Magnesium-calcium-based hydrolysis hydrogen production composite block material as well as preparation method and application thereof
The preparation method of hydrogen-generating composite bulk material by magnesium calcium-based hydrolysis, combined with the addition of expanded graphite and chloride and polyethylene glycol coating, the safety and convenience of magnesium calcium-based hydrogen-generating materials in humid environments are solved. Problem, improving hydrolysis performance and air tolerance.
Patent Information
- Application Number
- CN202410974780.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-05
AI Technical Summary
Magnesium-calcium-based hydrogen production materials are prone to hydrogen production in humid environments, increasing the risk of combustion and explosion, and attenuating hydrolysis performance in low-humidity environments, affecting its safety and convenience.
The hydrogen-producing composite bulk material is made of magnesium-calcium-based hydrolysis, including MgxCa1-x alloy hydride, expanded graphite and chloride. It is coated with polyethylene glycol after ball milling and hydrogenation. The bulk material is made by press molding process to improve the Hydrolysis conversion and safety.
It significantly improves the hydrolysis performance, safety and air tolerance of the material, reduces the particle size, promotes the complete hydrogenation and molding of the material, delays the contact between water molecules in the air and the material, and adapts to different environmental conditions.
Smart Images

Figure CN118894492A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrolysis hydrogen production materials, and in particular to a magnesium-calcium-based hydrolysis hydrogen production composite block material and a preparation method and application thereof. Background Art
[0002] As a clean, efficient, safe and sustainable renewable energy, hydrogen energy is regarded as the clean energy with the greatest development potential in the 21st century. However, its application is limited by three technologies: hydrogen production, hydrogen storage and hydrogen transportation. The magnesium-based material hydrolysis hydrogen production technology, which integrates online hydrogen production, storage and transportation, has become an ideal portable hydrogen source because of its advantages such as low raw material cost, high hydrogen storage density, simple operation and mild working conditions.
[0003] However, the hydrolysis of magnesium-based materials to produce hydrogen is affected by the byproduct Mg(OH)2, which usually covers the surface of the material to form a passivation layer, which prevents water from entering the interior of the particles and thus reduces the hydrolysis conversion rate. Chinese patent CN103787273A discloses a "magnesium-calcium-based hydride powder for hydrolysis and hydrogen production in a wide temperature range and its preparation method", which contains Ca4Mg3H 14 , MgH2 and Mg, among which Ca4Mg3H 14 The hydrolysis byproducts are Ca(OH)2 and Mg(OH)2. Ca(OH)2 has a higher solubility than Mg(OH)2, thus providing a channel for water to enter the particles. Compared with MgH2 and Mg, Ca4Mg3H 14 The hydrolysis conversion rate is higher, but because magnesium-calcium-based hydrides are exposed to humid air, when the humidity of the air is high, they are easy to react directly with water vapor in the air to produce hydrogen. Hydrogen is a flammable and explosive gas. Once it is produced in large quantities, it will greatly increase the risk of combustion or even explosion, which will lead to serious safety hazards. When the humidity of the air is low, it is also susceptible to poisoning by water vapor, causing its hydrolysis performance to decay. In addition, hydrogen production materials cannot be separated from convenient and efficient transfer and operation in actual use and large-scale storage and transportation. Therefore, how to solve the safety, convenience and air tolerance of magnesium-calcium-based hydrogen production materials is one of the keys to its engineering application. Summary of the invention
[0004] The present invention aims to provide a magnesium-calcium-based hydrolysis hydrogen production composite block material and a preparation method and application thereof, so as to improve the safety, convenience and air tolerance of the magnesium-calcium-based hydrogen production material.
[0005] To achieve the above object, the present invention adopts the following technical solution: a magnesium-calcium-based hydrolysis hydrogen production composite block material, comprising Mg x Ca 1-xThe mass ratios of alloy hydride, expanded graphite, chloride and polyethylene glycol are: (65-90): (2-7): (3-11): (5-17), wherein x is the mass fraction, and the value range of x is 0.7-0.9.
[0006] Preferably, the chloride is any one of aluminum chloride, ammonium chloride and calcium chloride.
[0007] Preferably, the molecular weight of polyethylene glycol is between 800-4000.
[0008] The present invention also provides another technical solution, a method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material, comprising the following steps:
[0009] S1: Mg x Ca 1-x After the alloy is crushed, expanded graphite is added and then ball milled to obtain Mg x Ca 1-x Alloy-expanded graphite composite powder material;
[0010] S2: Mg prepared in S1 x Ca 1-x The alloy-expanded graphite composite powder material is repeatedly activated and hydrogenated to obtain Mg x Ca 1-x Alloy hydride-expanded graphite composite powder material;
[0011] S3: Prepare Mg from S2 x Ca 1-x The alloy hydride-expanded graphite composite powder material is added with chloride and then ball-milled to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride composite powder material;
[0012] S4: Mg prepared in S3 by solution coating method x Ca 1-x The surface of alloy hydride-expanded graphite-chloride composite powder material is coated with polyethylene glycol to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite powder material;
[0013] S5: The Mg prepared in S4 is pressed into x Ca 1-x The alloy hydride-expanded graphite-chloride-polyethylene glycol composite powder material is pressed into blocks to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite bulk material.
[0014] Preferably, the Mg obtained in S2 x Ca 1-x The phases of alloy hydride-expanded graphite composite powder materials include Ca4Mg3H 14 and MgH2.
[0015] Preferably, in S2, the activation and hydrogenation temperature is 300-500°C and the time is 2-24h.
[0016] Preferably, in S4, the solvent of the solution coating method is acetone, Mg x Ca 1-x The ratio of the mixture of alloy hydride-expanded graphite-chloride composite powder material and polyethylene glycol to acetone is 0.5g: (10mL-20mL).
[0017] Preferably, in S3, the ball-to-material ratio of ball milling is 10:1-30:1, the rotation speed is 1200-2000 rpm, and the time is 0.5-1h.
[0018] Preferably, in S5, the pressure used in the press-molding process is 10-50 MPa, and after press-molding, the holding time is not less than 1 min.
[0019] The present invention also provides an application of a magnesium-calcium-based hydrolysis hydrogen production composite block material in hydrolysis hydrogen production.
[0020] The principle of this scheme is:
[0021] The present invention provides a magnesium-calcium-based hydrolysis hydrogen production composite block material, comprising Mg x Ca 1-x The mass ratios of alloy hydride, expanded graphite, chloride and polyethylene glycol are: (65-90): (2-7): (3-11): (5-17), wherein x is the mass fraction and the value range of x is 0.7-0.9. The preparation method is: Mg x Ca 1-x After the alloy is crushed, it is mixed with expanded graphite and ball-milled, then activated and hydrogenated, and then chloride is added and mixed with ball-milled, and then polyethylene glycol is coated on its surface by solution coating method; finally, it is pressed into blocks by pressing molding process to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite block material. The present invention provides a magnesium-calcium-based hydrolysis hydrogen production composite block material and a preparation method thereof. Due to the addition of expanded graphite, the expanded graphite is distributed as an additive in the Mg x Ca 1-xThe surface of the alloy can prevent Mg and CaMg2 from contacting each other during the ball milling process, thus improving the ball milling efficiency and reducing the particle size of the material, thereby helping to promote the complete hydrogenation of the material and improving the hydrolysis conversion rate of the material. Due to the reduction in the particle size of the material and the lubricating properties of the expanded graphite, it is more conducive to the filling and forming of the bulk material during the pressing process, making the pressed material less likely to collapse.
[0022] Due to the addition of chloride, chloride dissolves in water to form Cl - and H3O + , which makes water form a local acidic environment, can effectively destroy the byproduct Mg(OH)2 passivation layer, provide a channel for water molecules to enter the interior of the particles, and enhance the subsequent mass transfer; in addition, when chloride is dissolved in water, it will release a large amount of heat, which can improve the reaction kinetics of the micro-region, thereby promoting the hydrolysis performance of the material itself; the addition of chloride can also reduce the particle size of the material, and the smaller particle size and cracks on the particle surface observed under high magnification of SEM provide more initial reaction sites, so that the hydrolysis performance of the material itself is further improved. After pressing and molding, its hygroscopicity also improves the appearance retention of the block. The polyethylene glycol coating layer as an adhesive effectively promotes block molding and improves the appearance retention of the block, and effectively delays the direct contact between water molecules in the air and the material. In summary, the hydrolysis hydrogen production performance, safety, convenience and air tolerance of the material have been effectively improved.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Mg provided by the present invention x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite block material, polyethylene glycol coating layer and pressing molding process simultaneously improve the intrinsic safety and air poisoning resistance of the material. The polyethylene glycol coating layer thickness, molecular weight and pressing molding process parameters can be adjusted according to the exposure environment conditions (such as humidity and temperature), exposure time and other parameters to customize the suitable composite block material;
[0025] (2) Mg provided by the present invention x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite block material. The addition of expanded graphite and chloride effectively improves the hydrolysis performance of the material itself. The resulting smaller particle size and hygroscopicity of chloride are beneficial to pressing and block retention to a certain extent.
[0026] (3) The compression molding process adopted in the present invention is conducive to the convenient and efficient transfer and operation of materials during practical use and large-scale storage and transportation.
[0027] (4) The present invention adopts Mg x Ca 1-x Alloys, expanded graphite, chlorides and polyethylene glycol as raw materials have the advantage of low prices, which is conducive to the large-scale application of materials in the hydrogen energy industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The Mg-containing materials of Example 1 and Comparative Examples 1-2 of the present invention without adding expanded graphite, 3wt% expanded graphite, and 8wt% expanded graphite are respectively 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite composite powder materials;
[0029] Figure 2 Mg with 0wt%, 3wt%, and 8wt% expanded graphite added respectively in Example 1 and Comparative Examples 1-2 of the present invention 0.7 Ca 0.3 Bulk shape changes of alloy hydride-expanded graphite composite powder materials at different exposure times;
[0030] Figure 3 Mg with 0wt%, 3wt%, 6wt%, 9wt% and 12wt% AlCl3 added respectively in Examples 1-3 and Comparative Examples 3-4 of the present invention 0.7 Ca 0.3 The apparent morphology, particle size distribution and average particle size of alloy hydride-expanded graphite-AlCl3 composite powder materials;
[0031] Figure 4 Mg in which 0wt%, 6wt%, 12wt% and 18wt% of polyethylene glycol are added respectively in Example 1, Example 4 and Comparative Examples 5-6 of the present invention 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder materials;
[0032] Figure 5 Mg in which 6 wt %, 12 wt % and 18 wt % of polyethylene glycol are added respectively in Example 1, Example 4 and Comparative Example 6 of the present invention 0.7 Ca 0.3 Bulk shape change of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material;
[0033] Figure 6 Mg in Comparative Example 4 of the present invention with 12 wt% AlCl3 0.7 Ca 0.3 SEM-EDS results of alloy hydride-expanded graphite-AlCl3 composite powder materials;
[0034] Figure 7Mg added with 12 wt% polyethylene glycol in Example 1 of the present invention 0.7 Ca 0.3 XRD characterization patterns of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk materials after exposure for different times. DETAILED DESCRIPTION
[0035] The following is further described in detail through specific implementation methods:
[0036] Example 1
[0037] A magnesium-calcium-based hydrolysis hydrogen production composite block material, comprising Mg x Ca 1-x The mass ratios of alloy hydride, expanded graphite, chloride and polyethylene glycol are: (65-90): (2-7): (3-11): (5-17), wherein x is the mass fraction, and the value range of x is 0.7-0.9. x Ca 1-x The mass ratios of alloy hydride, expanded graphite, chloride, and polyethylene glycol are 77.6776:2.4024:7.92:12, respectively; the value of X is 0.7, Mg x Ca 1-x Alloy hydride is Mg 0.7 Ca 0.3 Alloy hydride.
[0038] Among them, Mg 0.7 Ca 0.3 The alloy hydride phases include Ca4Mg3H 14 and MgH2;
[0039] The manufacturer of expanded graphite is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the specification of expanded graphite is 80 mesh;
[0040] The chloride is any one of aluminum chloride, ammonium chloride and calcium chloride. In this embodiment, aluminum chloride (analytical grade) is selected as the chloride, and commercially available products can be used;
[0041] The molecular weight of polyethylene glycol is between 800 and 4000. In this embodiment, the molecular weight of polyethylene glycol is 2000, and a commercially available product can be used;
[0042] A method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material comprises the following steps:
[0043] S1: Mg 0.7 Ca 0.3 Alloy (purchased from Suzhou Chuanmao Metal Materials Co., Ltd., a specific ratio of Mg 0.7 Ca 0.3 Alloy, Mg0.7 Ca 0.3 The alloy phase includes CaMg2 and Mg) and is crushed and ground to less than 200 meshes, and expanded graphite is added, the amount of expanded graphite added is 3wt%, and high-energy ball milling is performed for 1-3h under normal pressure and argon atmosphere, the ball-to-material ratio is (10-30):1, and the rotation speed is 1200-2000 rpm to obtain Mg 0.7 Ca 0.3 Alloy-expanded graphite composite powder material, that is, Mg with 3wt% expanded graphite added 0.7 Ca 0.3 The alloy-expanded graphite composite powder material, in this embodiment, is subjected to high-energy ball milling for 2 h, the ball-to-material ratio is 20:1, the grinding balls are 3 mm and 10 mm in diameter (mass ratio is 1:1), and the rotation speed is 1800 rpm;
[0044] S2: Mg prepared in S1 0.7 Ca 0.3 The alloy-expanded graphite composite powder material is repeatedly activated and hydrogenated. Specifically, the Mg prepared in S1 0.7 Ca 0.3 The alloy-expanded graphite composite powder material is placed in a Sieverts reactor, and repeatedly activated (evacuated the reactor to a vacuum degree of 1 Pa) and hydrogenated (hydrogen is added to the reactor to maintain the hydrogen pressure at 3-4 MPa) at a temperature of 300-500°C. The repeated activation and hydrogenation process is: the activation for 60 minutes and the hydrogenation for 60 minutes are performed alternately, and the duration is 2-24 hours to obtain Mg 0.7 Ca 0.3 Alloy hydride-expanded graphite composite powder material, that is, Mg with 3wt% expanded graphite added 0.7 Ca 0.3 Alloy hydride-expanded graphite composite powder material, in this embodiment, the activation and hydrogenation temperature is 400°C and the duration is 8h;
[0045] S3: Mg prepared by adding 3wt% expanded graphite to S2 0.7 Ca 0.3 AlCl3 (analytical grade) was added to the alloy hydride-expanded graphite composite powder material, the addition amount of AlCl3 was 9wt%, and after mixing, high-energy ball milling was performed for 0.5-1h under normal pressure and argon atmosphere, the ball-to-material ratio was (10-30):1, and the rotation speed was 1200-2000 rpm to obtain Mg 0.7 Ca 0.3 Alloy hydride-expanded graphite-chloride composite powder material, that is, Mg with 9wt% AlCl3 added 0.7 Ca 0.3Alloy hydride-expanded graphite-AlCl3 composite powder material, in this embodiment, high-energy ball milling for 0.5h, ball-to-material ratio of 20:1, grinding balls with diameters of 3mm and 10mm (mass ratio of 1:1), rotating speed of 1800 rpm;
[0046] S4: Mg with 9 wt% AlCl3 added prepared in S3 by solution coating method 0.7 Ca 0.3 The surface of the alloy hydride-expanded graphite-AlCl3 composite powder material is coated with polyethylene glycol 2000. Specifically, Mg 0.7 Ca 0.3 The alloy hydride-expanded graphite-chloride composite powder material and polyethylene glycol 2000, the addition amount of polyethylene glycol 2000 is 12wt%, put into a three-necked flask in a glove box (argon atmosphere protection) and then transferred to a fume hood, and acetone was injected at room temperature. 0.7 Ca 0.3 The mixture of alloy hydride-expanded graphite-chloride composite powder material and polyethylene glycol 2000 and acetone is mixed in a ratio of 0.5 g: (10 mL-20 mL), and the stirring bar is turned on and stirred for 20 min at a stirring speed of 50 r / min. Then, the vacuum pump is turned on and the acetone is extracted. The dried material is processed and stored in a glove box to obtain Mg 0.7 Ca 0.3 Alloy hydride-expanded graphite-chloride-polyethylene glycol composite powder material, that is, Mg with 12wt% polyethylene glycol added 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, in this embodiment, Mg 0.7 Ca 0.3 The ratio of the mixture of alloy hydride-expanded graphite-chloride composite powder material and polyethylene glycol to acetone is 0.5 g:10 mL;
[0047] S5: The Mg prepared in S4 is pressed into 0.7 Ca 0.3 The alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is pressed into blocks. Specifically, a cylindrical mold with a diameter of 10 mm is used, and the pressure applied is 10-50 MPa. After pressing and molding, the pressure holding time is not less than 1 min. The mass of a single block after pressing and molding is 0.1 g. Mg 0.7 Ca 0.3 The alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material, in this embodiment, the applied pressure is 25 MPa, and the pressure holding time is 1.5 min.
[0048] In this example, the amount of each component is shown in Table 1.
[0049] The obtained Mg 0.7 Ca 0.3 The alloy hydride-expanded graphite-chloride-polyethylene glycol composite bulk material can be used in hydrogen production by hydrolysis.
[0050] Detection of Mg with 3 wt% expanded graphite added prepared in S2 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite composite powder materials are as follows:
[0051] The Mg2O3 prepared by adding 3 wt% expanded graphite in S2 was detected by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite composite powder material, the results are shown in Table 2;
[0052] Dynamic light scattering measurement of Mg prepared in S2 with 3 wt% expanded graphite 0.7 Ca 0.3 The hydraulic diameter of alloy hydride-expanded graphite composite powder material, the results are shown in Table 2;
[0053] TEM observation of Mg2O3 prepared in S2 with 3 wt% expanded graphite 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite composite powder material is shown in Figure 1 (b);
[0054] Detection of Mg with 3 wt% expanded graphite added prepared in S2 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite composite powder material is as follows: 0.7 Ca 0.3 The alloy hydride-expanded graphite composite powder material was placed in a reactor at a constant temperature of 25°C, 10 mL of deionized water at a temperature of 25°C was injected, and the reaction was carried out for 10 minutes. Hydrogen was collected by drainage method, and the hydrogen production was converted into the volume under standard conditions (the subsequent hydrolysis performance test operation process is the same as here, and will not be repeated). The results are shown in Table 2;
[0055] Mg with 3 wt% expanded graphite added prepared in S2 0.7 Ca 0.3 The alloy hydride-expanded graphite composite powder material was subjected to a pressing process, using a cylindrical mold with a diameter of 10 mm, the applied pressure was 25 MPa, the holding time after pressing was 1.5 min, and the mass of a single block after pressing was 0.1 g, thereby obtaining Mg with 3 wt% expanded graphite added. 0.7 Ca 0.3Alloy hydride-expanded graphite composite bulk material, measuring Mg with 3wt% expanded graphite added 0.7 Ca 0.3 The apparent density of the alloy hydride-expanded graphite composite bulk material is shown in Table 2;
[0056] Detection of Mg with 3 wt% expanded graphite added prepared in S2 0.7 Ca 0.3 The air tolerance of the alloy hydride-expanded graphite composite bulk material is to expose the bulk material to air at room temperature and humidity <80% RH (the subsequent air tolerance test conditions of the bulk material are the same as here and will not be repeated here), and the shape change of the bulk material is recorded. The results are as follows: Figure 2 (b) shows: Mg with 3wt% expanded graphite added after exposure 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride-expanded graphite composite block material was tested, and the hydrogen production was converted into volume under standard conditions. The results are shown in Table 2.
[0057] Detection of Mg with 9 wt% AlCl3 added prepared in S3 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite-AlCl3 composite powder materials are as follows:
[0058] The Mg prepared by adding 9wt% AlCl3 in S3 was characterized by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3 composite powder material was characterized, and the results are shown in Table 2;
[0059] The Mg prepared by adding 9wt% AlCl3 in S3 was characterized by SEM. 0.7 Ca 0.3 The morphology of alloy hydride-expanded graphite-AlCl3 composite powder was characterized, and its particle size was analyzed using Nano Measurer 1.2. The results are shown in Figure 3 , Figure 3 (d) is the apparent morphology of the material, Figure 3 (j) is the particle size distribution and average particle size of the material;
[0060] Detection of Mg with 9 wt% AlCl3 added prepared in S3 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3 composite powder material, the results are shown in Table 2;
[0061] XRD analysis of Mg with 9wt%AlCl3 0.7 Ca 0.3The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3 composite powder material were characterized. The byproduct treatment steps included: filtering the byproducts in a suction filtration bottle, drying them in a 50°C vacuum drying oven for 2-4 hours, and then performing XRD testing in an XRD vacuum accessory to avoid oxidation by air. (The subsequent hydrolysis byproduct treatment steps are the same as here and will not be repeated). The characterization results are shown in Table 2;
[0062] The Mg prepared in S3 with 9 wt% AlCl3 added 0.7 Ca 0.3 After the alloy hydride-expanded graphite-AlCl3 composite powder material was pressed and formed, its hydrolysis performance was tested after being exposed to air for 4 hours. The results are shown in Table 2.
[0063] Detection of Mg prepared in S4 with 12 wt% polyethylene glycol added 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder materials are as follows:
[0064] The Mg prepared in S4 with 12 wt% polyethylene glycol added was detected by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the results are shown in Table 2;
[0065] TEM observation of Mg prepared in S4 with 12 wt% polyethylene glycol added 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is shown in the following figure. Figure 4 (c)
[0066] The Mg prepared in S4 with 12 wt% polyethylene glycol added 0.7 Ca 0.3 After the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material was pressed and formed, its hydrolysis performance was tested after being exposed to air for 4 hours. The results are shown in Table 2;
[0067] XRD analysis of Mg with 12 wt% polyethylene glycol 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material were characterized, and the characterization results are shown in Table 2;
[0068] Mg with 12 wt% polyethylene glycol added 0.7 Ca 0.3The alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material was exposed to air for 24 hours, and the changes in its block shape and hydrolysis properties were detected. Figure 5 (b) Mg with 12 wt% polyethylene glycol added 0.7 Ca 0.3 Shape change of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material, 12wt% polyethylene glycol Mg 0.7 Ca 0.3 The hydrolysis performance change and attenuation rate test results of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material after exposure for 24 hours are shown in Table 2;
[0069] Mg with 12 wt% polyethylene glycol added 0.7 Ca 0.3 The samples of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material exposed for different times were characterized by XRD, such as Figure 7 shown.
[0070] Example 2
[0071] The difference from Example 1 is that in S3, the amount of AlCl3 added is 3wt%, and S4-5 is not included. Mg with 3wt% AlCl3 added is prepared in S3. 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3 composite powder material, the amount of each component is shown in Table 1.
[0072] The Mg prepared by adding 3wt% AlCl3 in S3 was characterized by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3 composite powder material was characterized, and the results are shown in Table 2;
[0073] The Mg prepared by adding 3wt% AlCl3 in S3 was characterized by SEM. 0.7 Ca 0.3 The morphology of alloy hydride-expanded graphite-AlCl3 composite powder was characterized, and its particle size was analyzed using Nano Measurer 1.2. The results are shown in Figure 3 , Figure 3 (b) is the apparent morphology of the material. Figure 3 (h) is the particle size distribution and average particle size of the material;
[0074] Detection of Mg with 3 wt% AlCl3 added prepared in S3 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3 composite powder material, the results are shown in Table 2;
[0075] XRD analysis of Mg with 3 wt% AlCl3 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3 composite powder material were characterized, and the characterization results are shown in Table 2.
[0076] Example 3
[0077] The difference from Example 1 is that in S3, the amount of AlCl3 added is 6wt%, and S4-5 is not included. Mg with 6wt% AlCl3 added is prepared in S3. 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3 composite powder material, the amount of each component is shown in Table 1.
[0078] The Mg prepared by adding 6wt% AlCl3 in S3 was characterized by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3 composite powder material was characterized, and the results are shown in Table 2;
[0079] The Mg prepared by adding 6wt% AlCl3 in S3 was characterized by SEM. 0.7 Ca 0.3 The morphology of alloy hydride-expanded graphite-AlCl3 composite powder was characterized, and its particle size was analyzed using Nano Measurer 1.2. The results are shown in Figure 3 , Figure 3 (c) is the apparent morphology of the material, Figure 3 (i) is the particle size distribution and average particle size of the material;
[0080] Detection of Mg with 6 wt% AlCl3 added prepared in S3 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3 composite powder material, the results are shown in Table 2;
[0081] XRD analysis of Mg with 6 wt% AlCl3 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3 composite powder material were characterized, and the characterization results are shown in Table 2.
[0082] Example 4
[0083] The difference from Example 1 is that in S4, the amount of polyethylene glycol 2000 added is 6 wt %, and S5 is not included. Mg with 6 wt % polyethylene glycol added is prepared in S4. 0.7 Ca 0.3Alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the amount of each component is shown in Table 1.
[0084] XRD analysis of the Mg prepared in S4 with 6 wt% polyethylene glycol added 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the results are shown in Table 2;
[0085] TEM observation of Mg prepared in S4 with 6 wt% polyethylene glycol added 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is shown in the following figure. Figure 4 (b)
[0086] The Mg prepared in S4 and added with 6 wt% polyethylene glycol 0.7 Ca 0.3 After the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material was pressed and formed, its hydrolysis performance was tested after being exposed to air for 4 hours. The results are shown in Table 2;
[0087] XRD analysis of Mg with 6 wt% polyethylene glycol 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material were characterized, and the characterization results are shown in Table 2;
[0088] Mg with 6 wt% polyethylene glycol added 0.7 Ca 0.3 The alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material was exposed to air for 24 hours, and the changes in its block shape and hydrolysis properties were detected. Figure 5 (a) Mg with 6 wt% polyethylene glycol added 0.7 Ca 0.3 Shape change of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material, Mg with 6wt% polyethylene glycol 0.7 Ca 0.3 The hydrolysis performance changes and attenuation rate test results of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material after exposure for 24 hours are shown in Table 2.
[0089] Comparative Example 1
[0090] The difference from Example 1 is that in S1, no expanded graphite is added, that is, the amount of expanded graphite added is 0wt%, and S3-5 is not included. Mg without adding expanded graphite is obtained in S2. 0.7 Ca 0.3Alloy hydride powder material, the amount of each component is shown in Table 1.
[0091] The Mg prepared in S2 without adding expanded graphite was detected by XRD 0.7 Ca 0.3 The physical phase of alloy hydride powder material, the results are shown in Table 3;
[0092] Dynamic light scattering measurement of Mg prepared in S2 without adding expanded graphite 0.7 Ca 0.3 The hydraulic diameter of alloy hydride powder material, the results are shown in Table 3;
[0093] TEM observation of Mg prepared in S2 without adding expanded graphite 0.7 Ca 0.3 The apparent morphology of alloy hydride powder material is shown in Figure 1 (a);
[0094] Detection of Mg2O3 without adding expanded graphite in S2 0.7 Ca 0.3 The hydrolysis performance of alloy hydride powder materials, the results are shown in Table 3;
[0095] Mg without adding expanded graphite was prepared in S2 0.7 Ca 0.3 Alloy hydride powder material is processed by pressing molding process, and Mg without adding expanded graphite is measured. 0.7 Ca 0.3 The apparent density of the alloy hydride bulk material is shown in Table 3;
[0096] Detection of Mg without adding expanded graphite 0.7 Ca 0.3 The air resistance of alloy hydride bulk materials is measured by recording the shape changes of the bulk materials. Figure 2 (a) shows: Mg without adding expanded graphite after exposure 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride bulk material was tested, and the results are shown in Table 3.
[0097] Comparative Example 2
[0098] The difference from Example 1 is that in S1, the amount of expanded graphite added is 8wt%, and S3-5 is not included. In S2, Mg with 8wt% expanded graphite added is prepared. 0.7 Ca 0.3 Alloy hydride-expanded graphite composite powder material, the amount of each component is shown in Table 1.
[0099] The Mg2O3 prepared by adding 8 wt% expanded graphite in S2 was detected by XRD. 0.7 Ca 0.3The physical phase of alloy hydride-expanded graphite composite powder material, the results are shown in Table 3;
[0100] Dynamic light scattering measurement of Mg2O3 prepared by adding 8 wt% expanded graphite in S2 0.7 Ca 0.3 The hydraulic diameter of alloy hydride-expanded graphite composite powder material, the results are shown in Table 3;
[0101] TEM observation of Mg2O3 prepared by adding 8 wt% expanded graphite in S2 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite composite powder material is shown in Figure 1 (c);
[0102] Detection of Mg2O3 prepared by adding 8wt% expanded graphite in S2 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite composite powder material, the results are shown in Table 3;
[0103] Mg2O3 with 8 wt% expanded graphite added was prepared in S2 0.7 Ca 0.3 The alloy hydride-expanded graphite composite powder material was subjected to a pressing process, and the Mg 0.7 Ca 0.3 The apparent density of the alloy hydride-expanded graphite composite bulk material is shown in Table 3;
[0104] Detection of Mg with 8wt% expanded graphite 0.7 Ca 0.3 The air resistance of alloy hydride-expanded graphite composite bulk material, the shape change of the bulk material is recorded, and the results are as follows Figure 2 (c) shows: Mg with 8wt% expanded graphite added after exposure 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride-expanded graphite composite block material was tested, and the results are shown in Table 3.
[0105] Comparative Example 3
[0106] The difference from Example 1 is that in S3, AlCl3 is not added, that is, the amount of AlCl3 added is 0wt%, and S4-5 is not included. Mg without adding AlCl3 is obtained in S3. 0.7 Ca 0.3 Alloy hydride-expanded graphite composite powder material, the amount of each component is shown in Table 1.
[0107] The Mg prepared in S3 without adding AlCl3 was characterized by XRD. 0.7 Ca 0.3The physical phase of the alloy hydride-expanded graphite composite powder material was characterized, and the results are shown in Table 3;
[0108] The Mg prepared in S3 without adding AlCl3 was observed by SEM. 0.7 Ca 0.3 The morphology of the alloy hydride-expanded graphite composite powder was characterized, and the particle size was analyzed using Nano Measurer 1.2. The results are shown in Figure 3 , Figure 3 (a) is the apparent morphology of the material, Figure 3 (g) is the particle size distribution and average particle size of the material;
[0109] Detection of Mg prepared in S3 without adding AlCl3 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite composite powder material, the results are shown in Table 3;
[0110] XRD analysis of Mg without adding AlCl3 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite composite powder material were characterized, and the characterization results are shown in Table 3.
[0111] Comparative Example 4
[0112] The difference from Example 1 is that in S3, the amount of AlCl3 added is 12wt%, and S4-5 is not included. Mg with 12wt% AlCl3 added is prepared in S3. 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3 composite powder material, the amount of each component is shown in Table 1.
[0113] The Mg-containing ... 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3 composite powder material was characterized, and the results are shown in Table 3;
[0114] The Mg-containing ... 0.7 Ca 0.3 The morphology of alloy hydride-expanded graphite-AlCl3 composite powder was characterized, and its particle size was analyzed using Nano Measurer 1.2. The results are shown in Figure 3 , Figure 3 (e) is the apparent morphology of the material, Figure 3 (f) is the local surface morphology of the material at high magnification. Figure 3 (k) is the particle size distribution and average particle size of the material; Figure 6Mg with 12wt% AlCl3 added 0.7 Ca 0.3 SEM-EDS results of alloy hydride-expanded graphite-AlCl3 composite powder materials;
[0115] Detection of Mg with 12 wt% AlCl3 added prepared in S3 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3 composite powder material, the results are shown in Table 3;
[0116] XRD analysis of Mg with 6 wt% AlCl3 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3 composite powder material were characterized, and the characterization results are shown in Table 3.
[0117] Comparative Example 5
[0118] The difference from Example 1 is that in S4, the amount of polyethylene glycol 2000 added is 0wt%, and S5 is not included. Mg without adding polyethylene glycol is obtained in S4. 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the amount of each component is shown in Table 1.
[0119] TEM observation of Mg prepared in S4 without adding polyethylene glycol 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is shown in the following figure. Figure 4 (a) shown.
[0120] Comparative Example 6
[0121] The difference from Example 1 is that in S4, the amount of polyethylene glycol 2000 added is 18 wt %. In S4, Mg 0.7 Ca 0.3 Alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the amount of each component is shown in Table 1.
[0122] The Mg prepared in S4 with 18 wt% polyethylene glycol added was detected by XRD. 0.7 Ca 0.3 The physical phase of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material, the results are shown in Table 3;
[0123] TEM observation of Mg prepared in S4 with 18 wt% polyethylene glycol added 0.7 Ca 0.3The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is shown in the following figure. Figure 4 (d) as shown; Figure 4 (ei) is Mg with 18 wt% polyethylene glycol added 0.7 Ca 0.3 Element distribution of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder materials;
[0124] The Mg prepared in S4 and added with 18 wt% polyethylene glycol 0.7 Ca 0.3 After the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material was pressed and formed, its hydrolysis performance was tested after being exposed to air for 4 hours. The results are shown in Table 3;
[0125] XRD analysis of Mg with 18 wt% polyethylene glycol added 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material were characterized, and the characterization results are shown in Table 3;
[0126] 18 wt% of Mg in polyethylene glycol was added 0.7 Ca 0.3 The alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material was exposed to air for 24 hours, and the changes in its block shape and hydrolysis properties were detected. Figure 5 (c) Mg with 18 wt% polyethylene glycol added 0.7 Ca 0.3 Shape change of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material, 18wt% Mg of polyethylene glycol 0.7 Ca 0.3 The hydrolysis performance change and attenuation rate test results of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material after exposure for 24 hours are shown in Table 3;
[0127] Table 1 is a table of the dosage of each component in Examples 1-4 and Comparative Examples 1-6;
[0128] Table 2 is the test result table of Examples 1-4;
[0129] Table 3 is the test result table of Comparative Examples 1-4 and Comparative Example 6.
[0130] Table 1
[0131]
[0132] Table 2
[0133]
[0134]
[0135]
[0136] Table 3
[0137]
[0138]
[0139] Conclusion analysis:
[0140] Mg prepared in S2 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite composite powder materials are analyzed as follows:
[0141] Depend on Figure 1 It can be seen that the Mg with 0%, 3wt%, and 8wt% expanded graphite added was observed by TEM. 0.7 Ca 0.3 The apparent morphology of the alloy hydride-expanded graphite composite powder material shows that when 3wt% expanded graphite is added, the expanded graphite is partially coated on the Mg 0.7 Ca 0.3 When 8wt% expanded graphite is added to the surface of alloy hydride particles, the expanded graphite is almost completely covered on the Mg 0.7 Ca 0.3 Surface of alloy hydride particles.
[0142] As shown in Tables 2 and 3, the XRD results show that the Mg 0.7 Ca 0.3 Alloy hydride-expanded graphite composite powder material was tested and it was found that Mg 0.7 Ca 0.3 The phases of alloy hydride powder materials include Ca4Mg3H 14 , MgH2 and Mg, Mg with 3wt% and 8wt% expanded graphite 0.7 Ca 0.3 The phase of alloy hydride-expanded graphite composite powder material is only Ca4Mg3H 14 and MgH2, indicating that the addition of expanded graphite can promote the 0.7 Ca 0.3 Complete hydrogenation of alloy materials.
[0143] As shown in Tables 2 and 3, the Mg content of 0%, 3wt%, and 8wt% expanded graphite was measured by dynamic light scattering. 0.7 Ca 0.3The hydraulic diameter of the alloy hydride-expanded graphite composite powder material reaches 2869.66nm when no expanded graphite is added. After adding 3wt% and 8wt% expanded graphite respectively, the hydraulic diameter of the composite powder material can be significantly reduced. It can be seen that after adding expanded graphite, the particle size of the composite powder material can be significantly reduced, which is more conducive to improving the hydrolysis conversion rate of the composite powder material.
[0144] It can be seen from Tables 2 and 3 that the addition of 0%, 3wt%, and 8wt% expanded graphite to Mg 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride-expanded graphite composite powder material was tested, and it was found that after adding expanded graphite, the hydrogen production of the composite powder material increased. Among them, the composite powder material with 8wt% expanded graphite added had a hydrogen production of 825mL / g com It can be seen that with the increase of the amount of expanded graphite added, the particle size of the material can be significantly reduced, the material can be completely hydrogenated, and the expanded graphite coated on the Mg 0.7 Ca 0.3 The surface of the alloy hydride material hinders the agglomeration of the material during the hydrolysis process, thereby improving the hydrolysis conversion rate.
[0145] It can be seen from Tables 2 and 3 that the addition of 0%, 3wt%, and 8wt% expanded graphite to Mg 0.7 Ca 0.3 The apparent density of the alloy hydride-expanded graphite composite block material was measured, and it was found that the surface density after adding 8wt% expanded graphite reached 1.37g / cm 3 Without adding expanded graphite, the surface density of the material is only 1.28g / cm 3 It can be seen that the addition of expanded graphite reduces the particle size of the material, and the smaller particle size and the relatively fluffy expanded graphite coated on the surface of the particles are conducive to the filling and forming of the particles.
[0146] Depend on Figure 2 It can be seen that after exposure for 1 h, Mg 0.7 Ca 0.3 Cracks appeared on the surface of alloy hydride bulk material, Mg with 8wt% expanded graphite added 0.7 Ca 0.3 The alloy hydride-expanded graphite composite block material expands from the side, and Mg with 3wt% expanded graphite is added 0.7 Ca 0.3The alloy hydride-expanded graphite composite block material is relatively intact; after 2 hours of exposure, the sides of all block materials expand, and the block materials without expanded graphite and with 3wt% expanded graphite remain relatively intact, while the collapsed part of the block material with 8wt% expanded graphite accounts for a larger proportion; after 4 hours, the trend is more obvious, the block material with 8wt% expanded graphite almost completely collapses, and the middle part of the block material with 3wt% expanded graphite remains relatively intact. It can be seen that after adding expanded graphite, the shape of the material can be maintained, but when the amount of expanded graphite added is greater than 8wt%, it is not conducive to maintaining the shape of the material.
[0147] It can be seen from Tables 2 and 3 that the addition of 0%, 3wt%, and 8wt% expanded graphite to Mg 0.7 Ca 0.3 The hydrogen production of the alloy hydride-expanded graphite composite bulk material after exposure for 4 hours was tested. The hydrogen production of the bulk material without adding expanded graphite, adding 3wt% and 8wt% expanded graphite was 349mL / g respectively. com 、403mL / g com and 120mL / g com It can be seen that the addition of an appropriate amount of expanded graphite (for example, 3wt%) is beneficial to reducing the particle size, improving the hydrolysis performance of the material itself and facilitating compression molding, thereby improving the air tolerance of the bulk material; but when added in excess (for example, 8wt%), the particle surface is completely covered with graphite, the viscosity between the particles is reduced, the retention rate of the block integrity is reduced, and the air tolerance is correspondingly deteriorated.
[0148] Mg prepared in S3 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite-AlCl3 composite powder materials are analyzed as follows:
[0149] As shown in Tables 2 and 3, the XRD results show that the Mg with 0wt%, 3wt%, 6wt%, 9wt%, and 12wt% AlCl3 added 0.7 Ca 0.3 The phases of alloy hydride-expanded graphite-AlCl3 composite powder materials were characterized. All composite powder materials only contained MgH2 and Ca4Mg3H 14 Two phases indicate that the composite powder material has been completely hydrogenated.
[0150] The SEM images of Mg with 0wt%, 3wt%, 6wt%, 9wt%, and 12wt% AlCl3 were taken. 0.7 Ca 0.3The morphology of alloy hydride-expanded graphite-AlCl3 composite powder materials was characterized, and the particle sizes of different materials were analyzed using Nano Measurer 1.2. Figure 3 It can be seen that the SEM results show that the particles have undergone serious agglomeration, but it is still not difficult to observe from the agglomerated particles that as the AlCl3 content gradually increases, the Mg 0.7 Ca 0.3 The particle size of the alloy hydride-expanded graphite-AlCl3 composite powder material showed a decreasing trend, and the results of particle size analysis were consistent with this trend. 0.7 Ca 0.3 In the local surface morphology of alloy hydride-expanded graphite-AlCl3 composite powder material at high magnification, it was observed that there were obvious cracks on the particle surface. Figure 6 It can be seen that adding 12wt% AlCl3 to Mg 0.7 Ca 0.3 The SEM-EDS results of the alloy hydride-expanded graphite-AlCl3 composite powder material proved that the elements were evenly distributed. The Al and Cl elements proved the existence of AlCl3, and the C element also proved the existence of expanded graphite.
[0151] It can be seen from Tables 2 and 3 that the addition of 0wt%, 3wt%, 6wt%, 9wt%, and 12wt% AlCl3 to Mg 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3 composite powder materials was tested, and Mg with 0wt%, 3wt%, 6wt%, 9wt%, and 12wt% AlCl3 was added. 0.7 Ca 0.3 The hydrogen production of alloy hydride-expanded graphite-AlCl3 composite powder materials is 824mL / g com 、843mL / g com 、925mL / g com , 1002mL / g com and 954mL / g com It can be seen that the addition of AlCl3 effectively improves the Mg content of 3wt% expanded graphite added in Example 1. 0.7 Ca 0.3 Hydrolysis properties of alloy hydride-expanded graphite composite powder materials.
[0152] As shown in Tables 2 and 3, the XRD results show that the Mg with 0wt%, 3wt%, 6wt%, 9wt%, and 12wt% AlCl3 added 0.7 Ca 0.3The alloy hydride-expanded graphite-AlCl3 composite powder material was characterized, and the results showed that only by-product Mg(OH)2 and unhydrolyzed MgH2 were observed.
[0153] AlCl3 dissolves in a large amount of water to generate Cl - and H3O + , destroying the byproduct Mg(OH)2 passivation layer, thus providing a channel for water molecules to enter the interior of the particles and strengthening the subsequent mass transfer; in addition, AlCl3 releases heat after dissolving in water, which can improve the reaction kinetics of the micro-area. 0.7 Ca 0.3 The particle size of the alloy hydride-expanded graphite-AlCl3 composite powder material has also changed. The smaller particle size and the cracks on the particle surface observed under high magnification of SEM provide more initial reaction sites. The above points synergistically promote the improvement of the material's hydrolysis performance. However, adding too much AlCl3 will reduce the theoretical hydrogen production of the system, which is why the hydrolysis performance decreases instead of increases after adding 12wt% AlCl3.
[0154] For Mg with 9wt% AlCl3 added 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride-expanded graphite-AlCl3 composite block material was tested. As shown in Table 2, the hydrogen production after 4 hours of exposure was 624 mL / g. com , which is better than that of Mg in Example 1 when no AlCl3 is added 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite composite bulk material, adding AlCl3 not only improves Mg 0.7 Ca 0.3 The hydrolysis performance of the alloy hydride-expanded graphite composite block material itself can also improve the appearance retention of the block material by its own moisture absorption, thereby improving its air tolerance.
[0155] Mg prepared in S4 0.7 Ca 0.3 The properties of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder materials are analyzed as follows:
[0156] XRD was used to detect the Mg content of 6wt%, 12wt% and 18wt% polyethylene glycol. 0.7 Ca 0.3 The phases of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder materials are shown in Table 2 and Table 3. The phases of all composite powder materials are composed of Ca4Mg3H 14 and MgH2.
[0157] TEM observation of Mg with 0wt%, 6wt%, 12wt%, and 18wt% polyethylene glycol added 0.7 Ca 0.3 The apparent morphology of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material is Figure 4 It can be seen that when the composite powder material is not coated with polyethylene glycol 2000, independent particles can be observed; however, after being coated with polyethylene glycol 2000, the composite powder material is seriously aggregated. 0.7 Ca 0.3 The element distribution diagram of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material shows that Mg, Ca, Al, and Cl are evenly distributed, and the C element is distributed over a larger area. Figure 4 (g) Demonstrates the presence of polyethylene glycol 2000 as a coating layer.
[0158] It can be seen from Tables 2 and 3 that the addition of 6wt%, 12wt% and 18wt% polyethylene glycol to Mg 0.7 Ca 0.3 The hydrolysis performance of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material was tested after exposure for 4 hours. Mg coated with 6wt%, 12wt% and 18wt% polyethylene glycol 0.7 Ca 0.3 The hydrogen production of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material after 4 hours of exposure was 803 mL / g. com 、737mL / g com and 669mL / g com , both better than Mg 0.7 Ca 0.3 Properties of alloy hydride-expanded graphite-AlCl3 composite bulk materials (624mL / g com ); Mg with 6wt%, 12wt% and 18wt% polyethylene glycol added 0.7 Ca 0.3 The hydrolysis byproducts of the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite powder material were characterized by XRD, and the results showed that only Mg(OH)2 and unreacted MgH2 were detected.
[0159] Depend on Figure 5 It can be seen that the addition of 6wt%, 12wt% and 18wt% polyethylene glycol to Mg 0.7 Ca 0.3After the alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block material was exposed to air for 24 hours, all composite block materials began to collapse from the side wall. Among them, the composite block material with 6wt% polyethylene glycol added had the worst appearance retention. The side wall expanded slightly after 4 hours of exposure and almost completely collapsed after 24 hours. The composite block material with 12wt% polyethylene glycol added had a slight expansion of the side wall after 16 hours of exposure, and obvious cracks on the block surface after 24 hours. The composite block material with 18wt% polyethylene glycol added had a slight expansion of the side wall after 24 hours of exposure. It can be seen that after the introduction of polyethylene glycol as a coating layer, the appearance retention of all blocks is far better than that of Mg 0.7 Ca 0.3 Appearance retention of alloy hydride-expanded graphite composite block materials.
[0160] It can be seen from Tables 2 and 3 that the addition of 6wt%, 12wt% and 18wt% polyethylene glycol to Mg 0.7 Ca 0.3 The hydrolysis performance changes and attenuation rates of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite block materials exposed to air for 24 hours. The hydrolysis performance of all composite block materials did not change much within 4 hours of exposure (only the composite block material coated with 6wt% polyethylene glycol had a 2.4% attenuation), and the hydrolysis performance showed a regular arrangement of 6wt% better than 12wt%, and further better than 18wt%. This is mainly because polyethylene glycol does not directly participate in the hydrolysis reaction. When its content is low, the theoretical hydrogen production of the material is higher and the hydrolysis performance is better. When the exposure time exceeds 4 hours, the hydrolysis performance of all block materials begins to decay, and the attenuation rate gradually increases with the exposure time. As the content of polyethylene glycol increases from 6wt% to 18wt%, the attenuation rate at the same exposure time decreases significantly. The hydrolysis performance of the sample after exposure for 16 hours shows a regular arrangement of 18wt% better than 12wt%, and further better than 6wt%.
[0161] In addition, the addition of 12 wt% polyethylene glycol to Mg 0.7 Ca 0.3 The XRD characterization of the samples of alloy hydride-expanded graphite-AlCl3-polyethylene glycol composite bulk material exposed for different times showed that with the increase of exposure time, Ca4Mg3H 14 The peak intensity of Ca4Mg3H 14 More likely to react with water in the air).
[0162] Obviously, polyethylene glycol as a binder effectively promotes block forming and improves the appearance retention of the block for a certain period of time, effectively delays the direct contact between water molecules in the air and the material, and thus promotes the improvement of the air tolerance of the material.
[0163] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A magnesium-calcium-based hydrolysis hydrogen production composite block material, characterized in that: Including Mg x Ca 1-x The mass ratios of alloy hydride, expanded graphite, chloride and polyethylene glycol are: (65-90): (2-7): (3-11): (5-17), wherein x is the mass fraction, and the value range of x is 0.7-0.
9.
2. The magnesium-calcium-based hydrolysis hydrogen production composite block material according to claim 1, characterized in that: The chloride is any one of aluminum chloride, ammonium chloride and calcium chloride.
3. The magnesium-calcium-based hydrolysis hydrogen production composite block material according to claim 2, characterized in that: The molecular weight of polyethylene glycol is between 800-4000.
4. A method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material, characterized in that: The following steps are involved: S1: Mg x Ca 1-x After the alloy is crushed, expanded graphite is added and then ball milled to obtain Mg x Ca 1-x Alloy-expanded graphite composite powder material; S2: Mg prepared in S1 x Ca 1-x The alloy-expanded graphite composite powder material is repeatedly activated and hydrogenated to obtain Mg x Ca 1-x Alloy hydride-expanded graphite composite powder material; S3: Prepare Mg from S2 x Ca 1-x The alloy hydride-expanded graphite composite powder material is added with chloride and then ball-milled to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride composite powder material; S4: Mg prepared in S3 by solution coating method x Ca 1-x The surface of alloy hydride-expanded graphite-chloride composite powder material is coated with polyethylene glycol to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite powder material; S5: The Mg prepared in S4 is pressed into x Ca 1-x The alloy hydride-expanded graphite-chloride-polyethylene glycol composite powder material is pressed into blocks to obtain Mg x Ca 1-x Alloy hydride-expanded graphite-chloride-polyethylene glycol composite bulk material.
5. The method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material according to claim 4, characterized in that: Mg prepared in S2 x Ca 1-x The phases of alloy hydride-expanded graphite composite powder materials include Ca4Mg3H 14 and MgH2.
6. The method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material according to claim 5, characterized in that: In S2, the activation and hydrogenation temperature is 300-500°C and the time is 2-24h.
7. The method for preparing a magnesium-calcium-based composite block material for hydrogen production by hydrolysis according to claim 6, characterized in that: In S4, the solvent of the solution coating method is acetone, Mg x Ca 1-x The ratio of the mixture of alloy hydride-expanded graphite-chloride composite powder material and polyethylene glycol to acetone is 0.5g: (10mL-20mL).
8. The method for preparing a magnesium-calcium-based composite block material for hydrogen production by hydrolysis according to claim 7, characterized in that: In S3, the ball-to-material ratio of the ball mill is 10:1-30:1, the rotation speed is 1200-2000 rpm, and the time is 0.5-1h.
9. The method for preparing a magnesium-calcium-based hydrolysis hydrogen production composite block material according to claim 8, characterized in that: In S5, the pressure used in the press-forming process is 10-50 MPa, and after press-forming, the holding time is not less than 1 minute.