Denitrification deep nitrogen removal functional carrier as well as preparation process and application thereof

By loading the glue with magnetic amine cross-linked activated carbon on the polymer matrix, a deep denitrification functional carrier is formed, which solves the problems of low utilization rate of loading additives and poor denitrification effect in the prior art, and achieves high efficiency Low-concentration nitrogen-containing wastewater treatment and effective utilization of carrier resources.

CN118894594AActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310499268.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

When existing biological carriers treat low-concentration nitrogen-containing wastewater, the load additive utilization rate is low, and the additive covers the adsorption site, resulting in poor nitrogen removal effect and waste of resources.

Method used

The glue with magnetic amine cross-linked activated carbon, biodegradable adhesive, hydrophilic substance and bioaffinity substances on the surface of the polymer matrix is ​​connected by silane coupling agent to form a functional carrier for deep denitrification denitrification, which improves the The utilization rate and bioaffinity of the loaded substance.

Benefits of technology

It has achieved efficient nitrogen removal at low concentrations of nitrogen-containing wastewater, high utilization rate of load substances, adjustable carrier density, shortened membrane hanging time, nitrate removal rate reaches 94.5%-99%, and low carrier mass reduction rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a denitrification deep nitrogen removal functional carrier as well as a preparation process and application thereof, and belongs to the technical field of water treatment. The denitrification functional carrier comprises the following raw materials: a polymer matrix, a silane coupling agent-ethanol water solution and mixed mucilage in a ratio of 100: (4.5-7): (10-13). The magnetic amine cross-linked activated carbon loaded on the carrier has strong adsorption performance on nitrate radicals by utilizing ion exchange and electrostatic adsorption principles and has good biodegradation performance on low-concentration nitrogen-containing wastewater, and the removal rate of the nitrate radicals is 94.5%-99% two weeks before biofilm formation; a loaded substance is mixed by using a biodegradable adhesive, the bioavailability is high, and the mass of the carrier is reduced by 1-3.5% in the first two weeks; and the time for forming a mature biological membrane is advanced by 5-23 days.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical industry and environmental protection, and relates to a preparation process and application of a denitrification deep denitrification functional carrier. Background Art

[0002] Biofilm method is a research hotspot in the field of water treatment. It has the advantages of low sludge production and high treatment efficiency. It can meet the latest emission standards and is very suitable for deep denitrification. Biofilms form on the surface of the carrier, and there is a concentration gradient between the pollutants in the water phase and the biofilm phase. The pollutants enter the biofilm phase and are degraded.

[0003] At present, there are many types of polymer biological carriers, mainly made of polymer materials such as polypropylene, polyethylene, and polyvinyl chloride, which are mixed with some hydrophilic and bio-affinity substances to increase the hydrophilicity and bio-affinity of the carrier surface. However, the mixing of hydrophilic and bio-affinity substances to improve the biofilm effect of the carrier is still difficult to meet the actual needs. The hydrophilic and bio-affinity substances mixed in the carrier cannot be effectively utilized, and only the functional substances on the surface play a role, resulting in a waste of resources.

[0004] Chinese invention patent CN100537450C discloses a method for preparing a bio-affinity carrier by coating natural biological material powder, solvent, and coating latex on the surface of a water treatment carrier, which has good bio-affinity, short biofilm formation time, and good treatment effect. Chinese invention patent CN106430527B discloses a method for preparing a hydrophilic biological carrier by coating natural polymer materials and synthetic polymer materials on the surface of a carrier, which not only has good bio-affinity and short biofilm formation time, but also has enhanced chemical stability, thermal stability, and mechanical strength compared to the previous invention. When these two inventions treat low-concentration wastewater, the concentration gradient between the two phases is low, and there is a disadvantage of insufficient driving force.

[0005] Chinese patent CN110407334B discloses the preparation and application of a biological carrier for simultaneous denitrification and denitrification by adsorbing nitrate ions. The biological filler provided by the present invention is made of carbon microspheres with anionic layered magnesium-aluminum compounds on the surface and polycaprolactone organically combined, and has the function of actively adsorbing nitrate and providing a carbon source for denitrification. However, the filler uses a non-degradable binder so that only part of the loaded polycaprolactone can be utilized, resulting in waste, and the loaded polycaprolactone will cover the adsorption sites for nitrate, affecting the adsorption function.

[0006] In summary, when the biological carriers commonly used in the prior art are used to treat low-concentration nitrate-containing wastewater, there are disadvantages such as low utilization rate of the loading additive and coverage of the adsorption sites by the additive. Therefore, it is of great significance to develop a filler with high additive utilization rate and deep denitrification capability. Summary of the invention

[0007] In view of the existing technology for treating low-concentration nitrate-containing wastewater, there are problems such as the loaded additives covering the adsorption sites and the low utilization rate of the additives. The present invention provides a denitrification deep denitrification functional carrier, in which a slurry prepared by a biodegradable adhesive, a magnetic amine cross-linked activated carbon, a hydrophilic substance, and a bioaffinity substance is mixed in a certain proportion and loaded on the surface of a polymer matrix. The additives loaded on the surface of the matrix can be effectively utilized, and the treatment effect on low-concentration nitrate-containing wastewater is better.

[0008] The present invention uses polymer materials as a matrix and silane coupling agents as connecting materials, and mixes magnetic amine cross-linked activated carbon, bioaffinity materials, hydrophilic materials, biodegradable adhesives, and ultrapure water in a certain proportion to prepare a slurry that is loaded on the surface of the matrix and then dried to obtain a biological carrier.

[0009] The invention provides a denitrification functional carrier. The raw materials of the denitrification functional carrier contain a polymer matrix, an ethanol aqueous solution of a silane coupling agent and a mixed mortar in a mass ratio of 100:(4.5-7):(10-13); the polymer matrix is ​​selected from at least one of polypropylene, polyethylene, polyvinyl chloride and polyurethane; the mixed mortar contains magnetic amine cross-linked activated carbon, a hydrophilic substance, a bioaffinity substance, a biodegradable adhesive and water in a mass ratio of 1:(0.6-0.8):(0.6-0.8):(4-4.5):(5-5.5); the hydrophilic substance is selected from at least one of polyvinyl alcohol, agar, silica gel and diatomaceous earth; the bioaffinity substance is selected from at least one of starch, degummed bone meal and oyster shell powder.

[0010] Optionally, the shape of the polymer matrix can be selected from a ring shape, a saddle shape, a Raschig ring or a hollow sphere. The molecular weight of the polymer matrix is ​​not limited, and the molecular weight commonly used in the art can be used.

[0011] Optionally, the density of the denitrification functional carrier is 0.95-1.1 g / cm 3 , preferably 0.98 to 1.05 g / cm 3 .

[0012] Optionally, the biodegradable adhesive is selected from at least one of a carboxymethyl polysaccharide adhesive and a modified starch adhesive.

[0013] Optionally, the mass ratio of the polymer matrix to the ethanol aqueous solution of the silane coupling agent is 100:(4.5-7). There are two groups in the silane coupling agent, one is an organic group with affinity to the polymer surface, and the other is an active group with affinity to other active groups other than the polymer. It is precisely because of this characteristic that the bonding strength between the loaded mixed mortar and the polymer substrate is increased.

[0014] Optionally, the silane coupling agent model is KH550.

[0015] Optionally, the mass concentration of the silane coupling agent in the ethanol aqueous solution is 2 to 10 g / L, more preferably 4 to 8 g / L.

[0016] Optionally, the mass concentration of ethanol in the ethanol aqueous solution of the silane coupling agent is 70% to 80%.

[0017] The present invention also provides a method for preparing a denitrification functional carrier, the method comprising the steps of:

[0018] S1 pre-treats the polymer matrix: immerses the polymer matrix in an ethanol aqueous solution of a silane coupling agent; the usage ratio of the two is not specifically limited, and the polymer matrix can be immersed in the ethanol aqueous solution of the silane coupling agent.

[0019] S2: mixing the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive and water to obtain a mixed slurry;

[0020] S3: immersing the pretreated polymer matrix into the mixed slurry for 3 to 6 hours; taking it out and drying it, so that the mixed slurry forms a dense layer on the surface of the matrix, thereby obtaining the denitrification functional carrier.

[0021] The density of the carrier can be controlled according to the number of immersions in S3.

[0022] Optionally, in S1, the pretreatment time is 1 to 3 hours; preferably, the treatment time is 2 to 3 hours.

[0023] Optionally, in S2, the mixed slurry is obtained by stirring at 60 to 120 r / min for 1 hour, preferably by stirring at 70 to 100 r / min for 1 hour.

[0024] Optionally, in S3, the drying temperature is 60-80°C and the time is 1-3 hours; preferably, the drying temperature is 70-80°C and the time is 2-3 hours.

[0025] The present invention also provides the use of the denitrification functional carrier obtained by any of the above preparation methods in treating nitrate nitrogen wastewater.

[0026] Optionally, the concentration of nitrate ions in the nitrate-nitrogen wastewater is 50 mg / L to 100 mg / L.

[0027] The magnetic amine cross-linked activated carbon is composed of mixed solution I and mixed solution II; mixed solution I is composed of activated carbon powder, FeCl3·6H2O and sodium hydroxide solution; mixed solution II is composed of dimethylformamide, ethylenediamine, epichlorohydrin and triethylamine. The concentration of the sodium hydroxide solution is 4wt% to 8wt%. The weight ratio of the activated carbon powder, FeCl3·6H2O and sodium hydroxide solution is 1:(3-4):(8-10). The volume ratio of dimethylformamide, ethylenediamine, epichlorohydrin and triethylamine is 1:(0.9-1.1):(1.2-1.4):(3.1-3.4). The volume ratio of the mixed solution I to the mixed solution II is 1:(1-2).

[0028] The preparation steps of the magnetic amine cross-linked activated carbon include:

[0029] (1) The activated carbon particles are crushed and passed through a 50-100 mesh sieve, preferably a 60-80 mesh sieve;

[0030] (2) Activated carbon pretreatment: first pyrolyze the activated carbon, then acid wash the activated carbon, then wash with deionized water until neutral, and finally dry it; the pyrolysis is performed in a muffle furnace at 350-700°C for 8-13 hours, preferably at 400-650°C for 9-11 hours; the acid wash is performed in 1-3 mol / L nitric acid at 60-85°C for 1-3 hours, preferably at 1.5-2.5 mol / L nitric acid at 65-80°C for 1-1.8 hours; the drying is performed at 70-100°C for 8-12 hours, preferably at 75-90°C for 9-11 hours;

[0031] (3) mixing the pretreated activated carbon powder, FeCl3·6H2O, and 4-8 wt% NaOH solution in a weight ratio, stirring at 75-85° C. for 4-8 h, preferably at 78-83° C. for 5-7 h to obtain a mixed solution;

[0032] (4) Dimethylformamide, ethylenediamine, epichlorohydrin and triethylamine are uniformly mixed in a volume ratio and added to the mixed solution obtained in step (3), and stirred at 55-65° C. for 4-8 hours, preferably at 60-65° C. for 5-7 hours; after centrifugation, the product is washed with deionized water, and dried at 70-100° C. for 3-7 hours, preferably at 70-85° C. for 3-5 hours, to obtain the magnetic amine cross-linked activated carbon.

[0033] Magnetic amine cross-linked activated carbon is a carbon with superparamagnetic properties. It is easy to recover from wastewater with the help of an external magnetic field, and amine functional groups (NH+2Cl - ), has a good adsorption effect on nitrate ions. The adsorption principle is that Cl in the amine functional group -Ion exchange with nitrate, Fe 3+ , which has an electrostatic attraction to nitrate.

[0034] The denitrification deep denitrification functional carrier of the present invention has the following beneficial effects:

[0035] (1) The adhesive in the mixed mortar is biodegradable, and the utilization rate of the loaded functional substances is high;

[0036] (2) Magnetic amine cross-linked activated carbon has a good adsorption effect on nitrate in wastewater, and can achieve good denitrification effect for low-concentration wastewater;

[0037] (3) Bio-affinity and hydrophilic substances are mixed into the mixed slurry, and the carrier has good bio-affinity and hydrophilic properties;

[0038] (4) The magnetic amine cross-linked activated carbon scattered in the water can play a certain adsorption and flocculation role;

[0039] (5) Magnetic amine cross-linked activated carbon contains chelated Fe3O4 particles, which has a magnetic promotion effect on film growth;

[0040] (6) Using silane coupling agent as a "bridge" between the mixed slurry and the carrier makes the load more solid and not easy to fall off;

[0041] (7) As the bioaffinity substances are consumed, the surface roughness of the carrier increases, which is conducive to biofilm formation.

[0042] The magnetic amine cross-linked activated carbon loaded on the carrier of the present invention has strong adsorption performance for nitrate by utilizing the principles of ion exchange and electrostatic adsorption, and has good biodegradability for low-concentration nitrogen-containing wastewater, and the nitrate removal rate in the first two weeks of biofilm formation is 94.5% to 99%; the loaded material is mixed with a biodegradable adhesive, and has a high bioavailability, and the weight reduction percentage of the carrier in the first two weeks is 1 to 3.5%; the time for forming a mature biofilm is advanced by 5 to 23 days. DETAILED DESCRIPTION

[0043] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0044] The present invention is further described below in conjunction with the embodiments. It should be emphasized that the following description is merely exemplary and is not intended to limit the scope of the present invention and its application.

[0045] The test method of the carrier density of the present invention is the mass volume method, which uses a balance to directly measure the carrier mass, adopts the water displacement method to measure the carrier volume, and calculates the carrier density according to the formula ρ=m / V.

[0046] The mature biofilm of the present invention refers to a biofilm amount of 150 mg per 1 g of carrier;

[0047] The test method for nitrate is ion chromatography, and the removal rate formula = (influent nitrate concentration - effluent nitrate concentration) / influent nitrate concentration.

[0048] The wastewater in the following examples and comparative examples is artificially prepared low-concentration nitric nitrogen wastewater.

[0049] The degummed bone meal in the embodiment of the present invention was purchased from Jinan Jianhui Chemical Co., Ltd., with a product model of 1130; polyvinyl alcohol was purchased from Beijing Inokai Technology Co., Ltd., with a product model of PVA17-88; agar was purchased from Beijing Inokai Technology Co., Ltd., with a product number of B46657; silica gel was purchased from Beijing Inokai Technology Co., Ltd., with a product number of S157-212; diatomaceous earth was purchased from Beijing Inokai Technology Co., Ltd., with a product number of B42396; starch was purchased from Beijing Inokai Technology Co., Ltd., with a product number of A48874; oyster shell powder was purchased from Shaanxi Feimi Technology Co., Ltd., with a product number of FM-HKF.

[0050] The modified starch adhesive in the embodiment of the present invention was purchased from Hebei Yanxing Chemical Co., Ltd.; the product model is pregelatinized starch α-starch.

[0051] The carboxymethyl chitosan adhesive in the embodiment of the present invention was purchased from Xi'an Preus Bioengineering Co., Ltd., and the product model is PRS180321.

[0052] Calculation method of carrier weight reduction rate = (weight before use - weight after use) / weight before use Example 1

[0053] The raw materials of the denitrification functional carrier are composed of 100g of a polymer matrix, 4.5g of an ethanol aqueous solution of a silane coupling agent KH550, and 11.2g of a mixed glue.

[0054] The polymer matrix is ​​hollow spherical polyethylene. The mixed glue is a mixture of 0.6g hydrophilic substance, 0.6g bioaffinity substance, 4g biodegradable adhesive, 1g magnetic amine cross-linked activated carbon and 5g ultrapure water. The hydrophilic substance is a mixture of 0.3g polyvinyl alcohol and 0.3g diatomaceous earth. The bioaffinity substance is a mixture of 0.3g starch and 0.3g degummed bone powder. The biodegradable adhesive is a modified starch adhesive.

[0055] The preparation method of magnetic amine cross-linked activated carbon is:

[0056] (1) After the activated carbon particles were crushed and passed through a 65-mesh sieve, they were first pyrolyzed in a muffle furnace at 600°C for 10 h, then activated in 2 mol / L nitric acid at 75°C for 1.5 h, and finally washed with deionized water until neutral, and dried at 80°C for 12 h to obtain activated carbon powder;

[0057] (2) 1 g of activated carbon powder, 3.2 g of FeCl3·6H2O, and 10 ml of 4 wt% NaOH solution were mixed and stirred at 80°C for 6 h to prepare a mixed solution I;

[0058] (3) Mix 2.5 ml of dimethylformamide, 2 ml of ethylenediamine, 3 ml of epichlorohydrin, and 8 ml of triethylamine to prepare a mixed solution II, mix the mixed solution I and the mixed solution II in a volume ratio of 1:1, stir at 60°C for 2 h, centrifuge, wash the product with deionized water, and dry at 100°C for 2 h to obtain magnetic amine cross-linked activated carbon.

[0059] The preparation method of the denitrification functional carrier is as follows:

[0060] Step 1: Immerse the surface of the hollow spherical polyethylene with a 75% ethanol aqueous solution of 5 g / L silane coupling agent for 2 h.

[0061] Step 2: Mix 1 g of magnetic amine cross-linked activated carbon, 0.6 g of hydrophilic substance, 0.6 g of bioaffinity substance, 4 g of biodegradable adhesive, and 5 g of ultrapure water, and stir at 70 r / min for 1 h to obtain a mixed slurry.

[0062] Step 3: Immerse the treated hollow spherical polyethylene in the mixed slurry and stir for 3 hours until the mixed slurry adheres to the surface of the hollow spherical polyethylene. After taking it out, dry it at 80℃ for 2 hours to form a dense layer on the surface of the hollow spherical polyethylene to obtain a denitrification functional carrier. After testing, the density of the carrier is 1.0g / cm 3 .

[0063] The following experiments were conducted to test the nitrate removal rate and mixed slurry utilization rate of the denitrification functional carrier prepared in the above steps, as well as the biofilm forming performance of the carrier.

[0064] The prepared denitrification function carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitric nitrogen wastewater (nitric nitrogen concentration 51 mg / L) was pumped in from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge, and the temperature was controlled at 25°C to 30°C to start biofilm formation. The time for forming a mature biofilm using only hollow spherical polyethylene as a carrier was 23 days, and the time for forming a mature biofilm using the denitrification function carrier prepared in this embodiment was 8 days, which was 15 days shorter than that of hollow spherical polyethylene. The average nitrate removal rate of the denitrification function carrier of this embodiment in the first two weeks of biofilm formation was 99%, and the average nitrate removal rate of the hollow spherical polyethylene in the first two weeks of biofilm formation was 97.5%, and the average removal rate of the present embodiment increased by 1.5%. The weight reduction rate of the carrier after two weeks was 1.2%.

[0065] Example 2

[0066] The raw materials of the denitrification functional carrier are composed of 100g of polymer matrix, 5g of silane coupling agent-ethanol aqueous solution and 11.4g of mixed glue.

[0067] The polymer carrier is a polypropylene Raschig ring with a specification of Φ25; the mixed glue is a mixture of 0.6g hydrophilic substance, 0.6g bioaffinity substance, 4.2g biodegradable adhesive, 1g magnetic amine cross-linked activated carbon and 5g ultrapure water. The hydrophilic substance is a mixture of 0.3g agar and 0.3g silica gel; the bioaffinity substance is a mixture of 0.3g starch and 0.3g oyster shell powder; the biodegradable adhesive is carboxymethyl chitosan adhesive.

[0068] The preparation method of magnetic amine cross-linked activated carbon is:

[0069] (1) After the activated carbon particles were crushed and passed through a 70-mesh sieve, they were first pyrolyzed in a muffle furnace at 600°C for 10.5 h, then activated in 2 mol / L nitric acid at 75°C for 1.5 h, and finally washed with deionized water until neutral, and dried at 80°C for 12 h to obtain activated carbon powder;

[0070] (2) 1 g of activated carbon powder, 4 g of FeCl3·6H2O, and 6 ml of 5 wt% NaOH solution were mixed and stirred at 80°C for 6 h to prepare a mixed solution I;

[0071] (3) Mix 2.5 ml of dimethylformamide, 2.5 ml of ethylenediamine, 3.5 ml of epichlorohydrin, and 8 ml of triethylamine to prepare a mixed solution II, mix the mixed solution I and the mixed solution II in a volume ratio of 1:1.2, stir at 60°C for 2 h, centrifuge, wash the product with deionized water, and dry at 100°C for 2 h to obtain magnetic amine cross-linked activated carbon.

[0072] The preparation method of the denitrification denitrification functional carrier is as follows:

[0073] Step 1: Immerse the surface of the polypropylene Raschig ring with 6 g / L silane coupling agent in 80% ethanol aqueous solution for 2 h.

[0074] Step 2: Mix 1 g of magnetic amine cross-linked activated carbon, 0.6 g of hydrophilic substance, 0.6 g of bioaffinity substance, 4.2 g of biodegradable adhesive, and 5 g of ultrapure water, and stir at 80 r / min for 1 h to obtain a mixed slurry.

[0075] Step 3: Immerse the treated polypropylene Raschig ring in the mixed slurry and stir for 4 hours until the mixed slurry adheres to the surface of the polypropylene Raschig ring. Take it out and dry it at 80℃ for 2 hours to form a dense layer on the surface of the polypropylene Raschig ring to obtain a denitrification functional carrier. The density of the carrier is 1.01g / cm 3 .

[0076] The following experiments were conducted to test the nitrate removal rate and mixed slurry utilization rate of the denitrification functional carrier prepared in the above steps, as well as the biofilm formation ability of the carrier.

[0077] The prepared denitrification functional carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitric nitrogen wastewater (nitric nitrogen concentration 51 mg / L) was pumped in from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge, and the temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm using only polypropylene Raschig ring as a carrier was 20 days, and the time for forming a mature biofilm using the denitrification functional carrier prepared in this embodiment was 10 days, which was 10 days shorter than that of the polypropylene Raschig ring. The average nitrate removal rate of the denitrification functional carrier of this embodiment in the first two weeks of biofilm formation was 98%, and the average nitrate removal rate of the polypropylene Raschig ring in the first two weeks as a carrier was 96.5%, and the average removal rate of this embodiment increased by 2.5%. The weight reduction rate of the carrier after two weeks was 1.05%.

[0078] Example 3

[0079] The raw materials of the denitrification functional carrier are composed of 100g of polymer matrix, 5.5g of silane coupling agent-ethanol aqueous solution, and 11.8g of mixed glue. Among them, the polymer carrier is saddle-shaped polyvinyl chloride; the mixed glue is a mixture of 0.7g of hydrophilic substance, 0.7g of bioaffinity substance, 4.4g of biodegradable adhesive, 1g of magnetic amine cross-linked activated carbon and 5g of ultrapure water. The hydrophilic substance is a mixture of 0.3g agar and 0.4g of silica gel; the bioaffinity substance is a mixture of 0.3g starch and 0.4g oyster shell powder; the biodegradable adhesive is a modified starch adhesive.

[0080] The preparation method of magnetic amine cross-linked activated carbon is:

[0081] (1) After the activated carbon particles were crushed and passed through a 75-mesh sieve, they were first pyrolyzed in a muffle furnace at 600°C for 11 h, then activated in 23 mol / L nitric acid at 80°C for 1.5 h, and finally washed with deionized water until neutral, and dried at 80°C for 12 h to obtain activated carbon powder;

[0082] (2) 1 g of activated carbon powder, 4 g of FeCl3·6H2O, and 8 ml of 6% (wt) NaOH solution were mixed and stirred at 80°C for 6 h to prepare a mixed solution I;

[0083] (3) Mix 2.5 ml of dimethylformamide, 2.8 ml of ethylenediamine, 3.3 ml of epichlorohydrin, and 8 ml of triethylamine to prepare a mixed solution II, mix the mixed solution I and the mixed solution II in a volume ratio of 1:1.5, stir at 60°C for 2 h, centrifuge, wash the product with deionized water, and dry at 100°C for 2 h to obtain magnetic amine cross-linked activated carbon.

[0084] The preparation method of the denitrification functional carrier is as follows:

[0085] Step 1: Immerse the saddle-shaped polyvinyl chloride surface with 75% ethanol aqueous solution of 7g / L silane coupling agent for 2h.

[0086] Step 2: Mix 1 g of magnetic amine cross-linked activated carbon, 0.7 g of hydrophilic substance, 0.7 g of bioaffinity substance, 4.4 g of biodegradable adhesive, and 5 g of ultrapure water, and stir at 80 r / min for 1 h to obtain a mixed slurry.

[0087] Step 3: Immerse the treated saddle-shaped polyvinyl chloride in the mixed slurry and stir for 5 hours until the mixed slurry adheres to the surface of the saddle-shaped polyvinyl chloride. Take it out and dry it at 80°C for 2 hours to form a dense layer on the surface of the saddle-shaped polyvinyl chloride to obtain a denitrification functional carrier. After testing, the density of the carrier is 1.03g / cm 3 .

[0088] The following experiments were conducted to test the nitrate removal rate and mixed slurry utilization rate of the denitrification functional carrier prepared in the above steps, as well as the biofilm formation ability of the carrier.

[0089] The prepared denitrification function carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitric nitrogen wastewater (nitric nitrogen concentration 50 mg / L, water content and addition ratio: methanol 333 mg / L, sodium nitrate 303 mg / L, potassium dihydrogen phosphate 4 mg / L, urea 21 mg / L, and the configured wastewater nitric nitrogen content was 50 mg / L.), the denitrification sludge of a sewage treatment plant was used as inoculated sludge, the temperature was controlled at 27°C to start biofilm formation, and only saddle-shaped polyvinyl chloride was used as a carrier, and the time for forming a mature biofilm was 30 days. The denitrification function carrier prepared by this embodiment was used, and the time for forming a mature biofilm was 7 days, which was 23 days shorter than that of saddle-shaped polyvinyl chloride. The average nitrate removal rate of the denitrification function carrier of this embodiment in the first two weeks of biofilm formation was 98.5%, and the average nitrate removal rate of the saddle-shaped polyvinyl chloride in the first two weeks as a carrier was 94.5%, and the average removal rate of this embodiment increased by 4%. The weight reduction rate of the carrier after two weeks was 1.0%.

[0090] Example 4

[0091] The denitrification functional carrier was prepared by using the same process as in Example 2. The only change was that the masses of the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive, and the ultrapure water in step 2 were 1 g, 0.6 g, 0.6 g, 4.2 g, and 5.2 g, respectively. The density of the denitrification functional carrier prepared in step 3 was 1.0 g / cm 3 .

[0092] The prepared denitrification functional carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitric nitrogen wastewater (nitric nitrogen concentration 52 mg / L) was pumped in from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge, and the temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm using polypropylene Raschig rings as carriers was 20 days. The time for forming a mature biofilm using the denitrification functional carrier prepared in this embodiment was 15 days, which was 5 days shorter than that of the polypropylene Raschig rings. The average nitrate removal rate of the denitrification functional carrier of this embodiment in the first two weeks of biofilm formation was 98%, and the average nitrate removal rate of the polypropylene Raschig ring in the first two weeks as a carrier was 96.5%. The average removal rate of this embodiment increased by 1.5%. The weight reduction rate of the carrier after two weeks was 3.5%.

[0093] Example 5

[0094] The denitrification functional carrier was prepared by using the same process as in Example 2. The only change was that the masses of the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive, and the ultrapure water in step 2 were 1 g, 0.6 g, 0.6 g, 4.4 g, and 5.5 g, respectively. The density of the denitrification functional carrier prepared in step 3 was 1.03 g / cm 3 .

[0095] The prepared denitrification functional carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitric nitrogen wastewater was pumped from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge, and the temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 20 days using only polypropylene Raschig rings as carriers. The time for forming a mature biofilm using the denitrification functional carrier prepared in this embodiment was 13 days, which was 7 days shorter than that of the polypropylene Raschig rings. The average nitrate removal rate of the denitrification functional carrier in this embodiment in the first two weeks of biofilm formation was 97%, and the average nitrate removal rate of the polypropylene Raschig ring in the first two weeks as a carrier was 96.5%. The average removal rate of this embodiment increased by 0.5%. The weight reduction rate of the carrier after two weeks was 1.2%.

[0096] According to the implementation method of preparing low-concentration denitrification functional carriers in the above five embodiments, the carriers prepared by the present invention are suitable for low-concentration nitric nitrogen wastewater, the loaded substances are fully utilized, the carrier density can be adjusted, and the biofilm formation time is significantly shortened.

[0097] Example 6

[0098] The same process as in Example 4 was used, but the mass ratio of polymer matrix: silane coupling agent-ethanol aqueous solution: mixed glue was 100:5:12.

[0099] The prepared denitrification functional carrier was loaded into a fixed bed biofilm reactor to treat low-concentration nitrogen-containing wastewater. Artificially prepared low-concentration nitrate-containing water (nitrate nitrogen concentration 53 mg / L) was pumped in from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge. The temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 14 days, which was 6 days shorter than the 20 days of the polypropylene Raschig ring carrier. The average nitrate removal rate in the first two weeks of biofilm formation was 97%, which was 0.5% higher than the removal rate of the polypropylene Raschig ring as a carrier. The weight reduction rate of the carrier was 1.1% after two weeks.

[0100] Example 7

[0101] The same process as in Example 4 was used, but the mass ratio of polymer matrix: silane coupling agent-ethanol aqueous solution: mixed glue was 100:5:13.

[0102] The prepared denitrification functional carrier was loaded into a fixed bed biofilm reactor, and artificially prepared low-concentration nitrate nitrogen wastewater (52 mg / L) was pumped in from bottom to top. The denitrification sludge of a sewage treatment plant was used as inoculated sludge, and the temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 16 days, which was 4 days shorter than the 20 days of the polypropylene Raschig ring carrier. The average nitrate removal rate in the first two weeks of biofilm formation was 97.5%, which was 1% higher than the removal rate of the polypropylene Raschig ring as a carrier. The weight reduction rate of the carrier was 2.3% after two weeks.

[0103] Comparative Example 1

[0104] The denitrification function was prepared by using the same process as in Example 1, except that the silane coupling agent-ethanol aqueous solution was not used to treat the surface of the carrier in step 1, which resulted in the mixed slurry being difficult to adhere to the carrier during the impregnation process, and the mechanical strength of the carrier was not high, resulting in the phenomenon of falling off in pieces during use. It took 30 days to form a mature biofilm, and the average nitrate removal rate was 75% in the first two weeks of biofilm formation, and the carrier weight reduction rate was 20% after two weeks.

[0105] Comparative Example 2

[0106] The denitrification functional carrier was prepared by using the same process as in Example 2, except that the magnetic amine cross-linked activated carbon was not added in step 2, but an equal amount of activated carbon was added, which lacked active adsorption function. It took 15 days to form a mature biofilm, and the average nitrate removal rate was 93% in the first two weeks of biofilm formation, and the carrier weight reduction rate was 0.08% after two weeks.

[0107] Comparative Example 3

[0108] The carrier was prepared by the same process as in Example 3, but the biodegradable adhesive was replaced by a non-biodegradable epoxy resin in the preparation step 2. This is because when the epoxy resin is used, in the process of treating nitrate, only the hydrophilic and bioaffinity additives loaded on the surface of the denitrification carrier can participate in the reaction, and the utilization rate of the carrier is low. It takes 25 days to form a mature biofilm, and the average nitrate removal rate in the first two weeks of biofilm formation is 90%, and the carrier weight reduction rate after two weeks is 0.03%.

[0109] Comparative Example 4

[0110] The same process as in Example 4 was used, with the only change being that the masses of the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive, and the ultrapure water in step 2 were 0.8 g, 0.6 g, 0.6 g, 4.2 g, and 5.2 g, respectively. The density of the denitrification functional carrier obtained in step 3 was 1.02 g / cm 3 .

[0111] The prepared denitrification functional carrier was loaded into a fixed-bed biofilm reactor to treat low-concentration nitrogen-containing wastewater. Artificially prepared low-concentration nitrate-containing water (nitrate-nitrogen concentration 52 mg / L) was pumped in from bottom to top. The denitrification sludge from a sewage treatment plant was used as inoculated sludge. The temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 18 days. The average nitrate removal rate in the first two weeks of biofilm formation was 97%, and the carrier weight reduction rate was 3% after two weeks.

[0112] Comparative Example 5

[0113] The same process as in Example 4 was used, with the only change being that the masses of the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive, and the ultrapure water in step 2 were 0.5 g, 0.6 g, 0.6 g, 4.2 g, and 5.2 g, respectively. The density of the denitrification functional carrier obtained in step 3 was 1.0 g / cm 3 .

[0114] The prepared denitrification functional carrier was loaded into a fixed-bed biofilm reactor to treat low-concentration nitrogen-containing wastewater. Artificially prepared low-concentration nitrate-containing water (nitrate-nitrogen concentration of 52 mg / L) was pumped in from bottom to top. The denitrification sludge from a sewage treatment plant was used as inoculated sludge. The temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 20 days. The average nitrate removal rate in the first two weeks of biofilm formation was 96%, and the carrier weight reduction rate was 2.8% after two weeks.

[0115] Comparative Example 6

[0116] The same process as in Example 4 was used, but the mass ratio of polymer matrix: silane coupling agent-ethanol aqueous solution: mixed glue was 100:5:8.

[0117] The prepared denitrification functional carrier was loaded into a fixed-bed biofilm reactor to treat low-concentration nitrogen-containing wastewater. Artificially prepared low-concentration nitrate-containing water (nitrate-nitrogen concentration 52 mg / L) was pumped in from bottom to top. The denitrification sludge from a sewage treatment plant was used as inoculated sludge. The temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 17 days. The average nitrate removal rate in the first two weeks of biofilm formation was 96.5%, and the carrier weight reduction rate was 2.7% after two weeks.

[0118] Comparative Example 7

[0119] The same process as in Example 4 was used, but the mass ratio of polymer matrix: silane coupling agent-ethanol aqueous solution: mixed glue was 100:5:5.

[0120] The prepared denitrification functional carrier was loaded into a fixed-bed biofilm reactor to treat low-concentration nitrogen-containing wastewater. Artificially prepared low-concentration nitrate-containing water (nitrate-nitrogen concentration of 52 mg / L) was pumped in from bottom to top. The denitrification sludge from a sewage treatment plant was used as the inoculated sludge. The temperature was controlled at 30°C to start biofilm formation. The time for forming a mature biofilm was 15 days. The average nitrate removal rate in the first two weeks of biofilm formation was 97%, and the carrier weight reduction rate was 2.3% after two weeks.

Claims

1. A denitrification functional carrier, characterized in that: The raw materials of the denitrification functional carrier contain a polymer matrix, an ethanol aqueous solution of a silane coupling agent and a mixed glue in a mass ratio of 100:(4.5-7):(10-13); The polymer matrix is ​​selected from at least one of polypropylene, polyethylene, polyvinyl chloride and polyurethane; The mixed slurry contains magnetic amine cross-linked activated carbon, hydrophilic material, bio-affinity material, biodegradable adhesive and water in a mass ratio of 1: (0.6-0.8): (0.6-0.8): (4-4.5): (5-5.5); The hydrophilic substance is selected from at least one of polyvinyl alcohol, agar, silica gel and diatomaceous earth; The bioaffinity substance is selected from at least one of starch, degummed bone meal and oyster shell powder.

2. The denitrification functional carrier according to claim 1, characterized in that: The density of the denitrification functional carrier is 0.95-1.1 g / cm 3 , preferably 0.98 to 1.05 g / cm 3 .

3. The denitrification functional carrier according to claim 1 or 2, characterized in that: The biodegradable adhesive is selected from at least one of carboxymethyl chitosan adhesive and modified starch adhesive; And / or, the shape of the polymer matrix can be selected from a ring shape, a saddle shape, a Raschig ring or a hollow sphere.

4. The denitrification functional carrier according to any one of claims 1 to 3, characterized in that: The mass ratio of the polymer matrix to the ethanol aqueous solution of the silane coupling agent is 100:(4.5-7); Preferably, the silane coupling agent model is KH550; Preferably, the mass concentration of the silane coupling agent in the ethanol aqueous solution is 2 to 10 g / L, more preferably 4 to 8 g / L; Preferably, the mass concentration of ethanol in the ethanol aqueous solution of the silane coupling agent is 70% to 80%.

5. The method for preparing the denitrification functional carrier according to any one of claims 1 to 4, characterized in that: The method comprises the steps of: S1 pre-treats the polymer matrix: immerses the polymer matrix in an ethanol aqueous solution of a silane coupling agent; S2: mixing the magnetic amine cross-linked activated carbon, the hydrophilic substance, the bio-affinity substance, the biodegradable adhesive and water to obtain a mixed slurry; S3: immersing the pretreated polymer matrix into the mixed slurry for 3 to 6 hours; taking it out and drying it, so that the mixed slurry forms a dense layer on the surface of the matrix, thereby obtaining the denitrification functional carrier.

6. The preparation method according to claim 5, characterized in that: In S1, the pretreatment time is 1 to 3 hours; preferably, the treatment time is 2 to 3 hours.

7. The preparation method according to claim 5 or 6, characterized in that: In S2, the mixed mortar is obtained by stirring at 60 to 120 r / min for 1 hour, preferably at 70 to 100 r / min for 1 hour.

8. The preparation method according to claim 5 or 6, characterized in that: In S3, the drying temperature is 60-80°C and the time is 1-3 hours; preferably, the drying temperature is 70-80°C and the time is 2-3 hours.

9. Application of the denitrification functional carrier obtained by the preparation method according to any one of claims 1 to 9 in treating nitrate nitrogen wastewater.

10. The use according to claim 9, characterized in that: In the nitrate nitrogen wastewater, the concentration of nitrate ions is 50 mg / L to 100 mg / L.

Citation Information

Patent Citations

  • Method for preparing surface function modified polyurethane foaming plastic carriers

    CN102702567A

  • Method for modifying biological filler with oyster shell powder

    CN105565481A

  • Method for enhancing biofilm culturing performance of graphene oxide modified biological filler

    CN111647189A

  • Method for preparing magnetic filling with biological affinity, hydrophilicity and activity for water treatment

    CN1522972A

  • Magnetic composite containing polyethylenimine functionalized actived carbon and methods thereof

    US20210023533A1