Manufacturing method of carbon fiber bipolar plate

Through the superposition and directional reinforcement fiber technology of nonwoven carbon reinforced film and thermoplastic resin film, the problems of large weight and short service life of bipolar plates in electrochemical devices are solved, and the thin and efficient bipolar plate manufacturing is achieved, which improves electricity Performance and overall density of chemical devices.

CN118891758APending Publication Date: 2024-11-01SAS HYCCO
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380026478.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Due to the large material weight, short service life and complex manufacturing process, the bipolar plates in existing electrochemical devices are difficult to make thin and efficient bipolar plates, which affects the performance and overall size of the electrochemical conversion device.

Method used

The nonwoven carbon reinforced film is superimposed with a thermoplastic resin film, and the fibers are oriented to reinforcing the fibers along the axis of the battery stack, forming bipolar plates through low pressure and appropriate temperatures, and using high porosity and directional fibers to improve conductivity and mechanical strength.

Benefits of technology

The manufacturing of bipolar plates with thin, high mechanical strength and good conductivity is achieved, which simplifies the production process, reduces manufacturing costs, and improves the performance and overall density of the electrochemical device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891758A_ABST
    Figure CN118891758A_ABST
Patent Text Reader

Abstract

A method for manufacturing a bipolar plate (B), comprising a step of superposing a first release film (4), at least one reinforcing film (2), at least one thermoplastic resin film (3), and a second release film (4) along a stack axis (A) to form a stack (1); a step of placing the cell stack (1) in a compression system (M) for a second predetermined time at a predetermined molding pressure and a predetermined molding temperature; the reinforcing membrane (2) is a non-woven carbon reinforcing membrane (2) comprising a plurality of reinforcing fibers (21), each reinforcing fiber (21) extending along an orientation axis (F), at least 10%-60% of the orientation axis (F) of the reinforcing fibers (21) being oriented along the stack axis (A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical devices, and in particular to a method for manufacturing a bipolar plate made of a composite material installed in an electrochemical device. Background Art

[0002] An electrochemical device is any device capable of carrying out an electrochemical reaction, such as a fuel cell or a proton exchange membrane electrolyzer, thereby producing electricity or hydrogen, respectively, through a redox reaction. The term "electrochemical device" also refers to redox flow batteries that produce electricity from potential energy stored in the cell.

[0003] As is known, an electrochemical device comprises a plurality of cells extending along the axis of the stack and two end plates placed at the ends of the stack. The end plates are connected by compression members that can compress the cells and ensure the sealing of the electrochemical device.

[0004] refer to Figure 1 , which shows an electrochemical device 100, each cell 110 known to include a membrane electrode assembly 120 and two bipolar plates 130 (also referred to as separators), the two bipolar plates 130 sandwiching the membrane electrode assembly 120 and achieving fluid distribution in the cell 110. In order to form an electrochemical reaction in the electrochemical device, each cell 110 is supplied with an oxidizing fluid and a reducing fluid, such as hydrogen and oxygen, which circulate on either side of the membrane and react with the aid of a catalyst. Each cell 110 is also supplied with a heat-conducting fluid to regulate the temperature of the electrochemical device. In practice, two adjacent bipolar plates 130A, 130B of two adjacent cells 110A, 110B are fixed together to form a number of internal channels 140, thereby achieving the flow of a heat-conducting fluid between the cells 110.

[0005] refer to Figure 2 and Figure 3 The bipolar plates 130 include a plurality of openings 131 for allowing the oxidation fluid and the reduction fluid to flow in and out, and an inlet and an outlet 132 for the heat transfer fluid. Each bipolar plate 130 also includes an active center portion 133, which contacts the membrane electrode assembly and undergoes a redox reaction on the membrane electrode assembly; and a peripheral portion 134, which fixes the two bipolar plates 130 together.

[0006] The active portion 133 includes a recessed portion 135 and a protruding portion 136 (eg, Figure 3 As shown, the figure shows the Figure 2 The cross-sectional view of the bipolar plate 130 taken along the plane A:A shown in FIG. 1 is to enable the fluid to flow between the inlets / outlets 131 and 132. The recessed portions 135 of the two bipolar plates 130 are fixed together so that the protruding portions 136 form an internal channel 140 (such as Figure 1shown).

[0007] In the prior art, it is known that bipolar plates are made of graphite or metal (e.g., stainless steel, Inconel, aluminum or titanium) and are covered with a protective coating to reduce the effects of corrosion caused by the electrochemical device. However, such bipolar plates have many disadvantages. Graphite bipolar plates are heavy and have a large overall size because the thickness is usually more than 2 mm. Metal bipolar plates are heavy and have a limited service life despite the use of a protective coating because the environment of the electrochemical device in which they are located is acidic and corrosive.

[0008] Therefore, bipolar plates are increasingly made of composite materials. For this purpose, a bipolar plate comprising a conductive element dispersed in a resin is known. The conductive element includes carbon black, ground carbon fiber, graphite, expanded graphite, carbon nanotubes or graphene. The resin is generally a thermoplastic or thermosetting polymer. When forming such a bipolar plate, a large amount of conductive elements is mixed into the resin in a viscous state (the conductive element content of the bipolar plate as a whole is generally higher than 85% to ensure higher conductivity). The bipolar plate is formed by injecting the resin loaded with the conductive element into a mold or by pressing it with a hot press.

[0009] However, the addition of a large amount of conductive elements significantly increases the viscosity of the thermosetting or thermoplastic resin, making the mixture more viscous. The above-mentioned manufacturing method makes it impossible to manufacture thin bipolar plates, which are often very thick, usually more than 2 mm, which increases the overall size and weight of the electrochemical device. This is disadvantageous for electrochemical devices that are integrated into aircraft or any other mobile devices. In addition, injection molding or hot compression molding will leave a residual resin surface layer, which may be caused by, for example, the use of demolding products, which will increase the contact resistance, which is disadvantageous for electrochemical conversion devices that must minimize contact resistance. In order to reduce the contact resistance, the bipolar plate needs to be subjected to chemical or mechanical post-treatment, such as wear.

[0010] A bipolar plate made of a composite material including reinforcing fibers (eg, carbon fibers) impregnated with a thermoplastic or thermosetting polymer resin is known in the prior art. The bipolar plate has the advantage of being thin (less than 1 mm thick), thereby reducing its overall size and weight.

[0011] However, in this bipolar plate, the thermoplastic resin forms a residual layer similar to an insulating layer on the surface, which affects the conductivity. Therefore, the reinforcing fibers on the surface of the bipolar plate need to be exposed. Treatments such as polishing or plasma radiation dissolution may damage the reinforcing fibers and affect the mechanical properties of the bipolar plate, which is a significant disadvantage. It is also known from patent WO2016182131A1 that the use of a sacrificial layer can expose the reinforcing fibers on the surface of the bipolar plate without damaging them. The bipolar plate is then manufactured using a hot pressing process, thereby producing a thin bipolar plate. However, in patent WO2016182131A1, the manufacturing method cannot simply and quickly produce bipolar plates reinforced with carbon fibers.

[0012] In addition, the use of reinforcing fibers requires very high molding pressures (usually exceeding 15 MPa) to allow the fibers to be properly impregnated, reduce porosity, and expose surface fibers for good electrical conductivity. Significant pressures can deform the initial weave of the reinforcing fibers and lead to the formation of porous cavities, which alters the airtightness of the bipolar plate. Summary of the invention

[0013] The object of the present invention is to at least partially alleviate the aforementioned drawbacks by proposing a method for manufacturing bipolar plates which is simple, fast and does not require the use of expensive industrial machinery, so as to form light and thin bipolar plates.

[0014] The present invention relates to a method for manufacturing a bipolar plate, wherein the bipolar plate is configured to be installed in an electrochemical device, wherein the electrochemical device is configured to realize an electrochemical reaction, the method comprising:

[0015] - a step of stacking a first release film, at least one reinforcement film, at least one thermoplastic resin film and a second release film along the battery stack axis Z to form a battery stack;

[0016] - a step of placing said battery stack in a compression system;

[0017] - a step of pressurizing the battery stack in the compression system, the pressurizing step being performed at a predetermined molding pressure and at a predetermined molding temperature for a second predetermined period of time to melt the thermoplastic resin in the thermoplastic resin film and impregnate the reinforcement film with the thermoplastic resin to form a bipolar plate.

[0018] The manufacturing method is notable in that the reinforcement membrane is a non-woven carbon reinforcement membrane comprising a plurality of reinforcement fibers, each reinforcement fiber extends along a directional axis, and the ratio of the reinforcement fibers extending along the cell stack axis Z is between 10% and 60%.

[0019] Advantageously, the molding pressure for nonwoven carbon reinforced membranes is lower than that for textile reinforced membranes, which allows the use of cheaper industrial machinery, resulting in a simpler and faster manufacturing method. The lower molding pressure makes it possible to limit the deformation of the initial weaving of the reinforcing fibers and the formation of porous cavities that could affect the airtightness of the bipolar plate.

[0020] Orienting the reinforcing fibers along the stack axis can increase the conductivity of the material along the axis to ensure optimal electrical transfer between the surfaces of the bipolar plates for the electrochemical device.

[0021] The ratio of reinforcing fibers extending along the stack axis between 10% and 60% enables the bipolar plate to have good electrical conductivity while ensuring that the bipolar plate has high mechanical resistance. The high ratio of reinforcing fibers extending along the stack axis Z enables the dual functions of mechanical properties and electrical conductivity.

[0022] Preferably, the reinforcing fibers are oriented by stitching. Some of the reinforcing fibers can be mechanically oriented along the battery stack axis Z by means of stitching, which improves the conductivity of the bipolar plate, so that when the bipolar plate is installed in an electrochemical device, better electrical exchange can be achieved between batteries adjacent to the bipolar plate.

[0023] Alternatively, the orientation of the reinforcing fibers may be performed by different methods, for example by means of hydroentanglement.

[0024] In a preferred embodiment, the ratio of reinforcing fibers extending along the stack axis Z is between 15% and 45% to achieve optimal conductivity in the bipolar plate. This ratio also means that the ratio of random reinforcing fibers is kept high enough to ensure optimal mechanical strength of the bipolar plate.

[0025] Preferably, since the nonwoven carbon reinforced membrane includes open pores, the open porosity of the nonwoven carbon reinforced membrane before the pressurizing step is greater than 60%. The term "open porosity" will be described in more detail later.

[0026] In one embodiment, the nonwoven carbon reinforced membrane has an open porosity between 60% and 70%. Studies have shown that certain materials such as carbon paper or gas diffusion layers can have this open porosity, which is particularly effective for making light, thin, and strong bipolar plates.

[0027] Preferably, the non-woven carbon reinforced membrane is a carbon felt. The carbon felt has a high open porosity in the reinforced membrane, preferably greater than 70%, to achieve optimal flow of the thermoplastic resin in the reinforced membrane, more specifically between the reinforcing fibers. In this way, the reinforcing fibers can be optimally impregnated with the thermoplastic resin, thereby obtaining a bipolar plate with a high degree of consolidation and fewer pores. "Open pores" refer to cavities or channels that are open to the outside of the reinforced membrane. The open pores are accessible from the outside and can be filled with a polymer resin to ensure the mechanical strength of the bipolar plate. Carbon felt can also use known materials, such as those traditionally used as thermal insulators or as a medium for diffusion of liquid electrolytes in the case of redox flow batteries.

[0028] Preferably, since the nonwoven carbon reinforced membrane has open pores, the open porosity of the nonwoven carbon reinforced membrane before the pressurization step is greater than 80%. This open porosity enables optimal deformation of the reinforced membrane, thereby obtaining a high compression rate and enabling the reinforced membrane to adapt to complex morphologies. Even more preferably, the open porosity of the nonwoven carbon reinforced membrane is greater than 90%. In the following, for simplicity, "open porosity" may be referred to as "porosity".

[0029] The high porosity in the reinforcement membrane, combined with an optimal ratio of reinforcement fibers oriented along the stack axis Z, has the advantage of providing the bipolar plate with optimal performance for use in an electrochemical system. Specifically, the high porosity, combined with a high ratio of reinforcement fibers oriented along the stack axis Z, provides both a high conductivity of the bipolar plate to enable it to optimally fulfill its role as a conductive element, and a high porosity of the reinforcement membrane to enable it to be well impregnated and significantly deformed at low pressures in order to correctly form the channels of the bipolar plate and obtain a composite material with negligible porosity relative to hydrogen to fulfill its role as a fluid separator.

[0030] Preferably, the diameter of the open pores is between 1 μm and 250 μm. Preferably, at least 50% of the open pores in the reinforced membrane have a diameter greater than 125 μm. Even more preferably, at least 50% of the open pores in the reinforced membrane have a diameter greater than 150 μm. The pores can be easily filled with polymer resin without affecting the mechanical strength of the bipolar plate. The size of the pores also means that the component is highly compressible, making it possible to manufacture thin bipolar plates. The term "diameter of an open pore" refers to the diameter of an equivalent circle, that is, the diameter of a circle whose surface area is equal to the surface area of ​​the pore. Similarly, more precisely described here, preferably, at least 50% of the surface area of ​​the open pores of the reinforced membrane is occupied by pores having an equivalent circular diameter greater than 125 μm.

[0031] Preferably, the equivalent circular diameter of the open pores is between 1 μm and 300 μm. In one embodiment, at least 50% of the surface area of ​​the open pores of the reinforced membrane is occupied by pores with an equivalent circular diameter greater than 30 μm. Even more preferably, at least 50% of the surface area of ​​the open pores of the reinforced membrane is occupied by pores with an equivalent circular diameter greater than 80 μm, preferably greater than 90 μm.

[0032] Preferably, the molding temperature is between 140°C and 400°C to achieve a variety of thermoplastic polymer series.

[0033] In one embodiment, the molding temperature is between 240° C. and 360° C. to form a polyphenylene sulfide (PPS) or polyphenylene sulfone (PPSU) type polymer.

[0034] In one embodiment, the molding temperature is between 200° C. and 260° C. to form polyvinylidene fluoride (PVDF) or polyamide type polymer.

[0035] In one embodiment, the molding temperature is between 140° C. and 200° C. to form a polyolefin type polymer.

[0036] In one embodiment, the molding temperature is between 350° C. and 400° C. to form a polymer of the polyaryletherketone type (PEEK, PEK, PEKK, etc.).

[0037] Preferably, the preset molding pressure is between 6 MPa and 12 MPa. Due to the use of non-woven carbon, the molding pressure is sufficient to optimally impregnate the reinforcing fibers in the reinforced membrane and benefit from a bipolar plate with a high degree of consolidation, and thus benefit from the bipolar plate's significant airtightness to hydrogen in an electrochemical device.

[0038] Preferably, the preset molding pressure is between 8 MPa and 10 MPa. Due to the present invention, it is not necessary to increase the molding pressure to an excessively high pressure. This eliminates the need for particularly expensive industrial machinery. The manufacturing method is not only faster and simpler to implement, but also allows a high manufacturing rate. The molding pressure also limits the deformation of the reinforcing fibers in the initial reinforcement membrane, thereby avoiding the creation of porous cavities in the bipolar plate, thereby ensuring the effectiveness of the bipolar plate by reducing the risk of failure.

[0039] Preferably, the thickness of the reinforcement film is less than 5 mm. The thickness of the reinforcement film is sufficient to produce a bipolar plate with high mechanical resistance, while being flexible enough to enable the reinforcement film to adapt to complex geometries. Preferably, the initial thickness of the reinforcement film (i.e., the thickness before the battery stack is compressed to form the bipolar plate) is between 0.5 mm and 3.4 mm, so as to form a bipolar plate with a thickness of less than 0.5 mm after the battery stack is compressed.

[0040] Preferably, the mass per unit area of ​​the reinforced film is 500 g / m 2 or lower, thereby forming a lightweight bipolar plate. Preferably, the mass per unit area is between 50 g / m 2 -400 g / m 2 Even more preferably, the mass per unit area is between 50 g / m 2 -300 g / m 2 Thus, the shaped bipolar plate can be integrated into an electrochemical device, such as an aircraft or other vehicle where mass constraints are important.

[0041] In one embodiment, the manufacturing method includes the step of cooling the formed bipolar plate for a third predetermined period of time after the pressurizing step.

[0042] In a first embodiment, the cooling step is carried out at a cooling rate between 10°C / min-100°C / min. Such a high cooling rate causes the crystalline portion of the semi-crystalline polymer to crystallize so that the manufactured bipolar plate has good airtightness to the fluid used for energy conversion in the electrochemical device. At this cooling rate, a crystallization rate of 43%-47% can be achieved, which corresponds to the maximum crystallization rate that can be achieved by the thermoplastic resin used, which is usually between 40%-55%. Studies have shown that other types of thermoplastic resins, such as polyaryletherketones, can achieve a maximum crystallization rate between 20%-40%. Similarly, different types of thermoplastic resins (such as polyolefins) can achieve a maximum crystallization rate between 55%-80%.

[0043] Alternatively, for polymers known as "amorphous" polymers, ie, polymers containing no crystalline portions, the cooling step is performed at a cooling rate greater than 80°C / min in order to rapidly cool the bipolar plate, allowing for a faster production rate.

[0044] Preferably, the cooling rate is between 40°C / min and 90°C / min, which can achieve optimal crystallization of the crystallized portion of the battery stack, while minimizing the cooling time of the bipolar plate to shorten the manufacturing cycle, and obtaining a fast manufacturing method with a high production rate.

[0045] The present invention also relates to a bipolar plate configured to be installed in an electrochemical device, the bipolar plate being manufactured by means of the manufacturing method as described above.

[0046] According to one aspect, the bipolar plate includes a nonwoven carbon reinforced film including a plurality of reinforcing fibers, each reinforcing fiber extending along a directional axis, and a ratio of the reinforcing fibers extending along the stack axis Z is between 10% and 60%.

[0047] Preferably, the thickness of the bipolar plate is less than or equal to 0.5 mm, which advantageously enables to reduce the mass and overall size of the electrochemical device and increase its power density (kW / kg). Therefore, the electrochemical device can be easily installed on a vehicle such as an aircraft.

[0048] Even more preferably, the bipolar plate has a thickness of less than 0.4 mm.

[0049] Preferably, the surface specific resistance of the bipolar plate is less than 12 mΩ.cm 2 .

[0050] Preferably, the porosity of the bipolar plate is less than 1%, thereby ensuring optimal permeability of the bipolar plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The invention will be better understood on reading the following description, given by way of example, and with reference to the following drawings, given by way of non-limiting example, in which like references refer to similar objects.

[0052] Figure 1 It is a schematic diagram of a cell stack of a membrane electrode assembly and bipolar plates in an electrochemical device.

[0053] Figure 2 yes Figure 1 Schematic diagram of the bipolar plate in FIG.

[0054] Figure 3 yes Figure 2 Schematic diagram of the cross section of the bipolar plate.

[0055] Figure 4 Schematic diagram of a battery stack of a nonwoven carbon reinforcement film, a thermoplastic resin film and two release films for manufacturing a bipolar plate of the present invention.

[0056] Figure 5 yes Figure 4 Close-up of the nonwoven reinforcement membrane.

[0057] Figure 6 FIG. 1 is a schematic diagram of a first step of a manufacturing method according to an embodiment of the present invention.

[0058] Figure 7FIG. 1 is a schematic diagram of the second step of the manufacturing method according to an embodiment of the present invention.

[0059] Figure 8 is a schematic diagram of the third step of the manufacturing method according to an embodiment of the present invention.

[0060] Fig. 9 is a schematic diagram of the fourth step of the manufacturing method according to an embodiment of the present invention.

[0061] Fig.10 is a schematic diagram of the fifth step of the manufacturing method according to an embodiment of the present invention.

[0062] Fig.11 A graph showing changes in temperature and pressure during the manufacturing method of the present invention.

[0063] Fig.12 is a schematic diagram of the sixth step of the manufacturing method according to an embodiment of the present invention.

[0064] Fig.13 Schematic diagram of a bipolar plate manufactured using the manufacturing method of the present invention.

[0065] Fig.14 is a schematic diagram of the image obtained by tomographic characterization of the enhanced film.

[0066] Fig.15 yes Fig.14 Schematic diagram of the skeletonization of the reinforcing fibers of the reinforced membrane shown.

[0067] It should be noted that the drawings illustrate the invention in detail in order to implement the invention and, if necessary, said drawings can of course be used to better define the invention. DETAILED DESCRIPTION

[0068] The present invention relates to a method for producing a bipolar plate made of a composite material for an electrochemical device.

[0069] Hereinafter, as described above, the term "electrochemical device" refers equally to a fuel cell, a proton exchange membrane electrolyzer, a redox flow battery, or any other device capable of effecting an electrochemical reaction.

[0070] As mentioned above, the electrochemical device includes a battery stack composed of a plurality of cells, each of which includes a membrane electrode assembly and two bipolar plates, also known as separators, which sandwich the membrane electrode assembly and realize the fluid distribution in the cell. In order to form an electrochemical reaction in the electrochemical device, each cell is known to be supplied with an oxidizing fluid and a reducing fluid, such as hydrogen and oxygen, which react when contacted in the redox reaction. Each cell is also supplied with a heat transfer fluid for regulating the temperature of the electrochemical device. In order to allow the fluid to pass through, the bipolar plate includes a recessed portion and a protruding portion to form a circulation channel.

[0071] refer to Figure 4 According to the bipolar plate B (such as Fig.13 ) is composed of at least one non-woven carbon reinforced film 2 and at least one thermoplastic resin film 3. In this example, the bipolar plate B is composed of a non-woven carbon reinforced film 2 and a thermoplastic resin film 3. This embodiment introduces an example of a single non-woven carbon reinforced film 2 and a single thermoplastic resin film 3, but it goes without saying that the number of films may be different. Specifically, it goes without saying that the bipolar plate B may be composed of several non-woven carbon reinforced films 2 and / or several thermoplastic resin films 3. For simplicity, the non-woven carbon reinforced film will be referred to as the reinforced film 2 below.

[0072] refer to Figure 5 The reinforcement membrane 2 preferably extends in the plane (X, Y) and has two substantially flat and parallel outer surfaces 2A and 2B, namely the lower surface 2A and the upper surface 2B. The reinforcement membrane 2 also includes a plurality of reinforcement fibers 21. Preferably, the reinforcement fibers 21 are composed of carbon fibers. The thickness Ep2 of the reinforcement membrane 2 is defined along a vertical axis Z orthogonal to the plane (X, Y).

[0073] Each reinforcing fiber 21 includes a first end 21a and a second end 21b. At least a portion of the reinforcing fibers 21 in the reinforcing membrane 2 extends from the first end 21a to the second end 21b approximately along the orientation axis F. In this example, the orientation axis F extends from the lower surface 2A to the upper surface 2B. In other words, the first end 21a of the reinforcing fiber 21 is approximately located on the lower surface 2A, and the second end 21b is approximately located on the upper surface 2B, and each reinforcing fiber 21 extends to penetrate the thickness Ep2 of the reinforcing membrane 2. Still referring to Figure 5 , the orientation axis F is formed by forming an angle Thetaθ with the vertical axis Z and an angle Phi with the axis X on the projection plane (X, Y) Preferably, the orientation axis F extends such that the angle Thetaθ is less than 45° or greater than 135°, and the angle Phi For the sake of clarity, when the reinforcing fiber 21 meets the above conditions, it is considered that the reinforcing fiber 21 extends along the axis Z of the battery stack.

[0074] More specifically, the orientation axis F extends such that the angle Thetaθ is between 0°-45° or between 135°-180°, and the angle Phi Between 45°-135°.

[0075] Preferably, if Figure 5As shown, 10%-60% of the reinforcing fibers 21 in the reinforced membrane 2 extend between the lower surface 2A and the upper surface 2B of the reinforced membrane 2 along the battery stack axis Z. This orientation of the reinforcing fibers 21 can improve the electrical conductivity, so that once manufactured, significant mechanical properties are maintained in the bipolar plate B. As will be described in more detail later, the high conductivity of the thickness of the reinforced membrane 2, i.e., along the stacking axis Z, is advantageous because it ensures good conductivity of the thickness of the bipolar plate B. In one embodiment, the reinforcing fibers 21 are oriented along the battery stack axis Z by methods such as needling, stitching or sewing. These methods are known to those skilled in the art and will not be described in detail herein. Alternatively, the orientation of the reinforcing fibers 21 can be performed by different methods, such as by hydraulic entanglement.

[0076] For example, the orientation of the reinforcing fibers 21 in the reinforcing membrane 2 can be determined by analyzing images obtained by X-ray tomography. This method enables a three-dimensional 3D image of the reinforcing membrane 2 to be obtained and each reinforcing fiber 21 to be analyzed independently in order to define their orientation in the reinforcing membrane 2.

[0077] More specifically, in this example, the reinforcing fibers 21 are defined by a grayscale threshold to distinguish the reinforcing fibers 21 from the pores. This involves filtering the 3D image within a contrast range that highlights the reinforcing fibers 21. Image processing of the "morphological operator" class is used to identify the three-dimensional structure of the reinforcing fibers 21 in the image. Preferably, an image processing method of the "skeletonization" type, which is called "morphological skeleton" or "skeletonization" in English, is selected. This method is known to those skilled in the art and will not be described in detail herein.

[0078] In one example, to determine the orientation of the reinforcing fibers 21 in the reinforced membrane 2, RX Solutions TM The enhanced film 2 was analyzed using a micro-tomography scanner of a brand (e.g., EasyTom 230 model). The analysis was performed under the conditions of an accelerating voltage of 60 kV, a current of 80 μA, and a tungsten target. The exposure time was 0.4 s, an average of 10 s, and 1120 X-ray projections. The X-Act software (RX Solutions TM ) and used the “Avizo for Industrial Inspection” software (ThermoFisher Scientific TM ) for three-dimensional reconstruction.

[0079] Specifically, the following steps are performed:

[0080] -Import the X-ray tomography characterization image of the enhanced film 2 to Thermo Scientific TM In the software "AvizoSoftware", the schematic diagram is as follows Fig.14 As shown,

[0081] - thresholding within the contrast range to highlight the reinforcing fibers 21,

[0082] - Using the "Auto Skeleton" module in the software, the three-dimensional fiber filament structure of each reinforcing fiber 21 is identified, for example Fig.15 shown.

[0083] The properties of each reinforcement fiber 21 of the reinforcement membrane 2, such as its orientation, can then be studied. Fig.15 In the figure, reinforcing fibers 21 having similar orientations are represented by the same solid line or dotted line.

[0084] As mentioned above, the orientation axis F of each reinforcing fiber 21 is the angle Thetaθ formed by the orientation axis F and the vertical axis Z and the angle Phi formed by the orientation axis F and the central axis X of the reference system (X, Y, Z) In this reference frame, the angle Thetaθ and the angle Phi It varies between 0° and 180°. More precisely, in the reference frame (X, Y, Z), the space is defined by three different cones at 45° angles, whose vertices are the origin of the reference frame and are centered on the X, Y, and Z axes, respectively. Therefore, the three cones can be represented by the following pair of Thetaθ and Phi Angle definition:

[0085] - A cone oriented towards the Z axis: And 0°<θ<45° or 135°<θ<180°

[0086] - A cone oriented towards the Y axis: And 45°<θ<135°

[0087] - A cone oriented towards the X axis: or And 0<θ<180°

[0088] The reinforcing fiber 21 is The orientation of the angle between these three cones is classified, while the reinforcing fibers 21 belonging to two cones are not classified (fibers at the junction of the two cones). The ratio of the reinforcing fibers 21 oriented along each axis X, Y and Z of the reinforced membrane 2 can then be calculated.

[0089] In a preferred embodiment, the reinforced membrane 2 is a carbon felt, also known as a "carbon mat". Carbon felt enables the use of materials with high open porosity, thereby enabling efficient exchange between the liquid electrolyte and the bipolar plate of the electrochemical device. The term "open pores" refers to open cavities, i.e., not blocked by the arrangement of carbon reinforcing fibers 21 and / or the sizing agent thereon. Preferably, the open porosity in the reinforced membrane 2 is greater than 70%. Even more preferably, the porosity is greater than 80% to allow the thermoplastic resin to flow optimally in the reinforced membrane 2, thereby achieving good impregnation of the reinforcing fibers 21. Due to the high open porosity of the reinforced membrane 2, a bipolar plate B with a high degree of consolidation (the percentage of remaining pores is typically less than 1%) can be obtained after the above-mentioned manufacturing method. Carbon felt also has the advantage of being easy to deform, allowing the reinforced membrane 2 to adapt to complex morphologies. Another advantage of carbon felt is that the molding pressure required (typically between 6MPa-10 MPa) is lower than the molding pressure required for the textile reinforced membrane (typically more than 15MPa). Even more preferably, the nonwoven carbon reinforced membrane 2 has an open porosity greater than 90%, enabling the manufacture of a bipolar plate B having optimal mechanical properties.

[0090] Preferably, the open porosity of the reinforced membrane 2 is greater than 60%. In one embodiment, the reinforced membrane 2 has an open porosity between 60% and 70%. In fact, certain materials with this open porosity (such as carbon paper or gas diffusion layer) can produce thin, lightweight and durable bipolar plates.

[0091] In a preferred embodiment, the reinforced membrane 2 includes pores with a diameter between 1 μm and -250 μm, so that the reinforcing fibers 21 can be effectively impregnated and the bipolar plate B produced has a high degree of consolidation. Preferably, at least 50% of the pores have a diameter greater than 125 μm, and even more preferably greater than 150 μm. "The diameter of the pore" refers to the diameter of the equivalent circle of the pore, that is, the diameter of a circle with a surface area equal to the surface area of ​​the pore. In one embodiment, the reinforced membrane 2 has pores with an equivalent circular diameter between 1 μm and 300 μm.

[0092] In one embodiment, at least 50% of the surface area of ​​the open pores of the reinforced membrane 2 is occupied by pores having an equivalent circular diameter greater than 30 μm, preferably greater than 80 μm, even more preferably greater than 90 μm.

[0093] For example, to characterize the pores in the reinforced membrane 2, one method is to use images obtained by X-ray tomography and analyze these images in three dimensions or two dimensions. For example, two-dimensional cuts can be made in the desired direction. As described above, the reinforcing fibers 21 are defined by grayscale thresholds to distinguish them from the pores. The image is then filtered using a range of contrasts to highlight the reinforcing fibers 21. A "morphological operator" type of image processing (e.g., "morphological gradient") is then used to identify the two-dimensional structure of the pores in the image.

[0094] In fact, in one example, a 2D image is obtained by taking slices of a 3D image acquired from an X-ray tomography scan. In this example, this 2D image is imported into ImageJ TM The image is then thresholded in a grayscale range between 120-255 (in a mode known as "blackfield"). A morphological gradient operator in the software ("watershed" in this example) can then be used to highlight the two-dimensional structure of the pores.

[0095] Once the pores are identified, the area of ​​each pore is measured and the equivalent circular diameter is calculated from the measured area. The pores are then characterized and classified based on their equivalent circular diameter. For example, pores can be classified based on whether their equivalent circular diameter is smaller or larger than a certain percentage of the diameter threshold of all pores.

[0096] Preferably, the reinforcement membrane 2 is highly compressible in order to adapt to the complex geometry of the bipolar plate fluid circulation channels. It is also possible to form a bipolar plate B with a thickness of less than 1 mm. Preferably, as will be described in more detail below, the thickness of the formed bipolar plate B is less than 0.5 mm.

[0097] Still refer to Figure 5 , along the axis Z, the thickness of the reinforcement film 2 is Ep2, preferably less than or equal to 5 mm. Preferably, the thickness Ep2 is between 0.5 mm and 2.5 mm. This thickness Ep2 can advantageously reduce the overall size of the bipolar plate B after manufacture.

[0098] In a preferred embodiment, the mass per unit area of ​​the reinforcement film 2 is less than or equal to 500 g / m 2 Preferably, the mass per unit area is between 50 g / m 2 -300 g / m 2 This enables the use of a reinforced membrane 2 of limited mass, thereby reducing the mass of the bipolar plate B using the reinforced membrane 2. The bipolar plate B has a limited mass, thereby enabling it to be integrated into an electrochemical device installed in an aircraft or any other vehicle.

[0099] Thermoplastic resin film 3 (such as Figure 4) includes a polymer designated as a thermoplastic resin 31 to form a thermoplastic matrix of the bipolar plate B after manufacturing. For the sake of simplicity, the thermoplastic resin film 3 is simply referred to as a thermoplastic film 3 below.

[0100] Preferably, reference Figure 4 The thickness Ep3 of the thermoplastic film 3 is between 50 μm and 600 μm, which ensures a sufficient amount of the thermoplastic resin 31 to form the thermoplastic matrix of the bipolar plate B while reducing the volume and mass of the bipolar plate B.

[0101] In one embodiment, the thermoplastic resin of the thermoplastic film 3 is of a semi-crystalline type, which makes the bipolar plate B highly fluid-tight, especially hydrogen-tight. Semi-crystalline thermoplastic resins also have significant mechanical and chemical resistance, especially corrosion resistance. In one embodiment, the thermoplastic resin of the thermoplastic film 3 is of an amorphous type, which allows greater ductility and lower dimensional shrinkage during the cooling step.

[0102] The thermoplastic resin is able to adapt to the chemical environment of the electrochemical device in which the bipolar plate B is installed. In this regard, in order to install the bipolar plate B in a low-temperature proton exchange membrane (abbreviated as "PEM"), the thermoplastic resin preferably belongs to polyphenylene sulfide (abbreviated as "PPS"), polyphenylene sulfone (abbreviated as "PPSU"), polyvinylidene fluoride (abbreviated as "PVDF"), ethylene monochlorotrifluoroethylene (abbreviated as "ECTFE"), or polyolefin, polyaryletherketone, or polyamide.

[0103] In order to install the bipolar plate B in a high-temperature proton exchange membrane, the thermoplastic resin is preferably of the type of polyphenylene sulfide (PPS), polyphenylene sulfone (PPSU), ethylene chlorotrifluoroethylene (ECTFE) or polyaryletherketone.

[0104] In order to install the bipolar plate B in a redox flow battery with a vanadium or hydrogen bromide electrolyte or any liquid electrolyte (e.g., organic), if the electrolyte is alkaline, the thermoplastic resin is preferably of the polyphenylene sulfide (PPS) and polyphenylene sulfone (PPSU) type, and if the electrolyte is acidic, the thermoplastic resin is preferably of the polyvinylidene fluoride (PVDF) or ethylene chlorotrifluoroethylene (ECTFE) type, or of the polyaryletherketone class.

[0105] A method for manufacturing a bipolar plate B according to one embodiment of the present invention will now be described.

[0106] refer to Figure 4, the bipolar plate B in this embodiment is made of a battery stack 1 of a reinforcement film 2, a thermoplastic resin film 3 and two release films 4. As will be described in more detail below, the battery stack 1 extends along the battery stack axis A. The use of the release film 4 exposes the reinforcement fibers 21 on the surface of the formed bipolar plate B and makes the reinforcement fibers conductive. Preferably, the reinforcement film 2, the thermoplastic film 3 and the release film 4 are in a roll form for easy storage and handling.

[0107] like Figure 6 As shown, the method includes a first step E1: cutting the reinforcement film 2, the thermoplastic resin film 3 and the two release films 4 ( Figure 6 Only the reinforcement film 2 is shown in the figure). For example, the cutting is performed manually on a cutting table and allows each film to be cut into the size required for the final bipolar plate B. The reinforcement film 2 and the thermoplastic film 3 preferably have similar sizes. Even more preferably, the size of each release film 4 is larger than that of the reinforcement film 2 and the thermoplastic film 3 so that it protrudes from the battery stack 1 so that it can be removed more easily after the bipolar plate B is formed. Of course, the cutting can also be performed in different ways, such as using a punch or a robotic arm.

[0108] Then, refer to Figure 7 , the method includes a second step E2: superimposing a first release film 4, a reinforcement film 2, a thermoplastic film 3, and a second release film 4 along the battery stack axis A to form a battery stack 1. This arrangement enables the orientation axis F of the reinforcement fibers 21 of the reinforcement film 2 to be oriented along the battery stack axis A, thereby orienting the reinforcement fibers 21 so that their ends 21a, 21b are exposed on two opposite surfaces of the manufactured bipolar plate B. Therefore, the reinforcement fibers 21 can optimally conduct electricity into the bipolar plate B and thus into the electrochemical device to which the bipolar plate is mounted. In this embodiment, the battery stack 1 can be formed by placing the first release film 4, the reinforcement film 2, the thermoplastic film 3, the second release film 4 in sequence or by placing the first release film 4, the thermoplastic film 3, the reinforcement film 2, and the second release film 4 in sequence.

[0109] Alternatively, in the case where the battery stack 1 includes two thermoplastic resin films 3, in this step, the operator can also easily stack the first release film 4, the first thermoplastic film 3, the reinforcement film 2, the second thermoplastic film 3, and the second release film 4 in sequence. The use of two thermoplastic films 3 located on both sides of the reinforcement film 2 can minimize the movement of the thermoplastic resin through the reinforcement film 2 and facilitate the impregnation of the reinforcement film 2.

[0110] The first release film 4 , the reinforcement film 2 , the thermoplastic film 3 and the second release film 4 can be stacked manually or with the aid of a robot.

[0111] In one embodiment, the battery stack 1 is fixed to prevent the risk of one of the membranes being displaced relative to the other membranes. This fixing can be achieved, for example, by adding welding points (such as ultrasound or local heating) or by sewing all the membranes together. Fixing in this way makes it easier to transport the entire battery stack 1, such as using a robotic arm with a clamping device.

[0112] refer to Figure 8 , then the method includes step E3: placing the battery stack 1 in a compression system, in this example, in a mold M. In this example, the mold M includes a lower member and an upper member, each of which includes an inner surface having a recess G. The recess G is used to form a fluid flow channel in the bipolar plate B. In one embodiment, before the battery stack 1 is placed in the mold M, a release agent is applied to the mold M, such as a liquid that can be sprayed on the inner surface of each lower member and upper member, to facilitate subsequent demolding. Preferably, the mold M is at an initial temperature Ti. Preferably, the initial temperature Ti is between 20°C and 210°C.

[0113] When the mold M is closed to clamp the battery stack 1, the temperature gradually increases from the initial temperature Ti to the predetermined molding temperature Tm. Preferably, the molding temperature Tm is between 140°C and 400°C. For example, for PPS type thermoplastics, the molding temperature Tm is preferably between 305°C and 340°C. For PVDF type thermoplastics, the molding temperature Tm is between 200°C and 260°C, preferably between 210°C and 240°C. For PPSU type thermoplastics, the molding temperature Tm is between 240°C and 360°C, preferably between 290°C and 330°C. The temperature is raised from the initial temperature Ti to the predetermined molding temperature Tm for a first predetermined time Δt1 (such as Fig.11 Preferably, the first time Δt1 is less than 10 min, preferably less than or equal to 3 min, so as to quickly heat the mold M, thereby saving production time and achieving a higher output rate.

[0114] refer to Fig. 9 The method further comprises step E4: pressurizing the battery stack 1 in the compression mold M. The pressurizing step E4 is performed at the molding temperature Tm and the predetermined molding pressure Pm for a second predetermined time Δt2 (eg Fig.11 The pressurizing step E4 melts the thermoplastic resin in the thermoplastic film 3, thereby impregnating the reinforcement film 2 and forming the bipolar plate B.

[0115] Preferably, the molding pressure Pm is between 6MPa and 12MPa. Even more preferably, the molding pressure Pm is between 8MPa and 10MPa, which can prevent the deformation of the reinforcing fibers 21 in the initial reinforced membrane 2 from causing porous cavities in the bipolar plate B, and can easily achieve pressurization. Preferably, the second time Δt2 is less than 2min, preferably less than 1min, so as to ensure that the reinforcing fibers 21 are impregnated with the thermoplastic resin 31 while reducing the appearance of pores in the bipolar plate B.

[0116] The method then comprises a step E5: Fig.10 As shown, the molded bipolar plate B is cooled for a third predetermined time Δt3 (eg Fig.11 ) to consolidate the bipolar plate. The temperature drops from the molding temperature Tm to the demolding temperature Tr, at which time the pressurization is stopped. Preferably, the demolding temperature Tr is equal to the initial temperature Ti. In the case of a semi-crystalline polymer, the third predetermined time Δt3 is set to obtain a cooling rate between 10°C / min-100°C / min to achieve sufficiently slow cooling to allow the crystalline portion of the thermoplastic resin to crystallize, thereby ensuring that the manufactured bipolar plate has low permeability to hydrogen or any other fluid used in the energy conversion system, while minimizing the cooling time to shorten the manufacturing cycle. At this cooling rate, a crystallinity of between 43% and 47% can be obtained. Even more preferably, the cooling rate is between 40°C / min-90°C / min, which ensures optimal crystallization of the thermoplastic resin during the consolidation stage. In the case of an amorphous polymer, the cooling rate is preferably greater than 80°C / min so as to quickly cool the bipolar plate B and the mold M and increase the production rate.

[0117] The molding cycle (i.e., temperature rise, molding step, and cooling step) is as follows Fig.11 As shown, the figure shows the variation of temperature T and pressure P with time t during a complete molding cycle, as described above.

[0118] When the demoulding temperature Tr is reached, the mold M is opened and the formed bipolar composite plate B is taken out.

[0119] like Fig.12 As shown, in step E6, the release films 4 on both sides of the manufactured bipolar plate B are removed to expose the reinforcing fibers 21 on the surface of the bipolar plate B. The removal of the release film 4 can be performed manually or automatically, such as rolling up the release film 4 when it leaves the mold.

[0120] In one implementation, the method includes a step of cutting the bipolar plate B to remove the peripheral portion of the bipolar plate such as a manufacturing defect. For example, this is done by water jet cutting, milling, or using a punch. Preferably, centering is taken into account to ensure accurate cutting of the bipolar plate (cutting error is less than or equal to 0.1 mm).

[0121] Fig.13 A bipolar plate B formed by the above manufacturing method is shown. The bipolar plate B extends on the plane (X, Y). Advantageously, the method can form a bipolar plate B having a thickness Ep (along the axis Z, orthogonal to the plane (X, Y)) less than 1 mm. Preferably, the thickness Ep of the formed bipolar plate B is less than 0.5 mm.

[0122] Preferably, the quantitative ratio of the reinforcing fiber 21 to the thermoplastic resin 31 in the final bipolar plate B enables the electrical, thermal and mechanical properties of the bipolar plate B to meet the requirements of electrochemical device applications. Therefore, the volume ratio of the reinforcing fiber 21 of the final bipolar plate B is preferably between 20%-60%, and the volume ratio of its thermoplastic matrix 31 is between 40%-80%. Preferably, the volume ratio of the reinforcing fiber 21 is between 30%-50%, and the volume ratio of the thermoplastic matrix 31 is between 50%-70%. Compared with the production process of the prior art, the extremely thin bipolar plates produced in this way can compensate for the lower proportion of conductive elements while ensuring the best conductivity, while in the prior art, the proportion of conductive elements is greater than 80%. The mass of the manufactured bipolar plate is also reduced, thereby limiting the mass of the electrochemical device on which the bipolar plate is installed.

[0123] For example, the volume ratio of the reinforcing fibers 21 in the manufactured bipolar plate B can be determined after the thermoplastic matrix 31 is separated. The separation can be achieved by, for example, acid dissolution or calcination of the thermoplastic matrix 31. The mass of the conductive reinforcing fibers 21 is then measured by weighing and related to the initial mass of the material. The density of the material is used to convert the volume ratio.

[0124] The method according to the present invention describes suitable types of carbon reinforcement materials and their associated manufacturing cycles in order to provide a method for manufacturing bipolar plates that is simple, fast, and does not require the use of expensive industrial machinery while forming thin and light bipolar plates.

[0125] Preferably, the thickness of the bipolar plate is less than or equal to 0.4 mm, which advantageously makes it possible to limit the mass and overall size of the electrochemical device and increase its power density (kW / kg) without subsequent treatment of the material surface in order to increase its conductivity. Therefore, the electrochemical device can be easily installed on a vehicle such as an aircraft.

[0126] In a preferred manufacturing example, the present invention can manufacture a surface specific resistance (surface specific resistance, abbreviated as ASR) less than 12mΩ.cm 2 The flexible bipolar plate B has a porosity of less than 1%. Advantageously, these characteristics ensure that the surface permeability of the bipolar plate B is less than 5x10A-8mol / m / s / MPa, while having high hydrophobicity and a contact angle greater than 110°.

[0127] The porosity of the manufactured bipolar plate B may be measured by various means known to those skilled in the art.

[0128] For example, the actual density of the bipolar plate B can be measured using the Archimedean thrust method or the pycnometer analysis method and compared with the theoretical density. Both methods can accurately determine the exact volume of the sample and infer its density based on its mass.

[0129] In a second example, a different image analysis method may be used to distinguish pores in the bipolar plate B. In this case, the volume of the pores may be identified on a three-dimensional image (or the surface of the pores on a two-dimensional image) in a manner similar to that described above for the reinforced membrane 2 .

[0130] In a third example, the porosity of the final bipolar plate B may also be determined using wave absorption methods such as X-ray tomography or ultrasound.

[0131] These methods usually measure the exact composition of the target sample. To this end, the reinforcing fibers 21 are separated and weighed independently of the thermoplastic matrix 31. The separation can be achieved by dissolution or thermal degradation (calcination or combustion) or chemical degradation (acid dissolution) of the matrix. Knowing the mass and density of the initial element of the bipolar plate B, the corresponding volume can be inferred. This volume is compared with the exact volume of the sample, and the remaining volume corresponds to the volume of the pores.

[0132] Pore ​​volume ratio Tv p Calculated according to the following formula, where m t corresponds to the mass of the reinforcing fiber 21 obtained after the thermoplastic matrix 31 is dissolved by acid, ρ f corresponds to the density of the reinforcing fiber 21, and, r Corresponding to the density of the thermoplastic matrix 31:

[0133]

Claims

1. A method for manufacturing a bipolar plate (B), wherein the bipolar plate (B) is configured to be installed in an electrochemical device, wherein the electrochemical device is configured to realize an electrochemical reaction, the method comprising: - Step (E2): stacking a first release film (4), at least one reinforcement film (2), at least one thermoplastic resin film (3) and a second release film (4) along the battery stack axis Z to form a battery stack (1); - Step (E3): placing the battery stack (1) in a compression system (M); - step (E4): pressurizing the battery stack (1) in the compression system (M), the pressurizing step (E4) being continued for a second predetermined time (Δt2) at a predetermined molding pressure (Pm) and a predetermined molding temperature (Tm) to melt the thermoplastic resin (31) of the thermoplastic resin film (3) and impregnate the reinforcement film (2) with the thermoplastic resin (31) to form a bipolar plate (B); -characterized in that the reinforced membrane (2) is a non-woven carbon reinforced membrane (2) comprising a plurality of reinforcing fibers (21), each reinforcing fiber (21) extending along a directional axis (F), and the ratio of the reinforcing fibers (21) extending along the battery stack axis Z is between 10% and 60%.

2. The manufacturing method according to claim 1, characterized in that The ratio of the reinforcing fibers extending along the stack axis Z is between 15% and 45%.

3. The manufacturing method according to claim 1 or 2, characterized in that: The non-woven carbon reinforcement membrane (2) is carbon felt.

4. The manufacturing method according to any one of claims 1 to 3, characterized in that: The nonwoven carbon reinforced membrane (2) comprises open pores, and the open porosity of the nonwoven carbon reinforced membrane (2) is greater than 60% before the pressurizing step (E4).

5. The manufacturing method according to claim 4, characterized in that: The diameter of the open pores is between 1 μm and 300 μm.

6. The manufacturing method according to any one of claims 1 to 5, characterized in that: The molding temperature (Tm) is between 140°C and 400°C.

7. The manufacturing method according to any one of claims 1 to 6, characterized in that: The predetermined molding pressure (Pm) is between 6 MPa and 12 MPa.

8. The manufacturing method according to any one of claims 1 to 7, characterized in that: After the pressurizing step (E4), the method further comprises a step (E5): cooling the formed bipolar plate (B), wherein the cooling lasts for a third predetermined period of time (Δt3).

9. The manufacturing method according to claim 8, characterized in that: The cooling rate is between 40℃ / min-90℃ / min.

10. A bipolar plate (B) configured to be installed in an electrochemical device, characterized in that The bipolar plate (B) is manufactured by the manufacturing method according to any one of claims 1 to 9.

11. The bipolar plate (B) according to claim 10, characterized in that: Its thickness (Ep) is less than or equal to 0.5 mm.

12. The bipolar plate (B) according to claim 10 or 11, characterized in that: Its surface resistivity is less than 12mΩ.cm 2 .

13. The bipolar plate (B) according to any one of claims 10 to 12, characterized in that: Its porosity is less than 1%.

Citation Information

Patent Citations

  • Composite material separation plate for fuel cell and method for manufacturing same

    WO2016182131A1