Electrode for power storage device

By forming a thick active material layer containing carbon nanotubes on the surface of the current collector of the electrode and installing a carbon coating, the problems of peeling strength and long-term output of the electrode active material layer are solved, and the performance of the power storage device is improved.

CN118891745APending Publication Date: 2024-11-01TOYOTA INDUSTRIES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028619.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When the electrodes where the active material layer is formed into thick electrodes and carbon nanotubes are contained, the long-term output of the power storage device may decrease, and the peel strength of the active material layer relative to the current collector is insufficient.

Method used

The electrode current collector surface is formed with an active material layer of 250 μm or more. The layer contains active material that can absorb and release charge carriers, water-based binders and single-layer carbon nanotubes. The content of the carbon nanotubes is controlled at 0.035 Between % and 0.08%, and a carbon coating is provided on the surface of the current collector to increase peel strength.

Benefits of technology

The long-term output performance of the power storage device and the peel strength of the active material layer to the current collector are improved, and the ion conductivity decrease caused by excessive carbon nanotubes is avoided, and the energy density of the electrode is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891745A_ABST
    Figure CN118891745A_ABST
Patent Text Reader

Abstract

An electrode (100) for a power storage device is provided with a current collector (101) having a first surface (101a), and an active material layer (102) formed on the first surface (101a) of the current collector (101). The thickness of the active material layer (102) is 250 [mu] m or more. A carbon coating layer (C) is provided on a first surface (101a) of the current collector (101). The active material layer (102) contains an active material capable of absorbing and releasing a charge carrier, an aqueous binder, and single-layer carbon nanotubes. The content of single-layer carbon nanotubes in the active material layer (102) is from 0.035% by mass to 0.08% by mass (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrode for an electricity storage device. Background Art

[0002] The power storage device disclosed in Patent Document 1 includes a positive electrode and a negative electrode, each with an active material layer formed on one side of a current collector, and a separator disposed between the positive and negative electrodes. The positive and negative electrodes are arranged with the separator sandwiched between them, with the active material layers facing each other. The active material layers of the positive and negative electrodes contain conductive fibers as a conductive additive to enhance electron conductivity within the active material layers.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 2016-189325 Summary of the Invention

[0006] Problems to be solved by the invention

[0007] One method for increasing the energy density of these energy storage devices is to thicken the active material layer of the electrode to increase the proportion of the active material layer in the device. The inventors of this application have newly discovered that, in electrodes with thick active material layers, the inclusion of carbon nanotubes in the active material layer can sometimes reduce the long-term output of the energy storage device. Furthermore, the inventors of this application have discovered that the inclusion of carbon nanotubes in the active material layer of the electrode improves the peel strength of the active material layer relative to the carbon-coated current collector.

[0008] Solutions for solving problems

[0009] An electrode for a power storage device that achieves the above-mentioned purpose comprises a current collector having a first surface and an active material layer formed on the first surface of the current collector, wherein the thickness of the active material layer is greater than 250 μm. In the electrode for the power storage device, a carbon coating is provided on the first surface of the current collector, and the active material layer contains an active material capable of absorbing and releasing charge carriers, an aqueous binder, and single-layer carbon nanotubes, and the content of the single-layer carbon nanotubes in the active material layer is greater than 0.035 mass % and less than 0.08 mass %.

[0010] Preferably, in the electrode for the power storage device, the density of the active material layer is 1.8 g / cm 3 above.

[0011] Preferably, in the above-mentioned electrode for a power storage device, the aqueous binder includes styrene-butadiene rubber, and the content of the styrene-butadiene rubber is 1.2% by mass or more and 1.8% by mass or less.

[0012] Preferably, in the above-mentioned electrode for an electricity storage device, the current collector is an aluminum current collector composed of aluminum and is used as a positive electrode.

[0013] Preferably, in the above-mentioned electrode for a power storage device, the content of the active material in the active material layer is 96% by mass or more.

[0014] Preferably, in the above-mentioned electrode for a power storage device, the carbon coating layer has a thickness of 0.1 μm or more and 5.0 μm or less.

[0015] Effects of the Invention

[0016] According to the present invention, the long-term output of the power storage device and the peel strength of the active material layer with respect to the current collector are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a cross-sectional view of an electrode for a power storage device.

[0018] Figure 2 This is an electron microscope photograph of the first surface of the current collector from which the active material layer has been peeled off.

[0019] Figure 3 It is a cross-sectional view of the power storage device.

[0020] Figure 4 This is a cross-sectional view of an electrode embodied as a modified example of a bipolar electrode.

[0021] Figure 5 This is a graph showing the relationship between the carbon nanotube content and long-term output.

[0022] Figure 6 This is a graph showing the relationship between the carbon nanotube content and short-time output. DETAILED DESCRIPTION

[0023] Hereinafter, one embodiment of the present invention will be described with reference to the accompanying drawings.

[0024] (electrode)

[0025] The electrode of this embodiment is used as the positive electrode or negative electrode of an electrical storage device. The electrical storage device is, for example, a secondary battery such as a nickel-metal hydride secondary battery or a lithium-ion secondary battery. Alternatively, the electrical storage device may be an electric double-layer capacitor. The following describes the case of an electrode of a lithium-ion secondary battery.

[0026] like Figure 1As shown, the electrode 100 includes a current collector 101 and an active material layer 102 provided on a first surface 101 a of the current collector 101 .

[0027] [Current Collector]

[0028] The current collector 101 is a chemically inert electrical conductor that allows current to continuously flow through the active material layer 102 during discharge or charge of the lithium-ion secondary battery. The current collector 101 is, for example, in the form of a foil. The thickness of the foil-shaped current collector 101 is, for example, 1 μm to 100 μm, preferably 10 μm to 60 μm. Materials for constituting the current collector 101 include, for example, metal materials, conductive resin materials, and conductive inorganic materials.

[0029] Examples of the metal material include copper, aluminum, nickel, titanium, and stainless steel. Examples of the conductive resin material include conductive polymer materials and resins obtained by adding conductive fillers to non-conductive polymer materials as needed.

[0030] When the electrode 100 is used as a positive electrode in a power storage device, the current collector 101 is preferably an aluminum current collector composed of aluminum. The aluminum current collector may be composed of a single element of aluminum or an aluminum alloy. Examples of aluminum alloys include Al-Mn alloys, Al-Mg alloys, and Al-Mg-Si alloys. The aluminum content in the aluminum layer 11a is, for example, 50% by mass or greater, and preferably 70% by mass or greater.

[0031] A carbon coating C is provided on the entire surface of the first surface 101a of the current collector 101. The thickness of the carbon coating C is, for example, 0.1 μm or more, preferably 0.2 μm or more. By setting the thickness of the carbon coating C to 0.1 μm or more, the peel strength of the active material layer 102 relative to the current collector 101 is improved. The thickness of the carbon coating C is, for example, 5.0 μm or less, preferably 2.0 μm or less. By setting the thickness of the carbon coating C to 5.0 μm or less, the volume ratio of the active material layer 102 in the power storage device using the electrode 100 can be increased. As a result, the energy density of the power storage device using the electrode 100 can be improved.

[0032] The carbon coating C is not particularly limited, and any known carbon coating used for a current collector of an electrode can be applied. An example of the carbon coating C includes carbon particles and a coating binder. The carbon coating C may also contain other components in addition to the carbon particles and the coating binder as needed.

[0033] Examples of carbon particles include graphite, acetylene black, and carbon black, which are known carbon materials used in carbon coatings. The carbon particles contained in the carbon coating C may be a single type or a combination of two or more types. The carbon particle content in the carbon coating C is, for example, 30% to 90% by mass.

[0034] Examples of the material constituting the coating binder include acrylic resins, cellulose derivatives, and carboxyl-modified styrene-butadiene rubber.

[0035] Examples of acrylic resins include homopolymers of acrylic monomers such as acrylic acid, methacrylic acid, and (meth)acrylic acid esters, and (meth)acrylic acid copolymers containing these acrylic monomers. In the present embodiment, (meth)acrylic acid refers to acrylic acid or methacrylic acid.

[0036] Examples of the (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.

[0037] In the (meth)acrylic acid copolymers, other comonomers copolymerized with the acrylic monomers include α-olefins, styrene, α-methylstyrene, vinyltoluene, acrylonitrile, methacrylonitrile, and vinyl acetate. These comonomers can be present in the acrylic resin as random copolymers, graft copolymers, or block copolymers. Examples of the (meth)acrylic acid copolymers include silicon-modified acrylic styrene resins, carboxyl-modified acrylic styrene resins, and hydroxyl-modified acrylic resins.

[0038] Examples of cellulose derivatives include carboxymethyl cellulose and its salts. Examples of carboxymethyl cellulose salts include sodium or ammonium salts of carboxymethyl cellulose. The coating binder may be composed of a single material or a combination of two or more. The coating binder content in the carbon coating C is, for example, 10% to 70% by mass.

[0039] The carbon coating layer C can be formed, for example, by applying a carbon paste containing carbon particles and a coating binder to the first surface 101 a of the current collector 101 and then curing the applied carbon paste film.

[0040] [Active material layer]

[0041] Active material layer 102 is formed on carbon coating layer C on first surface 101a of current collector 101. Active material layer 102 contains an active material capable of occluding and releasing charge carriers such as lithium ions, an aqueous binder, and single-walled carbon nanotubes (SWCNTs). Hereinafter, single-walled carbon nanotubes are referred to as carbon nanotubes.

[0042] In the case of the electrode 100 used as the positive electrode of an electrical storage device, the active material contained in the active material layer 102 is a positive electrode active material. As the positive electrode active material, any material that can be used as a positive electrode active material for a lithium ion secondary battery, such as a lithium composite metal oxide with a layered rock salt structure, a metal oxide with a spinel structure, or a polyanion compound, can be used. In addition, two or more positive electrode active materials can also be used in combination. As a specific example of the positive electrode active material, olivine-type lithium iron phosphate (LiFePO4) as a polyanion compound can be cited.

[0043] In the case of the electrode 100 used as the negative electrode of the power storage device, the active material contained in the active material layer 102 is a negative electrode active material. As the negative electrode active material, any substance that can be used as a negative electrode active material for a lithium-ion secondary battery, such as Li or carbon, a metal compound, an element capable of alloying with lithium, or a compound thereof, can be used. Examples of carbon include natural graphite, artificial graphite, or hard carbon (difficult to graphitize carbon) or soft carbon (easily graphitizable carbon). Examples of artificial graphite include highly oriented graphite and mesophase carbon microbeads. Examples of elements capable of alloying with lithium include silicon and tin.

[0044] The active material content in active material layer 102 is not particularly limited. The active material content in active material layer 102 is, for example, 96% by mass or greater, preferably 97% by mass or greater. By setting the active material content in active material layer 102 to 96% by mass or greater, the volume ratio of the active material in active material layer 102 can be increased. Consequently, the energy density of a power storage device incorporating electrode 100 can be increased. The active material content in active material layer 102 is, for example, 98.965% by mass or less, preferably 98% by mass or less.

[0045] The aqueous binder is a binder that can be dissolved or dispersed in an aqueous solvent, and is a binder that is mixed with the positive electrode active material in a state of being dispersed or dissolved in an aqueous solvent. The aqueous binder is not particularly limited, and conventionally known materials can be used as the aqueous binder contained in the active material layer of the lithium ion secondary battery. As aqueous binders, for example, fluororesins such as polyvinylidene fluoride, polytetrafluoroethylene, fluororubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamide-imide, acrylic resins such as alkoxysilyl resins, poly(meth)acrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, sodium alginate, ammonium alginate, water-soluble cellulose ester crosslinked products, starch-acrylic acid graft polymers. The aqueous binder contained in the active material layer 102 can be one or more.

[0046] The content of the aqueous binder in active material layer 102 is not particularly limited. The content of the aqueous binder in active material layer 102 is, for example, 1.0% by mass or greater, preferably 1.3% by mass or greater. The content of the aqueous binder in active material layer 102 is, for example, 2.5% by mass or less, preferably 2.1% by mass or less.

[0047] Furthermore, the active material layer 102 preferably contains styrene-butadiene rubber as an aqueous binder. The content of styrene-butadiene rubber in the active material layer 102 is, for example, 1.2% by mass or greater and 2.5% by mass or less. Furthermore, when the content of styrene-butadiene rubber is 1.2% by mass or greater, the active material layer 102 is improved relative to the current collector 101. Furthermore, the content of styrene-butadiene rubber is preferably 1.8% by mass or less. In this case, the curvature of the active material layer 102 is reduced, thereby improving ionic conductivity and the output performance of the power storage device.

[0048] The fiber length and fiber diameter of the carbon nanotubes are not particularly limited. The fiber length of the carbon nanotubes is, for example, not less than 5 μm and not more than 1000 μm. The fiber diameter of the carbon nanotubes is, for example, not less than 1.6 nm and not more than 100 μm. Furthermore, the fiber length distribution of the carbon nanotubes is preferably one in which a main peak in a graph showing the fiber length distribution is only one.

[0049] The carbon nanotube content in active material layer 102 is 0.035 mass% or more and 0.08 mass% or less. By setting the carbon nanotube content to 0.035 mass% or more, the peel strength of active material layer 102 relative to current collector 101 is improved. Furthermore, by setting the carbon nanotube content to 0.08 mass% or less, the long-term output of the power storage device is improved.

[0050] The active material layer 102 can contain other components other than the three components of the above-mentioned active material, aqueous binder and carbon nanotube as needed. As other components, for example, a conductive aid, an electrolyte (polymer matrix, ion conductive polymer, electrolyte, etc.), and an electrolyte supporting salt (lithium salt) for improving ion conductivity can be cited. As a conductive aid, for example, acetylene black, carbon black, and graphite can be cited. The type and content of other components are not particularly limited, and can be appropriately referred to the previously known insights about lithium ion secondary batteries.

[0051] To improve the energy density of the power storage device, the active material layer 102 is formed thicker than usual. The thickness t of the active material layer 102 is 250 μm or greater. Alternatively, the thickness t of the active material layer 102 is, for example, 750 μm or less.

[0052] The density of the active material layer 102 is not particularly limited. The density of the active material layer 102 is, for example, 1.8 g / cm 3 When the density of the active material layer 102 is high, the long-term output of the power storage device is likely to decrease due to the inclusion of carbon nanotubes. 3 the following.

[0053] (Electricity Storage Device)

[0054] Next, an example of a power storage device to which the electrode 100 is applied will be described.

[0055] The power storage device to which the electrode 100 is applied is, for example, a power storage module used in batteries of various vehicles such as forklifts, hybrid vehicles, and electric vehicles. In this embodiment, a case where the power storage device 10 is a lithium ion secondary battery is exemplified.

[0056] like Figure 3 As shown, the power storage device 10 is constructed to include a unit stack 30 (stacked body) in which a plurality of power storage units (cells) 20 are stacked (stacked) in a stacking direction. Hereinafter, the stacking direction of the plurality of power storage units 20 is referred to as the stacking direction. Each power storage unit 20 includes a positive electrode 21, a negative electrode 22, a separator 23, and a spacer 24. Either or both of the positive electrode 21 and the negative electrode 22 of the power storage unit 20 are the above-mentioned electrodes 100. In addition, Figure 3 In the figure, the carbon coating C is omitted.

[0057] The positive electrode 21 includes a positive electrode current collector 21a and a positive electrode active material layer 21b provided on a first surface 21a1 of the positive electrode current collector 21a. When the positive electrode 21 is the electrode 100, the positive electrode current collector 21a is the current collector 101, and the positive electrode active material layer 21b is the active material layer 102.

[0058] In a plan view (hereinafter referred to as a plan view) viewed from the stacking direction, the positive electrode active material layer 21b is formed in the central portion of the first surface 21a1 of the positive electrode current collector 21a. The peripheral edge of the first surface 21a1 of the positive electrode current collector 21a in a plan view is a positive electrode uncoated portion 21c where the positive electrode active material layer 21b is not provided. The positive electrode uncoated portion 21c is arranged to surround the positive electrode active material layer 21b in a plan view.

[0059] The negative electrode 22 includes a negative electrode current collector 22a and a negative electrode active material layer 22b provided on a first surface 22a1 of the negative electrode current collector 22a. When the negative electrode 22 is the electrode 100, the negative electrode current collector 22a is the current collector 101, and the negative electrode active material layer 22b is the active material layer 102.

[0060] When viewed from above, the negative electrode active material layer 22b is formed in the center of the first surface 22a1 of the negative electrode current collector 22a. The peripheral edge of the first surface 22a1 of the negative electrode current collector 22a when viewed from above is a negative electrode uncoated portion 22c where the negative electrode active material layer 22b is not provided. The negative electrode uncoated portion 22c is configured to surround the positive electrode active material layer 21b when viewed from above. The positive electrode 21 and the negative electrode 22 are configured so that the positive electrode active material layer 21b and the negative electrode active material layer 22b face each other in the stacking direction. In other words, the direction in which the positive electrode 21 and the negative electrode 22 face each other coincides with the stacking direction. The negative electrode active material layer 22b is formed to be the same size as the positive electrode active material layer 21b, or slightly larger than the positive electrode active material layer 21b. When the negative electrode active material layer 22 b is formed slightly larger than the positive electrode active material layer 21 b , the entire region where the positive electrode active material layer 21 b is formed is located within the region where the negative electrode active material layer 22 b is formed in a plan view.

[0061] The positive electrode current collector 21a has a second surface 21a2, which is the surface opposite to the first surface 21a1. The positive electrode 21 is a unipolar electrode, in which neither the positive electrode active material layer 21b nor the negative electrode active material layer 22b is formed on the second surface 21a2 of the positive electrode current collector 21a. The negative electrode current collector 22a has a second surface 22a2, which is the surface opposite to the first surface 22a1. The negative electrode 22 is a unipolar electrode, in which neither the positive electrode active material layer 21b nor the negative electrode active material layer 22b is formed on the second surface 22a2 of the negative electrode current collector 22a.

[0062] The separator 23 is a member disposed between the positive electrode 21 and the negative electrode 22 , and prevents a short circuit caused by contact between the positive electrode 21 and the negative electrode 22 by isolating the positive electrode 21 and the negative electrode 22 while allowing charge carriers such as lithium ions to pass therethrough.

[0063] Separator 23 is, for example, a porous sheet or nonwoven fabric containing a polymer that absorbs and retains electrolytes. Examples of materials constituting separator 23 include polyolefins such as polypropylene and polyethylene, and polyesters. Separator 23 can have a single-layer structure or a multi-layer structure. A multi-layer structure can include, for example, an adhesive layer and a ceramic layer serving as a heat-resistant layer.

[0064] The separator 24 is disposed between the first surface 21a1 of the positive electrode current collector 21a of the positive electrode 21 and the first surface 22a1 of the negative electrode current collector 22a of the negative electrode 22, and is positioned on the outer periphery of the positive electrode active material layer 21b and the negative electrode active material layer 22b. The separator 24 adheres to both the positive electrode current collector 21a and the negative electrode current collector 22a. The separator 24 maintains a gap between the positive electrode current collector 21a and the negative electrode current collector 22a to prevent short circuits between the current collectors and to provide a liquid-tight seal between the current collectors.

[0065] The spacer 24 extends along the periphery of the positive electrode collector 21a and the negative electrode collector 22a in a plan view and is formed into a frame shape surrounding the positive electrode collector 21a and the negative electrode collector 22a. The spacer 24 is arranged between the positive electrode uncoated portion 21c of the first surface 21a1 of the positive electrode collector 21a and the negative electrode uncoated portion 22c of the first surface 22a1 of the negative electrode collector 22a.

[0066] Examples of the material constituting the spacer 24 include various resin materials such as polyethylene (PE), modified polyethylene (modified PE), polystyrene (PS), polypropylene (PP), modified polypropylene (modified PP), ABS resin, and AS resin.

[0067] Inside the electricity storage cell 20 , a sealed space S is formed, which is surrounded by a frame-shaped separator 24 , the positive electrode 21 , and the negative electrode 22 . A separator 23 and an electrolyte are accommodated in the sealed space S. The peripheral edge of the separator 23 is embedded in the separator 24 .

[0068] As the electrolyte, for example, liquid electrolytes and polymer gel electrolytes containing electrolytes retained in a polymer matrix can be cited. As the liquid electrolyte, for example, liquid electrolytes containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent can be cited. As the electrolyte salt, known lithium salts such as LiClO4, LiAsF6, LiPF6, LiBF4, LiCF3SO3, LiN(FSO2)2, and LiN(CF3SO2)2 can be used. In addition, known solvents such as cyclic carbonates, cyclic esters, chain carbonates, chain esters, and ethers can be used. In addition, two or more of these known solvent materials can be combined for use.

[0069] The separator 24 seals the sealed space S between the positive electrode 21 and the negative electrode 22, thereby preventing leakage of the electrolyte contained in the sealed space S to the outside. Furthermore, the separator 24 prevents the intrusion of moisture from the outside of the electricity storage device 10 into the sealed space S. Furthermore, the separator 24 prevents gas generated from the positive electrode 21 or the negative electrode 22 due to, for example, charge and discharge reactions from leaking to the outside of the electricity storage device 10.

[0070] The cell stack 30 has a structure in which a plurality of power storage cells 20 are stacked with the second surface 21a2 of the positive electrode current collector 21a in contact with the second surface 22a2 of the negative electrode current collector 22a.

[0071] Here, in the cell stack 30, two adjacent storage cells 20 in the stacking direction form a pseudo-bipolar electrode 25, where the positive electrode current collector 21a and the negative electrode current collector 22a in contact with each other are considered to be a single current collector. The pseudo-bipolar electrode 25 includes a current collector having a structure in which the positive electrode current collector 21a and the negative electrode current collector 22a are stacked, a positive electrode active material layer 21b formed on one surface of the current collector, and a negative electrode active material layer 22b formed on the other surface of the current collector.

[0072] The power storage device 10 includes a pair of current-carrying members, namely a positive current-carrying plate 40 and a negative current-carrying plate 50, arranged in the stacking direction of the cell stack 30 so as to sandwich the cell stack 30. The positive current-carrying plate 40 and the negative current-carrying plate 50 are each made of a material having excellent electrical conductivity.

[0073] The positive electrode current conducting plate 40 is electrically connected to the second surface 21a2 of the positive electrode current collector 21a of the outermost positive electrode 21 at one end in the stacking direction. The negative electrode current conducting plate 50 is electrically connected to the second surface 22a2 of the negative electrode current collector 22a of the outermost negative electrode 22 at the other end in the stacking direction.

[0074] The charging and discharging of the power storage device 10 is performed by terminals provided on the positive electrode current plate 40 and the negative electrode current plate 50. As the material constituting the positive electrode current plate 40, for example, the same material as the material constituting the positive electrode current collector 21a can be used. The positive electrode current plate 40 can also be composed of a metal plate thicker than the positive electrode current collector 21a used in the unit stack 30. As the material constituting the negative electrode current plate 50, for example, the same material as the material constituting the negative electrode current collector 22a can be used. The negative electrode current plate 50 can also be composed of a metal plate thicker than the negative electrode current collector 22a used in the unit stack 30.

[0075] Next, the operation of this embodiment will be described.

[0076] Figure 2 The image shown is an electron microscope photograph of first surface 101a of current collector 101 of electrode 100 after the active material layer 102 has been peeled off. In this image, the spherical objects are the active material, and the fibrous objects are carbon nanotubes. The carbon nanotubes are entangled on the surface of the active material and are also rooted in the carbon coating C of current collector 101. By setting the carbon nanotube content in active material layer 102 to 0.035% by mass or more, the carbon nanotubes can be suitably bonded to the active material and carbon coating C. As a result, the peel strength of active material layer 102 relative to current collector 101 is improved.

[0077] As described above, when carbon nanotubes are included in the active material layer 102, in addition to the effect of a conductive additive that improves the electron conductivity of the active material layer 102, the peel strength of the active material layer 102 relative to the current collector 101 can also be improved. On the other hand, in electrodes having an active material layer 102 with a thickness of 250 μm or greater, the inclusion of carbon nanotubes in the active material layer 102 can lead to a problem of reduced output over long periods of time in the power storage device.

[0078] This problem arises because the carbon nanotubes within active material layer 102 reduce the ionic conductivity of active material layer 102. Specifically, incorporating carbon nanotubes into active material layer 102 increases the curvature of active material layer 102, resulting in a decrease in the ionic conductivity of active material layer 102. Furthermore, as the thickness of active material layer 102 increases, the ease of movement of charge carriers such as lithium ions within active material layer 102 becomes the primary factor limiting the long-term output of the power storage device, i.e., the upper limit of the long-term output. Consequently, the decrease in ionic conductivity of active material layer 102 manifests itself as a decrease in the long-term output of the power storage device.

[0079] The inventors of this application have discovered that the aforementioned decrease in the long-term output of the power storage device can be suppressed by setting the carbon nanotube content in the active material layer 102 to 0.08 mass % or less. Therefore, by using the electrode 100 of this embodiment having a carbon nanotube content of 0.08 mass % or less in the active material layer 102, the long-term output of the power storage device can be improved.

[0080] Next, the operation and effects of this embodiment will be described.

[0081] (1) An electrode 100 for a power storage device includes a current collector 101 having a first surface 101a and an active material layer 102 formed on the first surface 101a of the current collector 101. The thickness of the active material layer 102 is 250 μm or greater. A carbon coating layer C is provided on the first surface 101a of the current collector 101. The active material layer 102 contains an active material capable of occluding and releasing charge carriers, an aqueous binder, and carbon nanotubes. The carbon nanotube content in the active material layer 102 is 0.035% by mass or greater and 0.08% by mass or less.

[0082] According to the above configuration, the long-term output of the power storage device is improved. In addition, according to the above configuration, the peel strength of the active material layer 102 with respect to the current collector 101 is improved.

[0083] (2) The density of the active material layer 102 is 1.8 g / cm 3 above.

[0084] The higher the density of active material layer 102, the greater the curvature of active material layer 102 when it contains carbon nanotubes. As a result, the decrease in the long-term output of the power storage device also increases. Therefore, when the density of active material layer 102 is high, the effect of improving the long-term output of the power storage device described in (1) above can be more significantly achieved.

[0085] (3) The aqueous binder contains styrene-butadiene rubber. The content of styrene-butadiene rubber in active material layer 102 is 1.2% by mass or more and 1.8% by mass or less.

[0086] By setting the styrene-butadiene rubber content to 1.2% by mass or greater, the peel strength of active material layer 102 relative to current collector 101 is improved. Furthermore, by setting the styrene-butadiene rubber content to 1.8% by mass or less, the curvature of active material layer 102 is reduced. As a result, the ionic conductivity of active material layer 102 is enhanced, and the output performance of the power storage device is improved.

[0087] (4) The content of the active material in active material layer 102 is 96% by mass or more.

[0088] According to the above configuration, the energy density of the power storage device to which the electrode 100 is applied can be improved.

[0089] (5) The thickness of the carbon coating layer C is 0.1 μm or more and 5.0 μm or less.

[0090] According to the above configuration, the peel strength of the active material layer 102 with respect to the current collector 101 is improved. In addition, according to the above configuration, the energy density of the power storage device to which the electrode 100 is applied can be improved.

[0091] In addition, this embodiment can be implemented by modifying as follows: This embodiment and the following modification examples can be implemented in combination with each other within the scope of no technical contradiction.

[0092] The formation range of the carbon coating layer C on the first surface 101a of the current collector 101 may be changed. For example, the carbon coating layer C may be formed only on the area of ​​the first surface 101a where the active material layer 102 is formed, or may be formed locally on a portion of the area.

[0093] ○Electrode 100 can also be a bipolar structure electrode. Figure 4 An example of the electrode 100 embodied as an electrode with a bipolar structure will be described.

[0094] Figure 4The illustrated bipolar electrode 100 includes a bipolar current collector 103. Bipolar current collector 103 is a laminate formed by joining a foil-shaped positive electrode current collector 104 and a foil-shaped negative electrode current collector 105 together in the thickness direction. Examples of bipolar current collector 103 include those formed by laminating aluminum foils together or those formed by laminating aluminum foil and copper foil.

[0095] A carbon coating layer C is provided on a first surface 103a of the bipolar current collector 103, formed by the positive electrode current collector 104. Furthermore, an active material layer 102a, which is a positive electrode active material layer, is provided on the first surface 103a via the carbon coating layer C. Furthermore, a carbon coating layer C is provided on a second surface 103b of the bipolar current collector 103, formed by the negative electrode current collector 105. Furthermore, an active material layer 102b, which is a negative electrode active material layer, is provided on the second surface 103b via the carbon coating layer C.

[0096] Either or both of the active material layer 102a and the active material layer 102b are active material layers that meet the requirements of the active material layer 102 described in the above embodiment. Furthermore, if the active material layer 102a does not meet the requirements of the active material layer 102 described in the above embodiment, the carbon coating layer C on the first surface 103a can be omitted. Similarly, if the active material layer 102b does not meet the requirements of the active material layer 102 described in the above embodiment, the carbon coating layer C on the second surface 103b can be omitted.

[0097] The specific configuration of the power storage device 10 incorporating the electrode 100 is not particularly limited, as long as at least one positive electrode or at least one negative electrode corresponds to the electrode 100. For example, the number of power storage cells 20 constituting the power storage device 10 may be one. Alternatively, the power storage device 10 may include a restraining member that applies a restraining load to the cell stack 30 in the stacking direction. Furthermore, the power storage device 10 may include an electrode 100 configured as a bipolar electrode.

[0098] Example

[0099] The following describes examples that further embody the above-described embodiment.

[0100] <Making the positive electrode>

[0101] LiFePO₄, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), and single-walled carbon nanotubes (CNTs) were mixed in the proportions shown in Tables 1 and 2, and water was added to the mixture to prepare a positive electrode composite material having a solid content of 64% by mass. LiFePO₄ served as the positive electrode active material. Styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) served as aqueous binders.

[0102] As a positive electrode collector, a carbon-coated aluminum foil with a thickness of 30 μm was prepared. A carbon coating with a thickness of 1 μm was provided on one side of the carbon-coated aluminum foil. The positive electrode composite material was applied to the surface of the positive electrode collector provided with the carbon coating in a film-like form using a doctor blade method. The applied positive electrode composite material was heated at 50°C to dry and solidify the positive electrode composite material, thereby producing positive electrode sheets of Test Examples 1 to 10 in which a positive electrode active material layer with a thickness of 250 μm was formed on the positive electrode collector. The density of the positive electrode active material layer of each of the obtained positive electrode sheets was measured. As a result, the density of the positive electrode active material layer of each positive electrode sheet was 1.8 g / cm 3 .

[0103] <Peel Strength Measurement>

[0104] The positive electrode sheets of Test Examples 1 to 10 were cut into 2.5 cm × 4 cm pieces as test samples. A 90-degree peel test in accordance with JIS K 6854-1 was performed using a peel tester (LTS-50N-S300 manufactured by MINEBEA). The peel strength of the positive electrode active material layer relative to the positive electrode current collector in the test sample was calculated by dividing the strength measured in the 90-degree peel test by the line width (2.5 cm). The results are shown in Tables 1 and 2.

[0105] [Table 1]

[0106]

[0107] [Table 2]

[0108]

[0109] As shown in Tables 1 and 2, the peel strength of the positive electrode active material layer relative to the positive electrode current collector increases with increasing CNT content. Furthermore, the peel strength increases significantly between 0.03% by mass (Test Example 4) and 0.035% by mass (Test Example 5) of the CNT content, and increases slowly in other ranges. This result shows that by setting the CNT content in the active material layer to 0.035% by mass or more, the peel strength of the active material layer relative to the current collector is significantly improved.

[0110] <Production of Power Storage Device>

[0111] Electrode batteries were fabricated by combining the positive electrode sheets of Test Examples 1 to 10, cut into rectangular shapes measuring 30 mm long by 25 mm wide, with the negative electrode and separator. The electrode batteries were housed in a battery case, electrolyte was injected, and the case was sealed to produce lithium-ion secondary batteries.

[0112] The negative electrode used consisted of a copper current collector and a negative electrode active material layer composed of graphite as the negative electrode active material, styrene-butadiene rubber as the binder, and carboxymethyl cellulose as the dispersant. A polyethylene separator was used. The electrolyte used was lithium hexafluorophosphate dissolved to a concentration of 1.2 M in a mixed solvent of methyl propionate and ethylene carbonate at a volume ratio of 15:85.

[0113] <Evaluation of Output Performance of Power Storage Device>

[0114] (Evaluation of long-term output)

[0115] In this evaluation, lithium-ion secondary batteries obtained from the positive electrode sheets of Test Examples 6 to 10 that showed high peel strength were used. Each lithium-ion secondary battery was charged with a constant current (CC) until the voltage reached 3.75V. Then, a constant power discharge was performed at 200 to 300mW at 40°C, and the power that could be output for 2500 seconds (2500s output) was calculated. Figure 5 Graphs are shown in which the values ​​of the 2500 s output relative to the CNT content in each test example are plotted.

[0116] (Evaluation of short-time output)

[0117] In this evaluation, lithium-ion secondary batteries obtained using the positive electrode sheets of Test Examples 2 to 4 and 6 to 10 were used. Each lithium-ion secondary battery was charged with a constant current (CC) of 10 mA DC until the voltage of the negative electrode relative to the positive electrode became 3.75 V, and then discharged to an SOC (State of Charge) of 80%. Then, the battery was discharged at a current of 10C at 25°C for 10 seconds, and the output during the 10-second discharge (10s output) was calculated. Figure 6 Graphs are shown in which the 10s output values ​​are plotted against the CNT content in each test example.

[0118] like Figure 5As shown in the graph, the 2500s output, which is a parameter representing the long-term output, is roughly constant within the range of 0.04 to 0.08 mass% of CNT content, but decreases significantly when the CNT content increases to 0.10 mass%. Figure 6 As shown in the graph, 10s output, a parameter representing short-term output, increases with increasing CNT content within the CNT content range of 0.04% by mass or less, but remains roughly constant within the range of 0.04% by mass or greater. These results indicate that adding 0.10% or more CNTs has no effect on short-term output, but does reduce long-term output.

[0119] In addition, although detailed test data is omitted, the same test was conducted using a positive electrode sheet in which the thickness of the positive electrode active material layer of the positive electrode sheet of Test Examples 1 to 10 was changed from 250 μm to 120 μm. As a result, no decrease in short-term output or long-term output was confirmed when 0.10% by mass or more of CNTs was added. Therefore, it can be seen that the decrease in long-term output caused by the addition of 0.10% by mass or more of CNTs is a phenomenon unique to the case where the active material layer is formed thick. From these results, it can be seen that when the thickness of the active material layer is 250 μm or more, by setting the CNT content in the active material layer to 0.08% by mass or less, the long-term output is improved compared to the case where it exceeds 0.08% by mass.

[0120] <Evaluation of curvature>

[0121] Symmetrical model cells for curvature measurement were prepared using positive electrodes cut into predetermined shapes from the positive electrode sheets of Test Examples 7 and 9, separators, and electrolytes. Polyethylene separators were used. The electrolyte used was lithium hexafluorophosphate dissolved at a concentration of 1.2 M in a mixed solvent of methyl propionate and ethylene carbonate at a volume ratio of 15:85.

[0122] The curvature τ of the positive electrode active material layer of the positive electrode sheet of each test example was calculated based on the following formula (1).

[0123] Curvature τ=(R ion ·A·K·ε) / 2d…(1)

[0124] R ion : Ionic resistance

[0125] A: Electrode area (8.06 cm 2 )

[0126] K: ionic conductivity of the electrolyte

[0127] ε: Porosity of the positive electrode active material layer

[0128] d: thickness of the positive electrode active material layer (250 μm)

[0129] Ionic resistance R ion The symmetrical unit impedance of the symmetrical model unit is measured, and the real number component of the extremely low frequency of the measured symmetrical unit impedance (= ionic resistance R ion / 3)Exported.

[0130] The ion conductivity K of the electrolyte solution was calculated from the measured resistance value at 25° C. and 10 kHz of a sample in which the electrolyte solution of the above composition was sealed in a cell having a platinum electrode.

[0131] The porosity ε of the positive electrode active material layer was measured using mercury intrusion porosimetry.

[0132] [Table 3]

[0133]

[0134] As shown in Table 3, the curvature of Test Example 9, which has a relatively high CNT content, is higher than that of Test Example 7, which has a relatively low CNT content. This result shows that the CNTs contained in the active material layer are the main factor that increases the curvature of the active material layer, and in other words, the main factor that reduces the ionic conductivity of the active material layer. Therefore, it can be assumed that the decrease in long-term output caused by the addition of 0.10% by mass or more of CNTs is due to the decrease in the ionic conductivity of the active material layer caused by the CNTs.

[0135] Furthermore, when the active material layer is thick, the impact of the decrease in ionic conductivity becomes greater. Therefore, based on the idea that the long-term output decrease is due to the decrease in ionic conductivity of the active material layer caused by CNTs, it can be explained that the long-term output decrease is a phenomenon unique to the case of thick active material layers.

[0136] <Tests related to styrene-butadiene rubber (SBR) content>

[0137] The positive electrode sheets of Test Examples 11 to 13 were prepared in the same manner as in Test Examples 1 to 10, except that the compounding ratios were changed to those shown in Table 4. The density of the positive electrode active material layer of each of the obtained positive electrode sheets was measured. The density of the positive electrode active material layer of each positive electrode sheet was 2.0 g / cm3. 3In addition, the positive electrode sheet of Test Example 14 was prepared by the same method as Test Examples 1 to 10, except that the thickness of the positive electrode active material layer was changed from 250 μm to 370 μm and the mixing ratio was changed to the mixing ratio shown in Table 4. The density of the positive electrode active material layer of the positive electrode sheet of Test Example 14 was measured and the result was that the density was 2.0 g / cm 3 .

[0138] The peel strength between the positive electrode active material layer and the positive electrode current collector in the positive electrode sheets of Test Examples 11 to 13 and the positive electrode sheet of Test Example 14 was calculated using the same method as above. Furthermore, the curvature of the positive electrode active material layer in Test Examples 11 to 13 was calculated using the same method as above. These results are shown in Table 4.

[0139] In addition, lithium ion secondary batteries were prepared using the positive electrode sheets of Test Examples 11 to 13 in the same manner as above. Each of the prepared lithium ion secondary batteries was charged at a constant current (CC) until the voltage relative to the positive electrode reached 3.75 V, and the capacity C when discharged at 0.01 C was determined. 0.01 And the capacity C1 when discharged at 1C. And, based on the following formula (2), from the capacity C 0.01 The results are shown in Table 4.

[0140] ΔSOC (%) = (C1 / C 0.01 )×100…(2)

[0141] [Table 4]

[0142]

[0143] As shown in Table 4, the peel strength of the positive electrode active material layer relative to the positive electrode collector increases with the increase in the SBR content. The curvature of the positive electrode active material layer increases with the increase in the SBR content. ΔSOC is a parameter that represents the output performance assuming stable driving. With respect to ΔSOC, the values ​​of Test Examples 11 and 12 are of the same degree, and the value of Test Example 13, which has a higher SBR content than Test Examples 11 and 12, is lower than the values ​​of Test Examples 11 and 12. From these results, it can be seen that from the viewpoint of improving the peel strength of the active material layer, it is preferred to increase the SBR content. In addition, from the viewpoint of improving the output performance, it is preferred to set the SBR content to 1.8% by mass or less.

[0144] As shown in Table 4, the peel strength of Test Example 14, in which the thickness of the positive electrode active material layer was changed from 250 μm to 370 μm, was 0.35 N / cm. The results show that the thickness of the active material layer does not significantly affect the peel strength.

[0145] Next, technical ideas that can be grasped from the above-mentioned embodiment and modified examples are described below.

[0146] (i) A power storage device comprising an electrode having an active material layer formed on a first surface of a current collector, wherein a carbon coating is provided on the first surface of the current collector, the active material layer has a thickness of 250 μm or more, the active material layer contains an active material capable of absorbing and releasing charge carriers, an aqueous binder, and carbon nanotubes, and the content of the carbon nanotubes in the active material layer is not less than 0.035 mass % and not more than 0.08 mass %.

[0147] Description of Reference Numerals

[0148] C…Carbon coating

[0149] 100...electrode

[0150] 101…current collector

[0151] 101a…1st surface

[0152] 102 ...active material layer.

Claims

1. An electrode for a power storage device, comprising a current collector having a first surface and an active material layer formed on the first surface of the current collector, wherein the thickness of the active material layer is 250 μm or more, wherein the electrode for a power storage device is characterized in that: A carbon coating is provided on the first surface of the current collector, The active material layer contains an active material capable of absorbing and releasing charge carriers, an aqueous binder, and a single-walled carbon nanotube. The content of the single-walled carbon nanotubes in the active material layer is 0.035 mass % or more and 0.08 mass % or less.

2. The electrode for an electrical storage device according to claim 1, wherein The density of the active material layer is 1.8 g / cm 3 above.

3. The electrode for an electrical storage device according to claim 1 or claim 2, wherein: The water-based binder comprises styrene-butadiene rubber, The content of the styrene-butadiene rubber is 1.2 mass % or more and 1.8 mass % or less.

4. The electrode for an electrical storage device according to any one of claims 1 to 3, wherein: The current collector is an aluminum current collector composed of aluminum and is used as a positive electrode.

5. The electrode for an electrical storage device according to any one of claims 1 to 4, wherein: The content of the active material in the active material layer is 96 mass % or more.

6. The electrode for an electrical storage device according to any one of claims 1 to 5, wherein: The carbon coating layer has a thickness of 0.1 μm or more and 5.0 μm or less.