Method and device for synthesizing perovskite quantum dots based on supercritical CO2
Through the supercritical CO2 fluid-improved anti-solvent method, the problem of difficult control of perovskite quantum dot particle size is solved, narrow particle size and efficient luminescence are achieved, and the stability and optical performance of perovskite quantum dots are improved. It is suitable for high-quality Fine display technology.
Patent Information
- Application Number
- CN202410973942.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-05
AI Technical Summary
Existing perovskite quantum dot synthesis methods are difficult to stabilize the control of particle size, resulting in a wide particle size distribution, affecting the optical performance and application potential of the material, especially in large-scale preparation and blue-light quantum dot synthesis.
The perovskite quantum dot synthesis method based on supercritical CO2 is adopted. The anti-solvent method of supercritical CO2 fluid is improved to control the narrow particle size distribution and allow free selection of small molecules to modify the surface of the quantum dot to improve stability and luminous efficiency.
It realizes stable synthesis of small-sized perovskite quantum dots, with narrow particle size distribution, improves luminescence efficiency and stability, reduces material costs, and enhances color gamut breadth and color purity. It is suitable for high-fine quantum dot display technology .
Smart Images

Figure CN118892778A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor materials, relates to a perovskite quantum dot synthesis technology, and specifically relates to a perovskite quantum dot synthesis method and a synthesis device based on supercritical CO2. Background Art
[0002] Quantum dots are a new type of nanomaterial, with a size usually between 1 and 10 nm, consisting of an inorganic core and organic or inorganic molecules coated on the surface of the core. At the nanoscale, quantum dots have special structural characteristics and exhibit some wonderful properties, such as small size effect, quantum size effect, macroscopic quantum tunneling effect and surface effect. Compared with the common fluorescent materials in LEDs, quantum dots have the advantages of wide excitation spectrum, narrow emission spectrum, adjustable emission wavelength, high quantum yield, and low light bleaching. They are currently ideal fluorescent materials and have great application prospects in the fields of display, laser, lighting, solar cells, and bioluminescent labeling. There are many types of quantum dots, the most common of which are CdSe quantum dots, carbon quantum dots, ZnO quantum dots, CuInS2 quantum dots, CdTe quantum dots, InP quantum dots and perovskite quantum dots. Perovskite quantum dots are the most popular quantum dot materials in recent years.
[0003] Since the first synthesis of CdSe quantum dots in the 1990s, quantum dot materials have experienced great development in preparation technology, optical properties and device applications. However, traditional cadmium-based quantum dot materials have two disadvantages. First, cadmium is a highly toxic metal element, which limits its application in healthy lighting and high-quality display. Second, the reproducibility of preparing cadmium-based quantum dot samples with short-wavelength luminescence is poor, which affects the production design of its products. Therefore, it is urgent to develop relatively low-toxic, low-cost and high-quality luminescent quantum dot materials. In recent years, all-inorganic halogen perovskite CsPbX3 (X=Cl, Br, and I) quantum dot materials have attracted widespread attention due to their high fluorescence quantum yield (Photoluminescence Quantum Yield, PLQY), high carrier mobility, low preparation cost, low defect state density and adjustable band gap. These excellent properties make perovskite quantum dots the most popular quantum dot materials in recent years. In addition to display technology, perovskite quantum dots have begun to emerge in many application fields, such as X-ray imaging, micro-spectrometers, optical sensors and other fields. Thanks to the high atomic number component of perovskite materials, many perovskite materials have excellent X-ray fluorescence conversion performance and can achieve X-ray fluorescence imaging. Thanks to the high transparency and high luminescence characteristics of lead perovskite quantum dot optical films, they can be used as light conversion materials to enhance the near-infrared absorption of silicon-based devices, improve the solar energy efficiency of fluorescent concentrators, and respond to optical sensing media. Thanks to the finely adjustable absorption characteristics of perovskite quantum dots, perovskite quantum dots can be integrated with CCD as adjustable filter materials to build a micro-hyperspectrometer. In addition, perovskite quantum dot optical films are also expected to be used in agricultural lighting and health lighting.
[0004] At present, there are two main ways to prepare all-inorganic perovskite CsPbX3 quantum dots using solution technology: high-temperature hot injection method and room-temperature supersaturated crystallization method. The quantum dot materials prepared by the high-temperature hot injection method have high crystallinity and excellent optical properties. However, this method requires harsh conditions such as high temperature, inert gas protection and local injection, making it difficult to achieve large-scale production and application. The room-temperature solution crystallization method is much simpler than the high-temperature hot injection method. It uses the fact that the perovskite precursor ions have very low solubility in non-polar solvents. After the ions are injected into the solvent, the solubility drops rapidly to a supersaturated state, resulting in crystallization in a short time. In 2016, the team of Professor Zeng Haibo of Nanjing University of Science and Technology first proposed a method for synthesizing all-inorganic perovskite CsPbX3 quantum dots at room temperature without the need for inert gas protection. In 2017, WEI Song et al. synthesized a highly efficient luminescent CsPbBr3 quantum dot at room temperature by adding tetraoctylammonium bromide (TOAB) to the precursor solution to accelerate the dissolution of PbBr2, and prepared the corresponding quantum dot light emitting diode (QLED) device. Since then, researchers have prepared all-inorganic perovskite quantum dot materials with better performance by regulating the type and amount of surfactants and controlling the reaction time. However, in the process of mass preparation of CsPbX3 quantum dots, due to the uneven dissolution and dispersion of the precursor solution, the synthesized quantum dots will show phenomena such as reduced PLQY and widened emission peak half-height width, resulting in a decrease in the optical quality of the material. Therefore, how to maintain the excellent optical properties of CsPbX3 quantum dots synthesized in large quantities is a key step for the material to move from experiment to practical application.
[0005] Selecting appropriate ligands for perovskite quantum dots can further improve the luminescence efficiency of perovskite quantum dots and also improve the stability of perovskite quantum dots. However, this effect is still insufficient in the practical application of quantum dot materials and needs substantial improvement and enhancement. However, due to the limitations of existing perovskite quantum dot synthesis methods, it is impossible to arbitrarily select and combine small molecule compounds that have excellent coordination and surface defect passivation effects with perovskite quantum dots. Using such small molecule compounds to modify the surface of quantum dots can further reduce the surface defects of perovskite quantum dots, thereby improving the luminescence efficiency of quantum dots. At the same time, the synthesis of efficient blue light quantum dots is still very difficult. The main reason is that it is difficult to stably control the size of quantum dots below 10nm during the synthesis of conventional perovskite quantum dots. Even if the blue light quantum dots are compressed by other means, the particle size distribution is wide and the luminescence position cannot be accurately controlled. This will cause the perovskite quantum dots to increase the half-peak width (FWHM) of the luminescence peak, making the luminescence advantages of perovskite quantum dots (good monochromaticity and wide color gamut) impossible to achieve. Summary of the invention
[0006] Purpose of the invention: In order to overcome the shortcomings of the prior art that the size of perovskite quantum dots is difficult to stably control and the particle size distribution is too wide, a method and a synthesis device for perovskite quantum dots based on supercritical CO2 are provided. The method improves the anti-solvent synthesis method by supercritical CO2 fluid, so that perovskite quantum dots with smaller size and narrower particle size distribution can be obtained, and small molecules with good coordination and passivation effects on the perovskite quantum dots can be arbitrarily selected to perform surface modification on them, which can greatly improve the stability and luminescence efficiency of the perovskite quantum dots.
[0007] Technical solution: To achieve the above-mentioned purpose, the present invention provides a perovskite quantum dot synthesis device based on supercritical CO2, including a perovskite precursor solution container, a CO2 cylinder group, a high-pressure reactor and a recovery tank, wherein the perovskite precursor solution container is connected to the high-pressure reactor through a high-pressure isochoric double-plunger pump, the CO2 cylinder group is connected to the high-pressure reactor through a high-pressure large-flow pump, and the high-pressure reactor is connected to the recovery tank. The perovskite precursor solution container is used to store the precursor solution A, and the CO2 cylinder group is used to store the high-pressure CO2 liquid. A heating jacket and a back pressure valve are provided on the high-pressure reactor. The high-pressure reactor controls the temperature and pressure in the high-pressure reactor through the heating jacket and the back pressure valve respectively, so as to make the mixed fluid in the high-pressure reactor reach a supercritical state. The recovery tank is used to collect the perovskite quantum dot dispersion, and a quick pressure relief valve is provided between the high-pressure reactor and the recovery tank.
[0008] Furthermore, a quick injection valve is provided between the high-pressure isochoric double-plunger pump and the high-pressure reactor, a vent valve is provided on the high-pressure reactor, and a recovery valve is provided at the bottom liquid outlet of the recovery tank.
[0009] Furthermore, a ceramic filter is arranged in the recovery tank, and a pressure relief valve and a flushing valve are arranged on the top of the recovery tank.
[0010] Furthermore, an electric heating device is provided between the high-pressure and high-flow pump and the high-pressure reactor.
[0011] Based on the above-mentioned perovskite quantum dot synthesis device, the present invention also provides a perovskite quantum dot synthesis method based on supercritical CO2, comprising the following steps:
[0012] S1: preparing a good solution A of a predetermined concentration of a perovskite precursor, which also contains a predetermined concentration of a ligand and a surface modification small molecule, and introducing it into a perovskite precursor solution container 1 for standby use, which is recorded as precursor solution A;
[0013] S2: Prepare a good solution B of a predetermined concentration of a perovskite precursor, denoted as precursor solution B;
[0014] S3: Inject the precursor solution B and the quantitative ligand or modifier small molecules into the high-pressure reactor, pump out the high-pressure CO2 liquid in the CO2 cylinder group through a high-pressure and high-flow pump, and heat the high-pressure CO2 liquid to supercritical CO2 through an electric heater, and the supercritical CO2 enters the high-pressure reactor to form a mixed fluid;
[0015] S4: controlling the temperature and pressure in the high-pressure reactor by means of the heating jacket and the back pressure valve of the high-pressure reactor to maintain the supercritical state of the mixed fluid mainly composed of supercritical CO2 to form a supercritical mixed fluid;
[0016] S5: heating the precursor solution A to a specified temperature, and pumping a predetermined amount of the precursor solution A into the high-pressure reactor at a specified flow rate by a high-pressure isochoric double-plunger pump;
[0017] S6: The precursor solution A and the supercritical mixed fluid containing the precursor B are fully and evenly mixed by stirring in the high-pressure reactor to form a reaction solution;
[0018] S7: Open the quick pressure relief valve, and the reaction liquid is transferred to the recovery tank. In this process, the supercritical CO2 dissolved in the reaction liquid quickly loses pressure and turns into gas in an instant and is separated from the reaction liquid. The gaseous supercritical CO2 passes through the ceramic filter in the recovery tank and is discharged from the pressure relief valve. The remaining crude perovskite quantum dot crystal containing ligands or organic small molecule modifiers will be dispersed in a small amount of organic solvent;
[0019] S8: Open the recovery valve to recover the crude dispersion of perovskite quantum dots;
[0020] S9: Refining and purifying the crude dispersion of perovskite quantum dots to obtain a sample dispersion of perovskite quantum dots in a predetermined solvent.
[0021] Furthermore, the preparation method of the precursor solution A in step S1 is: weigh cesium carbonate or other cesium source and add it into a three-necked bottle, and at the same time add octadecene or other solvents, oleic acid or other ligands, turn on magnetic stirring and evacuate with a vacuum pump, heat to a specified temperature and then keep warm, continue to heat until the cesium source is completely dissolved and keep warm, fill the system with N2 protective gas, evacuate again, repeat this process N times, keep warm for later use, and use the solution at this time as precursor solution A.
[0022] Furthermore, the preparation method of the precursor solution B in the step S2 is: weigh lead bromide or other lead source, octadecene or other solvent, add them into a three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to a specified temperature and then keep warm, continue to heat until the lead source is completely dissolved and keep warm, fill the system with N2 protective gas; use a syringe to extract oleic acid or other ligands and oleylamine or other modified small molecules, respectively, and inject them into the reactor, re-evacuate the system until there are no bubbles, then fill with N2 protective gas and cool to a specified temperature range, and use the solution at this time as precursor solution B.
[0023] Furthermore, the ligand or modifier small molecule in step S3 can form a stable coordination structure with a certain element on the surface of the perovskite quantum dots, thereby improving the luminescence efficiency and stability of the perovskite quantum dots, or significantly improving the optical properties and stability of the perovskite quantum dots by modifying the surface of the perovskite quantum dots.
[0024] Furthermore, in step S4, the temperature in the high-pressure reactor is controlled to be between 60° C. and 90° C., and the pressure is controlled to be between 12 MPa and 30 MPa.
[0025] Furthermore, in step S5, the heating temperature range of the precursor solution A is 100° C. to 200° C., the pressure setting value of the high-pressure isochoric double-plunger pump is greater than the pressure value in the high-pressure reactor, and the precursor solution A is injected into the high-pressure reactor through the fast injection valve.
[0026] Furthermore, the crude perovskite quantum dot dispersion in step S8 includes a dispersion obtained by washing the filter element and a dispersion directly recovered by a recovery tank, wherein the dispersion obtained by washing the filter element is obtained by taking out a ceramic filter from the recovery tank and immersing it in a predetermined organic solvent, and obtaining the dispersion after ultrasonic washing.
[0027] Furthermore, the step S9 is specifically as follows: adding a predetermined solvent to the crude perovskite quantum dot product and transferring it to a centrifuge tube, washing it with high-speed shaking, and then centrifuging it under specified conditions of an ultra-high-speed centrifuge, removing the supernatant, and then adding the predetermined solvent to the centrifuge tube. After repeated washing and ultra-high-speed centrifugation treatment for more than 3 times, a refined perovskite quantum dot sample dispersion containing a ligand or an organic small molecule modifier is obtained.
[0028] The upper limit of the average particle size of the perovskite quantum dots obtained in the present invention should be below 50nm, preferably below 30nm, more preferably below 20nm, and most preferably below 10nm. The average particle size of the perovskite quantum dots obtained in the present invention has no lower limit, such as above 1nm, more preferably above 2nm, preferably above 3nm, and most preferably above 4nm.
[0029] The present invention provides a kind of quantum dot display technology that can be used for the next generation of high-precision (4K / 8K), which can obtain high-quality perovskite nanocrystals with wider color gamut (BT.2020), higher color purity and high quantum luminescence efficiency. When the perovskite nanocrystal is synthesized, the solubility of a mixed solvent of a large excess of supercritical CO2 and a small amount of organic solvent on small molecule compounds and the high uniform dispersion characteristics of small molecule compounds in the mixed solvent are utilized. By manipulating the pressure of the supercritical mixed fluid, CO2 is separated from the supercritical mixed fluid, and the solubility of the perovskite molecular structure in a small amount of organic solvent is sharply reduced, and it has to be precipitated from the organic solvent in the form of nanocrystals instantly. The surface of the perovskite nanocrystal can selectively form a stable surface passivation layer and the required surface modification effect while the nanocrystal is precipitated, thereby simultaneously ensuring the higher dimensional stability, higher luminous efficiency, narrower half-peak width (better monochromaticity, higher color purity) and high stability of the nanocrystal as a quantum dot luminescent material, and high dispersibility and independent dispersion effect in a predetermined resin dispersion. The use of supercritical CO2 reduces the amount of organic solvents used in conventional perovskite quantum dot synthesis methods. Compared with traditional perovskite quantum dot synthesis methods, it reduces material costs and environmental impact, and can obtain smaller particle sizes and narrower particle size distributions. In addition, it can freely select small molecules that have surface passivation and coordination effects on perovskite molecules to implement stable surface modification on the perovskite surface, which can greatly improve the stability of perovskite crystals.
[0030] In the present invention, the precursor good solvent dispersion of perovskite quantum dots is used to reprecipitate in a lean solvent composed of supercritical fluid with super-large excess supercritical CO2. The supersaturation of perovskite quantum dots in the supercritical fluid under such conditions is particularly high. At the moment when the precursor solution A and the precursor solution B in the supercritical fluid collide, the crystal nucleus is precipitated from the supercritical fluid as a crystal nucleus. Because the supercritical fluid is a super-uniform reaction field at the molecular level, the crystal nucleus is uniformly precipitated in the supercritical fluid at all places at the same time, and the perovskite quantum dots have quickly completed the reaction under conditions that are not conducive to nuclear growth. Therefore, the method of the present invention can obtain small-sized quantum dot materials (for example, within a particle size of 10nm or even within 5nm) that are not easy to obtain by existing synthesis methods, and the quantum dot particle size distribution is narrower. In addition, since the mixing of excess supercritical CO2 and lower alcohols can dissolve numerous small molecule compounds, the surface passivation and surface modification of various perovskite quantum dots have many selectable combinations, and the perovskite quantum dots can also be easily dispersed independently in different dispersion solvents because of the selection of appropriate modification molecules, thereby improving their optical properties. The quantum efficiency of perovskite quantum dots will be affected by the surface or internal defects of the quantum dots. Appropriate ligand molecules can not only reduce the surface defects of quantum dots, thereby improving the quantum efficiency of quantum dot luminescence, but also improve the optical properties and stability of quantum dot crystals.
[0031] The perovskite quantum dot material synthesized by the present invention comprises a perovskite structure crystal and a ligand on the surface of the crystal and a modified small molecule compound, wherein the perovskite structure crystal is represented by the following general formula (P1):
[0032] ABCl 3-x-y Br x I y :M n+ ······(P1)
[0033] Wherein, A represents at least one alkali metal cation (Cs) and one organic cation (FA: formamidine, MA: methylamine); B represents at least one divalent metal cation of Pb, Sn, Ge, Zn, Cu; M n+ is a cation of at least one metal element selected from the group consisting of Ge, Sn, Pb, Sb, Bi, Cu, Ni, Co, Fe, Mn, Cr, Pd, Cd, Eu, Yb and Ag; 0≤x≤3, 0≤y≤3;
[0034] The perovskite structure compounds described in the present invention include MAPbI3, MASnI3, MAPbBr3, MASnBr3, MAPbCl3, MASnCl3, FAPbI3, FAPbI3, FASnI3, FAPbBr3, FAPbBr2I, FASnBr3, FAPbCl3, FASnCl3, FASnBr2I, CsPbI3, CsSnI3, CsPbBr3, CsSnBr3, CsPbCl3, CsSnCl3, RbPbI3, RbSnI3, RbPbBr3, RbSnBr3, RbPbCl3 and RbSnCl3, etc.
[0035] Beneficial effects: Compared with the prior art, the present invention can synthesize perovskite quantum dots with stable small size and narrow particle size distribution through the synthesis method of the anti-solvent method improved by supercritical CO2 fluid, and the perovskite quantum dots can freely select surface modification molecules, and are more easily independently dispersed in a specified solvent or resin to achieve higher optical properties; the method of the present invention can also select ligands suitable for reducing surface defects of perovskite quantum dots, and the obtained perovskite quantum dots can have higher quantum luminescence efficiency and higher stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of the perovskite quantum dot synthesis device provided by the present invention. DETAILED DESCRIPTION
[0037] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0038] Embodiment 1:
[0039] like Figure 1 As shown, this embodiment provides a perovskite quantum dot synthesis device based on supercritical CO2, including a perovskite precursor solution container 1, a CO2 cylinder group 2, a high-pressure reactor 5 and a recovery tank 11, the perovskite precursor solution container 1 is connected to the high-pressure reactor 5 through a high-pressure isochoric double-plunger pump 3, a fast injection valve 17 is arranged on the pipeline between the high-pressure isochoric double-plunger pump 3 and the high-pressure reactor 5, the CO2 cylinder group 2 is connected to the high-pressure reactor 5 through a high-pressure large-flow pump 4, and the pipeline between the high-pressure large-flow pump 4 and the high-pressure reactor 5 is provided with a fast injection valve 17. An electric heating device 16 is provided, the bottom of the high-pressure reactor 5 is connected to the recovery tank 11 through a pipeline, and a quick pressure relief valve 9 is provided on the pipeline between the high-pressure reactor 5 and the recovery tank 11, a heating jacket 6 is provided on the high-pressure reactor 5, a back pressure valve 7 and a vent valve 8 are provided on the top of the high-pressure reactor 5, a ceramic filter 12 is provided in the recovery tank 11, a pressure relief valve 13 and a flushing valve 14 are provided on the top of the recovery tank 11, a recovery valve 15 is provided at the bottom liquid outlet of the recovery tank 11, and high-pressure CO2 liquid is stored in the CO2 cylinder group 2.
[0040] Embodiment 2:
[0041] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbBr3 green light quantum dots. Figure 1 , the specific synthesis process is:
[0042] 1) Weigh 0.1 g of cesium carbonate and add it to a 50 ml three-necked bottle, add 10 ml of octadecene and 0.7 ml of oleic acid, start magnetic stirring and evacuate with a vacuum pump, heat to 100 ° C and keep warm for 1 hour, continue to heat to 120 ° C and keep warm for 15 minutes, fill the system with N2 protective gas for 5 minutes, evacuate again, repeat this process 3 times, put it into the perovskite precursor solution container 1 and keep warm for standby use, recorded as precursor solution A;
[0043] 2) Weigh 0.138g of lead bromide and 10ml of octadecene into a 50ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0044] 3) Use a syringe to extract the ligands (4.5 ml of oleic acid and 4.5 ml of oleylamine) respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to below 80°C to form a precursor solution B. Then, 2.4 ml of the precursor solution B is extracted and transferred to the high-pressure reactor 5;
[0045] 4) After closing the high-pressure reactor 5, the high-flow high-pressure pump 4 is started to inject the high-pressure CO2 liquid in the CO2 cylinder group 2 into the high-pressure reactor 5. In this process, according to actual needs, the pipeline between the high-flow high-pressure pump 4 and the high-pressure reactor 5 can be appropriately heated (above 50° C.) and heat-insulated by the electric heating device 16 to heat the high-pressure CO2 liquid to a supercritical state CO2, and the supercritical state CO2 is injected into the high-pressure reactor 5;
[0046] The high-pressure reactor 5 is stirred by a stirring device to form a uniform mixed fluid, and the mixed fluid is heated by a heating jacket 6 until the temperature in the high-pressure reactor 5 reaches 60° C. The pressure in the high-pressure reactor 5 is adjusted to 12 MPa by a back pressure valve 7 to maintain a supercritical state of the mixed fluid mainly composed of supercritical CO2, thereby forming a supercritical mixed fluid;
[0047] 5) Reheat the precursor solution A in the perovskite precursor solution container 1 to 120° C. Use a syringe to extract 1.6 ml of the precursor solution A and inject it into the high-pressure reactor 5 through the isochoric high-pressure double-plunger pump 3. During this process, the pressure setting value of the high-pressure isochoric double-plunger pump 3 is slightly greater than the pressure value in the high-pressure reactor 5, and the injection is completed within 1.6 seconds by opening the fast injection valve 17. After continuous stirring in the high-pressure reactor 5 for 3 seconds, open the fast pressure relief valve 9 at the bottom of the high-pressure reactor 5 to transfer the reaction solution to the recovery tank 11. During this process, the supercritical CO2 dissolved in the reaction solution quickly loses pressure and instantly becomes gas and is separated from the reaction solution. Open the pressure relief valve 13, and the gaseous supercritical CO2 passes through the ceramic filter 12 in the recovery tank 11 and is discharged from the pressure relief valve 13. The remaining crude perovskite quantum dot crystals containing ligands or organic small molecule modifiers will be dispersed in a small amount of organic solvent;
[0048] 6) After the pressure in the recovery tank 11 drops to normal pressure, the recovery valve 15 is opened, and flushing is performed through the flushing valve 14 to recover the crude dispersion of perovskite quantum dots;
[0049] 7) taking out the ceramic filter 12 from the recovery tank 11 and immersing it in a predetermined organic solvent, and then washing it by ultrasonic wave for 10-20 minutes (the above operation can be repeated depending on the degree of clogging of the filter element by quantum dots) to obtain a dispersion, and mixing the dispersion with the dispersion of step 6 to obtain a final crude perovskite quantum dot dispersion;
[0050] 8) Take out the crude dispersion of perovskite quantum dots, add 40 ml of methyl acetate and stir for 5 minutes, put it into a centrifuge and centrifuge it at 10,000 rpm for 15 minutes, take out the precipitate and add 10 ml of n-hexane, centrifuge it again at 10,000 rpm for 10 minutes, and take the supernatant, which is CsPbBr3 green light quantum dots (excitation 365 nm, luminescence peak 508 nm).
[0051] Embodiment 3:
[0052] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbBr3 green light quantum dots. Figure 1 , the specific synthesis process is:
[0053] 1) Weigh 0.1 g of cesium carbonate and add it to a 50 ml three-necked bottle, add 10 ml of octadecene and 0.7 ml of oleic acid, start magnetic stirring and evacuate with a vacuum pump, heat to 100 ° C and keep warm for 1 hour, continue to heat to 120 ° C and keep warm for 15 minutes, fill the system with N2 protective gas for 5 minutes, evacuate again, repeat this process 3 times, put it into the perovskite precursor solution container 1 and keep warm for standby use, recorded as precursor solution A;
[0054] 2) Weigh 0.165g of lead bromide and 10ml of octadecene into a 50ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0055] 3) Use a syringe to extract 4.0 ml of oleic acid and 4.0 ml of oleylamine respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to below 80° C. to form a precursor solution B. Then, 1.0 ml of the precursor solution B is extracted and transferred to the high-pressure reactor 5;
[0056] 4) After closing the high-pressure reactor 5, the high-flow high-pressure pump 4 is started to inject the high-pressure CO2 liquid in the CO2 cylinder group 2 into the high-pressure reactor 5. In this process, according to actual needs, the pipeline between the high-flow high-pressure pump 4 and the high-pressure reactor 5 can be appropriately heated (above 50° C.) and heat-insulated by the electric heating device 16 to heat the high-pressure CO2 liquid to a supercritical state CO2, and the supercritical state CO2 is injected into the high-pressure reactor 5;
[0057] The high-pressure reactor 5 is stirred by a stirring device to form a uniform mixed fluid, and the mixed fluid is heated by a heating jacket 6 until the temperature in the high-pressure reactor 5 reaches 90° C. The pressure in the high-pressure reactor 5 is adjusted to 30 MPa by a back pressure valve 7 to maintain a supercritical state of the mixed fluid mainly composed of supercritical CO2, thereby forming a supercritical mixed fluid;
[0058] 5) Reheat the precursor solution A in the perovskite precursor solution container 1 to 120° C. and extract 1.0 ml of the precursor solution A with a syringe and inject it into the high-pressure reactor 5 through the isochoric high-pressure double-plunger pump 3. In this process, the pressure setting value of the high-pressure isochoric double-plunger pump 3 is slightly greater than the pressure value in the high-pressure reactor 5, and the injection is completed within 0.5 seconds by opening the fast injection valve 17. After continuous stirring in the high-pressure reactor 5 for 3 seconds, open the fast pressure relief valve 9 at the bottom of the high-pressure reactor 5 to transfer the reaction solution to the recovery tank 11. In this process, the supercritical CO2 dissolved in the reaction solution quickly loses pressure and instantly becomes gas and is separated from the reaction solution. Open the pressure relief valve 13, and the gaseous supercritical CO2 passes through the ceramic filter 12 in the recovery tank 11 and is discharged from the pressure relief valve 13. The remaining crude perovskite quantum dot crystals containing ligands or organic small molecule modifiers will be dispersed in a small amount of organic solvent;
[0059] 6) After the pressure in the recovery tank 11 drops to normal pressure, the recovery valve 15 is opened, and flushing is performed through the flushing valve 14 to recover the crude dispersion of perovskite quantum dots;
[0060] 7) taking out the ceramic filter 12 from the recovery tank 11 and immersing it in a predetermined organic solvent, and then washing it by ultrasonic wave for 10-20 minutes (the above operation can be repeated depending on the degree of clogging of the filter element by quantum dots) to obtain a dispersion, and mixing the dispersion with the dispersion of step 6 to obtain a final crude perovskite quantum dot dispersion;
[0061] 8) Take out the crude dispersion of perovskite quantum dots, add 40 ml of methyl acetate and stir for 5 minutes, put it into a centrifuge and centrifuge it at 10,000 rpm for 15 minutes, take out the precipitate and add 10 ml of n-hexane, centrifuge it again at 10,000 rpm for 10 minutes, and take the supernatant, which is CsPbBr3 green light quantum dots (excitation 365 nm, luminescence peak 506 nm).
[0062] Embodiment 4:
[0063] In this example, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPb 0.6 Sn 0.4 Br3 green light quantum dots, reference Figure 1 , the specific synthesis process is:
[0064] 1) Weigh 0.1 g of cesium carbonate and add it to a 50 ml three-necked bottle, add 10 ml of octadecene and 0.7 ml of oleic acid, start magnetic stirring and evacuate with a vacuum pump, heat to 100 ° C and keep warm for 1 hour, continue to heat to 120 ° C and keep warm for 15 minutes, fill the system with N2 protective gas for 5 minutes, evacuate again, repeat this process 3 times, put it into the perovskite precursor solution container 1 and keep warm for standby use, recorded as precursor solution A;
[0065] 2) Weigh 0.147g of lead bromide, 0.167g of tin bromide, and 10ml of tri-n-octylphosphine oxide (TOPO) into a 50ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 90°C and keep warm for 1h, continue heating to 190°C and keep warm for 15min, fill the system with N2 protective gas and continue cooling to room temperature for use;
[0066] 3) Use a syringe to extract 4.0 ml of oleic acid and 4.0 ml of oleylamine respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to below 80° C. to form a precursor solution B. Then, 1.0 ml of the precursor solution B is extracted and transferred to the high-pressure reactor 5;
[0067] 4) After closing the high-pressure reactor 5, the high-flow high-pressure pump 4 is started to inject the high-pressure CO2 liquid in the CO2 cylinder group 2 into the high-pressure reactor 5. In this process, according to actual needs, the pipeline between the high-flow high-pressure pump 4 and the high-pressure reactor 5 can be appropriately heated (above 50° C.) and heat-insulated by the electric heating device 16 to heat the high-pressure CO2 liquid to a supercritical state CO2, and the supercritical state CO2 is injected into the high-pressure reactor 5;
[0068] The high-pressure reactor 5 is stirred by a stirring device to form a mixed fluid, and the mixed fluid is heated by a heating jacket 6 until the temperature in the high-pressure reactor 5 reaches 80° C. The pressure in the high-pressure reactor 5 is adjusted to 18 MPa by a back pressure valve 7 to maintain a supercritical state of the mixed fluid mainly composed of supercritical CO2, thereby forming a supercritical mixed fluid;
[0069] 5) Reheat the precursor solution A in the perovskite precursor solution container 1 to 120° C. and extract 1.0 ml of the precursor solution A with a syringe and inject it into the high-pressure reactor 5 through the isochoric high-pressure double-plunger pump 3. In this process, the pressure setting value of the high-pressure isochoric double-plunger pump 3 is slightly greater than the pressure value in the high-pressure reactor 5, and the injection is completed within 0.5 seconds by opening the fast injection valve 17. After continuous stirring in the high-pressure reactor 5 for 3 seconds, open the fast pressure relief valve 9 at the bottom of the high-pressure reactor 5 to transfer the reaction solution to the recovery tank 11. In this process, the supercritical CO2 dissolved in the reaction solution quickly loses pressure and instantly becomes gas and is separated from the reaction solution. Open the pressure relief valve 13, and the gaseous supercritical CO2 passes through the ceramic filter 12 in the recovery tank 11 and is discharged from the pressure relief valve 13. The remaining crude perovskite quantum dot crystals containing ligands or organic small molecule modifiers will be dispersed in a small amount of organic solvent;
[0070] 6) After the pressure in the recovery tank 11 drops to normal pressure, the recovery valve 15 is opened, and flushing is performed through the flushing valve 14 to recover the crude dispersion of perovskite quantum dots;
[0071] 7) taking out the ceramic filter 12 from the recovery tank 11 and immersing it in a predetermined organic solvent, and then washing it by ultrasonic wave for 10-20 minutes (the above operation can be repeated depending on the degree of clogging of the filter element by quantum dots) to obtain a dispersion, and mixing the dispersion with the dispersion of step 6 to obtain a final crude perovskite quantum dot dispersion;
[0072] 8) Take out the crude dispersion of perovskite quantum dots, add 40 ml of methyl acetate and stir for 5 min, put it into a centrifuge and centrifuge it at 10000 rpm for 15 min, take out the precipitate and add 10 ml of n-hexane, centrifuge it at 10000 rpm again for 10 min, take out the supernatant, which is CsPb 0.6 Sn 0.4 Br3 green light quantum dots (excitation 365nm, luminescence peak 506nm).
[0073] Comparative Example 1:
[0074] In this comparative example, the existing hot injection method is used to prepare CsPbBr3 green light quantum dots, and the specific process is as follows:
[0075] 1) Weigh 0.1g of cesium carbonate and add it to a 50ml three-necked bottle, add 10ml of octadecene and 0.7ml of oleic acid, start magnetic stirring and evacuate with a vacuum pump, heat to 100℃ and keep warm for 1h, continue to heat to 120℃ and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, finally cool to 50℃, take out and bottle for use, recorded as precursor A;
[0076] 2) Weigh 0.138g of lead bromide and 10ml of octadecene into a 50ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0077] 3) Use a syringe to extract 4.5 ml of oleic acid and 4.5 ml of oleylamine respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C;
[0078] 4) Reheat the precursor A to 120°C and inject 1.6 ml of it into the reaction solution in step 3 using a syringe, and quickly cool the system to room temperature using an ice water bath;
[0079] 5) Take out the reaction solution in step 4, add 40 ml of methyl acetate and stir for 5 minutes, put it into a centrifuge and centrifuge it at 8000 rpm for 5 minutes, take out the precipitate and add 10 ml of n-hexane, centrifuge it again at 5000 rpm for 3 minutes, and take the supernatant, which is CsPbBr3 green light quantum dots (excitation 365 nm, luminescence peak 516 nm).
[0080] In the present invention, the performance of the perovskite quantum dots obtained in Examples 2 to 4 and Comparative Example 1 is compared and analyzed, as follows:
[0081] The key condition setting data of Examples 2 to 4 and Comparative Example 1 are shown in Table 1:
[0082] Table 1
[0083]
[0084] Take a small amount of the upper layer of the perovskite quantum dot dispersion and dilute it with toluene or n-hexane, observe it under FE-TEM or HR-TEM, select a representative area (the number of quantum dots in the area is greater than 100) in the observation field of a specified magnification, take a photo, magnify the photo at a specified ratio, scan it with special software, and automatically calculate the average particle size and the number of quantum dots in each particle size range. Select at least 5 representative areas, and take their average value as the average particle size and particle size distribution of the perovskite quantum dot sample.
[0085] Based on the above method for obtaining the average particle size and particle size distribution, the properties of the perovskite quantum dots obtained in Examples 2 to 4 and Comparative Example 1 are shown in Table 2:
[0086] Table 2
[0087]
[0088] It can be seen from Table 1 and Table 2 that the perovskite quantum dots obtained in Examples 2 to 4 have the following advantages compared with Comparative Example 1:
[0089] The average particle size of Examples 2 to 4 can be controlled below 10 nm, and the particle size distribution is significantly narrowed, and both the particle size and the particle size distribution are adjustable; while achieving a small size of quantum dots, the wavelength of the maximum luminescence peak is significantly shifted toward the short wavelength direction, which is reflected in the significant reduction in the half-peak width index of the monochromatic luminescence purity (better monochromaticity); by controlling the supersaturation of the two stages of supercritical fluid reprecipitation and instantaneous opening of supercritical CO2, the precursor raw materials can be utilized as much as possible to obtain a higher quantum dot material yield; due to the mixing of a large excess of supercritical CO2 and a small amount of lower alcohol, under conditions close to the critical point of supercritical CO2, almost all known small molecule compounds can be dissolved, and the screening of these small molecule compounds can refer to other research results on reducing the effect of surface defects of perovskite quantum dots on quantum luminescence efficiency, so as to improve the final effect of perovskite quantum dots at any time.
[0090] According to the data in Table 1 and Table 2, it can be seen that the present invention utilizes a supercritical mixed fluid with supercritical CO2 as the vast majority of components as a reaction field, and can arbitrarily adjust the combination of quantum dot material ligands and surface modifier molecules, and the resulting perovskite quantum dots have the following characteristics: 1) The average particle size is all below 10 nm, and the particle size distribution is less than ±3 nm; 2) It is easy to maintain an independent dispersion state in a given solvent; 3) The maximum luminescent peak wavelength of perovskite quantum dots with the same composition obtained by other conventional methods produces an obvious short-wavelength side shift, and the half-peak width is also significantly reduced; 4) Due to the possibility of free combination of ligands and modifier molecules, the luminescent quantum efficiency and stability of the quantum dots can be simultaneously improved.
Claims
1. A perovskite quantum dot synthesis device based on supercritical CO2, characterized in that: It includes a perovskite precursor solution container, a CO2 cylinder group, a high-pressure reactor and a recovery tank. The perovskite precursor solution container is connected to the high-pressure reactor through a high-pressure isochoric double-plunger pump, the CO2 cylinder group is connected to the high-pressure reactor through a high-pressure large-flow pump, and the high-pressure reactor is connected to the recovery tank. The perovskite precursor solution container is used to store precursor solution A, and the CO2 cylinder group is used to store high-pressure CO2 liquid. The high-pressure reactor is provided with a heating jacket and a back pressure valve. The high-pressure reactor controls the temperature and pressure in the high-pressure reactor through the heating jacket and the back pressure valve respectively, so as to make the mixed fluid in the high-pressure reactor reach a supercritical state. The recovery tank is used to collect perovskite quantum dot dispersion, and a quick pressure relief valve is provided between the high-pressure reactor and the recovery tank.
2. A supercritical CO2-based perovskite quantum dot synthesis device according to claim 1, characterized in that: A quick injection valve is arranged between the high-pressure isochoric double-plunger pump and the high-pressure reactor, a vent valve is arranged on the high-pressure reactor, and a recovery valve is arranged at the bottom of the recovery tank.
3. A supercritical CO2-based perovskite quantum dot synthesis device according to claim 1, characterized in that: A ceramic filter is arranged in the recovery tank, and a pressure relief valve and a flushing valve are arranged on the top of the recovery tank.
4. A supercritical CO2-based perovskite quantum dot synthesis device according to claim 1, characterized in that: An electric heating device is arranged between the high-pressure and large-flow pump and the high-pressure reactor.
5. A method for synthesizing perovskite quantum dots based on supercritical CO2, characterized in that: The steps include: S1: preparing a good solution A of a predetermined concentration of a perovskite precursor, which also contains a predetermined concentration of a ligand and a surface modification small molecule, and introducing it into a perovskite precursor solution container 1 for standby use, which is recorded as precursor solution A; S2: Prepare a good solution B of a predetermined concentration of a perovskite precursor, denoted as precursor solution B; S3: Inject the precursor solution B and the quantitative ligand or modifier small molecules into the high-pressure reactor, pump out the high-pressure CO2 liquid in the CO2 cylinder group through a high-pressure and high-flow pump, and heat the high-pressure CO2 liquid to supercritical CO2 through an electric heater, and the supercritical CO2 enters the high-pressure reactor to form a mixed fluid; S4: controlling the temperature and pressure in the high-pressure reactor by means of the heating jacket and the back pressure valve of the high-pressure reactor to maintain the supercritical state of the mixed fluid mainly composed of supercritical CO2 to form a supercritical mixed fluid; S5: heating the precursor solution A to a specified temperature, and pumping a predetermined amount of the precursor solution A into the high-pressure reactor at a specified flow rate by a high-pressure isochoric double-plunger pump; S6: The precursor solution A and the supercritical mixed fluid containing the precursor B are fully and evenly mixed by stirring in the high-pressure reactor to form a reaction solution; S7: Open the quick pressure relief valve, and the reaction liquid is transferred to the recovery tank. In this process, the supercritical CO2 dissolved in the reaction liquid quickly loses pressure and turns into gas in an instant and is separated from the reaction liquid. The gaseous supercritical CO2 passes through the ceramic filter in the recovery tank and is discharged from the pressure relief valve. The remaining crude perovskite quantum dot crystal containing ligands or organic small molecule modifiers will be dispersed in a small amount of organic solvent; S8: Open the recovery valve to recover the crude dispersion of perovskite quantum dots; S9: Refining and purifying the crude dispersion of perovskite quantum dots to obtain a sample dispersion of perovskite quantum dots in a predetermined solvent.
6. A method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: The preparation method of the precursor solution A in step S1 is as follows: weigh cesium carbonate or other cesium source and add it into a three-necked bottle, add octadecene or other solvents, oleic acid or other ligands at the same time, start magnetic stirring and evacuate with a vacuum pump, heat to a specified temperature and then keep warm, continue to heat until the cesium source is completely dissolved and keep warm, fill the system with N2 protective gas, evacuate again, repeat this process N times, keep warm for later use, and use the solution at this time as the precursor solution A.
7. The method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: The preparation method of the precursor solution B in the step S2 is as follows: lead bromide or other lead source, octadecene or other solvent are weighed and added into a three-necked flask, and vacuumized with a vacuum pump while stirring magnetically, and then heated to a specified temperature and kept warm, and the temperature is continued to be heated and kept warm, and N2 protective gas is filled into the system; oleic acid or other ligands and oleylamine or other modifiers are respectively extracted with a syringe, and injected into the reactor, and the system is vacuumized again until there are no bubbles, and then N2 protective gas is filled and the temperature is lowered to a specified temperature range, and the solution at this time is used as the precursor solution B.
8. The method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: In step S4, the temperature in the high-pressure reactor is controlled to be between 60° C. and 90° C., and the pressure is controlled to be between 12 MPa and 30 MPa.
9. The method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: In step S5, the precursor solution A is heated to a temperature in the range of 100°C to 200°C, the pressure setting value of the high-pressure isochoric double-plunger pump is greater than the pressure value in the high-pressure reactor, and the precursor solution A is injected into the high-pressure reactor through a fast injection valve.
10. The method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: The crude perovskite quantum dot dispersion in step S8 includes a dispersion obtained by washing the filter element and a dispersion directly recovered by a recovery tank, wherein the dispersion obtained by washing the filter element is obtained by taking out a ceramic filter from the recovery tank and immersing it in a predetermined organic solvent, and then washing it by ultrasonic wave to obtain the dispersion.
11. The method for synthesizing perovskite quantum dots based on supercritical CO2 according to claim 5, characterized in that: The step S9 specifically comprises: adding a predetermined solvent to the crude perovskite quantum dot product and transferring it to a centrifuge tube; washing it with high-speed shaking; and then centrifuging it under specified conditions of an ultra-high-speed centrifuge; removing the supernatant; and then adding the predetermined solvent to the centrifuge tube; and after repeated washing and ultra-high-speed centrifugation for more than 3 times, a refined perovskite quantum dot sample dispersion containing a ligand or an organic small molecule modifier is obtained.