Preparation method and application of alkali lignin-based porous carbon material
By using alkali lignin and formaldehyde to combine ammonia-dimethylamine-epoxychlorohydrin polymer to form a continuous three-dimensional network precursor, the problem of poor conductivity of alkali lignin-based carbon materials is solved, and the lead-carbon battery is realized. Highly efficient conductivity and extended life.
Patent Information
- Application Number
- CN202410929289.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The alkali lignin-based carbon material has poor electrical conductivity in lead-carbon batteries, resulting in serious irreversible sulfation of active substances, limiting its application in the field of lead-carbon batteries.
Using alkali lignin and formaldehyde as carbon sources, ammonia-dimethylamine-epoxychlorohydrin polymer as nitrogen sources, it self-assembles through hydrogen bonds to form a continuous three-dimensional network precursor, and carbonizes at high temperatures to prepare high-efficiency conductivity The alkaline lignin-based porous carbon material of the network.
The efficient conductivity of alkali lignin-based porous carbon materials is achieved, the growth of lead sulfate crystals is inhibited, and the service life of lead charcoal batteries is extended.
Smart Images

Figure CN118894516A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkali lignin-based carbon materials, and specifically relates to a preparation method and application of an alkali lignin-based porous carbon material. Background Art
[0002] Lead-carbon battery is a new type of battery that combines the high power of supercapacitors and the long life of lead-acid batteries. Especially as a hybrid vehicle battery, it has unparalleled advantages over other types of batteries. The main reason for the life of hybrid vehicles is the irreversible sulfation of the negative electrode. Adding carbon materials as additives to the negative electrode can give full play to its high conductivity and the dispersibility of substances with discharge activity on the negative electrode, which can improve the utilization rate of active substances and inhibit the growth of lead sulfate crystals.
[0003] my country is a large agricultural country, and a large amount of agricultural biomass waste is produced every year, such as straw, fruit shells, leaves, etc. Using biomass as raw materials to prepare carbon material additives can achieve effective utilization of agricultural waste and reduce the manufacturing cost of carbon materials. At present, the application of carbon materials prepared from biomass in the field of electrochemical energy storage has been relatively mature, such as the biomass porous carbon material and its preparation method and its application in lead-acid batteries disclosed in patent CN115367750B, and the modified carbon material, its preparation method, negative electrode lead paste, plate and lead-carbon battery disclosed in patent CN105958076B.
[0004] Lignin is a major component of biomass materials, the second largest renewable resource in nature after cellulose, and the most abundant aromatic natural polymer. In the pulp and paper industry, alkali lignin is the main by-product, with a global annual total output of about 50 billion tons. Due to the lack of efficient and complete utilization technology, most alkali lignin is directly burned in the form of industrial waste for power generation or heat supply. The carbon content in alkali lignin is as high as 50-60%, which is also an ideal precursor for the preparation of carbon materials. However, alkali lignin has a low degree of cross-linking and is a discontinuous carbon material precursor. Direct carbonization will cause the pore structure formed by the carbon material to be unstable, easy to collapse, and the porosity to deteriorate. Using it as an additive for lead-carbon battery carbon materials cannot form a complete three-dimensional conductive network, and the conductivity is poor, resulting in serious irreversible sulfation of active substances, so that alkali lignin-based carbon materials are rarely used in the field of lead-carbon batteries.
[0005] Therefore, it is of great significance to develop a method that can comprehensively utilize alkali lignin, a renewable resource, as an additive for lead-carbon battery carbon materials with excellent conductive properties. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for preparing an alkali lignin-based porous carbon material and its application, wherein alkali lignin and formaldehyde are used as carbon sources, and ammonia-dimethylamine-epichlorohydrin polymer is used as nitrogen source. The carbon source and the template are self-assembled through hydrogen bonds, and further cross-linked by the ammonia-dimethylamine-epichlorohydrin polymer to form a continuous three-dimensional network precursor, and finally carbonized under high temperature to obtain an alkali lignin-based porous carbon material with a high-efficiency conductive network and conductive properties.
[0007] In order to achieve the above purpose, the following technical solutions are adopted:
[0008] A method for preparing an alkali lignin-based porous carbon material comprises the following steps:
[0009] 3) adding an alkali lignin solution and a formaldehyde aqueous solution to a reaction kettle and mixing them evenly, heating and heating the reaction for the first time under stirring conditions, adding an ammonia-dimethylamine-epichlorohydrin polymer solution and a template solution after the reaction, heating and heating the reaction for the second time under stirring conditions, cooling to room temperature after the reaction, filtering, washing, and drying to obtain a precursor for standby use;
[0010] 4) The precursor is heated and carbonized in an inert atmosphere, and then cooled to obtain an alkali lignin-based porous carbon material.
[0011] Furthermore, in step 1), the alkali lignin solution is obtained by uniformly mixing alkali lignin and a mixed solvent, and the mixed solvent is a mixture of water and an organic solvent in a volume ratio of 1-2:1; preferably, the organic solvent is selected from one or a combination of two or more of acetone, tetrahydrofuran, and acetone dioxane; more preferably, the mass volume ratio of the alkali lignin to the mixed solvent is 1g:20-30mL.
[0012] Furthermore, in step 1), the alkali lignin has a weight average molecular weight of 1000-3000. Lignin is an aggregate with many polar groups in its structure, especially more hydroxyl groups, forming strong intramolecular and intermolecular hydrogen bonds. Therefore, lignin is insoluble in water and any solvent. However, alkali lignin is degraded lignin and can be dissolved in dilute water, alkaline or neutral polar solvents.
[0013] Furthermore, in step 1), the alkali lignin is selected from at least one of wood pulp alkali lignin, bamboo pulp alkali lignin, wheat straw pulp alkali lignin, reed pulp alkali lignin, bagasse pulp alkali lignin, and asparagus pulp alkali lignin.
[0014] Furthermore, in step 1), the concentration of the formaldehyde aqueous solution is 35-40wt%.
[0015] Furthermore, in step 1), the stirring speed is 200-300 r / min, the first heating temperature is raised to 50-60° C., and the reaction time is 1-3 h.
[0016] Further, in step 1), in step 1), the viscosity of the ammonia-dimethylamine-epichlorohydrin polymer solution at 25° C. is 3-4 Pa·s, and the concentration is 45-50wt%. The ammonia-dimethylamine-epichlorohydrin polymer solution can be commercially available or homemade. If it is homemade, its preparation method is as follows: in a flask equipped with a thermometer, a stirrer, a reflux condenser and a feeding funnel, add a dimethylamine aqueous solution and ammonia water, control the temperature at 25-40° C., dropwise add part of epichlorohydrin, heat up to react, add the remaining epichlorohydrin during the reaction, cool after the reaction, and adjust the pH value to obtain the ammonia-dimethylamine-epichlorohydrin polymer solution.
[0017] Furthermore, the mass ratio of the dimethylamine aqueous solution, ammonia water and epichlorohydrin is 400-450:60-65:450-480, the concentration of the dimethylamine aqueous solution is 40-45wt%, the concentration of ammonia water is 25-30wt%, the epichlorohydrin is dripped in 1-2.5h, the temperature is raised to 80-100°C, the reaction time is 1-3h, the remaining epichlorohydrin is added, the remaining epichlorohydrin accounts for 1 / 5-1 / 4 of the total amount of epichlorohydrin, the remaining epichlorohydrin is added in 1-3 times, each addition is separated by 10-30min, the cooling is cooled to 60-80°C, and the pH is adjusted to 2-3 with sulfuric acid.
[0018] Furthermore, in step 1), the template is one or a combination of two of the triblock copolymers F127 and P123, the solvent of the template solution is ethanol, and the concentration of the template solution is 3-5wt%.
[0019] Furthermore, in step 1), the mass ratio of the alkali lignin, the formaldehyde solution, the ammonia-dimethylamine-epichlorohydrin polymer solution, and the template agent is 1:1.5-1.8:1.4-1.7:0.1-0.13.
[0020] Furthermore, in step 1), the stirring speed is 200-300 r / min, the second heating temperature is raised to 60-90°C, and the reaction time is 3-5h. The washing is performed by washing with ethanol and water alternately for 1-3 times, and the drying is performed at 80-100°C to constant weight.
[0021] Step 1) During the first heating and temperature-raising reaction, the phenolic hydroxyl groups on the alkali lignin react with formaldehyde to generate hydroxymethyl, that is, to generate resol phenolic aldehyde, and during the second heating and temperature-raising reaction, the amine groups on the resol phenolic aldehyde and the ammonia-dimethylamine-epichlorohydrin polymer are condensed and dehydrated to generate a dense cross-linked precursor. The ammonia-dimethylamine-epichlorohydrin polymer plays the role of a cross-linking agent in the preparation process of the precursor. Because it belongs to a quaternary ammonium salt surfactant, it also has the role of a template agent. However, since most of the ammonia-dimethylamine-epichlorohydrin polymer is interspersed and buried in the continuously cross-linked precursor, it is still necessary to use a small amount of template agent to form a porous carbon structure with a good specific surface area. The ratio of ammonia-dimethylamine-epichlorohydrin polymer and template agent and its ratio relative to alkali lignin and formaldehyde solution have a great influence on the prepared alkali lignin-based porous carbon material. The relative proportion of template agent is small, which will cause excessive cross-linking and poor pore structure; too much relative proportion cannot form a continuous precursor matrix, and the pore structure after carbonization is unstable and easy to collapse. Therefore, the mass ratio of alkali lignin, formaldehyde solution, ammonia-dimethylamine-epichlorohydrin polymer solution and template agent needs to be strictly controlled.
[0022] In step 2), the heating graphitization treatment is to increase the temperature to 1700-1900° C. at a speed of 3-5° C. / min and keep the temperature for 1-3 hours.
[0023] The present invention also provides an alkali lignin-based porous carbon material prepared by the method.
[0024] The present invention also provides a negative electrode lead paste for a lead-carbon battery, using the alkaline lignin-based porous carbon material as a negative electrode lead paste additive.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention uses alkali lignin and formaldehyde as carbon sources and ammonia-dimethylamine-epichlorohydrin polymer as nitrogen source. The carbon source and the template agent are self-assembled through hydrogen bonds, and further cross-linked by the ammonia-dimethylamine-epichlorohydrin polymer to form a continuous three-dimensional network precursor, and finally carbonized under high temperature to obtain an alkali lignin-based porous carbon material with a high-efficiency conductive network and conductive properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is an electron microscope photo of the porous carbon material prepared in Example 1;
[0028] Figure 2 This is a pore size structure distribution diagram of the porous carbon material prepared in Example 1;
[0029] Figure 3 This is the specific surface test data of the porous carbon material prepared in Example 1. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.
[0031] Alkali lignin was purchased from Xinyi Feihuang Chemical Co., Ltd. with a weight average molecular weight of 2500.
[0032] Preparation of alkali lignin-based porous carbon materials:
[0033] Example 1
[0034] 1) In a 2000mL flask equipped with a thermometer, a stirrer, a reflux condenser and a charging funnel, add 450g of a 40wt% dimethylamine aqueous solution and 60.8g of a 29wt% ammonia solution. Then, at a temperature below 40°C, add 412.9g of epichlorohydrin dropwise to the mixed solution within 2h, heat to 90°C and react for 1h, then add a total of 45.9g of epichlorohydrin in 3 times, the time interval between each addition must be maintained at 20min, and the temperature is maintained at 90°C until all the additions are completed. Finally, the reaction mixture is cooled to 80°C, and concentrated sulfuric acid is added to reduce the pH value of the reaction solution to 2.5, to obtain a 50wt% ammonia-dimethylamine-epichlorohydrin polymer solution with a viscosity of 3.55Pa.s.
[0035] 2) Add 100g of alkali lignin and 3000mL of a mixed solvent (the mixed solvent is a mixture of water and tetrahydrofuran in a volume ratio of 2:1) and 180g of a 37wt% formaldehyde solution into a reactor and mix them evenly. Heat to 75°C for the first time at 200r / min stirring for 2h. After the reaction, add 170g of ammonia-dimethylamine-epichlorohydrin polymer solution and 200g of a 5wt% template F127 (purchased from Sigma) solution. Heat to 90°C for the second time at 200r / min stirring for 5h. After the reaction, cool to room temperature, filter, wash 3 times with ethanol and alcohol water alternately, and dry to obtain a precursor for standby use;
[0036] 5) In a nitrogen atmosphere, the precursor was heated to 1700°C at a rate of 3.5°C / min, and carbonized for 3 hours, and then cooled to room temperature to obtain an alkali lignin-based porous carbon material. Graphitization degree I D / I G It is 0.86.
[0037] Example 2
[0038] The rest is the same as Example 1, except that the amount of ammonia-dimethylamine-epichlorohydrin polymer solution used is 140 g.
[0039] Example 3
[0040] The rest is the same as Example 1, except that the amount of template F127 (purchased from Sigma) solution used is 260 g.
[0041] Example 4
[0042] The rest is the same as Example 1, except that the amount of template F127 (purchased from Sigma) solution used is 300 g.
[0043] Example 5
[0044] The rest is the same as Example 1, except that the amount of template F127 (purchased from Sigma) solution used is 180 g.
[0045] Example 6
[0046] The rest is the same as Example 1, except that, 2) an alkali lignin solution prepared by 100 g of alkali lignin and 3000 mL of a mixed solvent (the mixed solvent is a mixture of water and tetrahydrofuran in a volume ratio of 2: 1) and 150 g of a 37 wt % formaldehyde solution are added to the reactor and mixed evenly, and the mixture is heated to 75 ° C for the first time at 200 r / min stirring for 2 h. After the reaction, 140 g of ammonia-dimethylamine-epichlorohydrin polymer solution and 260 g of a 5 wt % template F127 (purchased from Sigma) solution are added, and the mixture is heated to 90 ° C for the second time at 200 r / min stirring for 5 h. After the reaction, the mixture is cooled to room temperature, filtered, washed alternately with ethanol and alcohol water for 3 times, and dried to obtain a precursor for standby use.
[0047] Comparative Example 1
[0048] The rest is the same as Example 1, except that 340 g of a 25 wt % diethylenetriamine aqueous solution is used to replace 170 g of ammonia-dimethylamine-epichlorohydrin polymer solution.
[0049] Comparative Example 2
[0050] The rest is the same as Example 1, except that the template F127 is not added.
[0051] Application Example 1
[0052] Assembling lead-carbon batteries:
[0053] (1) Paste: 50 g of lead powder, 10 g of lead oxide, 0.7 g of the alkali lignin-based porous carbon material prepared in Example 1, 0.8 g of barium sulfate, 0.2 g of acetylene black, 0.8 g of sodium lignosulfonate, 0.8 g of barium stearate, and 0.9 mL of water were stirred for 10 min to obtain a lead paste.
[0054] (2) Apply lead paste evenly to the positive and negative grids (the lead-calcium alloy negative grid was purchased from Baoding Meilun Nonferrous Metals Co., Ltd., and the lead dioxide positive grid was purchased from Baoji Changli Special Metals Co., Ltd. The size of the positive and negative grids is 70mm×50mm×2mm.), dry in an oven at 65℃ for 8h, and then dry at 75℃ for 6h to obtain the positive and negative plates of the lead-carbon battery. Add 150mL of 1.035g / cm 3 Sulfuric acid, insert the positive and negative plates on both sides of the beaker, separate them with industrial battery AGM, simulate lead-carbon battery, connect it to LAND5.8 battery test system, and perform formation to obtain qualified positive and negative plates. Among them, the formation conditions are: first stand for 2 hours, then charge at 0.05C constant current for 1 hour, then charge at 0.1C constant current for 20 hours; after standing for 2 hours, discharge at 0.1C constant current for 1 hour, then charge at 0.1C constant current for 10 hours, charge at 0.2C constant current for 12 hours, and finally charge at 0.1C constant current for 4 hours.
[0055] (3) Lead-carbon batteries are assembled in the form of 1 positive and 2 negative plates: welding of positive and negative plates, battery acid filling (sulfuric acid density 1.27g / cm 3 ), battery sealing, battery detection machine activation.
[0056] Application Example 2-6, Comparative Application Example 1-2
[0057] The rest is the same as Application Example 1, except that the biomass graphitized carbon material is prepared according to Examples 2-6 and Comparative Examples 1-2.
[0058] The alkali lignin-based porous carbon materials prepared in the above examples and comparative examples were tested for pore structure and specific surface area, and the lead-carbon batteries of the corresponding examples and comparative application examples were tested for cycle performance:
[0059] 1. Pore structure and specific surface area: measured by NOVA 1000e pore structure specific surface area tester. The sample was degassed at 350℃ for 2h, and liquid nitrogen was used as the adsorption medium at 77K and relative pressure (P / P 0 )10 -6 N in the range of -1 2 The specific surface area was calculated by the BET equation.
[0060] 2. Cycle performance: In order to study the life of lead-carbon batteries under high rate charge and discharge (HRPSoC) conditions, a cycle test experiment was carried out. The battery tester model used in the experiment is BTS-5V / 6A, produced by Shenzhen Xinwei Electronics Co., Ltd. The charge and discharge system used in the test is as follows: First, the battery is left for 30 minutes, discharged at 2A current for 84 minutes, reaching 50% of the theoretical capacity, that is, 50% SoC, and after leaving for 5 minutes, the following steps are cycled: 4A current charge for 1 minute, leave for 1 minute, 4A current discharge for 1 minute, and leave for 1 minute. The upper and lower limits of the charge and discharge voltage are set to 2.9V and 1.7V respectively. When any of the aforementioned cut-off voltages of the battery is reached, the cycle terminates.
[0061] Table 1
[0062] project <![CDATA[Specific surface area m 2 / g]]> Mesoporosity % Cycle life times Application Example 1 442 80.3 81890 Application Example 2 366 84.7 80113 Application Example 3 343 78.5 79222 Application Example 4 521 66.8 72325 Application Example 5 319 60.4 68894 Application Example 6 418 83.6 81006 Comparative application example 1 179 36.9 32067 Comparative Application Example 2 408 51.2 55571
[0063] As can be seen from Table 1, the present invention successfully prepared a porous carbon material with a mesoporous structure having high-efficiency conductive properties, and applying it to a lead-carbon battery can inhibit the growth of lead sulfate crystals and extend the service life of the battery. It can be clearly seen from Application Example 1 and Comparative Application Examples 1-2 that the relative ratio of ammonia-dimethylamine-epichlorohydrin polymer and template agent and their relative ratio to alkali lignin and formaldehyde solution have a great influence on the pore structure specific surface area and conductive properties of the porous carbon material. Although the inventor has not further explored, it is speculated that the mass ratio of alkali lignin, formaldehyde solution, ammonia-dimethylamine-epichlorohydrin polymer solution, and template agent affects nitrogen doping and pore structure and thus affects conductive properties.
[0064] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.
Claims
1. A method for preparing an alkali lignin-based porous carbon material, Its characteristics are that The steps include: 1) adding an alkali lignin solution and a formaldehyde aqueous solution to a reaction kettle and mixing them evenly, heating and heating the reaction kettle for the first time under stirring conditions, adding an ammonia-dimethylamine-epichlorohydrin polymer solution and a template solution after the reaction, heating and heating the reaction kettle for the second time under stirring conditions, cooling the reaction kettle to room temperature after the reaction, filtering, washing, and drying the reaction kettle to obtain a precursor for standby use; 2) The precursor is heated and carbonized in an inert atmosphere, and then cooled to obtain an alkali lignin-based porous carbon material.
2. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), the alkali lignin solution is obtained by uniformly mixing alkali lignin and a mixed solvent, wherein the mixed solvent is a mixture of water and an organic solvent in a volume ratio of 1-2:1; preferably, the organic solvent is selected from one or a combination of two or more of acetone, tetrahydrofuran, and acetone dioxane; more preferably, the mass volume ratio of the alkali lignin to the mixed solvent is 1g:20-30mL.
3. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), the weight average molecular weight of the alkali lignin is 1000-3000.
4. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), the concentration of the formaldehyde aqueous solution is 35-40 wt %.
5. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), in step 1), the viscosity of the ammonia-dimethylamine-epichlorohydrin polymer solution at 25° C. is 3-4 Pa·s, and the concentration is 45-50wt%.
6. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), the template is one or a combination of triblock copolymers F127 and P123, the solvent of the template solution is ethanol, and the concentration of the template solution is 3-5wt%.
7. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 1), the mass ratio of the alkali lignin, the formaldehyde solution, the ammonia-dimethylamine-epichlorohydrin polymer solution, and the template agent is 1:1.5-1.8:1.4-1.7:0.1-0.
13.
8. The method for preparing the alkali lignin-based porous carbon material according to claim 1, Its characteristics are that In step 2), the heating graphitization treatment is to increase the temperature to 1700-1900° C. at a speed of 3-5° C. / min and keep the temperature for 1-3 hours.
9. The alkali lignin based porous carbon material prepared by the method for preparing the alkali lignin based porous carbon material according to any one of claims 1 to 8.
10. A negative electrode lead paste for a lead-carbon battery, using the alkali lignin-based porous carbon material according to claim 9 as a negative electrode lead paste additive.
Citation Information
Patent Citations
Method for preparing sugary-lignin-based urea-formaldehyde resin capacitive carbon
CN107140637A
Preparation method of amination modified sodium alkali lignosulfonate oligomer cathode corrosion inhibitor
CN111662462A
Redox-active compounds and uses thereof
CN113166079A
Carbonaceous material and method for producing the same, and battery including carbonaceous material
JP2021116196A
Process for the preparation of hierarchically meso and macroporous structured materials
US20150284252A1
Cited By
Preparation method of high-strength composite bipolar plate
CN119252961A