Optical film and method for manufacturing optical film

By introducing regions with different orientation states and content ratios of liquid crystal polymers into the diffusion layer of the optical film, and controlling the polymerization of liquid crystal polymers by electric field intensity, the problem of difficulty in forming fine scattering degree patterns in the prior art is solved, and the optical film is realized patterned degree of scattering.

CN118891547APending Publication Date: 2024-11-01NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028349.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to form PDLC films with large and small parts with fine patterns, and it is impossible to effectively pattern the scattering degree of optical film.

Method used

By introducing regions with different orientation states and content ratios of liquid crystal polymers into the diffusion layer of the optical film, the liquid crystal polymer is polymerized by regions with different electric field strengths, thereby forming regions with different scattering degrees in the optical film.

Benefits of technology

The precise control of the scattering degree in different regions in the optical film is achieved, and the orientation state and content ratio of the liquid crystal polymer can be adjusted according to the pattern requirements, thereby obtaining the desired scattering degree pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891547A_ABST
    Figure CN118891547A_ABST
Patent Text Reader

Abstract

The present invention provides an optical film having a diffusion layer containing a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles containing a liquid crystal polymer that is a polymer of a polymerizable liquid crystal compound, the diffusion layer has a plurality of regions in which the orientation state of the liquid crystal polymer and / or the content ratio of the liquid crystal polymer differ.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical film having a diffusion layer and a method for producing the optical film. Background Art

[0002] The PDLC film having a polymer dispersed liquid crystal (PDLC; hereinafter sometimes referred to as "PDLC") layer between a pair of transparent electrode layers is a type of dimming film. By switching the voltage applied state and the non-applied state, it is possible to switch between a state where light is scattered (scattered state) and a state where light is transmitted (non-scattered state or transparent state). Specifically, the PDLC layer includes a polymer matrix and droplets of liquid crystal compounds dispersed in the polymer matrix (hereinafter sometimes referred to as "liquid crystal droplets"), and the liquid crystal droplets become scattering particles due to the difference in refractive index between the liquid crystal compounds in the liquid crystal droplets and the polymer matrix, thereby causing light scattering.

[0003] By utilizing the above scattering effect, the PDLC film can be used as a diffuser. For example, Patent Document 1 proposes to make a PDLC film including a portion with a large scattering degree and a portion with a small scattering degree by changing the ultraviolet irradiation intensity when making a polymer matrix according to the location, and use the PDLC film as a diffuser for a direct-type backlight.

[0004] However, in the technology disclosed in Patent Document 1, it is difficult to form a portion with a large degree of scattering and a small portion in a fine pattern.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-008005 Summary of the invention

[0008] Problems to be solved by the invention

[0009] A main object of the present invention is to provide an optical film having a diffusion layer and having regions with different degrees of scattering in a desired pattern.

[0010] Solutions to the problem

[0011] According to one aspect of the present invention, an optical film is provided, which has a diffusion layer, wherein the diffusion layer includes a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles include a liquid crystal polymer which is a polymer of a polymerizable liquid crystal compound, and the diffusion layer has a plurality of regions having different orientation states of the liquid crystal polymer and / or a plurality of regions having different content ratios of the liquid crystal polymer.

[0012] In one embodiment, the plurality of regions are arranged in a given pattern.

[0013] In one embodiment, the maximum value of the difference in haze between the portions corresponding to the plurality of regions in a plan view is 10% or more.

[0014] In one embodiment, the dispersed particles further include a liquid crystal compound.

[0015] In one embodiment, the content ratio of the liquid crystal polymer relative to the total content of the liquid crystal polymer and the liquid crystal compound is 5% by weight or more.

[0016] In one embodiment, the total content of the liquid crystal polymer and, if present, the liquid crystal compound in the diffusion layer is 30% by weight to 70% by weight.

[0017] In one embodiment, a first transparent substrate is disposed on the first main surface side of the diffusion layer.

[0018] In one embodiment, a second transparent substrate is disposed on the second main surface side of the diffusion layer.

[0019] In one embodiment, the optical film does not have an electrode layer.

[0020] According to another aspect of the present invention, an optical film is provided, which has a diffusion layer, wherein the diffusion layer comprises a polymer matrix and dispersed particles dispersed in the polymer matrix, wherein the dispersed particles comprise a liquid crystal polymer which is a polymer of a polymerizable liquid crystal compound, and wherein the optical film has a plurality of regions when viewed from above, and the plurality of regions exhibit different hazes corresponding to the orientation state of the liquid crystal polymer.

[0021] According to another aspect of the present invention, an optical film is provided, which has a diffusion layer, wherein the diffusion layer comprises a polymer matrix and dispersed particles dispersed in the polymer matrix, the diffusion layer having regions comprising dispersed particles containing polymerizable liquid crystal compounds, and regions comprising dispersed particles containing liquid crystal polymers which are polymers of the polymerizable liquid crystal compounds, and when viewed from above, these regions exhibit different hazes from each other.

[0022] According to another aspect of the present invention, there is provided a method for manufacturing an optical film, the method comprising:

[0023] Applying a coating liquid including a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent on a first substrate to obtain a coating layer;

[0024] Drying the coating layer to obtain a polymer dispersed liquid crystal layer, the polymer dispersed liquid crystal layer comprising a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound; and

[0025] Voltage is applied from the first main surface side and the second main surface side of the polymer-dispersed liquid crystal layer so as to generate regions with different electric field strengths, thereby polymerizing the polymerizable liquid crystal compound.

[0026] In one embodiment, the voltage is applied using a first electrode disposed on the first main surface side of the polymer dispersed liquid crystal layer and a second electrode disposed on the second main surface side, and the separation distance between the first electrode and the second electrode is controlled in a manner to generate regions with different electric field strengths.

[0027] According to another aspect of the present invention, there is provided a method for manufacturing an optical film, the method comprising:

[0028] Applying a coating liquid including a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent on a first substrate to obtain a coating layer;

[0029] Drying the coating layer to obtain a polymer dispersed liquid crystal layer, the polymer dispersed liquid crystal layer comprising a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound; and

[0030] While voltage is applied to the polymer dispersed liquid crystal layer, an active energy ray is irradiated to a predetermined region to polymerize the polymerizable liquid crystal compound.

[0031] In one embodiment, the coating liquid is an emulsion containing liquid crystal particles containing the polymerizable liquid crystal compound as a dispersoid.

[0032] In one embodiment, the coating liquid further includes a non-polymerizable liquid crystal compound.

[0033] Effects of the Invention

[0034] The optical film of the embodiment of the present invention has a diffusion layer, the diffusion layer includes a polymer matrix, and dispersed particles of a liquid crystal polymer dispersed in the polymer matrix and including a polymerizable liquid crystal compound, and the diffusion layer has a plurality of regions with different orientation states and / or content ratios of the liquid crystal polymer. Since the dispersed particles can show different scattering properties corresponding to the orientation state and / or content ratio of the liquid crystal polymer contained therein, in the optical film having such a structure, the plurality of regions can respectively show different scattering degrees corresponding to the orientation state and / or content ratio of the liquid crystal polymer. Thus, by adjusting the orientation state and / or content ratio of the liquid crystal polymer to a desired pattern, an optical film having regions with different scattering degrees in a desired pattern can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 (a) is a schematic plan view of an example of an optical film according to one embodiment of the present invention, and (b) is a schematic cross-sectional view of the optical film shown in (a).

[0036] Figure 2 It is a schematic cross-sectional view of an example of the optical film which is one embodiment of the present invention.

[0037] Figure 3 It is a schematic cross-sectional view of an example of the optical film which is one embodiment of the present invention.

[0038] Figure 4 It is a schematic cross-sectional view of an example of an optical film according to another embodiment of the present invention.

[0039] Figure 5 This is a schematic diagram for explaining step C of the method for producing an optical film according to one embodiment of the present invention.

[0040] Figure 6 It is a schematic cross-sectional view for explaining an electrode having a protrusion.

[0041] Figure 7 This is a schematic diagram for explaining step III of the method for producing an optical film according to another embodiment of the present invention.

[0042] Explanation of symbols

[0043] 100 Optical Film

[0044] 10 Diffusion layer

[0045] 12 Polymer matrix

[0046] 14 Dispersed particles

[0047] 14' LCD drop

[0048] 14a Liquid crystal compound (non-polymerizable liquid crystal compound)

[0049] 14b Liquid crystal polymer

[0050] 14c Polymerizable liquid crystal compound

[0051] 201st transparent substrate

[0052] 30 2nd transparent substrate

[0053] 40 1st electrode

[0054] 50 2nd electrode

[0055] 60 Power Supply DETAILED DESCRIPTION

[0056] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments. It should be noted that in the present specification, "to" indicating a numerical range includes the numerical values ​​of the upper limit and the lower limit.

[0057] A.Optical film

[0058] According to the first embodiment of the present invention, an optical film is provided, which has a diffusion layer, wherein the diffusion layer includes a polymer matrix and dispersed particles dispersed in the polymer matrix, wherein the dispersed particles include a liquid crystal polymer as a polymer of a polymerizable liquid crystal compound, and the diffusion layer has a plurality of regions with different orientation states of the liquid crystal polymer. The dispersed particles may further include a liquid crystal compound. In the dispersed particles, the liquid crystal compound may be oriented along the liquid crystal polymer. Thus, the dispersed particles can show different scattering properties corresponding to the orientation state of the liquid crystal polymer contained therein, and the optical film having such a structure can show a scattering degree (haze) corresponding to the orientation state of the liquid crystal polymer in the plurality of regions. Thus, in the optical film of the first embodiment, when there are a plurality of regions with different scattering degrees (haze) in the optical film (more specifically the diffusion layer) when viewed from above, it can be referred to as "the diffusion layer has a plurality of regions with different orientation states of the liquid crystal polymer". In addition, the optical film of the first embodiment can be the following optical film: it has a diffusion layer including a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles include a liquid crystal polymer which is a polymer of a polymerizable liquid crystal compound, and the above-mentioned optical film has a plurality of regions when viewed from above, and the plurality of regions have different hazes corresponding to the orientation state of the liquid crystal polymer.

[0059] A-1. Composition of optical film

[0060] Figure 1(a) is a schematic top view of an example of an optical film of the first embodiment, and (b) is a schematic cross-sectional view of the optical film shown in (a). The optical film 100a is composed of a diffusion layer 10 including a polymer matrix 12 and dispersed particles 14 dispersed in the polymer matrix 12, wherein the dispersed particles 14 include a liquid crystal compound 14a and a liquid crystal polymer 14b. The diffusion layer 10 has five regions (A1, A2, B1, B2, C). Among these regions, the orientation states of the liquid crystal polymer 14b in regions A1 and A2 are the same, the orientation states of the liquid crystal polymer 14b in regions B1 and B2 are the same, and the orientation states of the liquid crystal polymer 14b in regions A1 and A2, regions B1 and B2, and region C are different (the relationship between the orientation states of each region: A1 = A2 ≠ B1 = B2 ≠ C).

[0061] Specifically, the liquid crystal polymer 14b in the dispersed particles 14 is oriented approximately perpendicularly to the main surface of the optical film 100a (diffusion layer 10) in the regions A1 and A2, is in a non-oriented state in the region C, and is in an intermediate orientation state in the regions B1 and B2. In addition, the liquid crystal compound 14a in the dispersed particles 14 is oriented along the liquid crystal polymer 14b, and therefore is in the same orientation state as the liquid crystal polymer 14b. As a result, the dispersed particles in the above-mentioned multiple regions (A1, A2, B1, B2, C) can show different scattering properties in each region due to the different orientation states of the liquid crystal polymer and / or the liquid crystal compound. As a result, the optical film 100a, when viewed from above, shows the smallest haze (degree of diffusion) in the portion corresponding to the regions A1 and A2, shows the largest haze in the portion corresponding to the region C, and shows an intermediate haze in the portion corresponding to the regions B1 and B2.

[0062] Figure 2 and Figure 3 Each of them is a schematic cross-sectional view of another example of the optical film according to the first embodiment (dispersed particles are not shown). Figure 2 The optical film 100 b shown has a first transparent base material 20 on the first main surface side of the diffusion layer 10 . Figure 3 The optical film 100c shown has a first transparent substrate 20 on the first main surface side of the diffusion layer 10 and a second transparent substrate 30 on the second main surface side. The diffusion layer 10 and the first transparent substrate 20 and / or the second transparent substrate 30 may be laminated together via an adhesive layer or a pressure-sensitive adhesive layer, or may be laminated together directly without interposing them.

[0063] exist Figure 1In the optical film 100a shown, the dispersed particles 14 include the liquid crystal compound 14a and the liquid crystal polymer 14b, but the dispersed particles 14 may not include the liquid crystal compound 14a. In addition, in the optical film according to the embodiment of the present invention, the orientation of the liquid crystal compound in the dispersed particles can be controlled by the liquid crystal polymer, so it is not necessary to control the orientation of the liquid crystal compound by applying a voltage. Therefore, the optical film according to the embodiment of the present invention may not have an electrode layer regardless of whether the dispersed particles include the liquid crystal compound.

[0064] It should be noted that in Figure 1 In the diffusion layer of the embodiment shown, there are three ways for the orientation state of the liquid crystal polymer in the dispersed particles, but the present invention is not limited to such an embodiment. Specifically, the orientation state of the liquid crystal polymer can be more than two ways without special limitation. In addition, the orientation state of the liquid crystal polymer in multiple regions with different orientation states of the liquid crystal polymer (in other words, the scattering property of the dispersed particles in the region or the haze of the region) is not limited, and the desired orientation state can be independently obtained in each region. In addition, the configuration pattern of these regions is not limited and can be freely designed into a given pattern. Thus, the above-mentioned optical film can display the desired haze in the desired pattern.

[0065] In addition, Figure 1 In the embodiment shown, a plurality of regions (A1, A2, B1, B2, C) of different orientation states of the liquid crystal polymer in the dispersed particles each have a certain degree of area, but such regions do not necessarily have an area greater than a given value. For example, in the optical film of the first embodiment, when the orientation state of the liquid crystal polymer changes continuously in the in-plane direction and the portion in a specific orientation state cannot be identified as a region with a certain area when viewed from above, it is also treated as a case where "the diffusion layer has a plurality of regions of different orientation states of the liquid crystal polymer". In one embodiment, when the haze of the optical film (more specifically the diffusion layer) changes continuously in the in-plane direction when viewed from above, it can be regarded as that the orientation state of the liquid crystal polymer changes continuously in the in-plane direction.

[0066] In the case of looking down at the optical film, the haze of the parts corresponding to the multiple regions with different orientation states of the liquid crystal polymer in the dispersed particles can be appropriately set according to the purpose of the optical film, etc. In one embodiment, the difference between the maximum value and the minimum value of the haze of the parts corresponding to the multiple regions can be, for example, more than 0%, preferably more than 10%, more preferably 20% to 100%, and further preferably 30% to 100%. In addition, the maximum value of the haze can be, for example, 30% to 100%, and the minimum value of the haze can be, for example, 0% to 70%.

[0067] A-2. Diffusion layer

[0068] The diffusion layer 10 includes a polymer matrix 12 and dispersed particles 14 containing a liquid crystal polymer 14b which is a polymerizable liquid crystal compound and is dispersed in the polymer matrix 12, and has a plurality of regions in which the liquid crystal polymer 14b in the dispersed particles 14 has different orientation states. The dispersed particles 14 may further contain a liquid crystal compound 14a. For example, Figure 1 In the embodiment shown, the dispersed particles 14 include a liquid crystal compound 14a and a liquid crystal polymer 14b. In addition, the diffusion layer 10 has regions A1, A2, B1, B2, and C, and the orientation state of the liquid crystal polymer 14b in the dispersed particles 14 in each region is in the relationship of "A1=A2≠B1=B2≠C". That is, the orientation states of the liquid crystal polymer 14b in the regions A1 and A2, the regions B1 and B2, and the region C are different from each other. In addition, the liquid crystal compound 14a in the dispersed particles 14 is oriented along the liquid crystal polymer 14b. According to such a configuration, the regions with different orientation states of the liquid crystal polymer 14b in the dispersed particles 14 can show different hazes. As a result, the haze of each region of the diffusion layer 10 can satisfy the relationship of "A1=A2≠B1=B2≠C".

[0069] The haze in each of the above-mentioned multiple regions of the diffusion layer can be appropriately set according to the purpose of the optical film, etc. The maximum value, minimum value, and difference between the haze in the above-mentioned multiple regions of the diffusion layer can be set in such a way as to obtain the maximum value, minimum value, and difference between the hazes desired for the optical film.

[0070] The polymer matrix 12 can be formed by any appropriate resin. The polymer matrix forming resin can be appropriately selected according to the light transmittance, the refractive index of the liquid crystal compound, the adhesion with the substrate, etc. For example, water-soluble resins or water-dispersible resins such as carbamate resins, polyvinyl alcohol resins, polyethylene resins, polypropylene resins, and acrylic resins can be preferably used. The polymer matrix forming resin can be used alone or in combination.

[0071] The content ratio of the polymer matrix in the diffusion layer is, for example, 30% to 70% by weight, preferably 35% to 65% by weight, and more preferably 40% to 60% by weight. When the content ratio of the polymer matrix is ​​within this range, it is possible to obtain good mechanical strength and prevent liquid crystal leakage from the end.

[0072] The liquid crystal polymer 14b is a polymer of a polymerizable liquid crystal compound and is non-liquid crystal, that is, the liquid crystal polymer does not undergo transitions to a liquid crystal phase, a glass phase, or a crystal phase due to temperature changes, which are unique to liquid crystal compounds.

[0073] The polymerizable liquid crystal compound constituting the liquid crystal polymer can be appropriately selected according to transmittance, compatibility with the non-polymerizable liquid crystal compound described later, etc. The polymerizable liquid crystal compound can be a cross-linked type with more than 2 functions. As the polymerizable liquid crystal compound, for example, the polymerizable mesogen compounds recorded in Japanese Patent Table 2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445, etc. can be used. As a specific example of such a polymerizable mesogen compound, for example, the trade name LC242 of BASF can be cited. As the polymerizable liquid crystal compound, for example, a nematic liquid crystal monomer is preferred. The birefringence Δn (=ne-no; ne is the refractive index in the long axis direction of the liquid crystal compound molecule, no is the refractive index in the short axis direction of the liquid crystal compound molecule) of the polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, more preferably 0.10 to 0.45.

[0074] As the liquid crystal compound 14a, any appropriate non-polymerizable liquid crystal compound can be used. As described in detail in item B, the diffusion layer can be formed by performing a polymerization reaction in a state where the orientation of the polymerizable liquid crystal compound is controlled. At this time, by using the non-polymerizable liquid crystal compound in combination with the polymerizable liquid crystal compound, the temperature range of the liquid crystal phase (for example, the nematic phase) can be expanded, thereby more appropriately performing the orientation control. As the liquid crystal compound, it is preferred to use a non-polymerizable liquid crystal compound having a birefringence Δn (=ne-no; ne is the refractive index of the liquid crystal compound molecule in the long axis direction, and no is the refractive index of the liquid crystal compound molecule in the short axis direction) of 0.05 to 0.50 at a wavelength of 589nm, and more preferably a non-polymerizable liquid crystal compound having a birefringence Δn of 0.10 to 0.45.

[0075] The dielectric anisotropy of the non-polymerizable liquid crystal compound may be positive or negative. The non-polymerizable liquid crystal compound may be, for example, a nematic, smectic, or cholesteric liquid crystal compound. Since excellent transparency can be achieved in a transparent state, a nematic liquid crystal compound is preferably used.

[0076] As nematic liquid crystal compounds, there can be mentioned: biphenyl compounds, phenyl benzoate compounds, cyclohexylbenzene compounds, azoxybenzene compounds, azobenzene compounds, azomethine compounds, terphenyl compounds, biphenyl benzoate compounds, cyclohexylbiphenyl compounds, phenylpyridine compounds, cyclohexylpyrimidine compounds, cholesterol compounds, fluorine compounds, etc. These low molecular weight liquid crystal compounds can be used alone or in combination.

[0077] The total content ratio of the liquid crystal polymer and the liquid crystal compound in the diffusion layer when present (the content ratio of the liquid crystal polymer when the liquid crystal compound is not present) is, for example, 30% to 70% by weight, preferably 35% to 65% by weight, and more preferably 40% to 60% by weight. In addition, the content ratio of the liquid crystal polymer in the diffusion layer (more specifically, the dispersed particles) relative to the total content of the liquid crystal polymer and the liquid crystal compound is, for example, 5% by weight or more, preferably 7% by weight or more, and more preferably 10% by weight or more, and for example, it can be 100% by weight or less, preferably 80% by weight or less, and more preferably 50% by weight or less. In addition, the total content ratio of the polymer matrix, the liquid crystal polymer, and the liquid crystal compound in the diffusion layer when present can be, for example, 90% to 99.9% by weight, and preferably 95% to 99.9% by weight.

[0078] As described in detail in item B, the diffusion layer can be formed by preparing a PDLC layer containing liquid crystal droplets containing a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound as an arbitrary component, applying a voltage from the first main surface side and the second main surface side of the PDLC layer in a manner to generate regions with different electric field strengths, and polymerizing the polymerizable liquid crystal compound. Thus, the diffusion layer (more specifically, the dispersed particles) can further contain a polymerization initiator. The content ratio of the polymerization initiator is as described in item B. In addition, unreacted polymerizable liquid crystal compounds may remain in the dispersed particles. The content ratio of unreacted polymerizable liquid crystal compounds in the diffusion layer (more specifically, the dispersed particles) is, for example, less than 3% by weight, preferably less than 1% by weight.

[0079] The average particle size of the dispersed particles can be, for example, 0.3 μm to 9 μm, and can preferably be 0.4 μm to 8 μm. When the average particle size of the dispersed particles is too small, the dispersed particle size is smaller than the wavelength of light, so the light will not be scattered but will pass through the dispersed particles, resulting in a problem that sufficient haze cannot be obtained. In addition, when the average particle size is too large, the dispersed particle size is too large compared to the wavelength of light, so a problem that sufficient haze cannot be obtained may be caused. It should be noted that the average particle size of the dispersed particles in the diffusion layer is the volume average particle size of the dispersed particles when observed from a direction perpendicular to the main surface of the optical film.

[0080] The thickness of the diffusion layer is typically 2 μm to 40 μm, preferably 3 μm to 35 μm, and more preferably 4 μm to 30 μm.

[0081] A-3. First transparent substrate

[0082] The first transparent substrate 20 includes a first transparent film. If necessary, the first transparent substrate may have a hard coating layer on one or both sides of the first transparent film.

[0083] The haze of the first transparent substrate is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0084] The total light transmittance of the first transparent substrate is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more. The total light transmittance can be measured in accordance with JIS K 7361.

[0085] The first transparent film can be formed using any appropriate material. Specific examples include glass films and polymer films. Polymer films are preferred because they have excellent smoothness and can significantly improve productivity through continuous production using a roll.

[0086] Typically, the polymer film is a polymer film with a thermoplastic resin as the main component. As thermoplastic resins, for example, polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; cellulose resins, etc. Among them, polyester resins, cycloolefin resins or acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, etc. The above-mentioned thermoplastic resins can be used alone or in combination of two or more. In addition, optical films such as low phase difference substrates, high phase difference substrates, phase difference plates, absorption-type polarizing films, polarization selective reflection films, etc. that can be used for polarizers can also be used as the first transparent substrate.

[0087] The total light transmittance of the first transparent film is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more.

[0088] The thickness of the first transparent film is preferably 200 μm or less, more preferably 3 μm to 150 μm, and even more preferably 5 μm to 100 μm.

[0089] A-4. Second transparent substrate

[0090] The second transparent substrate 30 includes a second transparent film. If necessary, the second transparent substrate may have a hard coating layer on one or both sides of the second transparent film.

[0091] The haze of the second transparent substrate is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0092] The total light transmittance of the second transparent substrate is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more.

[0093] The same description as that of the first transparent film described in the section A-3 can be applied to the second transparent film. The second transparent substrate may have the same structure as the first transparent substrate, or may have a different structure.

[0094] A-5. Second Embodiment

[0095] According to the second embodiment of the present invention, a polymer film is provided, which has a diffusion layer, the diffusion layer includes a polymer matrix, and dispersed particles dispersed in the polymer matrix, the dispersed particles include a liquid crystal polymer as a polymer of a polymerizable liquid crystal compound, and the diffusion layer has a plurality of regions with different content ratios of the liquid crystal polymer. Representatively, the diffusion layer has a region including dispersed particles containing liquid crystal polymers, and a region including dispersed particles containing polymerizable liquid crystal compounds. The content ratio of the liquid crystal polymer in the region including dispersed particles containing polymerizable liquid crystal compounds is less than the content ratio of the liquid crystal polymer in the region including dispersed particles containing liquid crystal polymers. The difference in the content ratio of the liquid crystal polymer is not limited as long as the effect of the present invention can be obtained. For example, the region including dispersed particles containing polymerizable liquid crystal compounds may be substantially free of liquid crystal polymers. In such a configuration, the liquid crystal polymer and the polymerizable liquid crystal compound take different orientation states, and thus, these regions can show different hazes.

[0096] In the case of looking down at the optical film, the haze of the parts corresponding to the plurality of regions having different content ratios of the liquid crystal polymer can be appropriately set according to the purpose of the optical film. In one embodiment, the difference between the maximum value and the minimum value of the haze of the parts corresponding to the plurality of regions can be, for example, more than 0%, preferably more than 10%, more preferably 20% to 100%, and further preferably 30% to 100%. In addition, the maximum value of the haze can be, for example, 30% to 100%, and the minimum value of the haze can be, for example, 0% to 70%.

[0097] Figure 41 is a schematic cross-sectional view of an example of an optical film according to the second embodiment of the present invention. The optical film 100d has a diffusion layer 10, a first transparent substrate 20 disposed on the first main surface side of the diffusion layer 10, and a second transparent substrate 30 disposed on the second main surface side. The diffusion layer 10 has a region E, and regions D1 and D2, wherein the region E includes a polymer matrix 12, and first dispersed particles 14 dispersed in the polymer matrix 12, wherein the dispersed particles 14 include a non-polymerizable liquid crystal compound 14a and a liquid crystal polymer 14b, and the regions D1 and D2 include a polymer matrix 12, and second dispersed particles 14' dispersed in the polymer matrix 12, wherein the second dispersed particles 14' include a non-polymerizable liquid crystal compound 14a and a polymerizable liquid crystal compound 14c. The second dispersed particles 14' may be droplets of a liquid crystal compound. In the region E, the non-polymerizable liquid crystal compound 14a and the liquid crystal polymer 14b are oriented substantially perpendicularly to the main surface. In the regions D1 and D2, the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14c are in a non-aligned state. Therefore, the regions D1 and D2 can show a higher haze than the region E in a plan view.

[0098] Regarding the diffusion layer 10, the same description as in item A-2 can be applied to the region containing the first dispersed particles 14. The same description as in item A-2 can be applied to the region containing the second dispersed particles 14' except that the polymerizable liquid crystal compound 14c is included instead of the liquid crystal polymer 14b. The dispersed particles 14' may not include the non-polymerizable liquid crystal compound 14a depending on the purpose, as with the dispersed particles 14.

[0099] The descriptions of Item A-3 and Item A-4 are applicable to the first transparent substrate 20 and the second transparent substrate 30, respectively. Depending on the purpose, one or both of the first transparent substrate 20 and the second transparent substrate 30 may be omitted.

[0100] A-6. Application of optical films

[0101] The optical film according to the embodiment of the present invention can show a desired haze in a desired pattern. Therefore, specific examples of the use of the optical film include a diffusion film, a design film, and the like.

[0102] As the diffusion film, a diffusion film for an image display device, more specifically, an image display device having a direct-type backlight can be preferably exemplified. Specifically, with respect to a direct-type backlight having a plurality of LED light sources arranged at a given interval, by using an optical film patterned in such a manner that the haze of the area directly above the LED light source is high and the haze decreases as the distance from the LED light source increases, the brightness distribution within the surface can be suitably uniformed.

[0103] As a design film, for example, a shielding film for shielding wiring and the like provided at the periphery of the image display area in an image display device such as a liquid crystal display device or an organic EL display device can be preferably exemplified. Generally speaking, shielding of wiring and the like can be performed by providing a frame-shaped printed layer directly or through a substrate film on a front panel such as a cover glass or a cover film. According to such a structure, there is a problem that the interlayer adhesive cannot completely absorb the thickness difference between the portion provided with the printed layer and the other portions, and bubbles will be generated. In contrast, the optical film according to the embodiment of the present invention has no height difference between the shielding area (high haze area) and the display area (low haze area) and is smooth, so the problem of bubbles can be eliminated.

[0104] B. Method for manufacturing optical film

[0105] A method for producing an optical film according to a first embodiment of the present invention includes:

[0106] (Step A) applying a coating liquid including a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent onto a first substrate to obtain a coating layer;

[0107] (Step B) drying the coating layer to obtain a PDLC layer, wherein the PDLC layer includes a polymer matrix and droplets dispersed in the polymer matrix and including the polymerizable liquid crystal compound; and

[0108] (Step C) A voltage is applied from the first main surface side and the second main surface side of the PDLC layer so as to generate regions with different electric field strengths, thereby polymerizing the polymerizable liquid crystal compound.

[0109] The method for manufacturing an optical film of the first embodiment may further include, before or after polymerizing the polymerizable liquid crystal compound, disposing a second substrate on the side of the PDLC layer or the diffusion layer opposite to the side on which the first substrate is provided (step D), as required. According to the method for manufacturing an optical film of the first embodiment, in each region with different electric field intensities, the polymerizable liquid crystal compound is polymerized in different orientation states corresponding to the electric field intensities, resulting in a diffusion layer having a plurality of regions with different orientation states of the liquid crystal polymer in the dispersed particles. Thus, according to the method for manufacturing an optical film of the first embodiment, the optical film described in item A (specifically, the optical film of the first embodiment) can be suitably obtained.

[0110] B-1. Process A

[0111] In step A, a coating liquid containing a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent is applied to the first substrate to obtain a coating layer. The coating liquid may further contain a non-polymerizable liquid crystal compound.

[0112] The coating liquid is preferably an emulsion containing liquid crystal particles as a dispersoid (hereinafter sometimes referred to as an "emulsion coating liquid"), wherein the liquid crystal particles contain a polymerizable liquid crystal compound and an optionally used non-polymerizable liquid crystal compound. In one embodiment, the coating liquid is an emulsion coating liquid in which a polymer matrix-forming resin particle and liquid crystal particles containing a polymerizable liquid crystal compound and an optionally used non-polymerizable liquid crystal compound are dispersed in a solvent. The emulsion coating liquid preferably further contains a polymerization initiator in the liquid crystal particles, and may further contain any appropriate additives depending on the purpose.

[0113] As the solvent, water or a mixed solvent of water and a water-miscible organic solvent can be preferably used. As the water-miscible organic solvent, C1-3 alcohol, acetone, DMSO, etc. can be mentioned. Regarding the polymerizable liquid crystal compound, the non-polymerizable liquid crystal compound and the polymer matrix forming resin, as described in item A-2. As any additive, a dispersant, a leveling agent, a cross-linking agent, etc. can be mentioned.

[0114] The content ratio of the liquid crystal compound in the solid component of the coating liquid (the total content ratio of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound when present) can be, for example, 30% to 70% by weight, preferably 35% to 65% by weight, and more preferably 40% to 60% by weight.

[0115] The weight ratio of the polymerizable liquid crystal compound to the non-polymerizable liquid crystal compound in the coating liquid (polymerizable liquid crystal compound:non-polymerizable liquid crystal compound) may be, for example, 5:95 to 100:0, preferably 7:93 to 80:20, and more preferably 10:90 to 50:50.

[0116] The content ratio of the polymer matrix-forming resin in the solid content of the coating liquid may be, for example, 30 to 70 wt %, preferably 35 to 65 wt %, and more preferably 40 to 60 wt %.

[0117] The weight ratio of the content of the liquid crystal compound (the total content of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound, if present) to the content of the polymer matrix-forming resin in the coating liquid (liquid crystal compound: polymer matrix-forming resin) may be, for example, 30:70 to 70:30, preferably 35:65 to 65:35, and more preferably 40:60 to 60:40. In addition, the total content ratio of the polymer matrix-forming resin, the polymerizable liquid crystal compound, and the non-polymerizable liquid crystal compound, if present, in the solid content of the coating liquid may be, for example, 90% by weight to 99.9% by weight, preferably 95% by weight to 99.9% by weight.

[0118] The average particle size of the liquid crystal particles is preferably 0.3 μm or more, more preferably 0.4 μm or more. In addition, the average particle size of the liquid crystal particles is preferably 9 μm or less, more preferably 8 μm or less. When the average particle size of the liquid crystal particles is within this range, the average particle size of the dispersed particles in the diffusion layer can reach a desired range. It should be noted that the average particle size of the liquid crystal particles is a volume average particle size.

[0119] The average particle size of the liquid crystal particles preferably has a relatively narrow particle size distribution. The coefficient of variation (CV value) of the average particle size of the liquid crystal particles may be, for example, less than 0.40, preferably less than 0.35, and more preferably less than 0.30. In one embodiment, an emulsion coating liquid that substantially does not contain liquid crystal particles having a particle size less than 0.3 μm or greater than 9 μm (for example, an emulsion coating liquid in which the volume of liquid crystal particles having a particle size less than 0.3 μm or greater than 9 μm is less than 10% of the total volume of the liquid crystal particles) may be used.

[0120] The average particle size of the polymer matrix-forming resin particles is preferably 10 nm to 500 nm, more preferably 30 nm to 300 nm, and further preferably 50 nm to 200 nm. Two or more resin particles having different types of resins and / or average particle sizes may be used. The average particle size of the polymer matrix-forming resin particles refers to the volume average median particle size, which can be measured using a dynamic light scattering particle size distribution measuring device.

[0121] As the polymerization initiator, any appropriate photopolymerization initiator or thermal polymerization initiator may be used depending on the purpose, desired properties, etc., but a photopolymerization initiator is preferably used. Specific examples of the photopolymerization initiator include 2,2-dimethoxy-2-phenylacetophenone, acetophenone, benzophenone, xanthone, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, benzoin propyl ether, benzoin dimethyl ether, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dipentyloxyphenylphosphine oxide, bis(2,6-dimethoxy-benzoyl)-(2,4,4-trimethyl-pentyl)-phosphine oxide, and thioxanthone compounds. The polymerization initiator may be used alone or in combination of two or more thereof. The content of the polymerization initiator is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the polymerizable liquid crystal compound.

[0122] Examples of the dispersant include anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. The content of the dispersant is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, based on 100 parts by weight of the emulsion coating liquid.

[0123] Examples of the leveling agent include acrylic leveling agents, fluorine leveling agents, silicone leveling agents, etc. The content of the leveling agent is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, based on 100 parts by weight of the emulsion coating liquid.

[0124] Examples of the crosslinking agent include aziridine crosslinking agents, isocyanate crosslinking agents, etc. The content of the crosslinking agent is preferably 0.5 to 10 parts by weight, more preferably 0.8 to 5 parts by weight, based on 100 parts by weight of the emulsion coating liquid.

[0125] The emulsion coating liquid can be prepared, for example, by mixing a resin emulsion or resin particle dispersion containing polymer matrix-forming resin particles, a liquid crystal emulsion containing liquid crystal particles containing a polymerizable liquid crystal compound, a polymerization initiator, and an optionally used non-polymerizable liquid crystal compound, and any additives (e.g., a dispersant, a leveling agent, a cross-linking agent). As required, a solvent may be further added during mixing. Alternatively, the emulsion coating liquid may also be prepared by adding a polymerizable liquid crystal compound, a polymer matrix-forming resin, a polymerization initiator, and an optionally used non-polymerizable liquid crystal compound and an additive to a solvent and dispersing them mechanically.

[0126] The above-mentioned resin emulsion and liquid crystal emulsion can be prepared, for example, by mechanical emulsification, microchannel method, membrane emulsification method, etc. Among them, the liquid crystal emulsion is preferably prepared by membrane emulsification. According to the membrane emulsification method, an emulsion with a uniform particle size distribution can be suitably obtained. For details of the membrane emulsification method, reference can be made to the disclosures of Japanese Patent Laid-Open No. 4-355719, Japanese Patent Laid-Open No. 2015-40994 (which are cited as references in this specification), etc.

[0127] The solid content concentration of the emulsion coating liquid may be, for example, 20% to 60% by weight, and preferably 30% to 50% by weight.

[0128] The viscosity of the emulsion coating liquid can be appropriately adjusted in a manner that allows the coating on the first substrate to be carried out appropriately. The viscosity of the emulsion coating liquid during coating is preferably 20mPas to 400mPas, more preferably 30mPas to 300mPas, and further preferably 40mPas to 200mPas. When the viscosity is less than 20mPas, the convection of the solvent becomes significant when the solvent is dried, and there is a risk that the thickness of the PDLC layer (and consequently the diffusion layer) becomes unstable. In addition, when the viscosity exceeds 400mPas, there is a risk that the beads of the emulsion coating liquid are unstable. The viscosity of the emulsion coating liquid can be measured, for example, by a rheometer MCR302 manufactured by Anton Paar. The viscosity here uses the shear viscosity value under the conditions of 20°C and a shear rate of 1000 (1 / s).

[0129] As the first substrate, any appropriate substrate can be used. By using the first transparent substrate recorded in item A-3 as the first substrate, an optical film with the first transparent substrate and a diffusion layer can be obtained appropriately. According to the purpose, the first substrate can also be peeled off and removed from the diffusion layer after step C finishes.

[0130] As a coating method, any appropriate method can be used. For example, roll coating, spin coating, wire rod coating, dip coating, die coating, curtain coating, spray coating, blade coating (Comma Coating method, etc.) and the like can be cited. Among them, roll coating is preferred. For example, for coating based on a roll coating method using a slit die, reference can be made to the records of Japanese Patent Publication No. 2019-5698.

[0131] The thickness of the coating layer is preferably 3 μm to 40 μm, more preferably 4 μm to 30 μm, and even more preferably 5 μm to 20 μm. Within such a range, a PDLC layer (resulting in a diffusion layer) having excellent thickness uniformity can be obtained.

[0132] B-2. Process B

[0133] In step B, the coating layer is dried to obtain a PDLC layer, which includes a polymer matrix and droplets dispersed in the polymer matrix and including a polymerizable liquid crystal compound and an optionally used non-polymerizable liquid crystal compound. The solvent is removed from the coating layer by drying, and the polymer matrix-forming resin particles are fused together, thereby forming a PDLC layer having a structure in which liquid crystal droplets are dispersed in the polymer matrix.

[0134] The coating layer may be dried by any appropriate method. Specific examples of the drying method include natural drying, heating drying, hot air drying, etc. When the emulsion coating liquid contains a crosslinking agent, a crosslinked structure of the polymer matrix may be formed during drying.

[0135] The drying temperature is preferably 20° C. to 150° C., more preferably 25° C. to 80° C. The drying time is preferably 1 minute to 100 minutes, more preferably 2 minutes to 10 minutes.

[0136] B-3. ​​Process C

[0137] In step C, voltage is applied from the first main surface side and the second main surface side of the PDLC layer so as to generate regions with different electric field strengths, and the polymerizable liquid crystal compound is polymerized. Thus, a diffusion layer including a polymer matrix and dispersed particles of a liquid crystal polymer dispersed in the polymer matrix and including a polymer of the polymerizable liquid crystal compound can be formed.

[0138] The polymerization of the polymerizable liquid crystal compound can be performed by irradiation with active energy rays, heating, or a combination thereof, and is preferably performed by irradiation with active energy rays.

[0139] As the active energy ray, ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays, and electron beams can be used. Among them, ultraviolet rays are preferred. In addition, the active energy ray is preferably collimated light with high straightness from the irradiation source.

[0140] The ultraviolet irradiation conditions can be appropriately set according to the type of polymerizable liquid crystal compound, the transmittance of the substrate, the absorption wavelength of the photopolymerization initiator, etc. The irradiation intensity can be, for example, 0.1 mW / cm 2 ~1000mW / cm 2 , preferably 1 mW / cm 2 ~100mW / cm 2 The irradiation dose can be, for example, 10 mJ / cm 2 ~10000mJ / cm 2 , preferably 100 mJ / cm 2 ~5000mJ / cm 2 The irradiation temperature may be, for example, -20°C to 80°C, and preferably -20°C to 60°C.

[0141] In one embodiment, the voltage is applied using a first electrode disposed on the first main surface side of the PDLC layer and a second electrode disposed on the second main surface side, and regions with different electric field strengths are formed by controlling the separation distance between the first electrode and the second electrode. Figure 5 Step C is described. It should be noted that Figure 5In the illustrated embodiment, step D is performed before step C, and a first transparent substrate 20 as a first substrate is disposed on the first main surface side of the PDLC layer 10a, and a second transparent substrate 30 as a second substrate is disposed on the second main surface side. Different from the illustrated example, the first main surface and / or the second main surface of the PDLC layer may be exposed.

[0142] Figure 5 (a) is a cross-sectional schematic diagram showing a state where no voltage is applied to the PDLC layer obtained in step B. The PDLC layer 10a includes a polymer matrix 12 and liquid crystal droplets 14' dispersed in the polymer matrix 12, and the liquid crystal droplets 14' include non-polymerizable liquid crystal compounds 14a and polymerizable liquid crystal compounds 14c. A first electrode 40 is arranged on the outer side of the first transparent substrate 20 (the side opposite to the side where the PDLC layer is arranged), and a second electrode 50 capable of transmitting active energy rays is arranged on the outer side of the second transparent substrate 30 (the side opposite to the side where the PDLC layer is arranged). For the electrodes 40 and 50, since no voltage is applied by the power supply 60, no electric field is generated between them, and therefore, the non-polymerizable liquid crystal compounds 14a and polymerizable liquid crystal compounds 14c in the liquid crystal droplets 14' exist in a non-oriented state. In addition, the first electrode 40 is formed in such a way that the surface height of the PDLC layer 10a side is different depending on the location, thereby forming regions with different distances between electrodes.

[0143] The regions with different inter-electrode distances can be freely designed, for example, by changing the surface shape of the PDLC layer side of the first electrode and / or the second electrode. Specifically, by providing concavities and convexities, height differences, inclinations, etc. on the surface of the first electrode and / or the second electrode in an arbitrary pattern, a desired inter-electrode distance can be achieved in a desired pattern. For example, by Figure 6 As shown in FIG. 1 , by providing a conical protrusion 42 on the surface of the electrode 40a, the distance between the electrodes can be continuously changed, and as a result, the orientation state of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound in the liquid crystal droplet can be continuously changed in the plane. At this time, by changing the height H and the tilt angle θ, the change amount and the rate of change of the distance between the electrodes can be controlled, and as a result, the obtained optical film can have a haze with an arbitrary gradient. The height H and the tilt angle θ can be set to any appropriate value according to the desired haze pattern of the optical film.

[0144] Figure 5(b) is a schematic diagram showing an embodiment of polymerizing the polymerizable liquid crystal compound 14c by UV irradiation. UV irradiation is performed in a state where a voltage is applied between the first electrode 40 and the second electrode 50 by the power supply 60. By applying the voltage, an electric field of an intensity corresponding to the separation distance between the first electrode 40 and the second electrode 50 is generated, resulting in multiple regions with different electric field intensities. In each of the multiple regions, the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14c in the liquid crystal droplet 14' are oriented in accordance with the electric field intensity. Specifically, in the region where the separation distance between the first electrode 40 and the second electrode 50 is the smallest, the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14 are oriented approximately perpendicularly to the main surface of the PDLC layer 10a, and as the separation distance increases, the degree of orientation becomes weaker. By polymerizing the polymerizable liquid crystal compound 14c in such a state, as Figure 5 As shown in (c), the diffusion layer 10 having a plurality of regions in which the orientation states of the liquid crystal polymer 14 b in the dispersed particles 14 are different can be formed.

[0145] The voltage applied during polymerization is not limited as long as the polymerizable liquid crystal compound exhibits a desired orientation, and can be appropriately set according to the desired haze of the optical film, the separation distance of the electrodes, etc. The voltage may be, for example, 10 V to 100 kV, preferably 100 V to 10 kV.

[0146] B-4. Process D

[0147] In step D, a second substrate is disposed on the side (second main surface side) opposite to the side (first main surface side) where the first substrate is disposed on the PDLC layer or the diffusion layer. As the first substrate, any appropriate substrate can be used, and the second transparent substrate described in item A-4 can be preferably used. Step D can be performed before step C, that is, before polymerizing the polymerizable liquid crystal compound, or after step C, that is, after polymerizing the polymerizable liquid crystal compound.

[0148] According to the manufacturing method of an optical film including step D, by using the first transparent substrate described in item A-3 and the second transparent substrate described in item A-4 as the first substrate and the second substrate, respectively, an optical film having the first transparent substrate and the second transparent substrate, and a diffusion layer directly sandwiched between them can be obtained.

[0149] From the viewpoint of obtaining sufficient adhesion, the second substrate is preferably laminated on the second main surface side of the PDLC layer or the diffusion layer while applying a lamination pressure of 0.006 MPa / m to 7 MPa / m, more preferably 0.06 MPa / m to 0.7 MPa / m, using a laminator.

[0150] A method for producing an optical film according to a second embodiment of the present invention includes:

[0151] (Step I) applying a coating liquid comprising a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent onto a first substrate to obtain a coating layer;

[0152] (Step II) drying the coating layer to obtain a polymer dispersed liquid crystal layer, wherein the polymer dispersed liquid crystal layer comprises a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound; and

[0153] (Step III) While voltage is applied to the polymer dispersed liquid crystal layer, an active energy ray is irradiated to a predetermined region to polymerize the polymerizable liquid crystal compound.

[0154] The manufacturing method of the optical film of the second embodiment can be configured as needed on the side opposite to the side where the first substrate is provided in the PDLC layer or the diffusion layer before or after the polymerization of the polymerizable liquid crystal compound (process IV). According to the manufacturing method of the optical film of the second embodiment, in the area irradiated with active energy rays, the polymerizable liquid crystal compound is polymerized in an oriented state, thereby generating a liquid crystal polymer whose oriented state is fixed. On the other hand, in the area not irradiated with active energy rays, the polymerizable liquid crystal compound is not polymerized and becomes a non-oriented state in the state where no voltage is applied. As a result, a diffusion layer having multiple regions with different liquid crystal polymer content ratios is formed, and the haze of the region (irradiated region) with a large content ratio of the liquid crystal polymer is lower than the haze of the region (non-irradiated region) with a small content ratio. According to the manufacturing method of the optical film of the second embodiment, the optical film described in item A (for example, the optical film of the second embodiment) can be appropriately obtained. In addition, according to the manufacturing method of the optical film of the second embodiment, the boundary between the irradiated area and the non-irradiated area is clear, and an optical film with a high contrast of the haze of these regions can be appropriately obtained.

[0155] The same description as that of step A, step B, and step D in the method for producing an optical film of the first embodiment can be applied to step I, step II, and step IV, respectively. However, a photopolymerization initiator can be used as the polymerization initiator.

[0156] In step III, while a voltage is applied to the PDLC layer, an active energy ray is irradiated to a predetermined region to polymerize the polymerizable liquid crystal compound. Typically, the active energy ray irradiation is performed through a photomask having openings of a predetermined pattern.

[0157] As active energy rays, ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays and electron beams can be used. Among them, ultraviolet rays are preferred. In addition, the active energy rays are preferably collimated light with high straightness from the irradiation source. The irradiation conditions of ultraviolet rays can be the same as those described in the method for producing the optical film of the first embodiment.

[0158] Figure 7 This is a schematic diagram for explaining an embodiment of step III. Figure 7 In the illustrated embodiment, step IV is performed before step III, and a first transparent substrate 20 as a first substrate is disposed on the first main surface side of the PDLC layer 10a, and a second transparent substrate 30 as a second substrate is disposed on the second main surface side. Different from the illustrated example, the first main surface and / or the second main surface of the PDLC layer may be exposed.

[0159] The PDLC layer 10a includes a polymer matrix 12 and liquid crystal droplets 14' dispersed in the polymer matrix 12, and the liquid crystal droplets 14' include non-polymerizable liquid crystal compounds 14a and polymerizable liquid crystal compounds 14c. A first electrode 40 is disposed on the outer side of the first transparent substrate 20 (opposite to the side where the PDLC layer is disposed), and a second electrode 50 capable of transmitting active energy rays is disposed on the outer side of the second transparent substrate 30 (opposite to the side where the PDLC layer is disposed).

[0160] exist Figure 7 In (a), a voltage is applied to the electrodes 40 and 50 by a power supply 60, and an electric field is generated between them, so that the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14c in the liquid crystal droplet 14' are oriented in a substantially vertical direction. Preferably, the orientation state of the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14c is uniform in the entire PDLC layer. In such a state, active energy rays (ultraviolet rays in the example shown) are irradiated through a photomask 70 having an opening in a given pattern. As a result, the polymerizable liquid crystal compound 14c in the irradiated area is polymerized to generate a liquid crystal polymer 14b.

[0161] like Figure 7 As shown in (b), after irradiation with active energy rays, the irradiated area of ​​the diffusion layer 10 includes the first dispersed particles 14 containing the non-polymerizable liquid crystal compound 14a and the liquid crystal polymer 14b, and the non-irradiated area includes the second dispersed particles (liquid crystal droplets) 14' containing the non-polymerizable liquid crystal compound 14a and the polymerizable liquid crystal compound 14c. In the first dispersed particles 14, the orientation state of the liquid crystal polymer 14b is fixed, and the non-polymerizable liquid crystal compound 14a is oriented along the liquid crystal polymer 14b. In this embodiment, the irradiated area can show a lower haze than the non-irradiated area.

[0162] The voltage applied during polymerization is not limited as long as the polymerizable liquid crystal compound exhibits a desired orientation, and can be appropriately set according to the desired haze of the optical film, the separation distance of the electrodes, etc. The voltage may be, for example, 10 V to 100 kV, preferably 100 V to 10 kV.

[0163] If necessary, after step III, the non-irradiated region may be irradiated with active energy rays without applying voltage, thereby polymerizing the polymerizable liquid crystal compound contained in the non-irradiated region while maintaining a non-aligned state to generate a liquid crystal polymer.

[0164] Alternatively, in step III, the polymerizable liquid crystal compound may be polymerized through a photomask without applying a voltage, and then the non-irradiated area may be irradiated with active energy rays while a voltage is applied. That is, the method for manufacturing an optical film according to the third embodiment of the present invention includes:

[0165] (Step I) applying a coating liquid comprising a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent onto a first substrate to obtain a coating layer;

[0166] (Step II) drying the coating layer to obtain a polymer dispersed liquid crystal layer, wherein the polymer dispersed liquid crystal layer comprises a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound;

[0167] (Step IIIα) irradiating a predetermined region with active energy rays without applying a voltage to the polymer dispersed liquid crystal layer to polymerize the polymerizable liquid crystal compound;

[0168] (Step IIIβ) While voltage is applied to the polymer dispersed liquid crystal layer, the other regions are irradiated with active energy rays to polymerize the polymerizable liquid crystal compound.

[0169] The method for producing an optical film according to the third embodiment may further include, before or after polymerizing the polymerizable liquid crystal compound, disposing a second substrate on the side of the PDLC layer or the diffusion layer opposite to the side on which the first substrate is provided (step IV), if necessary.

[0170] According to these methods, the optical film described in the section A (specifically, the optical film of the first embodiment) can be preferably obtained.

[0171] Example

[0172] Hereinafter, the present invention will be specifically described in conjunction with the examples, but the present invention is not limited to these examples. The measuring methods of each characteristic are as follows. In addition, unless otherwise specifically stated, the "parts" and "%" in the examples and comparative examples are weight references.

[0173] (1) Thickness

[0174] The measurement was performed using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C").

[0175] (2) Volume average particle size of liquid crystal particles in liquid crystal emulsion

[0176] 0.1 wt% of liquid crystal emulsion was added to 200 ml of electrolyte aqueous solution (manufactured by Coulter, "ISOTON II"), and the obtained mixed solution was used as a measurement sample. Multisizer 3 (manufactured by Coulter, pore size = 20 μm) was used to divide 256 parts at equal intervals from 0.4 μm to 12 μm on a logarithmic basis, and the volume statistics of each discretized particle size were obtained to calculate the volume average particle size. It should be noted that in the case of particles of 12 μm or more, the pore size was set to 30 μm, and 256 parts were divided at equal intervals from 0.6 μm to 18 μm on a logarithmic basis, and the volume statistics of each discretized particle size were obtained, thereby calculating the volume average particle size.

[0177] (3) Average particle size of resin particles

[0178] A few drops of the resin dispersion were added to 100 mL of water to prepare a measurement sample. A dynamic light scattering particle size distribution measuring device (Microtrac, Inc., device name "Nanotrac 150") was used, the measurement sample was set on the measuring stand of the device, and the measurement was performed after confirming the measurable concentration on the monitor of the device.

[0179] (4) Haze

[0180] The measurement was performed in accordance with JIS K 7136 using the product name "NDH4000" manufactured by Nippon Denshoku Co., Ltd.

[0181] [Example 1]

[0182] (Preparation of emulsion coating liquid)

[0183] A liquid crystal emulsion was prepared by mixing 53.7 parts of a non-polymerizable liquid crystal compound (manufactured by JNC, product name "LX-153XX", birefringence Δn = 0.149 (ne = 1.651, no = 1.502), viscosity = 48.5 mPa·s), 5.9 parts of a polymerizable liquid crystal compound (manufactured by BASF, product name "PALIOCOLOR LC-242"), 0.1 parts of a photopolymerization initiator (manufactured by IGM, product name "OMNIRAD651"), 39.8 parts of pure water, and 0.5 parts of a dispersant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Noigen ET159"), and stirring at 100 rpm for 10 minutes with a homogenizer. The average particle size of the liquid crystal particles in the obtained liquid crystal emulsion was 3.4 μm.

[0184] 38.4 parts of the above-mentioned liquid crystal emulsion, 19.1 parts of a polyether polyurethane resin aqueous dispersion (manufactured by DSM, trade name "NeoRez R967", polymer average particle size: 80 nm, CV value = 0.27, solid content: 40 wt%), 17.0 parts of a polyester polyurethane resin aqueous dispersion (manufactured by Sanyo Chemical Industry Co., Ltd., trade name "UCOAT C-102", polymer average particle size: 168 nm, CV value = 0.23, solid content: 45 wt%), 0.1 part of a leveling agent (manufactured by DIC Corporation, product name "F-444"), 1.1 parts of a crosslinking agent (trimethylolpropane tris [3- (2-methylaziridin-1-yl) propionate], propylidynetrimethyltris [3- (2-methylaziridin-1-yl) propionate]), and 24.3 parts of pure water were mixed to obtain an emulsion coating liquid (solid content concentration: 40 wt%).

[0185] (Application and drying of emulsion coating liquid)

[0186] The emulsion coating liquid was applied to one side of a PET film (125 μm thick) as the first transparent substrate to form a coating layer with a thickness of 20 μm. The coating was performed using a slot die head at a line speed of 6 m / min. Then, the coating layer was dried at 25° C. for 8 minutes, thereby forming a PDLC layer with a thickness of 8 μm.

[0187] (Lamination of the Second Transparent Substrate)

[0188] A PET film (thickness 125 μm) as a second transparent substrate was laminated on the PDLC layer using a laminator at a laminating pressure of 0.4 MPa / m. Thus, a laminate having a structure of [first transparent substrate / PDLC layer / second transparent substrate] was obtained. The obtained laminate showed uniform haze (haze: 90%) on the entire main surface.

[0189] (UV irradiation)

[0190] As the first electrode, a flat metal electrode having a concave portion with a depth of 2 mm on the upper surface was used. The above-mentioned laminate was arranged on the upper surface of the first electrode in a manner that the first transparent substrate was in contact, and a glass substrate with ITO as the second electrode was arranged thereon in a manner that the ITO surface was in contact with the second transparent substrate. Next, while applying a voltage of 2 kV to these electrodes using a high voltage power supply, a UV-LED lamp (manufactured by Hamamatsu Photonics, product name "C11924-101", peak wavelength 365 nm) was used at 10 mW / cm 2 An exposure treatment was performed at 25°C for 10 minutes. Thus, the polymerizable liquid crystal compound was polymerized to obtain an optical film having a structure of [first transparent substrate / diffusion layer / second transparent substrate]. It should be noted that the distance between electrodes in the region (region I) corresponding to the concave portion of the first electrode is about 2250 μm, and the electric field strength is 0.89 V / μm. In addition, the distance between electrodes in the region (region II) corresponding to the portion other than the concave portion of the first electrode is about 250 μm, and the electric field strength is 7.8 V / μm.

[0191] The haze of the obtained optical film was measured, and the result showed that the haze of region I was 90%, and the haze of region II was 8%. This shows that the orientation state of the liquid crystal polymer and the liquid crystal compound in the dispersed particles in region I of the diffusion layer is different from that in the dispersed particles in region II, and more specifically, the orientation degree of the liquid crystal polymer and the liquid crystal compound in the dispersed particles in region I is lower than that in the dispersed particles in region II.

[0192] Industrial Applicability

[0193] The optical film of the present invention can be suitably used for various applications such as a diffusion film and a design film.

Claims

1. An optical film comprising a diffusion layer, the diffusion layer comprising a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles comprising a liquid crystal polymer as a polymer of a polymerizable liquid crystal compound, The diffusion layer has a plurality of regions having different alignment states of the liquid crystal polymer and / or different content ratios of the liquid crystal polymer.

2. The optical film according to claim 1, wherein The plurality of regions are arranged in a given pattern.

3. The optical film according to claim 1 or 2, wherein: The maximum value of the difference in haze between the portions corresponding to the plurality of regions in a plan view is 10% or more.

4. The optical film according to any one of claims 1 to 3, wherein The dispersed particles further include a liquid crystal compound.

5. The optical film according to claim 4, wherein: The content ratio of the liquid crystal polymer to the total content of the liquid crystal polymer and the liquid crystal compound is 5% by weight or more.

6. The optical film according to any one of claims 1 to 5, wherein The total content ratio of the liquid crystal polymer and the liquid crystal compound, if present, in the diffusion layer is 30% by weight to 70% by weight.

7. The optical film according to any one of claims 1 to 6, wherein A first transparent substrate is disposed on the first main surface side of the diffusion layer.

8. The optical film according to any one of claims 1 to 7, wherein A second transparent substrate is disposed on the second main surface side of the diffusion layer. 9 . The optical film according to claim 1 , which does not have an electrode layer.

10. An optical film comprising a diffusion layer, the diffusion layer comprising a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles comprising a liquid crystal polymer as a polymer of a polymerizable liquid crystal compound, The optical film has a plurality of regions in a plan view, and the plurality of regions show different hazes according to the alignment states of the liquid crystal polymer.

11. An optical film comprising a diffusion layer, wherein the diffusion layer comprises a polymer matrix and dispersed particles dispersed in the polymer matrix. The diffusion layer has: A region including dispersed particles containing a polymerizable liquid crystal compound, and a region including dispersed particles of a liquid crystal polymer including a polymer of the polymerizable liquid crystal compound, When viewed from above, these areas show different haze levels.

12. A method for manufacturing an optical film, the method comprising: Applying a coating liquid including a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent on a first substrate to obtain a coating layer; Drying the coating layer to obtain a polymer dispersed liquid crystal layer, the polymer dispersed liquid crystal layer comprising a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound; and Voltage is applied from the first main surface side and the second main surface side of the polymer-dispersed liquid crystal layer so as to generate regions with different electric field strengths, thereby polymerizing the polymerizable liquid crystal compound.

13. The method for producing an optical film according to claim 12, wherein: The voltage is applied using a first electrode disposed on the first main surface side of the polymer dispersed liquid crystal layer and a second electrode disposed on the second main surface side. The separation distance between the first electrode and the second electrode is controlled so as to generate regions with different electric field strengths.

14. A method for manufacturing an optical film, the method comprising: Applying a coating liquid including a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent on a first substrate to obtain a coating layer; Drying the coating layer to obtain a polymer dispersed liquid crystal layer, the polymer dispersed liquid crystal layer comprising a polymer matrix and droplets dispersed in the polymer matrix and comprising the polymerizable liquid crystal compound; and In a state where a voltage is applied to the polymer dispersed liquid crystal layer, an active energy ray is irradiated to a predetermined region to polymerize the polymerizable liquid crystal compound.

15. The method for producing an optical film according to any one of claims 12 to 14, wherein: The coating liquid is an emulsion containing liquid crystal particles containing the polymerizable liquid crystal compound as a dispersoid.

16. The method for producing an optical film according to any one of claims 12 to 15, wherein: The coating liquid further includes a non-polymerizable liquid crystal compound.