more polymerizable compounds having a molecular weight of 500 or less, a photopolymerization initiator having an absorption effect in at least a portion of the wavelength range of visible light, and an ultraviolet-absorbing compound, and in the illumination, the photopolymerization initiator has an absorption effect in at least a portion of the period from the start of the illumination, and the ultraviolet-absorbing compound has an absorption effect in at least a portion of the period from the start of the illumination. The illumination is performed by disposing an ultraviolet cut-off filter between the light source and the coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an optical article. Background Art

[0002] Many optical articles have one or more coating layers on a substrate, and the coating layers impart various properties to the optical articles. In recent years, it has been widely practiced to form such coating layers as cured layers cured by photopolymerization (for example, see Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-181455 Summary of the invention

[0006] Problems to be solved by the invention

[0007] Compared with the coating formation methods such as thermal curing, penetration / evaporation drying, and oxidative polymerization, the formation of a coating layer (cured layer) by photopolymerization has the advantages of reduced environmental burden due to reduced use of volatile organic compounds and improved productivity due to short-term curing. However, the inventors' research results have found that in optical articles obtained by forming a cured layer by photopolymerization, defects may occur on the surface of the cured layer, resulting in reduced transparency of the optical article.

[0008] In view of the above circumstances, an object of one embodiment of the present invention is to provide a new method for producing an optical article, which can produce an optical article having a cured layer formed by photopolymerization and having excellent transparency.

[0009] Solutions to the problem

[0010] One embodiment of the present invention relates to a method for manufacturing an optical article, the method comprising:

[0011] coating the polymerizable composition on a substrate to form a coating layer; and

[0012] The coating layer is cured by irradiating the coating layer with light from a light source, the light source emitting light in a wavelength range from ultraviolet light to visible light,

[0013] The polymerizable composition comprises:

[0014] One or more polymerizable compounds having a molecular weight of 500 or less,

[0015] A photopolymerization initiator having absorption in at least a part of the wavelength range of visible light, and

[0016] UV absorbing compounds,

[0017] In the irradiation, the irradiation is performed with an ultraviolet cut filter disposed between the light source and the coating layer during at least a portion of the period from the start of the irradiation.

[0018] The present inventors have newly discovered during repeated studies that the above-described surface defects of the cured layer tend to occur more easily in a cured layer formed by photopolymerizing a polymerizable composition containing an ultraviolet absorbing compound and a polymerizable compound having a molecular weight of 500 or less. The present inventors speculate as follows.

[0019] By irradiating light onto a coating layer formed by coating the polymerizable composition on a substrate, the coating layer can be cured by photopolymerization to form a cured layer.

[0020] On the other hand, the ultraviolet absorbing compound undergoes molecular motion when absorbing ultraviolet rays, which is presumed to cause the molecules to easily aggregate. It is thought that when the polymerizable composition contains the ultraviolet absorbing compound, the aggregation of the molecules at the initial stage of polymerization will hinder the polymerization of the polymerizable compound, and low molecular weight polymerizable compounds with a molecular weight of 500 or less are more susceptible to the above-mentioned polymerization hindrance. The inventors presume that this may be the main cause of defects on the surface of the cured layer.

[0021] In contrast, in the above-mentioned manufacturing method, on the basis of using a light source that emits light in the wavelength range from ultraviolet rays to visible light and a photopolymerization initiator that absorbs at least a part of the wavelength range of visible light, an ultraviolet cut filter is used to block the irradiation of ultraviolet rays to the coating layer of the polymerizable composition during at least a part of the period from the start of light irradiation for photopolymerization, that is, at least in the initial stage of polymerization. As a result, the ultraviolet absorption of the ultraviolet absorbing compound can be hindered in the initial stage of polymerization. Among them, the above-mentioned coating layer contains a photopolymerization initiator, which can function by being irradiated with light closer to the long wavelength side than the wavelength range of ultraviolet rays contained in the light emitted from the above-mentioned light source. Therefore, by using this photopolymerization initiator, the polymerization reaction of the polymerizable compound can be carried out in a state where the ultraviolet irradiation is blocked. Therefore, in the initial stage of polymerization when the ultraviolet rays are blocked by the above-mentioned filter, the influence caused by the aggregation of the molecules of the ultraviolet absorbing compound can be eliminated or reduced, and the polymerization of the low molecular weight polymerizable compound with a molecular weight of 500 or less can be carried out well. The inventors of the present invention speculate that this can suppress the occurrence of defects on the surface of the cured layer, which is the reason why an optical article with excellent transparency can be produced by the above-mentioned production method. However, it should be noted that the present invention is not limited to the speculation described in this specification.

[0022] Effects of the Invention

[0023] According to one embodiment of the present invention, a method for producing an optical article can be provided, which is capable of producing an optical article having a cured layer formed by photopolymerization and having excellent transparency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The transmission spectrum of the filter A used in the example and the transmission spectrum of the filter B used in the comparative example are shown.

[0025] Figure 2 The absorption spectrum of Omnirad819 manufactured by IGM Resin BV, a photoradical polymerization initiator, is shown.

[0026] Figure 3 The results of measuring the film thickness of the photochromic layer of the eyeglass lens produced in Example 1 and the eyeglass lens produced in Comparative Example 2 using a reflective non-contact film thickness measuring device are shown. DETAILED DESCRIPTION

[0027] In the present invention and this specification, “ultraviolet light” refers to electromagnetic waves in a wavelength range of 300 nm to 400 nm, and “visible light” refers to electromagnetic waves in a wavelength range exceeding 400 nm to 780 nm.

[0028] In the present invention and this specification, the "ultraviolet absorbing compound" refers to a compound having absorption at least at a wavelength of 400 nm.

[0029] In the present invention and this specification, "ultraviolet cut filter" refers to a filter whose transmittance to light in the wavelength range of ultraviolet light (300 nm to 400 nm) is less than 5%. That is, the maximum transmittance of the filter in the wavelength range of ultraviolet light (300 nm to 400 nm) is less than 5%.

[0030] In the present invention and this specification, "a photopolymerization initiator having absorption in at least a part of the wavelength range of visible light" refers to a compound that can function as a photopolymerization initiator, and is a compound that has absorption in at least a part of the wavelength range of visible light, i.e., the wavelength range exceeding 400nm and below 780nm.

[0031] In the present invention and this specification, "absorption" means that the molar absorption coefficient exceeds 0 L·mol -1 cm -1 The molar absorption coefficient is a coefficient obtained by converting the absorbance of a sample into a value when the sample concentration is 1 mol / L and a cell having an optical path length of 1 cm is used, and can be obtained by a known method.

[0032] In the present invention and this specification, “a light source emitting light in the wavelength range from ultraviolet light to visible light” means a light source having a light emission wavelength range in at least a part of the ultraviolet wavelength range and at least a part of the visible light wavelength range.

[0033] Hereinafter, the above-mentioned production method will be described in more detail.

[0034] <Base material>

[0035] In the above-mentioned manufacturing method, the polymerizable composition is coated on a substrate to form a coating layer. As for the substrate, it can be selected according to the type of optical article. Optical articles include various articles such as eyeglass lenses, goggles, the brim (brim) part of a sun hat, and a shielding member of a helmet. As an example of a substrate, the eyeglass lens substrate can be a plastic lens substrate or a glass lens substrate. The glass lens substrate can be, for example, a lens substrate made of inorganic glass. As a lens substrate, a plastic lens substrate is preferred from the viewpoint of being lightweight, not easy to break, and easy to handle. As plastic lens substrates, there can be listed styrene resins represented by (meth) acrylic resins, polycarbonate resins, allyl resins, allyl carbonate resins such as diethylene glycol bisallyl carbonate resin (CR-39), vinyl resins, polyester resins, polyether resins, carbamate resins obtained by reacting isocyanate compounds with hydroxy compounds such as diethylene glycol, thiocarbamate resins obtained by reacting isocyanate compounds with polythiol compounds, and cured products (generally referred to as transparent resins) formed by curing a curable composition containing a (thio) epoxy compound having one or more disulfide bonds in the molecule. As lens substrates, undyed substrates (colorless lenses) or dyed substrates (dyed lenses) can be used. The refractive index of the lens substrate can be, for example, about 1.50 to 1.75. However, the refractive index of the lens substrate is not limited to the above range, and can be within the above range or deviate above or below the above range. In the present invention and this specification, the refractive index refers to the refractive index relative to light with a wavelength of 500 nm. The lens substrate may be a lens having refractive power (so-called prescription lens) or a lens having no refractive power (so-called non-prescription lens).

[0036] The spectacle lens may be a single-focus lens, a multi-focus lens, a progressive-power lens, or any other lens. The type of lens may be determined based on the surface shapes of both sides of the lens substrate. In addition, the surface of the lens substrate may be any of a convex surface, a concave surface, and a flat surface. For a conventional lens substrate and a spectacle lens, the object-side surface is a convex surface and the eyeball-side surface is a concave surface, but the present invention is not limited thereto. When the spectacle lens is manufactured by the above-mentioned manufacturing method, the coating layer of the polymerizable composition may be formed on the surface side of the lens substrate on the object side and / or the surface side on the eyeball side.

[0037] The coating layer of the polymerizable composition may be directly provided on the surface of the substrate, or may be provided indirectly via one or more other layers formed on the substrate. Examples of other layers include a hard coating layer, and a primer layer for improving the adhesion between the cured layer formed by curing the polymerizable composition and the substrate. In addition, a substrate with a hard coating layer may be used as the substrate.

[0038] [Formation of coating layer of polymerizable composition]

[0039] <Coating method>

[0040] As a coating method of the polymerizable composition, a known coating method such as a spin coating method and a dip coating method can be adopted. From the viewpoint of coating uniformity, the spin coating method is preferred.

[0041] <Polymerizable composition>

[0042] (Polymerizable compound)

[0043] In the present invention and this specification, "polymerizable composition" refers to a composition containing one or more polymerizable compounds. "Polymerizable compound" refers to a compound having one or more polymerizable groups in one molecule. In the above-mentioned production method, a polymerizable composition containing at least one polymerizable compound with a molecular weight of 500 or less is used as a polymerizable compound. In the present invention and this specification, the molecular weight of the polymer is the theoretical molecular weight calculated based on the structural formula determined by the structural analysis of the compound or the feed ratio of the raw materials during production. As a specific example of a polymerizable compound with a molecular weight of 500 or less, (meth)acrylate can be cited. In the present invention and this specification, "(meth)acrylate" is used in the sense of including acrylate and methacrylate. "Acrylate" refers to a compound having one or more acryloyl groups in one molecule. "Methacrylate" refers to a compound having one or more methacryloyl groups in one molecule. With respect to (meth)acrylate, the number of functional groups is the number of groups selected from acryloyl and methacryloyl contained in one molecule. In the present invention and this specification, "methacrylate" refers to a compound containing only methacryloyl as a (meth)acryloyl group, and a compound containing both acryloyl and methacryloyl as a (meth)acryloyl group is called an acrylate. Acryloyl can be contained in the form of an acryloyloxy group, and methacryloyl can be contained in the form of a methacryloyloxy group. The "(meth)acryloyl" described below is used to mean that it includes acryloyl and methacryloyl groups, and the "(meth)acryloyloxy" is used to mean that it includes acryloyloxy and methacryloyloxy groups. In addition, unless otherwise specified, the group described may have a substituent or may be unsubstituted. In the case where a certain group has a substituent, as a substituent, an alkyl group (for example, an alkyl group having 1 to 6 carbon atoms), a hydroxyl group, an alkoxy group (for example, an alkoxy group having 1 to 6 carbon atoms), a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom), a cyano group, an amino group, a nitro group, an acyl group, a carboxyl group, etc. In addition, with respect to a group having a substituent, "the number of carbon atoms" refers to the number of carbon atoms of the part not containing the substituent.

[0044] As specific examples of polymerizable compounds having a molecular weight of 500 or less, the following components B and C can be cited. In addition, the polymerizable composition used to form the coating layer in the above-mentioned manufacturing method may contain only one or more polymerizable compounds having a molecular weight of 500 or less as polymerizable compounds in one embodiment. In another embodiment, the polymerizable composition used to form the coating layer in the above-mentioned manufacturing method may contain one or more polymerizable compounds having a molecular weight of 500 or less, and one or more polymerizable compounds having a molecular weight of more than 500 as polymerizable compounds. As specific examples of polymerizable compounds having a molecular weight of more than 500, the following component A can be cited. Hereinafter, polymerizable compounds having a molecular weight of 500 or less are referred to as "low molecular weight polymerizable compounds", and polymerizable compounds having a molecular weight of more than 500 are referred to as "high molecular weight polymerizable compounds". In the case where the polymerizable composition used to form the coating layer in the above-mentioned manufacturing method contains only low molecular weight polymerizable compounds as polymerizable compounds, the total amount of polymerizable compounds is set to 100% by mass, and the content rate of low molecular weight polymerizable compounds (the total of them when two or more low molecular weight polymerizable compounds are included) is 100% by mass. On the other hand, when the polymerizable composition for forming the coating layer in the above-mentioned manufacturing method contains a low molecular weight polymerizable compound and a high molecular weight polymerizable compound as the polymerizable compound, the total amount of the polymerizable compound is set to 100 mass%, and the content of the high molecular weight polymerizable compound (when containing two or more high molecular weight polymerizable compounds, their total) can be 50 mass% or less, or more than 50 mass%, or more than 60 mass%. In addition, the content of the above-mentioned high molecular weight polymerizable compound can be, for example, less than 90 mass%, less than 85 mass%, less than 80 mass%, or less than 75 mass%. When the polymerizable composition for forming the coating layer in the above-mentioned manufacturing method contains a low molecular weight polymerizable compound and a high molecular weight polymerizable compound, the total amount of the polymerizable compound is set to 100 mass%, and the content of the low molecular weight polymerizable compound (when containing two or more low molecular weight polymerizable compounds, their total) can exceed 50 mass%, or less than 50 mass%, or less than 40 mass%, and can be more than 5 mass%, more than 10 mass%, or more than 15 mass%.

[0045] Ingredient A

[0046] Component A is a non-cyclic (meth)acrylate having a molecular weight exceeding 500. In the present invention and this specification, "non-cyclic" means not containing a cyclic structure. In contrast, "cyclic" means containing a cyclic structure. Non-cyclic (meth)acrylate refers to a monofunctional or higher (meth)acrylate that does not contain a cyclic structure.

[0047] Component A may be a monofunctional or difunctional or higher (meth)acrylate, preferably a difunctional or trifunctional (meth)acrylate, and more preferably a difunctional (meth)acrylate. As a specific example of component A, polyalkylene glycol di(meth)acrylate may be cited. For example, polyalkylene glycol di(meth)acrylate may be represented by the following formula 2.

[0048] [Chemical formula 1]

[0049] (Formula 2)

[0050]

[0051] In formula 2, R 3 and R 4 Each independently represents a hydrogen atom or a methyl group, R represents an alkylene group, and n represents the number of repeating units of the alkoxy group represented by RO, which is 2 or more. As the alkylene group represented by R, ethylene, propylene, tetramethylene, etc. can be listed. n can be 2 or more and, for example, 30 or less, 25 or less, or 20 or less. Specific examples of polyalkylene glycol di(meth)acrylates include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, etc. In component A, as a (meth)acryloyl group, only an acryloyl group may be included, only a methacryloyl group may be included, or both an acryloyl group and a methacryloyl group may be included.

[0052] The molecular weight of component A may exceed 500, and may be 510 or more, 520 or more, 550 or more, 570 or more, 600 or more, 630 or more, or 650 or more. From the viewpoint of increasing the hardness of the cured layer, the molecular weight of component A may be, for example, 2000 or less, 1500 or less, 1200 or less, 1000 or less, or 800 or less.

[0053] Ingredient B

[0054] Component B is a (meth)acrylate represented by the following formula 1 having a molecular weight of 500 or less.

[0055] [Chemical formula 2]

[0056] (Formula 1)

[0057]

[0058] In formula 1, R 1 and R 2 Each independently represents a hydrogen atom or a methyl group, and m represents an integer greater than 1. m may be greater than 1 and, for example, less than 10, less than 9, less than 8, less than 7, or less than 6.

[0059] The molecular weight of component B is 500 or less, and may be 450 or less, 400 or less, 350 or less, or 300 or less. Alternatively, the molecular weight of component B may be, for example, 100 or more, 150 or more, or 200 or more.

[0060] Component B may contain only an acryloyl group as a (meth)acryloyl group, may contain only a methacryloyl group as a (meth)acryloyl group, or may contain both an acryloyl group and a methacryloyl group as a (meth)acryloyl group. Specific examples of component B include 1,9-nonanediol di(meth)acrylate (also referred to as "nonamethylene glycol di(meth)acrylate"), 1,6-hexanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate.

[0061] Ingredient C

[0062] Component C is a trifunctional to pentafunctional (meth)acrylate having a molecular weight of 500 or less, preferably a trifunctional or tetrafunctional (meth)acrylate, and more preferably a trifunctional (meth)acrylate. Specific examples of component C include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, etc. The molecular weight of component C is 500 or less, for example, it can be in the range of 200 to 400, but is not limited to this range. As a (meth)acryloyl group, component C may contain only an acryloyl group, may contain only a methacryloyl group, or may contain an acryloyl group and a methacryloyl group.

[0063] The total amount of the composition is set to 100 mass%, and the content of the polymerizable compound in the above-mentioned polymerizable composition can be, for example, 80 mass% or more, 85 mass% or more, or 90 mass% or more. In addition, the total amount of the composition is set to 100 mass%, and the content of the polymerizable compound in the above-mentioned polymerizable composition can be, for example, 99 mass% or less, 95 mass% or less, 90 mass% or less, or 85 mass% or less. In the present invention and this specification, with respect to the content, the "total amount of the composition" refers to the total amount of all components other than the solvent in the composition containing the solvent. The above-mentioned composition may contain a solvent or may not contain a solvent. In the case of containing a solvent, as a usable solvent, any solvent can be used in any amount as long as it does not hinder the polymerization reaction of the polymerizable composition.

[0064] <Photopolymerization initiator>

[0065] The polymerizable composition for forming the coating layer in the above-mentioned manufacturing method contains a photopolymerization initiator having absorption in at least a part of the wavelength range of visible light (i.e., the wavelength range of more than 400 nm and less than 780 nm) as a polymerization initiator. As such a polymerization initiator, from the viewpoint of making the polymerization reaction proceed well in the initial stage of polymerization using an ultraviolet cut filter, it is preferred that the molar absorption coefficient at a wavelength of 420 nm is 160 L·mol -1 cm -1 In addition, the above molar absorption coefficient can be, for example, 5300 L·mol -1 cm -1 Below. In addition, from the viewpoint of making the polymerization reaction after the ultraviolet cutoff filter is removed well, it is preferred to use a compound that also has absorption in at least a part of the wavelength range of ultraviolet rays as the above-mentioned photopolymerization initiator. As a photopolymerization initiator, a photoradical polymerization initiator is preferred. As a photoradical polymerization initiator, for example, α-hydroxyketone, α-aminoketone, oxime ester, phosphine oxide, 2,4,5-triaryl imidazole dimer, benzophenone compound, quinone compound, benzoin ether, benzoin compound, benzyl compound, acridine compound, etc. are mentioned. The total amount of the composition is set to 100% by mass, and the content of the photopolymerization initiator can be, for example, in the range of 0.1 to 5% by mass.

[0066] <Ultraviolet absorbing compounds>

[0067] The polymerizable composition used to form the coating layer in the above-mentioned manufacturing method contains an ultraviolet absorbing compound. For example, as an ultraviolet absorbing compound, a photochromic compound can be cited. A photochromic compound is a compound having the following properties: coloring (coloring) when irradiated with light in a wavelength range with photoresponsiveness, and fading without irradiation (photochromic performance). As an example, a photochromic compound is irradiated with light such as sunlight, and undergoes an excited state and its structure is converted into a colored body. The structure after the structural conversion after irradiation with light can be called a "colored body". In contrast, the structure before irradiation with light can be called a "colorless body". It should be noted that, with respect to the colorless body, "colorless" is not limited to being completely colorless, but also includes the case where the color is lighter than the colored body. With respect to the photochromic compound, the absorption characteristic refers to the absorption characteristic with respect to the colorless body. That is, the photochromic compound is an ultraviolet absorbing compound, which means that in the structure of the colorless body, there is absorption at least at a wavelength of 400nm. As photochromic compounds, fulgimide compounds, spiro Compounds having a known skeleton showing photochromic properties, such as oxazine compounds, chromene compounds, and indeno-condensed naphthopyran compounds. The photochromic compound may be used alone or in combination of two or more.

[0068] The content of the ultraviolet absorbing compound in the polymerizable composition for forming the coating layer in the above production method can be, for example, about 0.1 to 15% by mass, based on 100% by mass of the total amount of the composition, but is not limited to this range.

[0069] The polymerizable composition may further contain any known additives that are usually added to polymerizable compositions, such as surfactants, antioxidants, free radical scavengers, light stabilizers, anti-coloring agents, antistatic agents, fluorescent dyes, dyes, pigments, fragrances, plasticizers, silane coupling agents, etc. As these additives, known compounds may be used.

[0070] The polymerizable composition can be prepared by mixing the various components described above simultaneously or sequentially in any order.

[0071] [Curing treatment using light]

[0072] In the above production method, the coating layer of the polymerizable composition is irradiated with light from a light source emitting light in a wavelength range from ultraviolet light to visible light, and during the irradiation, an ultraviolet cut filter is arranged between the light source and the coating layer for at least a portion of the time from the start of the irradiation. Thus, the irradiation of the coating layer with ultraviolet light can be blocked in the initial stage of polymerization, so that the influence caused by the aggregation of molecules of the ultraviolet absorbing compound can be eliminated or reduced, and the polymerization reaction of the low molecular weight polymerizable compound can be carried out well.

[0073] <Light source>

[0074] In the above manufacturing method, a light source that emits light in the wavelength range from ultraviolet light to visible light is used. As described above, the light source is a light source that has a light emission band in at least a part of the wavelength range of ultraviolet light and at least a part of the wavelength range of visible light, for example, it can be a light source that has a light emission band in at least a part of the wavelength range of 300 nm to 600 nm (including at least a part of the wavelength range of ultraviolet light and at least a part of the wavelength range of visible light). As an example of the above light source, a metal halide lamp can be cited.

[0075] <UV cut filter>

[0076] As described above, the UV cutoff filter refers to a filter whose transmittance to light in the wavelength range of ultraviolet rays (above 300nm and below 400nm) is less than 5%. The inventors of the present invention believe that, in the initial stage of polymerization, using the above-mentioned filter to block the light in the wavelength range of ultraviolet rays in the light irradiated from the above-mentioned light source to the coating layer helps to suppress the generation of defects on the surface of the cured layer formed by curing the coating layer by photopolymerization. The details of this point are described in detail above. As an ultraviolet cutoff filter, any filter having the above-mentioned ultraviolet cutoff property can be used, and a commercially available product or a filter made by a known method can be used. In addition, the ultraviolet cutoff property of the ultraviolet cutoff filter can be a cutoff property based on reflection, a cutoff property based on absorption, or a cutoff property based on both reflection and absorption. In order to allow at least a portion of the light in the wavelength range of visible light in the light irradiated from the light source to pass through the ultraviolet cutoff filter and irradiate the coating layer in the initial stage of polymerization, the ultraviolet cutoff filter preferably has a transmittance of at least a portion of the light in the wavelength range of visible light (i.e., a wavelength range exceeding 400nm and below 780nm) of 5% or more, more preferably in the order of 10% or more, 20% or more, 30% or more, and 40% or more. The transmittance may be, for example, 100% or less, less than 100%, or 90% or less.

[0077] <Curing treatment>

[0078] For the illumination from the above-mentioned light source to the above-mentioned coating layer, an ultraviolet cut-off filter is arranged between the light source and the coating layer during at least a portion of the period from the start of illumination to block the irradiation of ultraviolet rays to the coating layer. It is also possible to illuminate the coating layer by arranging an ultraviolet cut-off filter between the light source and the coating layer during the entire period of illumination from the light source. From the viewpoint of making the polymerization reaction of the polymerizable compound proceed better, it is preferred to illuminate the coating layer by arranging an ultraviolet cut-off filter between the light source and the coating layer during a portion of the period from the start of illumination, and then remove the ultraviolet cut-off filter from the light source and the coating layer, and illuminate the coating layer without sandwiching the ultraviolet cut-off filter. In this case, for example, when the start of illumination is set to 0 seconds, the time for irradiating the coating layer from the light source via the ultraviolet cut-off filter can be set to more than 0 seconds and less than 5 seconds, but it is not limited thereto. The time for irradiating after removing the ultraviolet cut-off filter from the light source and the coating layer is not particularly limited.

[0079] Irradiation can be implemented by placing the irradiated object (i.e., a laminate comprising at least a substrate and a coating layer of the above-mentioned polymerizable composition) in an irradiation device. As the atmosphere in the irradiation device, a nitrogen atmosphere, an atmospheric atmosphere, etc. can be cited. The above-mentioned nitrogen atmosphere and the nitrogen atmosphere described later can be, for example, a nitrogen atmosphere with an oxygen concentration of less than 500 ppm (ppm is a volume basis). By performing nitrogen purging, the atmosphere in the device can be a nitrogen atmosphere. The configuration and removal of the ultraviolet cutoff filter between the light source and the coating layer can be performed automatically by providing an ultraviolet cutoff filter moving mechanism in the irradiation device and utilizing such a mechanism, or it can also be performed manually.

[0080] The thickness of the cured layer formed by the above-mentioned curing treatment may be determined according to the type of the cured layer. For example, when the cured layer is a layer containing a photochromic compound as an ultraviolet absorbing compound, that is, a photochromic layer, the thickness of the photochromic layer is preferably in the range of 5 to 80 μm, and more preferably in the range of 20 to 60 μm.

[0081] [Layers that can be set arbitrarily]

[0082] In the manufacturing method of the optical article, one or more layers may be further formed on the above-described cured layer. Such layers include: a hard coat layer, a protective layer, an antireflection layer, a water-repellent or hydrophilic antifouling layer, an antifogging layer, a primer layer for improving interlayer adhesion, and other layers known as functional layers of optical articles.

[0083] One form of the optical article is a spectacle lens. In addition, as one form of the optical article, a lens for goggles, a brim (brim) portion of a sun hat, a shielding member of a helmet, etc. can also be cited. In the case where the cured layer contains a photochromic compound as the ultraviolet absorbing compound, the optical article can be suitably used as an optical article with an anti-glare function.

[0084] By combining the above-mentioned eyeglass lenses with frames, eyeglasses can be manufactured. By providing such eyeglasses with, for example, an eyeglass lens having a cured layer (i.e., a photochromic layer) containing a photochromic compound, the photochromic compound contained in the photochromic layer can be colored by exposure to sunlight outdoors, thereby exerting an anti-glare effect like sunglasses, and when returning indoors, the photochromic compound can fade and restore transmittance. With regard to the configuration of eyeglasses, frames, etc., known techniques can be applied.

[0085] Example

[0086] The present invention will be further described below with reference to examples. However, the present invention is not limited to the embodiments shown in the examples. Unless otherwise specified, the following steps and evaluations were performed at room temperature (20°C ± 5°C) in the atmosphere.

[0087] [Preparation of polymerizable composition]

[0088] <Polymerizable composition A>

[0089] In a plastic container, polyethylene glycol dimethacrylate (in the above formula 2, n=14, R is ethylene, R is 3 and R 4 As component B, 68 parts by mass of nonamethylene glycol dimethacrylate (molecular weight 296) and as component C, 12 parts by mass of trimethylolpropane trimethacrylate (molecular weight 332) were used to obtain a mixture of polymerizable compounds.

[0090] With respect to the above mixture, 0.8 parts by mass of a photoradical polymerization initiator (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819 manufactured by IGM Resin BV)), 1.0 parts by mass of an antioxidant (ethylenebis(oxyethylene)bis(3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate), 1.0 parts by mass of a light stabilizer (a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate), and 3.7 parts by mass of a photochromic compound (an indeno-fused naphthopyran compound represented by the structural formula described in the specification of U.S. Patent No. 5,645,767) as an ultraviolet absorbing compound were mixed and stirred thoroughly. Then, degassing was performed using a rotation-revolution stirring degassing device.

[0091] Through the above operations, a polymerizable composition A was prepared.

[0092] <Polymerizable composition B>

[0093] Polymerizable composition B was prepared in the same manner as in the preparation of polymerizable composition A except that the total amount of the polymerizable compound was 100 parts by mass of nonamethylene glycol dimethacrylate (molecular weight: 296) as component B.

[0094] <Polymerizable composition C>

[0095] The total amount of the polymerizable compound is polyethylene glycol dimethacrylate as component A (in the above formula 2, n=14, R is ethylene, R 3 and R 4 A polymerizable composition C was prepared in the same manner as the preparation of the polymerizable composition A, except that the polymerizable composition C was 100 parts by mass and the molecular weight was 771 and 100 parts by mass. The polymerizable composition C is a polymerizable composition that does not contain a polymerizable compound having a molecular weight of 500 or less.

[0096] [Filter]

[0097] The filter A and the filter B described below are both commercially available products (Filter A: Sharp Cut Filter L39 (thickness 2.5 mm) manufactured by HOYA Corporation, Filter B: Sharp Cut Filter L42 (thickness 2.5 mm) manufactured by HOYA Corporation). Figure 1 The transmission spectra of filter A and filter B are shown in FIG. Figure 1 The transmission spectrum shown is a transmission spectrum obtained by measuring in the wavelength range of 300 to 800 nm using a UV-visible near-infrared spectrophotometer (Hitachi High-Tech Co., Ltd. UH4150) with a slit width of 5 nm and a scanning speed of 300 nm / min. Filter A is a filter that is an ultraviolet cut filter, and filter B is a filter that is not an ultraviolet cut filter.

[0098] [Photopolymerization initiator]

[0099] Figure 2 The absorption spectrum of the above-mentioned photoradical polymerization initiator Omnirad819 manufactured by IGM Resin BV is shown in FIG. The molar absorption coefficient at a wavelength of 420 nm is 169 L·mol -1 cm -1 .

[0100] It was prepared as follows Figure 2 Absorption spectrum shown.

[0101] A polymerizable composition A that does not contain a photochromic compound was used as a measurement sample and placed in a synthetic quartz cell (optical path length 0.05 mm), and the absorbance was measured. The measurement was performed using an ultraviolet-visible near-infrared spectrophotometer (Hitachi High-Tech Co., Ltd. UH4150) with a slit width of 5 nm and a scanning speed of 300 nm / min in the wavelength range of 300 to 800 nm. The same measurement was also performed on a reference sample that had the same composition as the measurement sample except that it did not contain a polymerization initiator. The value obtained by subtracting the absorbance obtained for the reference sample from the absorbance obtained for the measurement sample was taken as the absorbance of the polymerization initiator. Based on the measured absorbance, the molar absorption coefficient at each wavelength was calculated using the Lambert-Beer law, and a Figure 2 Absorption spectrum shown.

[0102] [Production of eyeglass lenses (photochromic lenses)]

[0103] <Example 1>

[0104] The polymerizable composition A was applied to the convex surface (object side surface) of a plastic lens substrate (trade name: PHOENIX, manufactured by HOYA Corporation; center wall thickness: 2.0 mm, radius: 70 mm, S0.00) by spin coating to form a coating layer.

[0105] A metal halide lamp was used as the light source. The metal halide lamp has a light emission wavelength band in at least a portion of the wavelength range of 300 nm to 600 nm (including at least a portion of the wavelength range of ultraviolet light and at least a portion of the wavelength range of visible light).

[0106] In the illumination device, the laminate of the substrate and the coating layer as the irradiated object was arranged so that the coating layer side was facing upward. During the period from the start of illumination (0 seconds) to 1 second, filter A was arranged between the light source and the coating layer to irradiate. Then, filter A was removed from between the light source and the coating layer, and light was continuously irradiated from the light source.

[0107] In this way, an eyeglass lens (photochromic lens) having a photochromic layer as a cured layer on a substrate was produced.

[0108] <Comparative Example 1>

[0109] A spectacle lens was produced as described in Example 1 except that filter B was used instead of filter A.

[0110] <Comparative Example 2>

[0111] A spectacle lens was produced in the same manner as described in Example 1 except that the filter A was not disposed between the light source and the coating layer and the illumination was performed for 1 second from the start of illumination.

[0112] <Comparative Example 3>

[0113] A spectacle lens was produced in the same manner as described in Comparative Example 2, except that the polymerizable composition B was used instead of the polymerizable composition A as the polymerizable composition.

[0114] <Example 2>

[0115] A spectacle lens was produced in the same manner as described in Example 1, except that the polymerizable composition B was used instead of the polymerizable composition A as the polymerizable composition.

[0116] <Reference Example 1>

[0117] A spectacle lens was produced in the same manner as described in Comparative Example 2, except that the polymerizable composition C was used instead of the polymerizable composition A as the polymerizable composition.

[0118] [Appearance evaluation]

[0119] The appearance of the eyeglass lenses produced in the above-mentioned embodiments, comparative examples and reference examples was evaluated by naked eye observation under indoor fluorescent lights and by projection inspection using a projector inspection machine (Optical ModuleX BA-H25 manufactured by Ushio Electric Co., Ltd.). With the eyeglass lenses arranged between the light source and the screen of the projector inspection machine, the projection inspection was performed by emitting 800 to 1200 Lux of light from the light source. The evaluation criteria are as follows.

[0120] Good: No turbidity or shadow was observed in the evaluation under indoor fluorescent light. No turbidity or shadow was observed in the projection test either.

[0121] Defective: Turbidity and / or shadows were observed in at least one of the evaluation under indoor fluorescent light and the projection inspection.

[0122] The above results are shown in Table 1.

[0123] [Table 1]

[0124]

[0125] The performance of the spectacle lenses produced in Example 1 and the spectacle lenses produced in Comparative Example 2 as photochromic lenses was evaluated by the following methods.

[0126] (1) Visible light transmittance without irradiation

[0127] The transmittance of each eyeglass lens was measured before the following color density measurement (measurement wavelength: 550 nm) using a spectrophotometer manufactured by Otsuka Electronics Co., Ltd. The larger the value of the transmittance measured in this way (hereinafter referred to as "initial transmittance"), the better the visible light transmittance under no irradiation.

[0128] (2) Color concentration

[0129] The color density was evaluated by the following method based on JIS T7333:2005.

[0130] For the photochromic layer of each eyeglass lens (a cured layer formed by curing the above-mentioned polymerizable composition), the surface of the photochromic layer was irradiated with light for 15 minutes (900 seconds) through a gas filter using a xenon lamp to color the photochromic compound in the photochromic layer. The transmittance during the color development was measured using a spectrophotometer manufactured by Otsuka Electronics Co., Ltd. (measurement wavelength: 550 nm). The above-mentioned irradiation was performed in accordance with JIS T7333: 2018 so that the irradiance and the allowable difference in irradiance were the values ​​shown in Table 2 below.

[0131] [Table 2]

[0132] Wavelength range (nm) <![CDATA[Irradiance (W / m 2 )]]> <![CDATA[Permissible difference in irradiance (W / m 2 )]]> 300~340 <2.5 - 340~380 5.6 ±1.5 380~420 12 ±3.0 420~460 12 ±3.0 460~500 26 ±2.6

[0133] The smaller the value of the measured transmittance (hereinafter referred to as "transmittance during color development") is, the higher the concentration of the photochromic compound developing color.

[0134] (3) Fading speed (half-decay time)

[0135] The fading speed of each spectacle lens was evaluated by the method described below.

[0136] After measuring the transmittance during color development in (2) above, the time (half-life time) required from the time when light irradiation is stopped until the transmittance (measurement wavelength: 550nm) reaches [(initial transmittance - transmittance during color development) / 2] is measured. The smaller the half-life time value measured in this way, the faster the fading speed can be considered.

[0137] The above results are shown in Table 3.

[0138] [Table 3]

[0139]

[0140] According to the results shown in Table 3, it can be confirmed that the spectacle lenses produced in Example 1 show the same color development concentration as the spectacle lenses produced in Comparative Example 2, and are superior in visible light transmittance without irradiation and have a faster fading speed than the spectacle lenses produced in Comparative Example 2. The present inventors believe that these results are due to the formation of a cured layer (photochromic layer) by the method described above, thereby suppressing the aggregation of molecules of the photochromic compound and allowing the polymerization reaction of the low molecular weight polymerizable compound to proceed well.

[0141] The film thickness of the photochromic layer of the eyeglass lens produced in Example 1 and the eyeglass lens produced in Comparative Example 2 was measured using a reflective non-contact film thickness measuring device. The film thickness measurement results are shown in FIG. Figure 3 As a reference, the measurement results of the substrate only without forming a photochromic layer are also shown. Figure 3 .

[0142] like Figure 3 As shown in FIG. 1 , a signal was detected for the eyeglass lens produced in Example 1, and thus the film thickness of the photochromic layer could be measured. In contrast, for the eyeglass lens produced in Comparative Example 2, a signal was detected for the eyeglass lens produced in Example 1, and thus the film thickness of the photochromic layer could be measured. Figure 3 Therefore, regarding the spectacle lens of Comparative Example 2, it is difficult to measure the film thickness of the photochromic layer using a reflective non-contact film thickness measuring device.

[0143] The above results are considered to be because the spectacle lens produced in Example 1 has a higher surface smoothness of the photochromic layer than the spectacle lens produced in Comparative Example 2.

[0144] Finally, summarize the above methods.

[0145] [1] A method for manufacturing an optical article, the method comprising:

[0146] coating the polymerizable composition on a substrate to form a coating layer; and

[0147] The coating layer is irradiated with light from a light source emitting light in a wavelength range from ultraviolet light to visible light, thereby subjecting the coating layer to a curing treatment.

[0148] The polymerizable composition comprises:

[0149] One or more polymerizable compounds having a molecular weight of 500 or less,

[0150] A photopolymerization initiator having absorption in at least a part of the wavelength range of visible light, and

[0151] UV absorbing compounds,

[0152] In the irradiation, the irradiation is performed with an ultraviolet cut filter disposed between the light source and the coating layer during at least a portion of the period from the start of the irradiation.

[0153] [2] The method for manufacturing an optical article according to [1], wherein:

[0154] The above-mentioned ultraviolet absorbing compound is a photochromic compound.

[0155] [3] The method for producing an optical article according to [1] or [2], wherein:

[0156] The wavelength band of the light emitted by the light source includes a wavelength range of 300 nm to 600 nm.

[0157] [4] The method for producing an optical article according to any one of [1] to [3], wherein:

[0158] The irradiation may further include irradiating light with the filter disposed thereon, removing the filter from between the light source and the coating layer.

[0159] [5] The method for producing an optical article according to any one of [1] to [4], wherein:

[0160] The polymerizable compound having a molecular weight of 500 or less is a (meth)acrylate.

[0161] [6] The method for producing an optical article according to any one of [1] to [5], wherein:

[0162] The polymerizable composition further contains one or more polymerizable compounds having a molecular weight exceeding 500.

[0163] [7] The method for producing an optical article according to any one of [1] to [6], wherein:

[0164] The above optical articles are eyeglass lenses.

[0165] [8] The method for producing an optical article according to any one of [1] to [6], wherein:

[0166] The above-mentioned optical article is a lens for goggles.

[0167] [9] The method for producing an optical article according to any one of [1] to [6], wherein:

[0168] The optical article is the brim portion of a sun hat.

[0169]

[10] The method for producing an optical article according to any one of [1] to [6], wherein:

[0170] The optical article is a shielding member of a helmet.

[0171] The various modes and aspects described in this specification may be combined in any combination of two or more.

[0172] The embodiments disclosed this time are merely illustrative in all aspects and are not intended to limit the scope of the present invention. The scope of the present invention is intended to include all modifications that are not described above but are indicated by the claims and are within the meaning and scope equivalent to the claims.

[0173] Industrial Applicability

[0174] The present invention is useful in the technical fields of glasses, goggles, sun hats, helmets, etc.

Claims

1. A method for manufacturing an optical article, the method comprising: Applying the polymerizable composition on a substrate to form a coating layer; and The coating layer is cured by irradiating the coating layer with light from a light source, the light source emitting light in a wavelength range from ultraviolet light to visible light, The polymerizable composition comprises: One or more polymerizable compounds having a molecular weight of 500 or less, A photopolymerization initiator having absorption in at least a part of the wavelength range of visible light, and UV absorbing compounds, In the irradiation, the irradiation is performed with an ultraviolet cut filter disposed between the light source and the coating layer during at least a portion of a period from the start of the irradiation.

2. The method for manufacturing an optical article according to claim 1, wherein: The ultraviolet absorbing compound is a photochromic compound.

3. The method for manufacturing an optical article according to claim 1 or 2, wherein: The wavelength band of the light emitted by the light source includes a wavelength range of 300 nm to 600 nm.

4. The method for producing an optical article according to any one of claims 1 to 3, wherein: In the irradiation, after the irradiation with the filter arranged, the method further comprises removing the filter from between the light source and the coating layer to irradiate the light.

5. The method for producing an optical article according to any one of claims 1 to 4, wherein: The polymerizable compound having a molecular weight of 500 or less is (meth)acrylate.

6. The method for producing an optical article according to any one of claims 1 to 5, wherein: The polymerizable composition further comprises one or more polymerizable compounds having a molecular weight exceeding 500.

7. The method for producing an optical article according to any one of claims 1 to 6, wherein: The optical article is a spectacle lens.

8. The method for producing an optical article according to any one of claims 1 to 6, wherein: The optical article is a lens for goggles.

9. The method for producing an optical article according to any one of claims 1 to 6, wherein: The optical article is a brim portion of a sun hat.

10. The method for producing an optical article according to any one of claims 1 to 6, wherein: The optical article is a shielding member of a helmet.