Size-controllable perovskite quantum dot synthesis method and synthesis device suitable for continuous production
By mixing the perovskite precursor solution with supercritical CO2 at high pressure and high temperature, the problems of perovskite quantum dot dimensional stability and particle size distribution uniformity are solved, and high efficiency is achieved continuous mass production and excellent performance of materials.
Patent Information
- Application Number
- CN202410973945.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-05
AI Technical Summary
The existing perovskite quantum dot synthesis methods are difficult to achieve dimensional stability control and uniform particle size distribution, and are difficult to achieve continuous mass production, resulting in low yields and waste of materials.
The supercritical CO2 assisted method is used to mix the precursor solution with supercritical CO2 at high pressure and high temperature to form a supercritical mixed fluid, and quickly cool to form perovskite quantum dots, leveraging the uniformity and high solubility of supercritical CO2. Achieve stability and size control of perovskite quantum dots.
The perovskite quantum dots are small and stable and controllable in size, suitable for continuous mass production, improve yield and material utilization, and reduce costs and environmental impact.
Smart Images

Figure CN118892779A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor materials and relates to a perovskite quantum dot synthesis technology, and specifically relates to a size-controllable perovskite quantum dot synthesis method and a synthesis device suitable for continuous production. Background Art
[0002] Perovskite quantum dots are a new type of nanomaterial with excellent optoelectronic properties, usually between 1 and 10 nm in size. Due to their unique structural characteristics, they exhibit some wonderful properties, such as small size effect, quantum confinement effect, macroscopic quantum tunneling effect, and surface effect, etc. They have broad application prospects in the fields of high color gamut display, solar cells, optoelectronic devices, biomedicine, lasers, catalysis, and sensing. With the deepening of research and the development of technology, perovskite quantum dots are expected to achieve breakthrough applications in more fields.
[0003] At present, there are two main ways to prepare perovskite quantum dots using solution technology: high-temperature crystallization method and room-temperature supersaturated crystallization method. Among them, the high-temperature crystallization method mainly includes hot injection method and solvothermal method. Its principle is to use the high-temperature process to promote the release of perovskite ions, and induce it to reach supersaturation and precipitate nanocrystals in the subsequent cooling process. For example, "DOI: 10.1021 / nl5048779" synthesized high-quality CsPbBr3 quantum dot nanocrystals by hot injection method, and its quantum efficiency is close to 90%. Although this method has high crystallization quality, it has extremely harsh requirements on reaction conditions. Temperature control and injection speed will greatly affect uniformity, and it is difficult to achieve mass production. At the same time, this method only crystallizes a small amount of precursor materials into quantum dots, and all others are lost, and the yield is low; the room-temperature supersaturated crystallization method is mainly the anti-solvent method. The principle is to dissolve the perovskite precursor material in a strong polar solvent in advance, and then quickly add a large amount of anti-solvent with poor solubility to make the precursor quickly reach supersaturation and precipitate nanocrystals. For example, DOI:10.1002 / adfm.201600109 first converts Cs + 、Pb2 + and Br - Dissolved in N,N-dimethylformamide solvent and then added dropwise into toluene solvent, CsPbBr3 quantum dot dispersion can be obtained after purification, and the quantum efficiency is close to 95%. This method has certain advantages in terms of simple operation and low equipment requirements, but it has significant disadvantages in terms of crystal quality, size control, reaction speed, stability and batch repeatability.
[0004] Therefore, the existing perovskite quantum dot synthesis methods can be summarized as follows:
[0005] The high-temperature crystallization method has extremely strict requirements on the control of reaction parameters. Conditions such as temperature and reaction environment uniformity will greatly affect the crystallization quality and product uniformity. It has high requirements on equipment and is difficult to scale up for mass production. At the same time, the precursor materials crystallized in this method are limited and cannot be fully utilized, resulting in a large amount of cost waste;
[0006] The room temperature supersaturated crystallization method has low crystal quality, a large number of defects that seriously affect the performance, and difficulty in controlling size and morphology. The reaction rate is slow and the batch repeatability is poor. In addition, there is also the problem of low yield and inability to fully utilize the precursor material.
[0007] These shortcomings limit their application in high-performance optoelectronic devices, and it is necessary to improve the quality and performance of perovskite quantum dots by improving the process or combining other methods. Summary of the invention
[0008] Purpose of the invention: In order to overcome the shortcomings of the prior art that the size of perovskite quantum dots is difficult to stably control and the particle size distribution is too wide and difficult to achieve continuous batch production, a method and a synthesis device for synthesizing perovskite quantum dots with controllable size and suitable for continuous production are provided, and a supercritical CO2-assisted method is used for the synthesis of perovskite quantum dots. The perovskite quantum dots have many advantages such as small size, stable and controllable size, and suitable for continuous batch production.
[0009] Technical solution: To achieve the above-mentioned purpose, the present invention provides a size-controllable perovskite quantum dot synthesis device suitable for continuous production, including a main pipeline, a CO2 cylinder, at least two precursor raw material bins, at least two product collecting bins, a product tank and a back pressure valve, the CO2 cylinder and the precursor raw material bin are connected to the main pipeline through a first branch pipeline and a second branch pipeline respectively, the first branch pipeline and the second branch pipeline are respectively provided with a high-pressure large-flow pump and a high-pressure constant-volume double-plunger pump, the first branch pipeline is provided with an electric heater, all the product collecting bins are connected to the main pipeline in parallel through a third branch pipeline, switching valves are provided between the product collecting bins, a piston is provided in the product collecting bin, the product collecting bin is divided into a pure water chamber and a collecting chamber by the piston, the pure water chamber is connected to the pure water bin through a constant pressure pump, the collecting chamber is connected to the product tank through a collecting valve, and the back pressure valve is respectively connected to the main pipeline and the pure water chamber of the product collecting bin.
[0010] Furthermore, the third branch pipeline is provided with an ultrafast cooling module for directly restoring the supercritical mixed fluid to a solution state through a subcritical state.
[0011] Furthermore, a filter module is provided on the pipeline of the back pressure valve for filtering the product mixed in the pure water.
[0012] Based on the above-mentioned perovskite quantum dot synthesis device, the present invention also provides a size-controllable perovskite quantum dot synthesis method suitable for continuous production, comprising the following steps:
[0013] S1: respectively preparing different types of precursor solutions of predetermined concentrations of perovskite precursors, adding a predetermined amount of ligands to the precursor solutions, and then respectively introducing them into the precursor raw material bin for standby use;
[0014] S2: Set the system pressure through the back pressure valve, evacuate the system, and then extract the liquid CO2 in the CO2 cylinder with a large flow high-pressure pump, and heat the extracted liquid CO2 with an electric heater to quickly reach a supercritical state;
[0015] S3: The precursor solution in the precursor raw material bin is heated to a specified temperature, and injected into the main pipeline at a stable speed under the action of a high-pressure constant-volume double-plunger pump. The precursor solution and the ligand are fully and evenly mixed with the supercritical CO2 in the main pipeline to form a mixed fluid. Under the action of the system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid.
[0016] S4: The supercritical mixed fluid passes through the subcritical state and directly returns to the solution state under the cooling effect of the ultrafast cooling module, and then enters the collection chamber of the product collection bin;
[0017] S5: When the pressure in the collection chamber exceeds the pressure in the pure water chamber, the solution in the collection chamber pushes the piston up to the limit mark, that is, the chamber is full, and then the switching valve switches the flow direction, and the solution enters the collection chamber of other products;
[0018] S6: The constant pressure pump pumps the water in the pure water tank out to the pure water chamber, and at the same time opens the collection valve. Under the action of water pressure, the piston moves downward, and the solution in the full collection chamber is pressed into the product tank;
[0019] S7: Open the discharge valve of the product tank to obtain a crude dispersion of perovskite quantum dots;
[0020] S8: Refining and purifying the crude perovskite quantum dot dispersion to obtain a fine perovskite quantum dot dispersion.
[0021] Further, the precursor solution in step S1 includes precursor solution A and precursor solution B;
[0022] The preparation method of the precursor solution A is as follows: weigh cesium carbonate and add it into a three-necked bottle, add octadecene and oleic acid at the same time, start magnetic stirring and evacuate with a vacuum pump, heat to a specified temperature and then keep the temperature, continue to heat and keep the temperature, fill the system with N2 protective gas, evacuate again, repeat this process N times, keep the temperature for later use, and use the solution at this time as the precursor solution A;
[0023] The preparation method of precursor solution B is as follows: weigh raw material B and octadecene and add them into a three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to a specified temperature and then keep warm, continue to heat and keep warm, fill the system with N2 protective gas; use a syringe to extract oleic acid and oleylamine respectively, inject them into the reaction liquid, re-evacuate the system until there are no bubbles, then fill with N2 protective gas and cool to a specified temperature range, and the solution at this time is used as precursor solution B.
[0024] The raw material B may be one of lead bromide, lead iodide and lead chloride.
[0025] Furthermore, the setting range of the system pressure in step S2 is 7.4-30 MPa.
[0026] Furthermore, in the step S2, only CO2 may be used in the CO2 cylinder, or other solvents may be mixed into the CO2 cylinder to change the critical point of the mixed system, and the other solvents include at least one of (water or lower alcohols); the conditions for CO2 to quickly reach a supercritical state include a temperature exceeding 31°C and a pressure exceeding 7.4MPa.
[0027] Furthermore, in step S3, the precursor solution A and the precursor solution B are heated to 120° C., and then the precursor solution A is injected into the main pipe at a rate of 1.6 ml / min, and the precursor solution B is injected into the main pipe at a rate of 10 ml / min.
[0028] The precursor solution A and precursor solution B injected in step S3 of the present invention and supercritical CO2 almost completely precipitate perovskite quantum dot crystal nuclei surrounded by ligands or modifier molecules at the moment of mixing. At the same time, due to the limitation of raw materials, the crystal nuclei cannot complete effective growth, so they have the characteristics of small size and narrow particle size distribution.
[0029] Furthermore, in step S4, a certain temperature and pressure are simultaneously met, and the sample is in a supercritical state, which can achieve ultra-fast crystallization. However, when collecting the sample, it must be kept at room temperature and pressure, and the process needs to pass through a subcritical state. In this state, the grains are unstable, so it is necessary to cool down quickly to keep the subcritical state as short as possible. The ultra-fast cooling module can achieve direct recovery to the solution state through the subcritical state, minimizing the time in the subcritical state.
[0030] Furthermore, in step S5, the solution that passes through the piston and enters the pure water chamber is filtered and recovered by the filtering module.
[0031] Furthermore, the step S8 is specifically as follows: adding a predetermined solvent to the crude perovskite quantum dot product and transferring it to a centrifuge tube, washing it with high-speed shaking, and then centrifuging it under specified conditions of an ultra-high-speed centrifuge, removing the supernatant, and then adding the predetermined solvent to the centrifuge tube. After repeated washing and ultra-high-speed centrifugation treatment for more than 3 times, a refined perovskite quantum dot dispersion containing a ligand or an organic small molecule modifier is obtained.
[0032] When synthesizing the perovskite nanocrystals in the present invention, the solubility of a mixed solvent of a large excess of supercritical CO2 and a small amount of organic solvent on small molecule compounds and the high uniform dispersion characteristics of small molecule compounds in the mixed solvent are utilized. By controlling the pressure of the supercritical mixed fluid, CO2 is separated from the supercritical mixed fluid, and the solubility of the perovskite molecular structure in a small amount of organic solvent is sharply reduced, and the perovskite molecular structure has to be instantly precipitated from the organic solvent in the form of nanocrystals. The surface of the perovskite nanocrystal can selectively form a stable surface passivation layer and a required surface modification effect while the nanocrystal is precipitated, thereby simultaneously ensuring the higher dimensional stability, higher luminous efficiency, narrower half-peak width (better monochromaticity, higher color purity) and high stability of the nanocrystal as a quantum dot luminescent material, as well as high dispersibility and independent dispersion effect in a predetermined resin dispersion. The use of supercritical CO2 reduces the amount of organic solvents used in conventional perovskite quantum dot synthesis methods. Compared with traditional perovskite quantum dot synthesis methods, it reduces material costs and environmental impact, and can obtain smaller particle sizes and narrower particle size distributions. In addition, it can freely select small molecules that have surface passivation and coordination effects on perovskite molecules to implement stable surface modification on the perovskite surface, which can greatly improve the stability of perovskite crystals.
[0033] In the present invention, the perovskite precursor can quickly reach a supersaturated state to a great extent under a supercritical CO2 environment, so that the supersaturation of the perovskite quantum dots in the supercritical fluid is particularly high, and the precursor solution A and the precursor solution B in the supercritical fluid collide at the moment of precipitation from the supercritical fluid as a crystal nucleus. Because the supercritical fluid is a super-uniform reaction field at the molecular level, the crystal nucleus is uniformly precipitated in the supercritical fluid at all places at the same time, and the perovskite quantum dots have quickly completed the reaction under conditions that are not conducive to nuclear growth. Therefore, the method of the present invention can obtain small-sized quantum dot materials (for example, within a particle size of 10nm, or even within 5nm) that are not easy to obtain by existing synthesis methods, and the quantum dot particle size distribution is narrower. In addition, since the mixing of excess supercritical CO2 and lower alcohols can dissolve numerous small molecule compounds, the surface passivation and surface modification of various perovskite quantum dots have many selectable combinations, and the perovskite quantum dots can also easily achieve independent dispersion in different dispersing solvents because of the selection of appropriate modified molecules, thereby improving their optical properties. The quantum efficiency of perovskite quantum dots will be affected by the surface or internal defects of the quantum dots. Appropriate ligand molecules can not only reduce the surface defects of quantum dots, thereby improving the quantum efficiency of quantum dot luminescence, but also improve the optical properties and stability of quantum dot crystals.
[0034] The perovskite quantum dot material synthesized by the present invention comprises a perovskite structure crystal and a ligand on the surface of the crystal and a modified small molecule compound, wherein the perovskite structure crystal is represented by the following general formula (P1):
[0035] ABCl 3-x-y Br x I y :M n+ ······(P1)
[0036] Wherein, A represents at least one alkali metal cation (Cs) and one organic cation (FA: formamidine, MA: methylamine); B represents at least one divalent metal cation of Pb, Sn, Ge, Zn, Cu; M n+ is a cation of at least one metal element selected from the group consisting of Ge, Sn, Pb, Sb, Bi, Cu, Ni, Co, Fe, Mn, Cr, Pd, Cd, Eu, Yb and Ag; 0≤x≤3, 0≤y≤3;
[0037] The perovskite structure compounds described in the present invention include MAPbI3, MASnI3, MAPbBr3, MASnBr3, MAPbCl3, MASnCl3, FAPbI3, FAPbI3, FASnI3, FAPbBr3, FAPbBr2I, FASnBr3, FAPbCl3, FASnCl3, FASnBr2I, CsPbI3, CsSnI3, CSPbBr3, CsSnBr3, CsPbCl3, CsSnCl3, RbPbI3, RbSnI3, RbPbBr3, RbSnBr3, RbPbCl3 and RbSnCl3, etc.
[0038] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0039] 1. The supercritical CO2-assisted method is used. Since the supercritical CO2 environment itself has the characteristics of uniformity, high solubility and stability, it can avoid the differentiation of the reaction environment of the precursor material, so that the crystallization process is almost under the same conditions, thereby avoiding the difference in the size of quantum dots and achieving better crystal quality;
[0040] 2. Under the supercritical CO2 environment, the precursor material can instantly reach a state of extreme supersaturation, so almost all the precursor materials can be crystallized to form crystal nuclei, avoiding material waste. At the same time, there is no more material to complete crystal growth, thereby achieving the purpose of cutoff reaction and controlling the size of quantum dot nanocrystals;
[0041] 3. The synthesis equipment proposed in the present invention has a microchannel and a plurality of switchable piston-type collection chambers, which can realize uninterrupted continuous batch production while collecting products, and also avoid the problem of batch product differences caused by batch production;
[0042] 4. The scheme of using supercritical CO2-assisted method to continuously batch prepare perovskite quantum dots can also be applied to the regulation method of traditional perovskite quantum dot preparation. The performance of quantum dots can be improved by adjusting parameters such as ligands, stoichiometric ratios, and reaction conditions. It has good universality and is suitable for mass production, which will help promote the industrialization process. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 Schematic diagram of the perovskite quantum dot synthesis device provided by the present invention. DETAILED DESCRIPTION
[0044] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0045] Embodiment 1:
[0046] like Figure 1 As shown, the present embodiment provides a size-controllable perovskite quantum dot synthesis device suitable for continuous production, including a main pipeline 100, a CO2 cylinder 1, a precursor raw material warehouse A4, a precursor raw material warehouse B5, a first product collection warehouse 104, a second product collection warehouse 105, a product tank 19, a back pressure valve 14, and a pure water warehouse 16. Supercritical CO2 liquid is stored in the CO2 cylinder 1. The CO2 cylinder 1 is connected to the inlet end of the main pipeline 100 through a first branch pipeline 101. The first product collection warehouse 104 and the second product collection warehouse 105 are connected to the outlet end of the main pipeline 100 in parallel through a third branch pipeline 103. The precursor raw material warehouse A4 and the precursor raw material warehouse B5 are both connected to the main pipeline 100 through a second branch pipeline 102. The connection positions of the precursor raw material warehouse A4 and the precursor raw material warehouse B5 in the main pipeline 100 are positions T1 and T2 respectively. Positions T1 and T2 are close to each other. The first branch pipeline 101 and the second branch pipeline A high-pressure, large-flow pump 2 and a high-pressure, constant-volume, double-plunger pump 6 are respectively provided on 102, an electric heater 3 is provided on the first branch pipeline 101, the outlet end of the main pipeline 100 is position T3, an ultra-fast cooling module 7 is provided on the third branch pipeline 103 near position T3, a switching valve 8 is provided between the first product collecting bin 104 and the second product collecting bin 105, a piston 11 is provided in the first product collecting bin 104 and the second product collecting bin 105, the product collecting bin is divided into a pure water chamber 12 and a collecting chamber 9 by the piston 11, the pure water chamber 12 is connected to the pure water bin 16 through a constant-pressure pump 15, the back pressure valve 14 is respectively connected to the system pipeline and the pure water chamber 12 of the product collecting bin, a filtering module 13 is provided on the pipeline of the back pressure valve 14, the bottom discharge ends of the first product collecting bin 104 and the second product collecting bin 105 are respectively provided with a first collecting valve 17 and a second collecting valve 18, and a discharge valve 20 is provided at the bottom of the product tank 19.
[0047] Embodiment 2:
[0048] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbBr3 green light quantum dots. Figure 1 , the specific synthesis process is:
[0049] 1) Weigh 1g of cesium carbonate and add it to a 500ml three-necked flask, add 100ml of octadecene and 7ml of oleic acid, turn on magnetic stirring and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, record it as precursor A, and load it into precursor raw material bin A4;
[0050] 2) Weigh 1.38g of lead bromide and 100ml of octadecene into a 500ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0051] 3) Use a syringe to extract 45 ml of oleic acid and 45 ml of oleylamine as ligands, respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C. This is recorded as precursor B and loaded into the precursor raw material bin B5;
[0052] 4) The closed reaction system is set to a system pressure of 7.4 MPa through the back pressure valve 14, the main line 100 is heated to no more than 150° C. through the heating jacket, and after evacuation, the high-flow high-pressure pump 2 is started to extract the CO2 in the CO2 cylinder 1, and the extracted liquid CO2 is heated by the electric heater 3 to quickly reach a supercritical state;
[0053] 5) Precursor solution A and precursor solution B are heated to 120° C., and then two high-pressure constant volume double plunger pumps 6 are used to respectively inject precursor solution A into the main pipe 100 at position T1 at a speed of 1.6 ml / min, and precursor solution B is injected into the main pipe 100 at position T2 at a speed of 10 ml / min. After the precursor solution A and the precursor solution B are injected, they are fully and evenly mixed with supercritical CO2 to form a mixed fluid, and under the action of system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid;
[0054] Among them, the precursor solution A and the precursor solution B and the supercritical CO2 almost completely precipitate the perovskite quantum dot crystal nuclei surrounded by ligands at the moment of mixing. At the same time, due to the limitation of raw materials, the crystal nuclei cannot complete effective growth, so they have the characteristics of small size and narrow particle size distribution.
[0055] 6) The supercritical mixed fluid passes through the subcritical state and directly recovers to the solution state under the cooling effect of the ultrafast cooling module 7, and then the solution enters the collection chamber 9 of the first product collection chamber 104 through the switching valve 8. When the pressure in the collection chamber 9 exceeds the pressure in the pure water chamber 12, the piston 11 in the collection chamber 9 is continuously pushed up to the limit mark, that is, the full-storage state is reached, and the constant-pressure pump 15 pumps the water in the pure water chamber 16 out to the pure water chamber 12, and at the same time opens the first collection valve 17. Under the action of water pressure, the piston 11 moves downward, and the solution in the collection chamber 9 of the first product collection chamber 104 in the full-storage state is pressed into the product tank 19;
[0056] At the same time, the switching valve 8 switches the flow direction, and the solution enters the second product collection chamber 105 and repeats the same process, thereby achieving continuous and uninterrupted recovery of the product.
[0057] 7) During the execution of step 6, a small amount of solution will pass through the piston 11 and enter the pure water chamber 12, and the solution can be filtered and recovered through the filter module 13;
[0058] 8) Open the discharge valve 20 of the product tank 19 to obtain a crude dispersion of perovskite quantum dots, and add the filtered portion in step 7 to obtain a crude CsPbBr3 product;
[0059] 9) Take 10 ml of CsPbBr3 crude product, add 40 ml of methyl acetate and stir for 5 min, centrifuge it at 8000 rpm for 5 min, take the precipitate, add 10 ml of n-hexane to disperse it, centrifuge it at 5000 rpm again for 3 min, and take the supernatant, which is the CsPbBr3 green light quantum dot dispersion.
[0060] Embodiment 3:
[0061] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbI3 red light quantum dots. Figure 1 , the specific synthesis process is:
[0062] 1) Weigh 1g of cesium carbonate and add it to a 500ml three-necked flask, add 100ml of octadecene and 7ml of oleic acid, turn on magnetic stirring and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, record it as precursor A, and load it into precursor raw material bin A4;
[0063] 2) Weigh 1.73 g of lead iodide and 100 ml of octadecene into a 500 ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100 ° C and keep warm for 1 h, continue to heat to 120 ° C and keep warm for 15 min, and fill the system with N2 protective gas for 5 min;
[0064] 3) Use a syringe to extract 45 ml of oleic acid and 45 ml of oleylamine as ligands, respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C. This is recorded as precursor B and loaded into the precursor raw material bin B5;
[0065] 4) The closed reaction system is set to a system pressure of 30 MPa through the back pressure valve 14, the main line 100 is heated to no more than 150° C. through the heating jacket, and after evacuation, the high-flow high-pressure pump 2 is started to extract the CO2 in the CO2 cylinder 1, and the extracted liquid CO2 is heated by the electric heater 3 to quickly reach a supercritical state;
[0066] 5) Precursor solution A and precursor solution B are heated to 120° C., and then two high-pressure constant volume double plunger pumps 6 are used to respectively inject precursor solution A into the main pipe 100 at position T1 at a speed of 1.6 ml / min, and precursor solution B is injected into the main pipe 100 at position T2 at a speed of 10 ml / min. After the precursor solution A and the precursor solution B are injected, they are fully and evenly mixed with supercritical CO2 to form a mixed fluid, and under the action of system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid;
[0067] Among them, the precursor solution A and the precursor solution B and the supercritical CO2 almost completely precipitate the perovskite quantum dot crystal nuclei surrounded by ligands at the moment of mixing. At the same time, due to the limitation of raw materials, the crystal nuclei cannot complete effective growth, so they have the characteristics of small size and narrow particle size distribution.
[0068] 6) The supercritical mixed fluid passes through the subcritical state and directly recovers to the solution state under the cooling effect of the ultrafast cooling module 7, and then the solution enters the collection chamber 9 of the first product collection chamber 104 through the switching valve 8. When the pressure in the collection chamber 9 exceeds the pressure in the pure water chamber 12, the piston 11 in the collection chamber 9 is continuously pushed up to the limit mark, that is, the full-storage state is reached, and the constant-pressure pump 15 pumps the water in the pure water chamber 16 out to the pure water chamber 12, and at the same time opens the first collection valve 17. Under the action of water pressure, the piston 11 moves downward, and the solution in the collection chamber 9 of the first product collection chamber 104 in the full-storage state is pressed into the product tank 19;
[0069] At the same time, the switching valve 8 switches the flow direction, and the solution enters the second product collection chamber 105 and repeats the same process, thereby achieving continuous and uninterrupted recovery of the product.
[0070] 7) During the execution of step 6, a small amount of solution will pass through the piston 11 and enter the pure water chamber 12, and the solution can be filtered and recovered through the filter module 13;
[0071] 8) Open the discharge valve 20 of the product tank 19 to obtain a crude dispersion of perovskite quantum dots, and add the filtered portion in step 7 to obtain a crude CsPbI3 product;
[0072] 9) Take 10 ml of CsPbI3 crude product, add 40 ml of methyl acetate and stir for 5 min, put it into a centrifuge and centrifuge it at 8000 rpm for 5 min, take the precipitate, add 10 ml of n-hexane to disperse it, put it into a centrifuge again and centrifuge it at 5000 rpm for 3 min, and take the supernatant, which is the CsPbI3 red light quantum dot dispersion.
[0073] Embodiment 4:
[0074] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbBr3 green light quantum dots. Figure 1 , the specific synthesis process is:
[0075] 1) Weigh 1g of cesium carbonate and add it to a 500ml three-necked bottle, add 100ml of octadecene and 7g of 4-dodecylbenzenesulfonic acid at the same time, turn on magnetic stirring and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, record it as precursor A, and load it into precursor raw material bin A4;
[0076] 2) Weigh 1.38g of lead bromide and 100ml of octadecene into a 500ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0077] 3) Use a syringe to extract 45g of 4-dodecylbenzenesulfonic acid as a ligand and inject it into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C. This is recorded as precursor B and loaded into the precursor raw material bin B5;
[0078] 4) The closed reaction system is set to a system pressure of 10 MPa through the back pressure valve 14, the main pipeline 100 is heated to no more than 150° C. through the heating jacket, and after evacuation, the high-flow high-pressure pump 2 is started to extract the CO2 in the CO2 cylinder 1, and the extracted liquid CO2 is heated by the electric heater 3 to quickly reach a supercritical state;
[0079] 5) Precursor solution A and precursor solution B are heated to 120° C., and then two high-pressure constant volume double plunger pumps 6 are used to respectively inject precursor solution A into the main pipe 100 at position T1 at a speed of 1.6 ml / min, and precursor solution B is injected into the main pipe 100 at position T2 at a speed of 10 ml / min. After the precursor solution A and the precursor solution B are injected, they are fully and evenly mixed with supercritical CO2 to form a mixed fluid, and under the action of system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid;
[0080] Among them, the precursor solution A and the precursor solution B and the supercritical CO2 almost completely precipitate the perovskite quantum dot crystal nuclei surrounded by ligands at the moment of mixing. At the same time, due to the limitation of raw materials, the crystal nuclei cannot complete effective growth, so they have the characteristics of small size and narrow particle size distribution.
[0081] 6) The supercritical mixed fluid passes through the subcritical state and directly recovers to the solution state under the cooling effect of the ultrafast cooling module 7, and then the solution enters the collection chamber 9 of the first product collection chamber 104 through the switching valve 8. When the pressure in the collection chamber 9 exceeds the pressure in the pure water chamber 12, the piston 11 in the collection chamber 9 is continuously pushed up to the limit mark, that is, the full-storage state is reached, and the constant-pressure pump 15 pumps the water in the pure water chamber 16 out to the pure water chamber 12, and at the same time opens the first collection valve 17. Under the action of water pressure, the piston 11 moves downward, and the solution in the collection chamber 9 of the first product collection chamber 104 in the full-storage state is pressed into the product tank 19;
[0082] At the same time, the switching valve 8 switches the flow direction, and the solution enters the second product collection chamber 105 and repeats the same process, thereby achieving continuous and uninterrupted recovery of the product.
[0083] 7) During the execution of step 6, a small amount of solution will pass through the piston 11 and enter the pure water chamber 12, and the solution can be filtered and recovered through the filter module 13;
[0084] 8) Open the discharge valve 20 of the product tank 19 to obtain a crude dispersion of perovskite quantum dots, and add the filtered portion in step 7 to obtain a crude CsPbBr3 product;
[0085] 9) Take 10 ml of CsPbBr3 crude product, add 40 ml of methyl acetate and stir for 5 min, centrifuge it at 8000 rpm for 5 min, take the precipitate, add 10 ml of n-hexane to disperse it, centrifuge it at 5000 rpm again for 3 min, and take the supernatant, which is the CsPbBr3 green light quantum dot dispersion.
[0086] Embodiment 5:
[0087] In this embodiment, the perovskite quantum dot synthesis device in Example 1 is used to synthesize CsPbCl3 blue light quantum dots. Figure 1 , the specific synthesis process is:
[0088] 1) Weigh 1g of cesium carbonate and add it to a 500ml three-necked flask, add 100ml of octadecene and 7ml of oleic acid, turn on magnetic stirring and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, record it as precursor A, and load it into precursor raw material bin A4;
[0089] 2) Weigh 1.31 g of lead chloride and 100 ml of octadecene into a 500 ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100 ° C and keep warm for 1 h, continue to heat to 120 ° C and keep warm for 15 min, and fill the system with N2 protective gas for 5 min;
[0090] 3) Use a syringe to extract 45 ml of oleic acid and 45 ml of oleylamine as ligands, respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C. This is recorded as precursor B and loaded into the precursor raw material bin B5;
[0091] 4) The closed reaction system is set to a system pressure of 20 MPa through the back pressure valve 14, the main pipeline 100 is heated to no more than 150° C. through the heating jacket, and after evacuation, the high-flow high-pressure pump 2 is started to extract the CO2 in the CO2 cylinder 1, and the extracted liquid CO2 is heated by the electric heater 3 to quickly reach a supercritical state;
[0092] 5) Precursor solution A and precursor solution B are heated to 120° C., and then two high-pressure constant volume double plunger pumps 6 are used to respectively inject precursor solution A into the main pipe 100 at position T1 at a speed of 1.6 ml / min, and precursor solution B is injected into the main pipe 100 at position T2 at a speed of 10 ml / min. After the precursor solution A and the precursor solution B are injected, they are fully and evenly mixed with supercritical CO2 to form a mixed fluid, and under the action of system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid;
[0093] Among them, the precursor solution A and the precursor solution B and the supercritical CO2 almost completely precipitate the perovskite quantum dot crystal nuclei surrounded by ligands at the moment of mixing. At the same time, due to the limitation of raw materials, the crystal nuclei cannot complete effective growth, so they have the characteristics of small size and narrow particle size distribution.
[0094] 6) The supercritical mixed fluid passes through the subcritical state and directly recovers to the solution state under the cooling effect of the ultrafast cooling module 7, and then the solution enters the collection chamber 9 of the first product collection chamber 104 through the switching valve 8. When the pressure in the collection chamber 9 exceeds the pressure in the pure water chamber 12, the piston 11 in the collection chamber 9 is continuously pushed up to the limit mark, that is, the full-storage state is reached, and the constant-pressure pump 15 pumps the water in the pure water chamber 16 out to the pure water chamber 12, and at the same time opens the first collection valve 17. Under the action of water pressure, the piston 11 moves downward, and the solution in the collection chamber 9 of the first product collection chamber 104 in the full-storage state is pressed into the product tank 19;
[0095] At the same time, the switching valve 8 switches the flow direction, and the solution enters the second product collection chamber 105 and repeats the same process, thereby achieving continuous and uninterrupted recovery of the product.
[0096] 7) During the execution of step 6, a small amount of solution will pass through the piston 11 and enter the pure water chamber 12, and the solution can be filtered and recovered through the filter module 13;
[0097] 8) Open the discharge valve 20 of the product tank 19 to obtain a crude dispersion of perovskite quantum dots, and add the filtered portion in step 7 to obtain a crude CsPbBr3 product;
[0098] 9) Take 10 ml of CsPbBr3 crude product, add 40 ml of methyl acetate and stir for 5 min, centrifuge it at 8000 rpm for 5 min, take the precipitate, add 10 ml of n-hexane to disperse it, centrifuge it at 5000 rpm again for 3 min, and take the supernatant, which is the CsPbCl3 blue light quantum dot dispersion.
[0099] Comparative Example 1:
[0100] In this example, the existing normal hot injection method is used to synthesize CsPbBr3 quantum dots. The specific synthesis process is as follows:
[0101] 1) Weigh 0.1g of cesium carbonate and add it to a 50ml three-necked bottle, add 10ml of octadecene and 0.7ml of oleic acid, start magnetic stirring and evacuate with a vacuum pump, heat to 100℃ and keep warm for 1h, continue to heat to 120℃ and keep warm for 15min, fill the system with N2 protective gas for 5min, evacuate again, repeat this process 3 times, finally cool to 50℃, take out and bottle for use, recorded as precursor A;
[0102] 2) Weigh 0.138g of lead bromide and 10ml of octadecene into a 50ml three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to 100°C and keep warm for 1h, continue to heat to 120°C and keep warm for 15min, and fill the system with N2 protective gas for 5min;
[0103] 3) Use a syringe to extract 4.5 ml of oleic acid and 4.5 ml of oleylamine respectively, and inject them into the reaction solution in step 2. The system is evacuated again until there are no bubbles, and then filled with N2 protective gas and cooled to 110°C;
[0104] 4) Reheat the precursor A to 120°C and inject 1.6 ml of it into the reaction solution in step 3 using a syringe, and quickly cool the system to room temperature using an ice water bath;
[0105] 5) Take out the reaction solution in step 4, add 40 ml of methyl acetate and stir for 5 minutes, put it into a centrifuge and centrifuge it at 8000 rpm for 5 minutes, take out the precipitate and add 10 ml of n-hexane, centrifuge it again at 5000 rpm for 3 minutes, and take the supernatant, which is the CsPbBr3 quantum dots.
[0106] Comparative Example 2:
[0107] In this example, the existing room temperature anti-solvent method is used to synthesize CsPbBr3 quantum dots. The specific synthesis process is as follows:
[0108] 1) Weigh 0.08 g of cesium bromide, 0.138 g of lead bromide, 4.5 ml of oleylamine, 4.5 ml of oleic acid, and 10 ml of dimethyl sulfoxide into a 50 ml beaker and stir magnetically until completely dissolved, which is recorded as precursor A;
[0109] 2) Weigh 50 ml of toluene into a 100 ml beaker, quickly add precursor A, and stir evenly;
[0110] 3) The reaction solution in step 2 was placed in a centrifuge and centrifuged at 8000 rpm for 5 min. The precipitate was added with 10 ml of n-hexane and centrifuged again at 5000 rpm for 3 min. The supernatant was taken, which was the CsPbBr3 quantum dots.
[0111] In the present invention, the performance of the perovskite quantum dots obtained in Examples 2 to 5 and Comparative Examples 1 and 2 is compared and analyzed, as shown in Table 1:
[0112] Table 1 Performance comparison of perovskite quantum dots obtained in the examples and comparative examples
[0113]
[0114] It can be seen from the data in Table 1 that by comparing the parameters of the quantum dots obtained in Examples 2-5 and Comparative Examples 1 and 2, the synthesis scheme proposed in the present invention has a higher yield, a smaller quantum dot size, and a more uniform size distribution, which makes the half-width of the luminescence peak narrower and has better monochromaticity. Examples 2 to 5 illustrate that this scheme is not only applicable to green perovskite quantum dots, but also to red and blue perovskite quantum dots.
[0115] In addition, the synthesis scheme proposed in the present invention can be continuously mass-produced to avoid batch differences and enhance production capacity.
Claims
1. A size-controllable perovskite quantum dot synthesis device suitable for continuous production, characterized in that: It includes a main pipeline, a CO2 cylinder, at least two precursor raw material bins, at least two product collecting bins, a product tank and a back pressure valve, the CO2 cylinder and the precursor raw material bin are connected to the main pipeline through a first branch pipeline and a second branch pipeline respectively, the first branch pipeline and the second branch pipeline are respectively provided with a high-pressure large-flow pump and a high-pressure constant-volume double-plunger pump, the first branch pipeline is provided with an electric heater, all the product collecting bins are connected to the main pipeline in parallel through a third branch pipeline, switching valves are provided between the product collecting bins, a piston is provided in the product collecting bin, the product collecting bin is divided into a pure water chamber and a collecting chamber by the piston, the pure water chamber is connected to the pure water bin through a constant pressure pump, the collecting chamber is connected to the product tank through a collecting valve, and the back pressure valve is respectively connected to the main pipeline and the pure water chamber of the product collecting bin.
2. A size-controllable perovskite quantum dot synthesis device suitable for continuous production according to claim 1, characterized in that: The third branch pipeline is provided with an ultrafast cooling module for directly restoring the supercritical mixed fluid to a solution state through a subcritical state.
3. A size-controllable perovskite quantum dot synthesis device suitable for continuous production according to claim 1, characterized in that: A filter module is arranged on the pipeline of the back pressure valve.
4. A method for synthesizing perovskite quantum dots with controllable size and suitable for continuous production, characterized in that: The steps include: S1: respectively preparing different types of precursor solutions of predetermined concentrations of perovskite precursors, adding a predetermined amount of ligands to the precursor solutions, and then respectively introducing them into the precursor raw material bin for standby use; S2: Set the system pressure through the back pressure valve, evacuate the system, and then extract the liquid CO2 in the CO2 cylinder with a large flow high-pressure pump, and heat the extracted liquid CO2 with an electric heater to quickly reach a supercritical state; S3: The precursor solution in the precursor raw material bin is heated to a specified temperature, and injected into the main pipeline at a stable speed under the action of a high-pressure constant-volume double-plunger pump. The precursor solution and the ligand are fully and evenly mixed with the supercritical CO2 in the main pipeline to form a mixed fluid. Under the action of the system pressure and temperature, the mixed fluid can maintain a supercritical state to form a supercritical mixed fluid. S4: The supercritical mixed fluid passes through the subcritical state and directly returns to the solution state under the cooling effect of the ultrafast cooling module, and then enters the collection chamber of the product collection bin; S5: When the pressure in the collection chamber exceeds the pressure in the pure water chamber, the solution in the collection chamber pushes the piston up to the limit mark, that is, the chamber is full, and then the switching valve switches the flow direction, and the solution enters the collection chamber of other products; S6: The constant pressure pump pumps the water in the pure water tank out to the pure water chamber, and at the same time opens the collection valve. Under the action of water pressure, the piston moves downward, and the solution in the full collection chamber is pressed into the product tank; S7: Open the discharge valve of the product tank to obtain a crude dispersion of perovskite quantum dots; S8: Refining and purifying the crude perovskite quantum dot dispersion to obtain a fine perovskite quantum dot dispersion.
5. A size-controllable perovskite quantum dot synthesis method suitable for continuous production according to claim 4, characterized in that: In step S1, the precursor solution includes a precursor solution A and a precursor solution B; The preparation method of the precursor solution A is as follows: weigh cesium carbonate and add it into a three-necked bottle, add octadecene and oleic acid at the same time, start magnetic stirring and evacuate with a vacuum pump, heat to a specified temperature and then keep the temperature, continue to heat and keep the temperature, fill the system with N2 protective gas, evacuate again, repeat this process N times, keep the temperature for later use, and use the solution at this time as the precursor solution A; The preparation method of precursor solution B is as follows: weigh raw material B and octadecene and add them into a three-necked flask, stir magnetically and evacuate with a vacuum pump, heat to a specified temperature and then keep warm, continue to heat and keep warm, fill the system with N2 protective gas; use a syringe to extract oleic acid and oleylamine respectively, inject them into the reaction liquid, re-evacuate the system until there are no bubbles, then fill with N2 protective gas and cool to a specified temperature range, and the solution at this time is used as precursor solution B.
6. A method for synthesizing perovskite quantum dots with controllable size and suitable for continuous production according to claim 4, characterized in that: The setting range of the system pressure in step S2 is 7.4-30 MPa.
7. A size-controllable perovskite quantum dot synthesis method suitable for continuous production according to claim 6, characterized in that: The conditions for CO2 to quickly reach a supercritical state in step S2 include a temperature exceeding 31° C. and a pressure exceeding 7.4 MPa.
8. The method for synthesizing perovskite quantum dots with controllable size and suitable for continuous production according to claim 5, characterized in that: In step S3, the precursor solution A and the precursor solution B are heated to 120° C., and then the precursor solution A is injected into the main pipe at a rate of 1.6 ml / min, and the precursor solution B is injected into the main pipe at a rate of 10 ml / min.
9. A method for synthesizing perovskite quantum dots with controllable size and suitable for continuous production according to claim 4, characterized in that: In step S5, the solution that passes through the piston and enters the pure water chamber is filtered and recovered by the filtering module.
10. A size-controllable perovskite quantum dot synthesis method suitable for continuous production according to claim 4, characterized in that: The step S8 specifically comprises: adding a predetermined solvent to the crude perovskite quantum dot product and transferring it to a centrifuge tube; washing it with high-speed shaking; and then centrifuging it under specified conditions of an ultra-high-speed centrifuge; removing the supernatant; and then adding the predetermined solvent to the centrifuge tube; and after repeated washing and ultra-high-speed centrifugation for more than 3 times, a refined perovskite quantum dot dispersion containing a ligand or an organic small molecule modifier is obtained.