Manganese dioxide with nanowire and nanosheet structure, preparation method and application in lithium-sulfur battery

Manganese dioxide in nanowire nanosheet structure was prepared by using polyvinyl alcohol and manganese sulfate in lithium sulfur batteries, which solved the problem of insufficient MnO2 active sites, significantly improved the performance and polysulfide of lithium sulfur batteries. The material suppression ability improves the cycle stability and Coulomb efficiency of the battery.

CN118894554APending Publication Date: 2024-11-05SHANDONG AEROSPACE WEINENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410951465.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The insufficient existing MnO2 active sites lead to its limited effect on inhibiting polysulfides, affecting the cyclic stability and Coulomb efficiency of lithium-sulfur batteries.

Method used

Polyvinyl alcohol is used to undergo solvothermal reaction with sulfuric acid solution and manganese sulfate to prepare manganese dioxide with nanowire nanosheet structure, increasing the active site to improve the inhibitory ability of polysulfides.

Benefits of technology

By preparing manganese dioxide with nanowire nanosheet structures, the performance of lithium-sulfur batteries is significantly improved, the inhibition ability of polysulfides is enhanced, and the circulation stability and Coulomb efficiency of lithium-sulfur batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894554A_ABST
    Figure CN118894554A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrode materials, and discloses manganese dioxide with a nanowire and nanosheet structure, a preparation method and application in a lithium-sulfur battery. The preparation method of the manganese dioxide with the nanowire and nanosheet structure comprises the following steps: firstly, mixing polyvinyl alcohol with a sulfuric acid solution, then adding manganese sulfate for dispersion, then adding potassium permanganate for mixing, and carrying out solvothermal reaction to obtain the manganese dioxide with the nanowire and nanosheet structure. The preparation method disclosed by the invention is simple, the nanosheet can be prepared by a one-step method, and the size of the obtained nanosheet is obviously reduced compared with a traditional preparation method; the one-dimensional line can prevent the two-dimensional sheets from being agglomerated, and the two-dimensional sheets can be connected with the one-dimensional line to provide a conductive path; due to the large length-width ratio of the one-dimensional line and the two-dimensional sheet, more active sites can be exposed; and the lithium-sulfur battery has good lithium-sulfur battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to manganese dioxide with a nanowire and nanosheet structure, a preparation method and application in a lithium-sulfur battery. Background Art

[0002] The energy crisis is a pressing problem facing mankind. To achieve a sustainable energy supply and alleviate the contradiction between energy supply and demand, the development and application of efficient and low-cost energy storage and conversion systems are indispensable. Lithium-sulfur batteries have a high theoretical specific capacity (1675mAh g -1 ), high theoretical specific energy (~2600Wh g -1 ), the positive electrode active material sulfur has abundant reserves, low toxicity and no pollution, and has become a strong competitor for the next generation of high-energy metal secondary batteries. During the charge and discharge process of lithium-sulfur batteries, sulfur will generate polysulfides and dissolve in the electrolyte and diffuse to the lithium negative electrode to produce a "shuttle effect", resulting in irreversible capacity loss of active materials during the cycle, reducing the cycle stability and coulombic efficiency of lithium-sulfur batteries.

[0003] Carbon materials are currently the most common sulfur carriers, which can better accommodate the volume expansion of sulfur and effectively improve the shuttle effect. However, the weak van der Waals force of carbon materials has limited adsorption effect on polysulfides. Therefore, carbon materials are doped or polar metal compound materials with stronger adsorption capacity, such as transition metal oxides, hydroxides, etc., are used as sulfur carriers to more effectively inhibit the diffusion of polysulfides by forming chemical bonds with polysulfides. At the same time, metal compounds can also improve the conversion efficiency of polysulfides through catalysis. Among them, MnO2 is an effective polysulfide medium, which fixes lithium polysulfide by reacting with lithium polysulfide to form a surface-bound intermediate of thiosulfate. However, the lack of active sites in bulk MnO2 leads to its limited effect in inhibiting polysulfides.

[0004] Therefore, improving the ability of MnO2 to inhibit polysulfides is of great significance for the development of lithium-sulfur batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a manganese dioxide with a nanowire nanosheet structure, a preparation method and an application in a lithium-sulfur battery, so as to solve the problem of insufficient active sites of MnO2 in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing manganese dioxide having a nanowire nanosheet structure, comprising the following steps:

[0008] Polyvinyl alcohol is first mixed with sulfuric acid solution, then manganese sulfate is added for dispersion, and then potassium permanganate is added for mixing, and manganese dioxide with nanowire and nanosheet structure is obtained through solvent thermal reaction.

[0009] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the temperature at which the polyvinyl alcohol and the sulfuric acid solution are mixed is 85-95°C.

[0010] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the concentration of the sulfuric acid solution is 4 to 15 wt %.

[0011] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the dosage ratio of the polyvinyl alcohol to the sulfuric acid solution is 0.03-0.8 g:35 mL.

[0012] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the molar ratio of manganese sulfate to potassium permanganate is 1:4 to 1:8.

[0013] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the dispersion time is 1 to 2 hours.

[0014] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the dosage ratio of potassium permanganate to sulfuric acid solution is 0.01-0.08 mmol:35 mL.

[0015] Preferably, in the above method for preparing manganese dioxide having a nanowire and nanosheet structure, the temperature of the solvothermal reaction is 150 to 180° C., and the time of the solvothermal reaction is 8 to 16 hours.

[0016] The invention also provides a method for preparing manganese dioxide with a nanowire and nanosheet structure to obtain manganese dioxide with a nanowire and nanosheet structure.

[0017] The present invention also provides an application of manganese dioxide with a nanowire nanosheet structure in a lithium-sulfur battery.

[0018] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0019] 1) The hydroxyl group of polyvinyl alcohol can play a role in bridging potassium permanganate and water molecules, while the non-hydrophilic polyethylene group can adjust the strength of the bridging effect, cooperate with the adsorption of polyvinyl alcohol on manganese dioxide, improve the growth crystal surface and morphology of manganese dioxide, and obtain manganese dioxide with small-sized nanowire and nanosheet structures;

[0020] 2) The preparation method is simple and can be prepared in one step, and the size of the obtained nanosheets is significantly reduced compared with the traditional preparation method;

[0021] 3) One-dimensional wires can prevent two-dimensional sheets from agglomerating, while two-dimensional sheets can connect one-dimensional wires to provide conductive pathways;

[0022] 4) The large aspect ratio of one-dimensional wires and two-dimensional sheets can expose more active sites;

[0023] 5) Has good lithium-sulfur battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.

[0025] Figure 1 is a SEM image of manganese dioxide having a nanowire nanosheet structure in Example 3;

[0026] Figure 2 This is the SEM image of the large flake manganese dioxide in Comparative Example 1. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing manganese dioxide having a nanowire nanosheet structure, comprising the following steps:

[0028] Polyvinyl alcohol is first mixed with sulfuric acid solution, then manganese sulfate is added for dispersion, and then potassium permanganate is added for mixing, and manganese dioxide with nanowire and nanosheet structure is obtained through solvent thermal reaction.

[0029] In the present invention, the temperature at which the polyvinyl alcohol and the sulfuric acid solution are mixed is preferably 85 to 95°C, more preferably 86 to 92°C, and even more preferably 88 to 90°C.

[0030] In the present invention, the concentration of the sulfuric acid solution is preferably 4 to 15 wt %, more preferably 5 to 14.5 wt %, and even more preferably 8 to 12 wt %.

[0031] In the present invention, the usage ratio of the polyvinyl alcohol to the sulfuric acid solution is preferably 0.03-0.8 g:35 mL, more preferably 0.03-0.6 g:35 mL, and even more preferably 0.1-0.5:35 mL.

[0032] In the present invention, the molar ratio of manganese sulfate to potassium permanganate is preferably 1:4 to 1:8, more preferably 1:5 to 1:7, and more preferably 1:5.5 to 1:6.

[0033] In the present invention, the dispersion time is preferably 1 to 2 hours, more preferably 1.5 to 2 hours, and more preferably 1.75 to 2 hours; the purpose of the dispersion is to better complex manganese sulfate and polyvinyl alcohol to prepare manganese dioxide with a nanowire nanosheet structure.

[0034] In the present invention, the usage ratio of potassium permanganate to sulfuric acid solution is preferably 0.01-0.08 mmol:35 mL, more preferably 0.03-0.06 mmol:35 mL, and more preferably 0.04-0.05:35 mL.

[0035] In the present invention, the temperature of the solvothermal reaction is preferably 150-180°C, more preferably 155-170°C, and more preferably 160-165°C; the time of the solvothermal reaction is preferably 8-16h, more preferably 10-15h, and more preferably 12-13h.

[0036] The invention also provides a method for preparing manganese dioxide with a nanowire and nanosheet structure to obtain manganese dioxide with a nanowire and nanosheet structure.

[0037] The present invention also provides an application of manganese dioxide with a nanowire and nanosheet structure in a lithium-sulfur battery. The specific method of the application is to prepare a positive electrode sulfur carrier of the lithium-sulfur battery.

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] 35 mL of a 5 wt% sulfuric acid solution was heated to 90°C, 0.03 g of polyvinyl alcohol was added and mixed, and then 0.0025 mmol of manganese sulfate was added and mixed, followed by stirring for 1 hour, and then 0.01 mmol of potassium permanganate was added and mixed, and then a solvothermal reaction was carried out at 150°C for 16 hours to obtain manganese dioxide having a nanowire nanosheet structure.

[0041] The manganese dioxide with nanowire and nanosheet structure prepared above was assembled into a battery for testing, and the performance under the test condition of 0.2C can reach 1074.1mAh g -1 .

[0042] The specific process of assembling the battery:

[0043] Preparation of sulfur positive electrode: sublimated sulfur and the manganese dioxide with nanowire nanosheet structure prepared above were mixed in a mass ratio of 3:1, and then heated in an ampoule at 155°C for 12h, the obtained mixture was dispersed in N-methylpyrrolidone (NMP) with carbon nanotubes and polyvinylidene fluoride (PVDF) in a weight ratio of 8:1:1, and the obtained slurry was coated on aluminum foil and dried at 60°C for 8h to obtain a sulfur positive electrode;

[0044] The obtained sulfur positive electrode, functional separator, lithium metal negative electrode and electrolyte (1.0M LiTFSI in DME:DOL=1:1Vol%&2%LiNO3) were assembled into a CR2016 button-type battery in an argon-filled glove box; the battery was left to stand for 8h before electrochemical testing.

[0045] Example 2

[0046] 35 mL of a 14.5 wt% sulfuric acid solution was heated to 90°C, 0.1 g of polyvinyl alcohol was added and mixed, and then 0.01 mmol of manganese sulfate was added and mixed, followed by stirring for 2 h, and then 0.08 mmol of potassium permanganate was added and mixed, and then a solvent thermal reaction was carried out at 180°C for 8 h to obtain manganese dioxide having a nanowire nanosheet structure.

[0047] The manganese dioxide with nanowire and nanosheet structure prepared above was assembled into a battery for testing, and the performance under the test condition of 0.2C can reach 996.2mAh g -1 .

[0048] The specific process of assembling the battery:

[0049] Preparation of sulfur positive electrode: sublimated sulfur and the manganese dioxide with nanowire nanosheet structure prepared above were mixed in a mass ratio of 3:1, and then heated in an ampoule at 155°C for 12h, the obtained mixture was dispersed in N-methylpyrrolidone (NMP) with carbon nanotubes and polyvinylidene fluoride (PVDF) in a weight ratio of 8:1:1, and the obtained slurry was coated on aluminum foil and dried at 60°C for 8h to obtain a sulfur positive electrode;

[0050] The obtained sulfur positive electrode, functional separator, lithium metal negative electrode and electrolyte (1.0M LiTFSI in DME:DOL=1:1Vol%&2%LiNO3) were assembled into a CR2016 button-type battery in an argon-filled glove box; the battery was left to stand for 8h before electrochemical testing.

[0051] Example 3

[0052] 34 mL of a 10 wt% sulfuric acid solution was heated to 90°C, 0.6 g of polyvinyl alcohol was added and mixed, and then 0.01 mmol of manganese sulfate was added and mixed, followed by stirring for 1 hour, and then 0.06 mmol of potassium permanganate was added and mixed, and then a solvothermal reaction was carried out at 170°C for 12 hours to obtain manganese dioxide having a nanowire nanosheet structure.

[0053] The SEM image of the manganese dioxide with nanowire nanosheet structure prepared above is as follows: Figure 1 In addition to the nanosheet structure, fine linear structures with a diameter of tens of nanometers can also be observed.

[0054] The manganese dioxide with nanowire and nanosheet structure prepared above was assembled into a battery for testing, and the performance under the test condition of 0.2C can reach 1182.6mAh g -1 .

[0055] The specific process of assembling the battery:

[0056] Preparation of sulfur positive electrode: sublimated sulfur and the manganese dioxide with nanowire nanosheet structure prepared above were mixed in a mass ratio of 3:1, and then heated in an ampoule at 155°C for 12h, the obtained mixture was dispersed in N-methylpyrrolidone (NMP) with carbon nanotubes and polyvinylidene fluoride (PVDF) in a weight ratio of 8:1:1, and the obtained slurry was coated on aluminum foil and dried at 60°C for 8h to obtain a sulfur positive electrode;

[0057] The obtained sulfur cathode, functional separator, lithium metal anode and electrolyte (1.0M LiTFSI in DME:DOL=1:1 Vol% & 2% LiNO3) were assembled into CR2016 button-type cells in an argon-filled glove box. The cells were left to stand for 8 h before electrochemical testing.

[0058] Comparative Example 1

[0059] 0.01 mmol of manganese sulfate was dissolved in 35 ml of deionized water, and after stirring for 2 hours, 0.06 mmol of potassium permanganate was added and mixed, and a solvent thermal reaction was carried out at 170° C. for 12 hours to obtain large flakes of manganese dioxide.

[0060] The SEM image of the large flake manganese dioxide obtained above is as follows Figure 2 shown. Figure 1 and Figure 2 In comparison, it can be seen that Figure 1 There are tiny linear structures with a diameter of tens of nanometers. Figure 2 The nanosheets in the sample are clearer, more complete and larger in size. Figure 1 The nanosheets in the sample are small and have a fuzzy structure. In addition, it can be seen from the scale that Figure 2 The scale bar is 3 μm, and Figure 1 The scale of the particle is 500nm, which is ten times the difference between the two. Figure 1 A villi structure can be seen in the .

[0061] The large flake manganese dioxide prepared above was assembled into a battery for testing, and the performance was found to be 942 mAh g under the test condition of 0.2C. -1 .

[0062] The specific process of assembling the battery:

[0063] Preparation of sulfur positive electrode: sublimated sulfur and the large flake manganese dioxide prepared above were mixed in a mass ratio of 3:1, and then heated in an ampoule at 155°C for 12h, the obtained mixture was dispersed in N-methylpyrrolidone (NMP) with carbon nanotubes and polyvinylidene fluoride (PVDF) in a weight ratio of 8:1:1, and the obtained slurry was coated on aluminum foil and dried at 60°C for 8h to obtain a sulfur positive electrode;

[0064] The obtained sulfur cathode, functional separator, lithium metal anode and electrolyte (1.0M LiTFSI in DME:DOL=1:1 Vol% & 2% LiNO3) were assembled into CR2016 button-type cells in an argon-filled glove box. The cells were left to stand for 8 h before electrochemical testing.

[0065] The functional separator described in Examples 1 to 3 and Comparative Example 1 is Celgard 2500.

[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing manganese dioxide having a nanowire nanosheet structure, characterized in that: The following steps are involved: Polyvinyl alcohol is first mixed with sulfuric acid solution, then manganese sulfate is added for dispersion, and then potassium permanganate is added for mixing, and manganese dioxide with nanowire and nanosheet structure is obtained through solvent thermal reaction.

2. The method for preparing manganese dioxide having a nanowire nanosheet structure according to claim 1, characterized in that: The temperature of mixing the polyvinyl alcohol and the sulfuric acid solution is 85-95°C.

3. The method for preparing manganese dioxide having a nanowire nanosheet structure according to claim 2, characterized in that: The concentration of the sulfuric acid solution is 4-15 wt %.

4. The method for preparing manganese dioxide having a nanowire nanosheet structure according to claim 3, characterized in that: The dosage ratio of the polyvinyl alcohol to the sulfuric acid solution is 0.03-0.8 g:35 mL.

5. The method for preparing manganese dioxide having a nanowire nanosheet structure according to claim 4, characterized in that: The molar ratio of manganese sulfate to potassium permanganate is 1:4 to 1:

8.

6. The method for preparing manganese dioxide having a nanowire nanosheet structure according to claim 4 or 5, characterized in that: The dispersion time is 1 to 2 hours.

7. The method for preparing manganese dioxide having a nanowire and nanosheet structure according to claim 6, characterized in that: The dosage ratio of the potassium permanganate to the sulfuric acid solution is 0.01-0.08 mmol:35 mL.

8. The method for preparing manganese dioxide having a nanowire and nanosheet structure according to claim 7, characterized in that: The temperature of the solvent thermal reaction is 150-180° C., and the time of the solvent thermal reaction is 8-16 hours.

9. Manganese dioxide with a nanowire or nanosheet structure obtained by the method for preparing manganese dioxide with a nanowire or nanosheet structure according to any one of claims 1 to 8.

10. Use of the manganese dioxide having a nanowire and nanosheet structure according to claim 9 in a lithium-sulfur battery.